Conductive flexible transparent wooden film, electronic device, and preparation method

By combining transparent wood film with origami technology, conductive ink is prepared using wood powder and multi-wall carbon nanotubes, and printed on the surface of the wood film to form a circuit, solving the problems of insufficient interface bonding and poor durability of the plastic substrate in flexible electronic devices, realizing the Flexible electronic devices with editable shapes expand their application areas and improve the value of wood.

WO2024234413A1PCT designated stage expired Publication Date: 2024-11-21NANJING FORESTRY UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/096820
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2023-05-29
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In existing flexible electronic devices, plastic substrates have problems such as insufficient interface bonding, poor durability and environmental pollution, and are difficult to apply to complex shape and shape transformation scenarios.

Method used

Using transparent wood film combined with origami technology and three-dimensional printing, flexible transparent wood film is prepared by delignin and dehemic cellulose treatment, and conductive ink is prepared using wood powder and multi-wall carbon nanotubes as raw materials, and printed on the surface of the wood film to form a circuit. , realize flexible electronic devices with editable shapes.

Benefits of technology

The mechanical strength and performance of flexible transparent wood membrane are achieved with flexibility, can be folded into a three-dimensional structure, expanding the application field of flexible electronic devices, and improving the utilization value of wood.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023096820_21112024_PF_FP_ABST
    Figure CN2023096820_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of novel wood technology development, and provides a conductive flexible transparent wooden film, an electronic device, and a preparation method. The preparation method for the conductive transparent wooden film provided by the present invention comprises: using natural wood pieces as raw materials; removing lignin and part of hemicellulose to prepare a transparent wooden film; and printing CNT / CNFs conductive ink on the surface of the transparent wooden film to form a circuit. The transparent wooden film provided by the present invention has high mechanical properties and flexibility, and excellent optical strength; conductive ink is deposited on the surface to form a conductive circuit, and a single-channel or multi-channel circuit is implemented by means of spatial transformation such as folding or cutting; the transparent wooden film is combined with the traditional paper folding and cutting techniques to realize the editable and adjustable design of the spatial structure, so that a flexible electronic device of the transparent wooden film transitions from a simple shape to a complex shape; moreover, the transparent wooden film can be customized to meet specific requirements or applications.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive flexible transparent wood film, electronic device and preparation method Technical Field

[0001] The present invention relates to the technical field of novel wood technology development, and in particular to a conductive flexible transparent wood film, an electronic device and a preparation method thereof. Background Art

[0002] With the development of science and technology and the in-depth study of electronic materials, flexible electronics has become one of the hottest multidisciplinary research fields in recent years. The use of metal and plastic substrates in traditional flexible electronic devices still faces challenges, such as the need for high-temperature and high-pressure preparation processes, insufficient interface bonding between the plastic substrate and the functional material, and poor durability. In addition, these plastic substrates are generally incinerated and landfilled after use in electronic devices. The large amount of carbon emissions generated by incineration pollutes the atmospheric environment. The landfilled plastic is difficult to degrade, which will also seriously affect the soil environment and disrupt the ecological balance. In order to alleviate the problem of dependence on non-renewable resources, research shows that vigorously developing resource-rich, green and environmentally friendly materials has become an important research topic in the field of flexible electronic devices.

[0003] Wood, a sustainable, renewable, and biodegradable natural material, possesses a unique natural pore structure, excellent mechanical properties, and a complex multilayered architecture. In recent years, with the improvement of traditional wood functions and the advancement of modern nanotechnology, researchers have developed multifunctional wood-based advanced functional materials with broad application prospects in energy-saving building materials, clean energy, wastewater treatment, and optoelectronic devices. Among them, transparent wood is a biomass-based material with high transparency, low thermal conductivity, and environmental friendliness. Currently, the construction of flexible electronic devices based on transparent wood mainly involves two strategies: bottom-up and top-down. The bottom-up approach involves self-assembling nanocellulose and introducing conductive materials to construct cellulose films with high conductivity, high transparency, and high flexibility, thereby achieving lightweight and flexible electronic device substrates. Alternatively, the top-down approach uses wood as a template, removes most of the lignin and some hemicellulose, and densifies the delignified template to produce wood films with high mechanical, flexibility, and optical properties.

[0004] Theoretical and applied research in optoelectronic devices has become a hot topic internationally. The use of conductive inks to form circuits on transparent wood films shows great potential as an alternative to plastic substrates. Related research has demonstrated that delignified wood can be used to create highly transparent anisotropic films. Furthermore, by coating with silver nanowire ink, ultrathin, highly transparent, and highly conductive films can be fabricated, promising applications in mobile phone screens. Electroluminescent devices constructed from flexible transparent wood films exhibit excellent thermal stability and water resistance. The low thermal expansion coefficient of the transparent wood film also provides good dimensional stability for the substrate in the device. By directly printing lignin-derived conductive inks onto transparent wood film substrates, all-wood flexible films can be fabricated for use in flexible strain sensors, demonstrating more stable conductivity than plastic. However, current research is still in its early stages, and the application scenarios are relatively limited, limited to simple planar device designs. The rapid development of flexible electronic devices requires substrates that can accommodate increasingly complex shapes, interfaces, and applications while maintaining mechanical strength and performance. Further breakthroughs are needed in the areas of shape transformation and editability.

[0005] Origami and paper cutting utilize the logical variations of spatial configurations to design, fold, and cut, transforming two-dimensional structures into three-dimensional structures. These processes allow for the design of deformations from simple to complex shapes, while also endowing them with inherent shape editability and shape deformation capabilities. Origami and paper cutting offer advantages such as simplicity, efficiency, and flexibility. Due to their excellent editability and shape repeatability, they are widely used to construct three-dimensional and thin film structures. For example, thin film folding and unfolding mechanisms developed using origami techniques offer advantages such as light weight, large area, foldability, and high storage ratios. These mechanisms are increasingly being used in spacecraft to replace traditional mechanical deployment methods. Furthermore, leveraging the natural chemical composition of wood to create highly efficient and conductive conductive inks will provide a path to effectively utilize all of wood's components.

[0006] In summary, by combining transparent wood film with origami technology and three-dimensionally printing conductive ink circuits made of wood components on the surface, single-pass or multi-pass conductivity can be achieved during the deformation process. By designing different forms of folding methods and rationally designing the spatial folding angle or cutting path, shape-editable all-wood-based flexible electronic devices can be realized. This is expected to expand the potential application areas of flexible electronic devices constructed with transparent wood film and increase the high added value of wood utilization.

[0007] Summary of the Invention

[0008] In view of this, the purpose of the present invention is to provide a conductive flexible transparent wood film, an electronic device and a preparation method. The flexible transparent wood film provided by the present invention ensures its flexibility while ensuring mechanical strength and performance, and can be folded into a three-dimensional structure.

[0009] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a conductive flexible transparent wood film, comprising the following steps:

[0010] (1) Delignification treatment of natural wood chips using NaClO2 solution in an acidic buffer solution;

[0011] (2) The wood chips after delignining are subjected to hemicellulose removal treatment in an alkaline solution, and then placed between a polyethersulfone membrane layer and a filter paper layer, and compressed under external force for 24 to 48 hours to obtain a transparent wood film;

[0012] (3) Preparation of CNT / CNFs conductive ink using wood powder and multi-walled carbon nanotubes as raw materials;

[0013] (4) Printing the obtained CNT / CNFs conductive ink on the surface of the transparent wood film obtained in step (2) to form a circuit.

[0014] Preferably, the method for preparing the CNT / CNFs conductive ink in step (3) comprises the following steps:

[0015] (S1) Using wood powder as raw material, high aspect ratio nanocellulose was prepared by TEMPO oxidation method, dissolved in deionized water, and a uniform TOCNFs suspension was obtained by stirring and ultrasonication;

[0016] (S2) Multi-walled carbon nanotubes are added to the TOCNFs suspension, stirred, and ultrasonicated, and the mixed solution is concentrated to obtain a gel-like CNT / CNFs conductive ink.

[0017] Further preferably, the amount of the TEMPO oxidant used in step (S1) is 8 mmol / g; the TOCNFs have a diameter of 5-15 nm and a length of 0.5-1 μm.

[0018] Further preferably, the TOCNFs content in the TOCNFs suspension in step (S1) is 0.2 to 0.8 wt%.

[0019] More preferably, the multi-walled carbon nanotubes in step (S2) have a diameter of 5-15 nm, a length of 0.5-2 μm, and a carboxyl content of 3-5 wt%.

[0020] Further preferably, the mass ratio of TOCNFs to multi-walled carbon nanotubes in the mixed solution of step (S2) is (1-2):(1-2).

[0021] Further preferably, the concentration of the mixed solution after concentration in step (S2) is 4 to 8 wt%.

[0022] The present invention also provides a conductive flexible transparent wood film prepared by the preparation method described in the above technical solution.

[0023] The present invention also provides an editable wood flexible electronic device, which is obtained by editing the conductive flexible transparent wood film described in the above technical solution.

[0024] Beneficial technical effects:

[0025] 1. The flexible transparent wood film provided by the present invention ensures its mechanical strength and performance while ensuring its flexibility and can be folded into a three-dimensional structure.

[0026] 2. The flexible transparent wood film provided by the present invention can be edited using origami geometric structures to give it programmable shape and deformation capabilities. By regulating the folding angle, folding direction, thickness of the transparent wood film and the thickness of the printed conductive ink during the folding / cutting process, it is possible to construct a transparent wood film flexible electronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 is a schematic diagram of the preparation process of the transparent wood film in Example 1;

[0028] FIG2 is a schematic diagram of the optical properties of the transparent wood film in Example 1;

[0029] FIG3 is an SEM image of logs, delignified wood, and alkali-treated wood in Example 1;

[0030] FIG4 is a graph showing the haze and transmittance of the transparent wood film in Example 1;

[0031] FIG5 is a schematic diagram of the mechanical properties of the transparent wood film, original wood, and delignified wood in Example 1;

[0032] FIG6 is a diagram showing the appearance of the CNT / CNFs conductive ink prepared in Example 1;

[0033] FIG7 is a graph showing the rheological properties of the CNT / CNFs conductive inks prepared in Examples 1 to 4;

[0034] FIG8 is a surface diagram of conductive ink printed on the transparent wood film surface in Example 1;

[0035] FIG9 is an atomic force microscope (AFM) microscopic morphology characterization of the transparent wood film in Example 1;

[0036] FIG10 is an SEM image of ink printed on the surface of the transparent wood film in Example 1.

[0037] FIG11 is a diagram showing the folding and application of the transparent wood film flexible electronic device in Example 4. DETAILED DESCRIPTION

[0038] In order to have a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be understood as limiting the scope of implementation of the present invention.

[0039] Natural wood is inherently opaque, so the preparation of transparent wood films for flexible electronics involves two key steps: removing light-absorbing components (including removing and modifying lignin) and reducing the refractive index difference between the wood and air. Delignification removes components in the wood that absorb visible light, while the natural wood's honeycomb cell wall structure, along with its original fiber orientation and multi-layered assembly, remains intact in the treated wood. To reduce the refractive index difference, the transparent wood film densifies the delignified wood to form a transparent film. Delignification reduces the rigidity of the cell wall, making it more flexible and more easily collapsed without breaking. The collapse process forms a stacked layered structure, and under the influence of water molecules, numerous hydrogen bonds are formed, resulting in a transparent wood film with dense cell wall interfacial bonding and a holocellulose content of 90-98%. The present invention utilizes a top-down approach to prepare the transparent wood film. Compared to the bottom-up method, the top-down approach eliminates the steps of separating and reorganizing cellulose, offering significant advantages in production efficiency, reduced chemical reagent use, and lower energy consumption. The top-down approach directly transforms natural wood into a transparent film with excellent mechanical and optical properties, making the entire process more environmentally friendly and efficient.

[0040] Based on the above principles, the present invention provides a method for preparing a conductive flexible transparent wood film, comprising the following steps:

[0041] (1) The natural wood chips are delignified using NaClO2 solution in an acidic buffer solution.

[0042] In the present invention, the acidic buffer solution is a sodium acetate-acetic acid buffer solution, and the pH of the acidic buffer solution is 4.6; the mass fraction of the NaClO2 is 1%; and the delignification treatment is heating in a water bath at 80°C for 6 hours.

[0043] (2) The wood chips from which lignin has been removed are subjected to hemicellulose removal treatment in an alkaline solution, and then placed between a polyethersulfone membrane layer and a filter paper layer. They are compressed under external force for 24 to 48 hours to obtain a transparent wood film. After densification, the thickness of the transparent wood film can be reduced by about 80% to 95%.

[0044] In the present invention, the concentration of the alkaline solution is 4 wt %; the alkaline solution is a NaOH solution; and the hemicellulose removal treatment time is 3-6 h.

[0045] (3) Preparation of CNT / CNFs conductive ink using wood powder and multi-walled carbon nanotubes as raw materials:

[0046] (S1) Using wood powder as a raw material, nanocellulose with a high aspect ratio was prepared by TEMPO oxidation, and dissolved in deionized water. A uniform TOCNFs suspension was obtained by stirring and ultrasonication. The TEMPO oxidant was used in an amount of 8 mmol / g. The TOCNFs had a diameter of 5-15 nm and a length of 0.5-1 μm. The TOCNFs content in the TOCNFs suspension was 0.2-0.8 wt%.

[0047] (S2) adding multi-walled carbon nanotubes to a TOCNFs suspension, stirring, and ultrasonicating the mixed solution to obtain a gel-like CNT / CNFs conductive ink; the multi-walled carbon nanotubes have a diameter of 5-15 nm, a length of 0.5-2 μm, and a carboxyl content of 3-5 wt%; the mass ratio of TOCNFs to multi-walled carbon nanotubes in the mixed solution is (1-2): (1-2); the concentration of the mixed solution after concentration is 4-8 wt%; in the present invention, the concentration also includes removing bubbles in the solution by passing the concentrated solution through a high-speed centrifugal degassing mixer.

[0048] (4) Printing the obtained CNT / CNFs conductive ink on the surface of the transparent wood film obtained in step (2) to form a circuit.

[0049] In the present invention, the printing is performed using a bioprinter equipped with a pneumatic dispenser, specifically, a syringe filled with ink is assembled with a needle (diameter = 1 mm) and connected to an air control dispenser to adjust the printing pressure. The printing speed is controlled using Newcreato software associated with the 3D printer. The printing thickness is 1 mm. The model is designed by 3D MAX 2019 software and then converted into G-code instructions for the printing stage using Newcreator software. By executing the G-code program, the circuit path is printed on the transparent wood film. After printing, the transparent wood film is frozen and freeze-dried at -4°C for 24 hours.

[0050] The present invention also provides a conductive flexible transparent wood film prepared by the preparation method described in the above technical solution.

[0051] The present invention also provides an editable wood flexible electronic device, which uses the conductive flexible transparent wood film described in the above technical solution as a substrate, and adopts a geometric design to fold the editable geometric shape, and the folded shape can form a conductive path; the editable folding or cutting shape design is mainly composed of polygons such as triangles, rectangles, rhombuses or hexagons, obtained according to a specific folding or cutting route, and the middle part is a simplified Kreseling fold structure. This configuration has rotational symmetry / folding / cutting; in the present invention, the size of the transparent wood film used is 50×50mm 2The crease / cutting methods involved have two states, allowing for deformation through folding, stretching, or rotation; the rotation angle range is -90° to 90°. Transparent wood film possesses high mechanical properties, flexibility, and excellent optical strength. Conductive ink deposited on the surface creates a conductive circuit. Through spatial transformations such as folding or cutting, single-pass or multi-pass circuits can be achieved. Transparent wood film flexible electronic devices are capable of rapid deformation.

[0052] In order to better understand the present invention, the content of the present invention is further illustrated below in conjunction with the examples, but the content of the present invention is not limited to the following examples.

[0053] Example 1

[0054] (1) Cut 1mm thick natural balsa wood into 70×70mm pieces 2 Wood chips of different sizes were delignified in an acidic (pH = 4.6) sodium acetate and acetic acid buffer solution with a mass fraction of 1% NaClO2 by heating at 80 ° C in a water bath for 6 h. After delignification, the obtained wood samples were washed three times with deionized water under low vacuum conditions to remove residual chemicals;

[0055] (2) The wood chips after delignining were immersed in NaOH solution at room temperature for 3 h to remove hemicellulose, then washed with deionized water, and then placed between a polyethersulfone membrane layer and a filter paper layer and compressed under external force for 24 h to obtain a transparent wood film;

[0056] SEM images of log, delignified, and alkali-treated wood were obtained. Figures 3a, b, and c show the SEM images of log, delignified, and alkali-treated wood, respectively. Figure 3 shows that the wood cell walls gradually become thinner with the removal of lignin and hemicellulose. Figures d, e, and f show the changes in the intercellular angles of log, delignified, and alkali-treated wood.

[0057] The transparency test of the transparent wood film was conducted. As shown in FIG2 , the prepared transparent wood film is light-transmissive and meets the transparency requirements.

[0058] The mechanical properties of the transparent wood film were tested. As shown in Figure 5, the tensile stress of the transparent wood film (TWF) can reach 393.9 MPa, which is much greater than that of the original wood (OW) and delignified (DW) templates, meeting the mechanical property requirements.

[0059] The component contents of the original wood and the transparent wood film were analyzed, as shown in Table 1. As shown in Table 1, most of the lignin and hemicellulose were removed from the transparent wood film.

[0060] Table 1

[0061] (3) Preparation of CNT / CNFs conductive ink:

[0062] (S1) Using wood powder as a raw material, cellulose nanofibers with a high aspect ratio were prepared by TEMPO oxidation using a TEMPO oxidant dosage of 8 mmol / g. The fibers were dissolved in deionized water, and a uniform TOCNF suspension was obtained by stirring and ultrasonication. The TOCNFs had a diameter of 5-15 nm and a length of 0.5-1 μm. The TOCNF content in the TOCNF suspension was 0.2 wt%.

[0063] (S2) Multi-walled carbon nanotubes were added to a TOCNFs suspension with a solid content mass ratio of 1:1. The mixed solution was stirred for 30 min and ultrasonicated at 300 W for 1 h, and then concentrated to a concentration of 4 wt%. The bubbles in the solution were removed by a high-speed centrifugal degassing mixer to obtain CNT / CNFs conductive ink.

[0064] (4) A Dr. INVIVO 4D bioprinter (ROKIT Healthcare, INC, South Korea) equipped with a pneumatic dispenser was used. The diameter of the syringe needle filled with ink was 1 mm and connected to an air control dispenser to adjust the printing pressure to 30 kPa. The Newcreato software associated with the 3D printer was used to control the printing speed. The printing thickness was 1 mm. The model was designed by 3D MAX 2019 software and then converted into G-code instructions for the printing stage using Newcreator software. By executing the G-code program, the circuit path was printed on the transparent wood film. After printing, the transparent wood film was frozen and freeze-dried at -4°C for 24 hours.

[0065] AFM micromorphology was performed on a transparent wood film printed with ink. Figure 9a shows the surface micromorphology of the transparent wood film, and Figure 9b shows the surface micromorphology of the transparent wood film after 3D printing with conductive ink. Surface roughness is a critical parameter when printing or coating conductive ink on electronic substrates. Figure 9 shows that the surface roughness of the TWF without conductive ink is approximately 150 nm in the Z-axis direction. After printing with conductive ink, the surface roughness reaches 2-3 μm in the Z-axis direction, with significant protrusions along the linear path, demonstrating that the ink is printed along the intended path.

[0066] The transparent wood film printed with CNT / CNFs conductive ink was characterized by SEM. Figure 10a shows the surface bonding between the transparent wood film and the wood film, Figure b shows the surface of the transparent wood film, and Figure c shows the microscopic morphology of the conductive ink surface; d, e, and f are cross-sections of the transparent wood film loaded with conductive ink at different magnifications. In d, the stacked brick-wall-like cell structure of the transparent wood film after load compression can be seen, in e, the bonding between the transparent wood film and the conductive ink can be seen, and in f, the microscopic morphology of the oxidized cellulose nanofibers in the conductive ink can be seen.

[0067] Example 2

[0068] (1) Cut 1mm thick natural balsa wood into 70×70mm pieces 2 Wood chips of different sizes were delignified in an acidic (pH = 4.6) sodium acetate and acetic acid buffer solution with a mass fraction of 1% NaClO2 by heating at 80 ° C in a water bath for 6 h. After delignification, the obtained wood samples were washed three times with deionized water under low vacuum conditions to remove residual chemicals;

[0069] (2) The delignified wood chips were immersed in a NaOH solution at room temperature for 6 h to remove hemicellulose, then washed with deionized water, and then placed between a polyethersulfone membrane layer and a filter paper layer and compressed under external force for 48 h to obtain a transparent wood film;

[0070] (3) Preparation of CNT / CNFs conductive ink:

[0071] (S1) Using wood powder as a raw material, cellulose nanofibers with a high aspect ratio were prepared by TEMPO oxidation using a TEMPO oxidant dosage of 8 mmol / g. The fibers were dissolved in deionized water, and a uniform TOCNF suspension was obtained by stirring and sonication. The TOCNFs had a diameter of 5-15 nm and a length of 0.5-1 μm. The TOCNF content in the TOCNF suspension was 0.4 wt%.

[0072] (S2) Multi-walled carbon nanotubes were added to a TOCNFs suspension at a solid content weight ratio of 1:2. The mixture was stirred for 30 minutes and ultrasonicated at 300W for 1 hour, and then concentrated to a concentration of 4 wt%. The bubbles in the solution were removed by a high-speed centrifugal degassing mixer to obtain a CNT / CNFs conductive ink.

[0073] (4) A Dr. INVIVO 4D bioprinter (ROKIT Healthcare, INC, South Korea) equipped with a pneumatic dispenser was used. The diameter of the syringe needle filled with ink was 1 mm and connected to an air control dispenser to adjust the printing pressure to 30 kPa. The Newcreato software associated with the 3D printer was used to control the printing speed. The printing thickness was 1 mm. The model was designed by 3D MAX 2019 software and then converted into G-code instructions for the printing stage using Newcreator software. By executing the G-code program, the circuit path was printed on the transparent wood film. After printing, the transparent wood film was frozen and freeze-dried at -4°C for 24 hours.

[0074] Example 3

[0075] (1) Cut 1mm thick natural balsa wood into 70×70mm pieces 2Wood chips of different sizes were delignified in an acidic (pH = 4.6) sodium acetate and acetic acid buffer solution with a mass fraction of 1% NaClO2 by heating at 80 ° C in a water bath for 6 h. After delignification, the obtained wood samples were washed three times with deionized water under low vacuum conditions to remove residual chemicals;

[0076] (2) The delignified wood chips were immersed in a NaOH solution at room temperature for 5 h to remove hemicellulose, then washed with deionized water, and then placed between a polyethersulfone membrane layer and a filter paper layer and compressed under external force for 36 h to obtain a transparent wood film;

[0077] (3) Preparation of CNT / CNFs conductive ink:

[0078] (S1) Using wood powder as a raw material, cellulose nanofibers with a high aspect ratio were prepared by TEMPO oxidation using a TEMPO oxidant dosage of 8 mmol / g. The fibers were dissolved in deionized water, and a uniform TOCNF suspension was obtained by stirring and ultrasonication. The TOCNFs had a diameter of 5-15 nm and a length of 0.5-1 μm. The TOCNF content in the TOCNF suspension was 0.6 wt%.

[0079] (S2) Multi-walled carbon nanotubes were added to a TOCNFs suspension with a solid content mass ratio of 2:1. The mixed solution was stirred for 30 min and ultrasonicated at 300 W for 1 h, and then concentrated to a concentration of 4 wt%. The bubbles in the solution were removed by a high-speed centrifugal degassing mixer to obtain CNT / CNFs conductive ink.

[0080] (4) A Dr. INVIVO 4D bioprinter (ROKIT Healthcare, INC, South Korea) equipped with a pneumatic dispenser was used. The diameter of the syringe needle filled with ink was 1 mm and connected to an air control dispenser to adjust the printing pressure to 30 kPa. The printing speed was controlled using Newcreato software associated with the 3D printer. The printing thickness was 1 mm. The model was designed using 3D MAX 2019 software and then converted into G-code instructions for the printing stage using Newcreator software. By executing the G-code program, the circuit path was printed on the transparent wood film. After printing, the transparent wood film was frozen and freeze-dried at -4°C for 24 hours.

[0081] Example 4

[0082] (1) Cut 1mm thick natural balsa wood into 70×70mm pieces 2Wood chips of different sizes were delignified in an acidic (pH = 4.6) sodium acetate and acetic acid buffer solution with a mass fraction of 1% NaClO2 by heating at 80 ° C in a water bath for 6 h. After delignification, the obtained wood samples were washed three times with deionized water under low vacuum conditions to remove residual chemicals;

[0083] (2) The delignified wood chips were immersed in a NaOH solution at room temperature for 5 h to remove hemicellulose, then washed with deionized water, and then placed between a polyethersulfone membrane layer and a filter paper layer and compressed under external force for 36 h to obtain a transparent wood film;

[0084] (3) Preparation of CNT / CNFs conductive ink:

[0085] (S1) Using wood powder as a raw material, cellulose nanofibers with a high aspect ratio were prepared by TEMPO oxidation using a TEMPO oxidant dosage of 8 mmol / g. The fibers were dissolved in deionized water, and a uniform TOCNF suspension was obtained by stirring and sonication. The TOCNFs had a diameter of 5-15 nm and a length of 0.5-1 μm. The TOCNF content in the TOCNF suspension was 0.8 wt%.

[0086] (S2) Multi-walled carbon nanotubes were added to a TOCNFs suspension with a solid content mass ratio of 2:1. The mixed solution was stirred for 30 min and ultrasonicated at 300 W for 1 h, and then concentrated to a concentration of 4 wt%. The bubbles in the solution were removed by a high-speed centrifugal degassing mixer to obtain CNT / CNFs conductive ink.

[0087] For extrusion-based direct 3D printing technology, the printability of the ink (e.g., extrudability, filament formation, shape fidelity, and geometric accuracy) depends largely on its rheological properties. 3D printable inks should have excellent shear thinning ability, and be able to smoothly extrude the ink through the deposition nozzle under shear force and form smooth filaments. The rheological properties of the CNT / CNFs conductive ink were characterized. As shown in Figure 7, in Examples 1-4, the CNT / CNFs suspensions with concentrations of 2%, 4%, 6%, and 8% showed good shear thinning performance at 10 -1 s -1 The steady-state viscosities at shear rates of 13.19 kPa s -1 , 20.13 kPa s -1 、32.87kPa s -1 , 40.43 kPa s -1 , and it can be found that the suspension has significant shear thinning behavior, which can ensure that the ink flows out of the narrow holes evenly under the driving of printing pressure to form a conductive circuit.

[0088] (4) A Dr. INVIVO 4D bioprinter (ROKIT Healthcare, INC, South Korea) equipped with a pneumatic dispenser was used. The diameter of the syringe needle filled with ink was 1 mm and connected to an air control dispenser to adjust the printing pressure to 30 kPa. The Newcreato software associated with the 3D printer was used to control the printing speed. The printing thickness was 1 mm. The model was designed by 3D MAX 2019 software and then converted into G-code instructions for the printing stage using Newcreator software. By executing the G-code program, the circuit path was printed on the transparent wood film. After printing, the transparent wood film was frozen and freeze-dried at -4°C for 24 hours.

[0089] The surface roughness of the transparent wood films obtained in Examples 1 to 4 was tested, and the test results are shown in Table 2:

[0090] Table 2

[0091] As shown in Table 2, the lower roughness of the transparent wood film surface is conducive to the good adhesion of the conductive ink to its surface during printing.

[0092] Example 5

[0093] The transparent wood film obtained in Example 1 was folded to obtain an editable wood flexible electronic device. FIG11 is a diagram showing the folding and application of the transparent wood film flexible electronic device.

[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing a conductive flexible transparent wood film, It is characterized in that The following steps are involved: (1) The natural wood chips are treated with NaClO in an acidic buffer solution. 2 The solution is subjected to delignification treatment; (2) removing hemicellulose from the wood chips after lignin removal in an alkaline solution, and then placing the wood chips between a polyethersulfone membrane layer and a filter paper layer, and compressing the wood chips under external force for 24 to 48 hours to obtain a transparent wood film; (3) Preparation of CNT / CNFs conductive ink using wood powder and multi-walled carbon nanotubes as raw materials; (4) Printing the obtained CNT / CNFs conductive ink on the surface of the transparent wood film obtained in step (2) to form a circuit.

2. The preparation method according to claim 1, It is characterized in that The method for preparing the CNT / CNFs conductive ink in step (3) comprises the following steps: (S1) Using wood powder as raw material, high aspect ratio nanocellulose was prepared by TEMPO oxidation method and dissolved in deionized water. A uniform TOCNFs suspension was obtained by stirring and ultrasound. (S2) Multi-walled carbon nanotubes are added to the TOCNFs suspension, stirred, and ultrasonicated, and then the mixed solution is concentrated to obtain a gel-like CNT / CNFs conductive ink.

3. The preparation method according to claim 2, It is characterized in that In step (S1), the dosage of the TEMPO oxidant is 8 mmol / g; the diameter of the TOCNFs is 5-15 nm and the length is 0.5-1 μm.

4. The preparation method according to claim 2, It is characterized in that The TOCNFs content in the TOCNFs suspension in step (S1) is 0.2-0.8wt%.

5. The preparation method according to claim 2, It is characterized in that The multi-walled carbon nanotubes in step (S2) have a diameter of 5-15 nm, a length of 0.5-2 μm, and a carboxyl content of 3-5 wt%.

6. The preparation method according to claim 2, It is characterized in that The mass ratio of TOCNFs to multi-walled carbon nanotubes in the mixed solution of step (S2) is (1-2):(1-2).

7. The preparation method according to claim 2, It is characterized in that The concentration of the mixed solution after concentration in step (S2) is 4-8wt%.

8. A conductive flexible transparent wood film prepared by the preparation method according to any one of claims 1 to 7.

9. An editable wood flexible electronic device, It is characterized in that It is obtained by editing the conductive flexible transparent wood film as described in claim 8.

Citation Information

Patent Citations

  • Preparation method of transparent and conductive flexible wood composite material

    CN109049215A

  • Flexible transparent conductive wood-based thin film and preparation method thereof

    CN115020033A

  • Cotton fiber dissolution and regeneration and 3D printing of cellulose based conductive composites

    US20170140848A1

  • Compositions comprising modified lignin useful for additive manufacturing

    WO2023062239A1