Polymer, electrolyte composition, and battery
The development of a polymer with specific structural units in batteries addresses the challenge of low ionic conductivity in polymer electrolytes, resulting in improved ion mobility and battery performance through optimized structural arrangement and uniform anion distribution.
Patent Information
- Application Number
- PCT/JP2024/016903
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-14
AI Technical Summary
Polymer electrolytes in batteries, such as lithium ion batteries, face challenges in achieving high ionic conductivity, which is essential for efficient ion movement and battery performance.
A polymer with a specific structural unit arrangement, represented by formulas (A) and (B), is developed, which allows for alternating copolymerization and uniform dispersion of structural units, enhancing ionic conductivity by optimizing the environment for alkali metal cations, thereby facilitating their movement.
The polymer exhibits improved ionic conductivity, as evidenced by narrow peaks in NMR spectra, leading to better performance in batteries by ensuring uniform anion distribution and easier cation mobility, thus enhancing battery efficiency.
Smart Images

Figure JP2024016903_14112024_PF_FP_ABST
Abstract
Description
Polymer, electrolyte composition, and battery
[0001] The present disclosure relates to polymers, electrolyte compositions and batteries.
[0002] Batteries such as lithium-ion batteries, which charge and discharge through the movement of metal ions between a positive electrode and a negative electrode, have been the subject of vigorous research due to their high capacity. Known electrolytes for lithium-ion batteries and the like include solutions of lithium salts containing organic solvents or ionic liquids. Meanwhile, research into solid electrolytes, polymer electrolytes, and the like is also underway from the standpoints of safety and processability (see Patent Document 1). In addition to lithium-ion batteries, research is also underway into batteries using other alkali ions, such as sodium and potassium, which are more abundant than lithium.
[0003] Japanese Patent Application Laid-Open No. 2001-176556
[0004] However, polymer electrolytes still have room for improvement in terms of ionic conductivity.
[0005] The present disclosure has been made in view of the above circumstances, and has an object to provide a polymer and an electrolyte composition having high ionic conductivity, and a battery using the same.
[0006] The present disclosure provides, for example, the following [1] to [8]. [1] A polymer comprising a structural unit (A) represented by the following formula (A) and a structural unit (B) represented by the following formula (B), which satisfies at least one of the following (1) to (3): (1) The solid state of the polymer at 25°C is 13 When CNMR is measured, the half-value width of the peak derived from the carbonyl carbon of the -COOA group (A is an alkali metal element) is 1,380 Hz or less. 13 When CNMR measurement is carried out in deuterated methanol, the half-value width of the peak derived from the carbonyl carbon of the -COOA group is 80 Hz or less. 13 When CNMR measurement was carried out in deuterated methanol, the ratio of the peak height to the half width of the peak derived from the carbonyl carbon of the -COOA group was 0.4 × 10 -4 abn / Hz or more. (In formula (A), R 1 is a -COOA group or a monovalent organic group having a -COOA group, and R 2 ~R 4 are each independently a hydrogen atom or a monovalent substituent, or R 2 and R 3 is a hydrogen atom or a monovalent substituent, and the other is R 4 and form a ring together. * indicates the bonding site of the structural unit (A) to another structural unit. (In formula (B), R 5 is a hydrogen atom or a monovalent substituent, and R 6 ~R 8 are each independently a hydrogen atom or a monovalent substituent, or R 6 and R 7 is a hydrogen atom or a monovalent substituent, and the other is R 8 and form a ring. * denotes a bonding site of the structural unit (B) with another structural unit.) [2] The polymer of [1], wherein A contains sodium or lithium. [3] An electrolyte composition comprising the polymer of [1] or [2]. [4] The electrolyte composition of [3], further comprising a plasticizer, wherein the plasticizer contains at least one selected from the group consisting of carbonate-based solvents, ether-based solvents, fluorine-based solvents, and phosphate ester-based solvents. [5] The electrolyte composition of [3] or [4], further comprising an anion receptor. [6] The electrolyte composition of any one of [3] to [5], further comprising an alkali metal salt. [7] A polymer obtained by polymerizing a monomer mixture containing a monomer (A) having a -COOA group (A is an alkali metal element) and a monomer (B) other than the monomer (A), wherein the reactivity ratio r1 of the monomer (A) and the reactivity ratio r2 of the monomer (B) in the polymerization reaction of the monomer (A) and the monomer (B) are both 0.5 or less. [8] A battery comprising the electrolyte composition according to any one of [3] to [6].
[0007] According to the present disclosure, it is possible to provide a polymer and an electrolyte composition having high ionic conductivity, and a battery using the same.
[0008] The polymer of this embodiment has a -COOA group (A is an alkali metal element). The polymer includes a structural unit (A) represented by the following formula (A) and a structural unit (B) represented by the following formula (B). The polymer may be one in which the structural unit (A) and the structural unit (B) tend to be arranged alternately, and may be an alternating copolymer. The structural units constituting the polymer may not include a structural unit having a carbonyl group other than the structural unit (A), or may consist of the structural unit (A) and the structural unit (B). (In formula (A), R 1 is a -COOA group or a monovalent organic group having a -COOA group, and R 2 ~R 4 are each independently a hydrogen atom or a monovalent substituent, or R 2 and R 3 is a hydrogen atom or a monovalent substituent, and the other is R 4 and form a ring together. * indicates the bonding site of the structural unit (A) to another structural unit. (In formula (B), R 5 is a hydrogen atom or a monovalent substituent, and R 6 ~R 8 are each independently a hydrogen atom or a monovalent substituent, or R 6 and R 7 is a hydrogen atom or a monovalent substituent, and the other is R 8 and form a ring. * indicates the bonding site of the structural unit (B) to another structural unit.
[0009] In the above polymer, each structural unit is introduced in a relatively uniformly dispersed manner in the molecular chain of the polymer, and in particular, the environment in which each structural unit (A) is placed in the polymer is highly uniform. Therefore, in the NMR spectrum of the above polymer measured under specified conditions, the half-width of the peak derived from carbonyl carbon is narrow. The presence of the structural units (A) dispersed in a similar environment in the molecular chain of the above polymer facilitates the movement of alkali metal element cations between the structural units (A), and excellent ionic conductivity can be exhibited. On the other hand, if the environment in which each structural unit (A) is placed differs for each structural unit, such as when the structural units (A) and (B) are randomly arranged in the molecular chain of the polymer, it is thought that there will be parts in the molecular chain of the polymer where the structural unit (A) is not present, and the distance between the structural units (A) will also vary, and once the alkali metal element cations are transferred to the -COO - If the anion strongly interacts with the group, subsequent movement requires energy, and the overall ionic conductivity is not as high as expected from the structure. Also, as described above, when structural units (A) with different environments exist, the resonance frequencies of the carbonyl carbons of the structural units (A) differ, and the peak width becomes wider. In other words, by uniformly distributing the anions immobilized on the polymer on the polymer chain, Li + Next to -COO - It becomes easier to interact with the adjacent -COO group. - On the other hand, if the immobilized anions are heterogeneous, the -COO groups on the polymer chains become more easily transferred. - This will result in a portion where no group exists, and this portion will be replaced with Li + Therefore, the Li atoms along the polymer chains are difficult to move. + When considering migration, it is considered important that the anions are uniformly dispersed. On the other hand, in a homopolymer consisting only of the structural unit (A), the immobilized anions are generally located close to each other. As a result, ionic interactions are strong, making it difficult for the alkali metal cations to migrate as counter cations. The polymer of this embodiment may have a region in which the structural unit (A) and the structural unit (B) are arranged alternately.
[0010] The polymer has a narrow half-width of the peak derived from carbonyl carbon in an NMR spectrum measured under predetermined conditions, and satisfies at least one of the following (1) to (3). In other words, the present disclosure is based on the idea that the half-width of the peak derived from carbonyl carbon in an NMR spectrum is useful as an index for understanding the intramolecular distribution of the structural unit (A) in the polymer. (1) The solid state of the polymer at 25°C is 13 When CNMR is measured, the half-value width of the peak derived from the carbonyl carbon of the -COOA group is 1,380 Hz or less. 13 When CNMR measurement is carried out in deuterated methanol, the half-value width of the peak derived from the carbonyl carbon of the -COOA group is 80 Hz or less. 13 When CNMR measurement was carried out in deuterated methanol, the ratio of the peak height to the half width of the peak derived from the carbonyl carbon of the -COOA group was 0.4 × 10 -4 abn / Hz or more.
[0011] Regarding condition (1), solid 13 The half-width of the peak derived from carbonyl carbon in the C-NMR spectrum may be 1350 Hz or less, 1330 Hz or less, 1300 Hz or less, 1280 Hz or less, or 1250 Hz or less. 13 The half-width of the peak derived from carbonyl carbon in the C-NMR spectrum may be 500 Hz or more, 600 Hz or more, 700 Hz or more, 750 Hz or more, or 800 Hz or more. It may be 1000 Hz or more, 1050 Hz or less, 1100 Hz or more, 1150 Hz or more, or 1200 Hz or less. In this specification, unless otherwise specified, the half-width refers to the full width at half maximum (FWHM). When multiple peaks derived from carbonyl carbon are observed, the half-width of the peak with the greatest intensity may be in the above range.
[0012] Regarding condition (2), deuterated methanol (CD 3 The half-width of the peak derived from the carbonyl carbon of the -COOA group of the polymer measured in deuterated methanol (CD 0D) may be 70 Hz or less, 60 Hz or less, 50 Hz or less, or 40 Hz or less. 3 The half-value width of the peak derived from the carbonyl carbon of the -COOA group of the polymer measured in a chromatographic method (OD) may be 5 Hz or more, 7 Hz or more, or 10 Hz or more.
[0013] Regarding condition (3), the ratio of the peak height to the half-width of the peak (peak height / half-width) is 0.5 × 10 -4 abn / Hz or more, and may be 0.75×10 -4 abn / Hz or more, and may be 1.0 x 10 -4 abn / Hz or more, and may be 1.2×10 -4 Regarding condition (3), the ratio of the peak height to the half width of the peak (peak height / half width) may be 5.0 × 10 -4 abn / Hz or less, and may be 3.0 × 10 -4 abn / Hz or less.
[0014] The polymer of this embodiment is an alkali metal-containing polymer having a carboxyl group modified with an alkali metal. In this specification, the alkali metal-modified carboxyl group refers to a group in which H of a —COOH group is substituted with an alkali metal element.
[0015] A in the -COOA group may contain at least one selected from the group consisting of potassium, sodium, and lithium, may contain at least one of sodium and lithium, or may contain lithium.
[0016] The content of one kind of alkali metal element among the alkali metal elements contained in the polymer may be 80 mol% or more, 85 mol% or 90 mol%. The one kind of alkali metal element may be potassium, sodium, or lithium, or may be sodium or lithium, or may be lithium.
[0017] In the above formula (A), R 1 may be a -COOA group itself, or may be a monovalent organic group having a -COOA group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. The monovalent organic group may have one or more -COOA groups, or may have one -COOA group. Examples of the organic group include monovalent groups having a -COOA group as a substituent, such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group of -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. The -COOA group is represented by R 1 is bonded to a carbon atom of another moiety in the above. The monovalent group may have a substituent that replaces a hydrogen atom bonded to the carbon atom. Examples of the substituent include an electron-withdrawing group such as a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be any of a linear hydrocarbon group, a branched hydrocarbon group, and a cyclic hydrocarbon group. The hydrocarbon group may be any of a saturated hydrocarbon group and an unsaturated hydrocarbon group. In this specification, an aromatic hydrocarbon group refers to a hydrocarbon group having an aromatic moiety such as a benzene ring, and may have an aliphatic moiety. In this specification, a cyclic hydrocarbon group refers to a hydrocarbon group having an aliphatic carbon ring moiety, and may have a linear or branched aliphatic moiety.
[0018] In the above formula (A), R 1 is -R 9 -COOA, where R 9is a divalent organic group. The divalent organic group may have 1 to 19 carbon atoms, 1 to 14 carbon atoms, 1 to 9 carbon atoms, 1 to 4 carbon atoms, or 1 or 2 carbon atoms. Examples of the divalent organic group include monovalent groups such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. The divalent group may also have a substituent substituting a hydrogen atom bonded to the carbon atom. Examples of the substituent include an electron-withdrawing group such as a halogen atom. The hydrocarbon group is not particularly limited and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group. The hydrocarbon group may also be a saturated hydrocarbon group or an unsaturated hydrocarbon group.
[0019] In the above formula (A), R 1 Examples of the electron-withdrawing group that may be contained include a halogen atom, a sulfonic acid group or a salt thereof, a sulfonic acid ester, a nitro group, a nitrile group, a carboxyl group or a salt thereof, etc. The halogen atom may be at least one of Cl and F, and may be F.
[0020] In the above formula (A), R 4 is a monovalent substituent, examples of the substituent include a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 1 to 10, 1 to 5, or 1 to 3. Examples of the monovalent organic group include monovalent groups such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group of -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle. R in the above formula (A) 4 may be a hydrogen atom or a methyl group. 4 is a monovalent organic group, R 2 or R 3may be a group having a —COOA group, or may be a —COOA group.
[0021] In the above formula (A), R 2 or R 3 When R is a monovalent substituent, the substituent may be a monovalent organic group. 4 Examples of the compounds are as follows: 2 and R 3 may be a hydrogen atom, and R 2 and R 3 Both of R in the above formula (A) may be hydrogen atoms. 2 or R 3 is a monovalent organic group, R 4 may be a group having a —COOA group, or may be a —COOA group.
[0022] In the above formula (A), R 2 and R 3 One of them is R 4 When the ring is formed together with the carbon atom, the number of ring members may be 4 to 10, 5 to 8, or 5 or 6. A substituent may be bonded to the carbon atom that is a ring member. Examples of the substituent include a halogen atom such as a fluorine atom.
[0023] The structural unit (B) is a structural unit other than the structural unit (A) and does not contain a —COOA group.
[0024] In the above formula (B), R 5 is a monovalent substituent, it may be a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 2 to 15, or 4 to 10. Examples of the organic group include monovalent groups such as hydrocarbon groups, groups having a chemical structure formed by substituting one or more carbon atoms (methylene groups) in the hydrocarbon group with a linking group of -O-, -S-, -C(=O)-, or -C(=O)O-, and groups having a heterocycle, and may be a group having an aromatic ring. The aromatic ring may have at least one of a carbocyclic ring and a heterocyclic ring, and may be a carbocyclic ring. R in the above formula (B) 5is a carbon atom of the ethylene group in formula (B) (R 5 may be bonded to the carbon atom to which R is directly bonded, 5 A carbon atom that is a ring member of the aromatic ring of formula (B) may be bonded to a carbon atom of the ethylene group in formula (B). The group having an aromatic ring may be either a monocyclic or condensed ring system, or may be a group having a benzene ring. The group having an aromatic ring may have a monovalent substituent, and the monovalent substituent may be bonded to a carbon atom that is a ring member of the aromatic ring.
[0025] In the above formula (B), R 5 is a group having an aromatic ring, and when the group having an aromatic ring has a monovalent substituent bonded to the aromatic ring, the monovalent substituent bonded to the aromatic ring is a monovalent organic group, an electron-withdrawing group such as a halogen atom (excluding those which are monovalent organic groups), an amino group (-NH 2 The monovalent substituent bonded to the aromatic ring may be a substituted or unsubstituted hydrocarbon group, a group represented by the formula: -R 41 - (W 1 -R 42 ) n -W 2 R 43 Examples of the group represented by the formula: -R 41 - (W 1 -R 42 ) n -W 2 R 43 The group represented by the formula (I) may be bonded to the para position of the benzene ring. 1 may be a divalent group such as -O-, -S-, -C(=O)- or -C(=O)O-, or may be -O-. 2 may be a divalent group such as —O—, —S—, —C(═O)— or —C(═O)O—, or may be —O—.
[0026] The above formula: -R 41 - (W 1 -R 42 ) n -W 2 R 43 In the group represented by41 is a covalent bond or a divalent organic group. The divalent organic group may be a divalent hydrocarbon group. The divalent hydrocarbon group may have 1 to 8 carbon atoms, 1 to 5 carbon atoms, or 1 to 3 carbon atoms. The hydrogen atoms bonded to the divalent hydrocarbon group may be substituted with a substituent such as a monovalent substituent (i.e., the divalent hydrocarbon group may be a substituted hydrocarbon group). Examples of the substituent include a halogen atom such as a fluorine atom. The divalent hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, or may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, or may be a linear or branched aliphatic hydrocarbon group. Specific examples of the divalent hydrocarbon group include a methylene group, an ethylene group, a 1,2-propylene group, a 1,3-propylene group, or a group in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine atoms, or may be a methylene group.
[0027] The above formula: -R 41 - (W 1 -R 42 ) n -W 2 R 43 In the group represented by 42 is a divalent organic group and may be a divalent hydrocarbon group. The divalent hydrocarbon group may have 1 to 8 carbon atoms, 1 to 5 carbon atoms, or 1 to 3 carbon atoms. The hydrogen atoms bonded to the divalent hydrocarbon group may be substituted with a substituent such as a monovalent substituent (i.e., the divalent hydrocarbon group may be a substituted hydrocarbon group). Examples of the substituent include a halogen atom such as a fluorine atom. The divalent hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, and may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, and may be a linear or branched aliphatic hydrocarbon group. Specific examples of the divalent hydrocarbon group include a methylene group, an ethylene group, a 1,2-propylene group, a 1,3-propylene group, or a group in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine atoms, and may be an ethylene group. The formula: -R 41 - (W1 -R 42 ) n -W 2 R 43 In the group represented by the formula (I), n may be 1 to 10, 1 to 5, or 1 to 3. The n may be an integer or a rational number (for example, n is an average value across the structural units (B) contained in the polymer). 42 When there are multiple, they may be different or the same.
[0028] The above formula: -R 41 - (W 1 -R 42 ) n -W 2 R 43 In the group represented by 43 may be a hydrogen atom or a divalent hydrocarbon group. The monovalent hydrocarbon group may have 1 to 8 carbon atoms, 1 to 5 carbon atoms, or 1 to 3 carbon atoms. The hydrogen atoms bonded to the monovalent hydrocarbon group may be substituted with a substituent such as a monovalent substituent (i.e., the monovalent hydrocarbon group may be a substituted hydrocarbon group). Examples of the substituent include a halogen atom such as a fluorine atom. The monovalent hydrocarbon group may be either an aromatic hydrocarbon group or an aliphatic hydrocarbon group, and may be an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, and may be a linear or branched aliphatic hydrocarbon group. Specific examples of the divalent hydrocarbon group include a methyl group, an ethyl group, an isopropyl group, an n-propyl group, or a group in which some or all of the hydrogen atoms in these groups have been substituted with halogen atoms such as fluorine atoms, and may be a methyl group.
[0029] The structural unit (B) may contain at least one structural unit derived from a monomer represented by the following formula (B1). (wherein m is 0 to 4 and n is 0 to 10. R 20 may be a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. The alkyl group may be a methyl group or an ethyl group, or may be a methyl group.
[0030] In the above formula (B1), m may be 1 to 3, may be 1 or 2, or may be 1. The above m may be an integer, or may be an average value across all structural units derived from the monomer represented by formula (B1) contained in the polymer (in this case, m is a rational number). In formula (B1), n may be 1 to 4, or may be 1 to 3. The above n may be an integer, or may be an average value across all structural units derived from the monomer represented by formula (B1) contained in the polymer (in this case, n is a rational number).
[0031] In the above formula (B), R 6 ~R 8 When at least one of the groups is a monovalent substituent, the substituent may be a monovalent organic group. 4 Examples of R in the above formula (B) include: 6 ~R 8 may be a hydrogen atom, and R 6 ~R 8 may all be hydrogen atoms.
[0032] The polymer according to the present disclosure contains a plurality of structural units (A), and the plurality of structural units (A) may be the same or different from one another, and may contain a plurality of types of structural units (A) with different chemical structures. The polymer according to the present disclosure may also contain a plurality of structural units (B), and when a plurality of structural units (B) is contained, the plurality of structural units (B) may be the same or different from one another, and may contain a plurality of types of structural units (B) with different chemical structures.
[0033] The number average molecular weight (Mn) of the polymer according to the present disclosure may be 5,000 to 400,000, 8,000 to 200,000, 10,000 to 150,000, 10,000 to 100,000, or 10,000 to 50,000. The number average molecular weight of the polymer can be measured by gel permeation chromatography.
[0034] The gel permeation chromatography (GPC) is performed under the following conditions: A standard sample of polymethyl methacrylate (manufactured by Polymer Laboratories, Mn 800 to 2,200,000) is used as the standard substance for preparing the calibration curve. <GPC measurement conditions> Apparatus: GPC-104 (Shodex) DU-H2000 precision pump 74S-RI refractive-index detector 41-UV UV / vis detector Column: Shodex LF-404 Temperature: 40°C Solvent: tetrahydrofuran (THF) Flow rate: 0.3 mL / min Back pressure: 3.0 MPa Detection: RI Sample concentration: 0.5% by mass THF solution Injection volume: 10 μL
[0035] An example of a method for producing a polymer according to this embodiment is a method of radically polymerizing a monomer composition containing a monomer such that the reactivity ratio of the monomer is 0.5 or less. The reactivity ratio of the monomer can be calculated using the Fineman-Ross method or the Kelen-Tuedos method. Specific examples of the method for producing a polymer include the following two production methods (production method (I) and production method (II)). (I) A method comprising the steps of: obtaining a raw polymer by polymerizing a monomer mixture containing a monomer (A') having a functional group capable of inducing a -COOA group and a monomer (B) other than the monomer (A') and the monomer (A') in which the functional group has been converted to a -COOA group; and converting the functional group in the raw polymer to a -COOA group. The monomers (A') and (B) can be selected such that the reactivity ratio r1' of the monomer (A') and the reactivity ratio r2' of the monomer (B) in the polymerization reaction between the monomer (A') and the monomer (B) are both 0.5 or less. (II) A method comprising a step of polymerizing a monomer mixture containing a monomer (A) having a -COOA group and a monomer (B) other than the monomer (A), wherein the reactivity ratio r1 of the monomer (A) and the reactivity ratio r2 of the monomer (B) in the polymerization reaction of the monomer (A) and the monomer (B) are both 0.5 or less.
[0036] In the production method (I), the structural unit derived from the monomer (A') becomes the structural unit (A) by converting a functional group capable of inducing a -COOA group into a -COOA group after the structural unit is incorporated into the raw polymer. In this specification, unless otherwise specified, the structural unit derived from the monomer means, in the case of radical polymerization, a structural unit having a chemical structure obtained directly by radical polymerization of the monomer.
[0037] The monomer (A') may be one represented by the following formula (MA'): 1 '~R 4 ' are R in formula (A), 1 ~R 4 may correspond to. (In formula (MA'), R 1 ' is a functional group capable of inducing a -COOA group, and R 2 ~R 4 are each independently a hydrogen atom or a monovalent substituent, or R 2 and R 3 is a hydrogen atom or a monovalent substituent, and the other is R 4 A forms a ring together with the above. A is an alkali metal element.
[0038] Examples of the functional group capable of inducing a -COOA group contained in the monomer (A') include a group that becomes a -COOH group upon hydrolysis. Examples of the group that becomes a -COOH group upon hydrolysis include a -COOR group (where R is a monovalent organic group, and may be a substituted or unsubstituted hydrocarbon group or a substituted or unsubstituted alkyl group), and include the following functional groups: (In the formula, * represents a bonding site for the functional group, and the hydrogen atom of the benzene ring may be substituted with a substituent.)
[0039] In the production method (I), the reactivity ratio r1' of the monomer (A') in the polymerization reaction of the monomer (A') with the monomer (B) may be 0.4 or less, 0.3 or less, 0.2 or less, or 0.05 or less. The reactivity ratio r2' of the monomer (B) in the polymerization reaction of the monomer (A') with the monomer (B) may be 0.4 or less, 0.3 or less, 0.2 or less, or 0.05 or less.
[0040] In production method (II), the reactivity ratio r1 of monomer (A) in the polymerization reaction of monomer (A) with monomer (B) may be 0.4 or less, 0.3 or less, 0.2 or less, or 0.05 or less. The reactivity ratio r2 of monomer (B) in the polymerization reaction of monomer (A) with monomer (B) may be 0.4 or less, 0.3 or less, 0.2 or less, or 0.05 or less.
[0041] In the production method (II), even when r1 and r2 are large (for example, both are larger than 0.5), the half width of the NMR spectrum of the obtained polymer can be set within a predetermined range by selecting, from among monomers (A') that can derive the same structural unit as the structural unit derived from monomer (A), one that has a low reactivity ratio in the polymerization reaction with monomer (B).
[0042] In the polymerization of two or more monomers having an ethylenically unsaturated group, alternating copolymerization generally increases when the monomer reactivity ratio of the monomers is less than 1. Furthermore, when a monomer X having an electron-deficient ethylenically unsaturated group is polymerized with a monomer Y having an electron-rich ethylenically unsaturated group, a copolymer in which the monomer X and the monomer Y are arranged alternately is likely to be obtained.
[0043] In production method (I), if the ethylenically unsaturated group in monomer (A') is electron-deficient and the ethylenically unsaturated group in monomer (B) is electron-rich, a polymer in which structural units derived from monomer (A') and structural units derived from monomer (B) are arranged alternately is likely to be obtained. Therefore, a monomer (A') having an electron-withdrawing group may be used. Furthermore, a monomer (B) having an aromatic ring directly bonded to the ethylenically unsaturated group may be used. Monomer (B) may further have an electron-donating group.
[0044] In production method (II), when the ethylenically unsaturated group in monomer (A) is electron-deficient and the ethylenically unsaturated group in monomer (B) is electron-rich, a polymer in which structural units derived from monomer (A) and structural units derived from monomer (B) are alternately arranged is easily obtained. Therefore, a monomer having an electron-withdrawing group may be used as monomer (A). Furthermore, a monomer having an aromatic ring directly bonded to the ethylenically unsaturated group may be used as monomer (B). Monomer (B) may further have an electron-donating group.
[0045] The polymer obtained by the production method of this embodiment can be used as a component of an electrolyte composition. One embodiment of the electrolyte composition may contain the above-mentioned polymer and, if necessary, components other than the above-mentioned polymer. Examples of such components include anion receptors, plasticizers, alkali metal salts, other resins (binder resins, etc.) such as fluorine-based resins, fabrics such as nonwoven fabrics, porous materials, and viscosity adjusters.
[0046] The electrolyte composition may contain an anion receptor. The anion receptor is a chemical species that captures anions by forming electrostatic interactions, hydrogen bonds, acid-base complexes, or the like with the anions. The anion receptor captures counter anions of alkali metal ions and promotes dissociation of the counter anions from the alkali metal ions. This increases the mobility of the metal ions. This also tends to improve the conductivity and transport number of the alkali metal ions in the electrolyte composition.
[0047] Low molecular weight chemical species (compounds, etc.) that function as the anion receptor are known, and examples of such compounds include those described in U.S. Patent Nos. 6,022,643, 5,705,689, and 6,120,941. The anion receptor may have a formula weight (molecular weight) of, for example, 1,000 or less, 800 or less, or 500 or less.
[0048] The anion receptor may have Lewis acidity. In this case, the anion receptor can capture the anion by accepting the unshared electron pair of the anion and forming an acid-base complex. Examples of such compounds include compounds having an electron-deficient atom. Note that an electron-deficient atom refers to an atom that is covalently bonded to another atom but has fewer than eight electrons in its outermost shell. Examples of the electron-deficient atom include atoms belonging to Group 13 of the periodic table, and more specifically, may be at least one of an aluminum atom and a boron atom, or may be a boron atom.
[0049] Examples of anion receptors having a boron atom include boron compounds that function as Lewis acids, such as diborane and compounds represented by the following chemical formulas IA to IE.
[0050]
[0051] In Formula IA, R 31is a halogen atom or a monovalent organic group. The halogen atom may be a fluorine atom or a chlorine atom, or may be a fluorine atom. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the boron atom (B) in Formula IA via a carbon atom in the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. 31 may be different from each other or may all be the same.
[0052] In formula IB, R 32is a hydrogen atom or a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. Here, the monovalent organic group is bonded to the oxygen atom (O) in Formula IB via a carbon atom in the monovalent organic group. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. In one molecule, there are multiple R 32 may be different from each other or may all be the same.
[0053] In formula IC, R 35 is a divalent organic group, Z 2 is a covalent bond or an oxygen atom. The number of carbon atoms in the divalent organic group may be 1 to 15, 2 to 10, or 3 to 8. In formula IC, R 35 , two Zs 2 and the boron atom (B) form a ring, and the ring may have 4 to 8 ring members, or may have 5 or 6 ring members. The divalent organic group is not particularly limited and may be a hydrocarbon group, a divalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-, etc. 2 When is an oxygen atom, the divalent organic group is connected to Z in formula IC by the carbon atom contained in the divalent organic group. 2 and the above Z 2is a covalent bond, the divalent organic group is bonded to the boron atom (B) in formula IC via a carbon atom contained in the divalent organic group. The hydrogen atom bonded to the hydrocarbon portion of the divalent organic group may be substituted with a substituent. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The divalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. In one molecule represented by formula IC, multiple Z 2 may be different from each other or may all be the same.
[0054] In formula IC, R 36 is a hydrogen atom or a monovalent organic group. The monovalent organic group may be a group that bonds to the boron atom (B) in formula IC via a carbon atom that the monovalent organic group has, but -OR 37 The above-mentioned —OR 37 R in the group represented by 37 is a hydrogen atom or a monovalent organic group. 37 The monovalent organic group represented by the formula (I) is -OR 37 The oxygen atom of the above R 36 When R is a monovalent organic group, the number of carbon atoms in the organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. 37The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the boron atom (B) in Formula IA via a carbon atom possessed by the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group.
[0055] In Formula ID, R 33 is a hydrogen atom, a halogen atom, or a monovalent organic group. The halogen atom may be a fluorine atom or a chlorine atom, or may be a fluorine atom. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the boron atom (B) in Formula ID via a carbon atom in the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. 33 may be different from each other or may all be the same.
[0056] In formula IE, R 34 is a hydrogen atom or a monovalent organic group. The number of carbon atoms in the monovalent organic group may be 1 to 20, 1 to 15, 2 to 10, or 2 to 6. The monovalent organic group is not particularly limited and may be a hydrocarbon group, a monovalent group having a chemical structure in which one or more carbon atoms (methylene groups) in a hydrocarbon group are substituted with a linking group such as -O-, -S-, -C(=O)-, or -C(=O)O-. The hydrogen atom bonded to the hydrocarbon portion of the monovalent organic group may be substituted with a substituent. Here, the monovalent organic group is bonded to the oxygen atom (O) in Formula IE via a carbon atom possessed by the monovalent organic group. The substituent may be a monovalent substituent such as a halogen atom, a monovalent electron-withdrawing group, or a fluorine atom. The monovalent organic group may be a hydrocarbon group or a halogen-substituted hydrocarbon group, and the halogen-substituted hydrocarbon group may be a partially or fully fluorinated hydrocarbon group. In one molecule represented by formula IE, multiple R 34 may be different from each other or may all be the same.
[0057] Specific examples of boron compounds include diborane, boron trifluoride, boric acid, boroxine, trimethylborane, triethylborane, tri-n-propylborane, triisopropylborane, triphenylborane, trimethylborate, triethylborate, triphenylborate, tri-n-propylborate, triisopropylborate, 2-methoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane, and 2-ethoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane. Examples thereof include organic boron compounds such as oran, 2,4,6-trimethylboroxine, 2,4,6-triethylboroxine, 2,4,6-trivinylboroxine, 2,4,6-trimethoxyboroxine, 2,4,6-trimethoxyboroxine, and triphenylboroxine; and halogen-substituted hydrocarbon groups such as tris(2,2,2-trifluoroethyl)borate, 2,4,6-tris(4-fluorophenyl)boroxine, and 2,4,6-tris(3,4,5-trifluorophenyl)boroxine.
[0058] The anion receptor having an aluminum atom includes an aluminum compound that functions as a Lewis acid, and has the formula AlX 1 3 (X in the formula 1 is a halogen atom, which may be a fluorine atom), the formula: Al(OR 35 ) 3 (R in the formula 35 is a hydrocarbon group, which may be an alkyl group.
[0059] The anion receptor may also be an azaether. An azaether is an ether compound in which —O— is replaced by —NR E - (where R E is a hydrogen atom or an organic group). The azaether may be either a linear azaether or a cyclic azaether. The azaether may have an electron-withdrawing group, for example, in the hydrocarbon moiety.
[0060] The content of the anion receptor in the electrolyte composition may be 10 to 200 parts by mass, 30 to 180 parts by mass, 50 to 150 parts by mass, or 80 to 130 parts by mass relative to 100 parts by mass of the polymer of the present embodiment.
[0061] The plasticizer may be an organic solvent. The organic solvent may be an aprotic solvent. The organic solvent may include one or more organic solvents selected from the group consisting of carbonate solvents, ether solvents, fluorine solvents, nitrile solvents, and phosphate ester solvents, and may include a phosphate ester.
[0062] Examples of carbonate solvents include chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; and cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate.
[0063] Examples of the ether solvent include cyclic ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, and 1,3-dioxolane; and chain ethers such as 1,2-diethoxyethane and ethoxymethoxyethane.
[0064] Examples of the fluorine-based solvent include hydrofluorocarbons such as perfluorooctane; hydrofluoroethers such as methyl nonafluorobutyl ether and ethyl nonafluorobutyl ether; and hydrofluoroolefins such as 1,3,3,3-tetrafluoropropene.
[0065] Examples of the phosphate ester include trimethyl phosphate (TMP), triethyl phosphate (TEP), and tris(2,2,2-trifluoroethyl) phosphate (TFEP).
[0066] In addition to the above, examples of organic solvents include solvents having a sulfonyl group such as dimethyl sulfoxide (DMSO); amide solvents such as dimethylformamide (DMF) and dimethylacetamide (DMA); organic solvents having a carbonyl group such as acetone (referring to carbonyl compounds other than amide compounds such as -C(=O)-, esters, ketones, and aldehydes); and nitrogen-containing aromatic compounds such as pyridine (compounds containing nitrogen as a ring member of the aromatic ring, which may be either monocyclic or fused ring systems). Only one organic solvent may be used, or a mixed solvent containing two or more organic solvents may be used.
[0067] The content of the organic solvent in the electrolyte composition may be 100 to 500 parts by mass, 150 to 450 parts by mass, 200 to 400 parts by mass, or 250 to 350 parts by mass relative to 100 parts by mass of the polymer of the present embodiment.
[0068] The content of the organic solvent in the electrolyte composition may be 30 to 90 mass %, 35 to 85 mass %, 40 to 80 mass %, 45 to 75 mass %, 50 to 70 mass %, or 60 to 70 mass %, relative to the total amount of the electrolyte composition.
[0069] The electrolyte composition may further contain other resins (binder resins, etc.) such as fluororesins, fabrics such as nonwoven fabrics, porous materials, viscosity adjusters, etc. The electrolyte composition may contain, as the fluororesin, a resin having a carbon chain as the main chain. The carbon chain may be formed by radical polymerization of an ethylenically unsaturated group. Examples of fluororesins include poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), polyvinylidene fluoride (PVDF), etc.
[0070] The content of the other resin in the electrolyte composition may be 10 to 100 parts by mass, 20 to 80 parts by mass, 30 to 70 parts by mass, or 40 to 60 parts by mass relative to 100 parts by mass of the polymer of the present embodiment.
[0071] The electrolyte composition may contain an alkali metal salt, such as MF, MCl, MBr, MI, or MClO, where M is an alkali metal. 4 , MPF 6 , MBF 4 , M 2 SO 4 , M[(C h F 2h+1 ) SO 3 ] (h is 0 to 3), M[(C h F 2h+1 ) SO 2 ] 2 N (h is 0 to 3), M{[(C h F 2h+1 ) SO 2 ]N[(C i F 2i+1 ) SO 2 ]} (h and i are 0 to 3). One or more types of alkali metal salts may be used. The alkali metal contained in the alkali metal salt may be the same alkali metal element as the alkali metal element contained in the structural unit (A) described in the description of the polymer of the present disclosure.
[0072] The content of the alkali metal salt in the electrolyte composition may be 10 to 200 parts by mass, 20 to 150 parts by mass, 30 to 100 parts by mass, or 40 to 75 parts by mass relative to 100 parts by mass of the polymer of the present embodiment.
[0073] The method for producing the electrolyte composition is not particularly limited, and examples thereof include a method in which a dry film of the polymer of this embodiment or a dry film is produced by mixing the polymer of this embodiment with a binder resin, and then the dry film is impregnated with an organic solvent. When the electrolyte composition contains an alkali metal salt or an anion receptor, the polymer, optionally a binder resin, and the alkali metal salt or anion receptor may be mixed to produce a dry film, and then an organic solvent may be added, or the alkali metal salt or anion receptor may be dissolved in an organic solvent and added to the dry film.
[0074] The electrolyte composition of this embodiment can be used as a composition for forming an electrolyte for batteries, capacitors, etc. That is, the electrolyte of this embodiment includes the above-described electrolyte composition. Examples of the battery include batteries that perform charging and discharging by the movement of alkali metal ions, such as lithium ion batteries and sodium ion batteries. The battery may be a primary battery, a secondary battery, or a solid-state battery.
[0075] The battery of this embodiment includes a positive electrode, a negative electrode, and an electrolyte disposed between the positive electrode and the negative electrode. The positive electrode may be a layer containing a positive electrode material formed on a current collector. The negative electrode may be a layer containing a negative electrode material formed on a current collector. The following description will be given taking a lithium-ion battery as an example.
[0076] The negative electrode of the lithium ion battery is not particularly limited and may contain a negative electrode active material and, if necessary, a conductive additive, a binder, etc. Examples of the negative electrode active material include simple elements such as Li, Si, P, Sn, Si—Mn, Si—Co, Si—Ni, In, and Au, alloys or composites containing these elements, carbon materials such as graphite, substances in which lithium ions are inserted between the layers of the carbon material, and oxides containing titanium.
[0077] The positive electrode of the lithium ion battery is not particularly limited, and may contain a positive electrode active material and, if necessary, a conductive additive, a binder, etc. Examples of the positive electrode active material include lithium composite metal oxides containing lithium and a transition metal element. The transition metal element may be at least one selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Cu, and Al, and may contain Ni. Examples of the lithium composite metal oxides include LiCoO 2 , LiNiO 2 , LiMn 2 O 4 , LiNi 0.5 Mn 1.5 O 4 , Li 2 MnO 3 , LiNi x Mn y Co 1-x-y O 2 [0<x+y<1]), LiNi x Co y Al 1-x-y O 2 [0<x+y<1]), LiCr 0.5 Mn 0.5 O 2 , LiFePO 4 , Li 2 FeP 2 O 7 , LiMnPO 4 , LiFeBO 3 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 CuO 2 , Li 2 FeSiO 4 , Li 2 MnSiO 4 When the positive electrode active material contains an alkali metal element other than Li, specific examples thereof include those in which Li in the above specific examples is replaced with another alkali metal.
[0078] The negative electrode (negative electrode material) and the positive electrode (positive electrode material) of this embodiment may further contain a solid electrolyte material, a binding resin (binder), a conductive assistant, and the like.
[0079] The battery may have a separator. The separator may be a porous material, such as a porous resin material. Specific examples of the separator include a porous polyolefin membrane and a porous ceramic membrane.
[0080] Example 1 A lithiated carboxyl group-containing copolymer of Example 1 was produced by the following method.
[0081] Saccharin methacrylamide (SacM) (1.8848 g, 7.5 mmol), styrene (St) (0.86 mL, 7.5 mmol), tetralin (0.15 mL), and azobisisobutyronitrile (24.7 mg, 0.15 mmol) were dissolved in a mixed solvent of dioxane and acetonitrile (dioxane:acetonitrile=1:1 (volume ratio)) (12.1 mL), and the solution was stirred at 60° C. for 24 hours to obtain a solution of a copolymer of saccharin methacrylamide and styrene (raw material copolymer).
[0082] Next, a 25 mM phenothiazine solution in 1,4-dioxane (45.0 mL, 1.13 mmol) and 100 equivalents of water were added to the resulting polymerization solution, and the mixture was stirred overnight. As a result, the structural units derived from saccharin methacrylamide in the raw copolymer were hydrolyzed, and the amide bonds containing saccharin moieties were converted to -COOH groups (i.e., the structural units derived from saccharin methacrylamide were converted to methacrylic acid (MAA) units), yielding a -COOH group-containing copolymer (0.61 g).
[0083] The composition ratio of the structural units in the polymer was MAA:St = 48:52 (molar ratio). 1 It was calculated by measuring the H-NMR spectrum.
[0084] Then, the -COOH group-containing copolymer (0.61 g, 3.21 mmol) was dissolved in dimethylformamide (12 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH (449.1 mg, 18.82 mmol) relative to the amount of SacM initially charged when producing the raw material copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days. As a result, a copolymer in which the -COOH groups of the -COOH group-containing copolymer had been converted to -COOLi (lithiated carboxyl group-containing copolymer) was obtained (0.43 g).
[0085] The raw copolymer was alcoholyzed with methanol instead of water to synthesize a copolymer of MMA and St, and the molecular weight of the copolymer was measured by gel permeation chromatography. The number average molecular weight of the copolymer was 18,200.
[0086] Example 2 A lithiated carboxyl group-containing copolymer of Example 2 was produced by the following method.
[0087] In Example 2, the monomer represented by the following formula (i.e., 4-(2-methoxyethoxy)methoxystyrene) was used in place of the styrene in Example 1. (where m=1 and n=1)
[0088] Saccharin methacrylamide (SacM) (628.8 mg, 2.5 mmol), 4-(2-methoxyethoxy)methoxystyrene (0.49 mL, 2.5 mmol), azobisisobutyronitrile (8.8 mg, 0.05 mmol), and tetralin (0.05 mL) were dissolved in a mixed solvent of dioxane and acetonitrile (dioxane:acetonitrile=1:1 (volume ratio)) (3.75 mL), and the solution was stirred at 60°C for 24 hours to obtain a copolymer of SacM and 4-(2-methoxyethoxy)methoxystyrene (raw copolymer).
[0089] Next, a 25 mM phenothiazine solution in 1,4-dioxane (15.0 mL, 0.38 mmol) and 100 equivalents of water were added to the resulting raw copolymer, and the mixture was stirred overnight. As a result, the structural units derived from saccharin methacrylamide in the raw copolymer were hydrolyzed, and the amide bonds containing saccharin moieties were converted to -COOH groups (i.e., the structural units derived from saccharin methacrylamide were converted to methacrylic acid (MAA) units), yielding a -COOH group-containing copolymer (0.28 g).
[0090] The composition ratio of the structural units in the polymer was MAA:4-(2-methoxyethoxy)methoxystyrene = 47:53 (molar ratio). 1 It was calculated by measuring the H NMR spectrum.
[0091] Then, the -COOH group-containing copolymer (0.28 g, 1.00 mmol) was dissolved in dimethylformamide (4.6 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH (149.0 mg, 6.22 mmol) relative to the amount of SacM initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days (24 hours). As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer were converted to -COOLi was obtained (0.23 g). In the synthesized copolymer, -COO - Because the groups were fixed on the copolymer, they did not move even when a voltage was applied, and the transference number of lithium ions was sufficiently high.
[0092] The raw copolymer was alcoholyzed with methanol instead of water to synthesize a copolymer of MMA and St, and the molecular weight of the copolymer was measured by gel permeation chromatography. The number average molecular weight of the copolymer was 30,100.
[0093] Comparative Example 1 A lithiated carboxyl group-containing copolymer of Comparative Example 1 was produced by the following method.
[0094] Tert-butyl methacrylate (tBMA) (1.22 mL, 7.5 mmol), styrene (St) (0.86 mL, 7.5 mmol), and azobisisobutyronitrile (20.0 mg, 0.12 mmol) were dissolved in toluene (13.0 mL) and stirred at 60°C for 24 hours to obtain a copolymer of tert-butyl methacrylate and styrene (raw copolymer) (0.59 g). The composition ratio of the structural units in the raw polymer was tBMA:St = 46:54 (molar ratio). The composition ratio was determined by dissolving the raw polymer in deuterated chloroform, 1 This was confirmed by measuring the H NMR spectrum.
[0095] Next, excess trifluoroacetic acid (15.0 mL, 196 mmol) was added to the obtained raw copolymer (0.59 g), and the mixture was stirred at 40° C. for 24 hours. As a result, the —C(═O)—O—C(CH 3 ) 3 The groups were substituted with —COOH groups (that is, the structural units derived from tBMA were converted to methacrylic acid (MAA) units), and a —COOH group-containing copolymer was obtained (0.36 g).
[0096] Then, the -COOH group-containing copolymer (0.36 g) was dissolved in dimethylformamide (3.0 mL) to obtain a solution. To this solution, 2.5 equivalents of LiOH relative to the amount of tBMA initially charged when producing the raw copolymer was added, and the mixture was stirred at room temperature (25°C) for 3 days. As a result, a copolymer (lithiated carboxyl group-containing copolymer) in which the -COOH groups of the -COOH group-containing copolymer had been converted to -COOLi was obtained (0.26 g). The obtained lithiated carboxyl group-containing copolymer was dissolved in deuterated dimethyl sulfoxide. 1 By measuring the H NMR spectrum, it was found that the composition ratio of the structural units in the lithiated carboxyl group-containing copolymer was lithiated MAA:St=47:53 (molar ratio).
[0097] <Solid 13Solid-state NMR was measured using a Bruker AVANCEIII 800 solid-state MAS BL4 probe at a resonance frequency of 201 MHz (external magnetic field) at room temperature (25° C.) and 8 kHz MAS. 13 The half-width of the peak derived from the carbonyl carbon of the lithiated MAA unit in each copolymer was determined from the CNMR spectrum. The results are shown in Table 1.
[0098] <Solution 13 CNMR Measurement> The apparatus used was a JNM-ECA500 spectrometer (manufactured by JEOL Ltd.), 1 The H-NMR measurement was carried out at room temperature (25°C) and a resonance frequency (external magnetic field) of 500.16 MHz. 13 The C-NMR measurement was carried out under the conditions of 55°C and a resonance frequency (external magnetic field) of 125.04 MHz. 3 For Comparative Example 1, 120 mg of the copolymer was dissolved in 0.6 mL of CD 3 The results are shown in Table 1.
[0099]
[0100] (Preparation of Electrolyte Compositions) Each component was mixed according to the composition shown in Table 2 to prepare each electrolyte composition.
[0101] The abbreviations in Table 2 are as follows: TMP: trimethyl phosphate TEP: triethyl phosphate EC: ethylene carbonate PC: propylene carbonate PVDF-HFP: vinylidene fluoride-co-hexafluoropropylene
[0102] <Measurement of Ionic Conductivity> The ionic conductivity of the electrolyte composition was measured by the following method. Ionic conductivity (σ 25 ) are shown in Table 2.
[0103] First, in a glove box under a dry argon atmosphere, an evaluation cell of the coin-type battery CR2032 was assembled. Specifically, a test laminate was prepared by laminating each layer in the following order in the evaluation cell: stainless steel plate / electrolyte composition / stainless steel plate.
[0104] Measurements are made using an impedance measuring device under the conditions of 25°C, a frequency range of 0.1 Hz to 1 MHz, and an applied voltage of 10 mV (vs. open circuit voltage). The ionic conductivity σ can be calculated using the following formula. In the formula, R represents the impedance value, A represents the area of the sample, and t represents the thickness of the sample. σ (S cm -1 )=t(cm) / (R(Ω)×A(cm 2 ))
[0105] <Activation Energy> Ion conductivity measurements using the above evaluation cell were also carried out under conditions of 25, 30, 40, 50, 60, and 70°C to measure the change in ionic conductivity with respect to temperature. Activation energy was calculated from the slope of a graph of the common logarithm of ionic conductivity versus the reciprocal of temperature using the Arrhenius equation (logk = logA - Ea / RT, where k is the reaction rate constant, A is the frequency factor, Ea is the activation energy, R is the gas constant, and T is the absolute temperature). The results are shown in Table 2.
[0106]
[0107] (Preparation of Electrolyte Compositions) Each component was mixed according to the compositions shown in Tables 3 and 4 to prepare each electrolyte composition containing an anion receptor, and the ionic conductivity and activation energy at 25° C. were determined by the methods described above.
[0108] The abbreviations in Tables 3 and 4 are as follows: In addition, lithium (bistrifluoromethanesulfonyl)imide (LiTFSI) was used as the lithium salt in Table 4. MTD: 2-methoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane TEB: tris(2,2,2-trifluoroethyl)borate TFB: 2,4,6-tris(4-fluorophenyl)boroxine PVDF-HFP: vinylidene fluoride-co-hexafluoropropylene
[0109] The electrolyte compositions of Examples A8 and A9 were produced by mixing a polymer and PVDF-HFP to form a dry film, and then impregnating the dry film with an organic solvent in which a lithium salt and an anion receptor had been dissolved.
[0110] The electrolyte composition of Example A10 was produced by mixing a polymer, PVDF-HFP, a lithium salt, and an anion receptor to form a dry film, and then impregnating the dry film with an organic solvent.
[0111]
[0112]
[0113] (Preparation of Electrolyte Compositions) Each component was mixed according to the composition shown in Table 5 to prepare each electrolyte composition containing an anion receptor, and the ionic conductivity and activation energy at 25° C. were determined by the above-mentioned method.
[0114]
[0115] <Measurement of Lithium Ion Transference Number> The lithium ion transference numbers of the electrolyte compositions prepared as described above were measured by the following method. The results are shown in Table 6.
[0116] First, in a glove box under a dry argon atmosphere, an evaluation cell of a coin-type lithium battery CR2032 was assembled. Specifically, each layer was laminated in the evaluation cell in the order of lithium / electrolyte composition / lithium to prepare a test laminate.
[0117] The lithium ion transport number measurement method is introduced in Polymer, 28, 2324 (1987). That is, 10 mV is applied to the test laminate at room temperature (25° C.), and the initial current value (I 0 ) and steady-state current value (I ss ) was measured, and the interface resistance measured value R 0 and the measured interface resistance R after voltage application SS The lithium ion transport number (t Li+ ) was calculated. V in the formula is the applied voltage. Li+ =I ss(V-I 0 R 0 ) / I 0 (V-I SS R SS )
[0118]
Claims
1. A polymer comprising a structural unit (A) represented by the following formula (A) and a structural unit (B) represented by the following formula (B), which satisfies at least one of the following (1) to (3): (1) The solid state of the polymer at 25° C. 13 When the polymer is subjected to CNMR measurement, the half-width of the peak derived from the carbonyl carbon of the -COOA group (A is an alkali metal element) is 1,380 Hz or less. 13 When the CNMR measurement is carried out in deuterated methanol, the half-value width of the peak derived from the carbonyl carbon of the -COOA group is 80 Hz or less. 13 When CNMR measurement was performed in deuterated methanol, the ratio of the peak height to the half-width of the peak derived from the carbonyl carbon of the -COOA group was 0.4 × 10 -4 abn / Hz or more. (In formula (A), R 1 is a -COOA group or a monovalent organic group having a -COOA group, and R 2 ~R 4 are each independently a hydrogen atom or a monovalent substituent, or R 2 and R 3 One of the groups is a hydrogen atom or a monovalent substituent, and the other is R 4 and form a ring. * indicates the bond between the structural unit (A) and another structural unit. (In formula (B), R 5 is a hydrogen atom or a monovalent substituent, R 6 ~R 8 are each independently a hydrogen atom or a monovalent substituent, or R 6 and R 7 One of the groups is a hydrogen atom or a monovalent substituent, and the other is R 8 and form a ring. * indicates the bond between the structural unit (B) and other structural units.
2. The polymer of claim 1, wherein A comprises at least one of sodium and lithium.
3. An electrolyte composition comprising the polymer according to claim 1 or 2.
4. The electrolyte composition according to claim 3, further comprising a plasticizer, the plasticizer comprising at least one solvent selected from the group consisting of carbonate-based solvents, ether-based solvents, fluorine-based solvents, and phosphate-based solvents.
5. The electrolyte composition of claim 3, further comprising an anion receptor.
6. The electrolyte composition of claim 3 further comprising an alkali metal salt.
7. A polymer obtained by polymerizing a monomer mixture containing a monomer (A) having a -COOA group (A is an alkali metal element) and a monomer (B) other than the monomer (A), wherein the reactivity ratio r1 of the monomer (A) and the reactivity ratio r2 of the monomer (B) in the polymerization reaction between the monomer (A) and the monomer (B) are both 0.5 or less.
8. A battery comprising the electrolyte composition of claim 3.
Citation Information
Patent Citations
Aza compounds as anion receptors
US5705689A
Boron compounds as anion binding agents for nonaqueous battery electrolytes
US6022643A
Anion receptor compounds for non-aqueous electrolytes
US6120941A
Water-absorbing composite and its production
JP1984230046A
High molecular electrolyte gel
JP2001176556A
Cited By
Polymer, electrolyte composition, and battery
WO2026014389A1