Photocurable composition and use thereof
By using an improved photocuring composition in optical fiber coated resin, photoinitiator containing specific alkyl and alkoxy structures, the volatile problem under high-speed wire drawing conditions is solved, the curing speed and efficiency are improved, and the fiber performance is ensured stability.
Patent Information
- Application Number
- PCT/CN2024/091360
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-21
AI Technical Summary
Under high-speed wire drawing conditions, the volatile amount increases during the curing process of the fiber-coated resin, resulting in the surface of the photocuring equipment being covered with volatiles, affecting the curing effect. The thermal stability of the existing photoinitiator TPO during the high-speed curing process is also the same. Inadequate, it is difficult to meet the needs of efficient solidification.
Using a new photocuring composition, including photocuring oligomers, photocuring active monomers and improved photoinitiators, the thermal stability of the initiator is enhanced by introducing photoinitiators of specific alkyl and alkoxy structures. , reduce volatility, improve curing efficiency, and appropriately add additives to the composition to optimize curing effect.
It effectively improves the curing speed of fiber coating, reduces the loss of volatiles during curing, improves the curing density and efficiency, and ensures the stability of fiber performance and production capacity.
Smart Images

Figure CN2024091360_21112024_PF_FP_ABST
Abstract
Description
Photocurable composition and its application Technical Field
[0001] The present invention relates to the technical field of photocuring, and in particular to a photocuring composition and application thereof. Background Art
[0002] Optical fiber is a key material for the construction of information industry infrastructure, especially the key transmission carrier and core component of optical fiber communication, and plays an important supporting role in the national economy.
[0003] Optical fiber is a dielectric cylindrical optical waveguide that can confine and guide light waves to propagate forward along its axis within or near its surface. Generally, an optical fiber is composed of a glass core layer, a glass cladding layer, and an organic coating layer. The glass portion of a single-mode or multimode communication optical fiber is generally composed of high-purity silica and germanium dioxide doped therein. Quartz glass fiber has high longitudinal tensile strength, but it is also very brittle and easily breaks when bent. Quartz glass itself is also not resistant to moisture and acidic and alkaline corrosive gases or liquids in the environment. To make quartz glass fiber practical, the outer surface of the glass fiber is generally coated with one or more layers of organic polymer materials (generally referred to as optical fiber coating materials) to effectively protect the quartz glass fiber. This not only improves the environmental reliability of the quartz glass fiber, but also improves its optical performance.
[0004] With the development of the optical fiber industry, light-curing coatings have found more and more applications in optical fibers. Currently, optical fiber inner and outer coatings, optical fiber coloring layers, optical fiber ribbon layers, and optical fiber tight jacket layers are all formed by light-curing coating resins that are cured by ultraviolet light under specific process conditions.
[0005] In the prior art, in the photocurable compositions used in the field of optical fiber materials, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (also known as photoinitiator TPO) is used as a photoinitiator. It has excellent properties such as a wide absorption band in the ultraviolet band of 200nm-400nm, high initiation efficiency, and low yellowing after curing. It is particularly suitable for optical fiber coating production that requires rapid curing. Due to the current development of LED curing, the wavelength of LED ultraviolet light sources is generally relatively single. The three most commonly used bands in optical fibers are 365nm, 385nm, and 395nm, and the photoinitiator TPO is mainly used.
[0006] At the same time, with the advancement of fiber optic technology, fiber and cable manufacturers are demanding increasingly higher fiber drawing speeds to increase production capacity. High-speed drawing places higher demands on fiber cooling, coating, and curing, and also on the fiber coating resin. As fiber speeds increase, the time the curing composition is exposed to light during the curing process decreases. During the resin curing process, the amount of volatiles released increases. As these volatiles accumulate, the surface of the light-curing equipment becomes easily coated with them. In particular, coating the surface of the light-curing lampshade with volatiles can affect the curing effect of the light-curing composition, compromising the performance of the optical fiber.
[0007] Chinese invention patent application publication CN101549962A discloses a method and apparatus for removing volatiles from coating curing during optical fiber drawing, and Chinese utility model patent CN214654487U discloses an apparatus for removing volatiles from coating curing during optical fiber drawing. Both publications indicate that optical fiber manufacturers hope to reduce volatiles by adjusting equipment.
[0008] Based on the problems existing in the prior art, the present invention provides a photocurable composition, in which a more environmentally friendly and efficient photoinitiator is used to replace the photoinitiator TPO. Combined with other substances in the formula, it also effectively improves the volatilization problem of the coating under high-speed drawing conditions.
[0009] Summary of the Invention
[0010] Purpose of the invention: The purpose of the present invention is to provide a photocurable composition which, when applied to optical fiber coating, can effectively increase the curing speed and effectively improve the volatilization problem occurring during the drawing process.
[0011] Furthermore, the present invention aims to provide applications of the photocurable composition.
[0012] Technical solution: A photocurable composition comprising: a photocurable oligomer, a photocurable reactive monomer, and a photoinitiator, wherein the photoinitiator comprises at least one compound represented by general formula I:
[0013] wherein R1, R2, and R3 are the same or different and are each independently selected from a substituted or unsubstituted alkyl or alkoxy group of 1 to 5 carbon atoms, wherein the substituent is selected from an alkyl or alkoxy group of 1 to 3 carbon atoms;
[0014] n=1, 2 or 3.
[0015] Alkyl groups of 1 to 5 carbon atoms are selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, -CH(CH3)CH2CH2CH3, -CH2CH(CH3)CH2CH3, -CH2CH2CH(CH3)2, -CH(C2H5)CH2CH3, -C(CH3)2CH2CH3, -CH(CH3)CH(CH3)2 and -CH2C(CH3)3;
[0016] The alkoxy group having 1 to 5 carbon atoms is selected from methoxy, ethoxy, propoxy, butoxy and pentoxy.
[0017] In some embodiments of the present invention, R1, R2 and R3 are each independently selected from methyl, ethyl, propyl or isopropyl; in some embodiments of the present invention, R3 is preferably methyl.
[0018] After the above-mentioned alkyl group is introduced into the structure, the thermal stability of the initiator is further improved, which can reduce the volatilization of the initiator during the photocuring process.
[0019] In some embodiments of the present invention, the R3 substitution position can be ortho, meta or para; in some embodiments of the present invention, the R3 substitution position is preferably ortho and para.
[0020] In some embodiments of the present invention, n is preferably 3.
[0021] In some embodiments of the present invention, the photoinitiator preferably comprises at least one compound represented by formula II:
[0022] The definition of R1 and R2 is the same as that of the compound represented by general formula I.
[0023] In some embodiments of the present invention, R1 and R2 are each independently selected from methyl, ethyl, propyl or isopropyl; in some embodiments of the present invention, R1 and R2 are each independently preferably methyl.
[0024] In some embodiments of the present invention, the substitution positions of R1 and R2 may be ortho, meta or para; in some embodiments of the present invention, the substitution positions of R1 and R2 are preferably para.
[0025] In some embodiments of the present invention, R1 and R2 are each a para-substituted methyl group.
[0026] There are two more methyl groups at the para position of the two benzene rings connected to the phosphorus oxygen group. The methyl groups and the structure of the benzene ring form a σ-π hyperconjugated structure. Compared with the conjugated structure of the benzene ring, the σ-π hyperconjugated structure has lower conjugation energy and higher activity. Under the condition of free radical formation under light, it is easier to initiate polymerization, thereby increasing the cross-linking density of the system, thereby improving the curing efficiency and reducing the volatilization of small molecular monomers in the system.
[0027] In some embodiments of the present invention, the photocurable composition comprises: 35-95 wt % of a photocurable oligomer, 1-50 wt % of a photocurable reactive monomer, and 1-15 wt % of a photoinitiator, based on the weight of the photocurable composition.
[0028] In some embodiments of the present invention, the weight percentage of the photocurable oligomer in the photocurable composition is 35-95%, for example, 35%-90%, 40%-90%, 45%-90%, 50%-90%, 55%-90%, 60%-90%, 65%-90%, 70%-90%, 75%-90%, 80%-90%, 85%-90%, 35%-85%, 40%-90%, 45%-90%, 50%-90%, 55%-90%, 60%-90%, 65%-90%, 70%-90%, 75%-90%, 80%-90%, 85 ... 0%-85%, 45%-85%, 50%-85%, 55%-85%, 60%-85%, 65%-85%, 70%-85%, 75%-85%, 80%-85%, 35%-80%, 40%-80%, 45%-80%, 50%-80%, 55%-80%, 60%-80%, 65%-80%, 70%-80%, 75%-80 %, 35%-75%, 40%-75%, 45%-75%, 50%-75%, 55%-75%, 60%-75%, 65%-75%, 70%-75%, 35%-70%, 40%-70%, 45%-70%, 50%-70%, 55%-70%, 60%-70%, 65%-70%, 35%-65%, 40%-65%, 45% -65%, 50%-65%, 55%-65%, 60%-65%, 35%-60%, 40%-60%, 45%-60%, 50%-60%, 55%-60%, 35%-55%, 40%-55%, 45%-55%, 50%-55%, 35%-50%, 40%-50%, 45%-50%, 35%-45% or 40%-45%.
[0029] In some embodiments of the present invention, the photocurable oligomer is selected from at least one of a polyurethane acrylate oligomer and an epoxy acrylate oligomer.
[0030] In some embodiments of the present invention, the polyurethane acrylate oligomer is one or more of a monofunctional polyurethane acrylate oligomer, a difunctional polyurethane acrylate oligomer, or a trifunctional polyurethane acrylate oligomer, preferably a difunctional polyurethane acrylate oligomer or a trifunctional polyurethane acrylate oligomer.
[0031] In some embodiments of the present invention, the epoxy acrylate oligomer is one or more of a monofunctional epoxy acrylate oligomer, a difunctional epoxy acrylate oligomer, or a trifunctional epoxy acrylate oligomer, preferably a difunctional epoxy acrylate oligomer.
[0032] The polyurethane acrylate oligomer of the present invention is prepared from diisocyanate and acrylate containing hydroxyl groups. During the preparation process, a chain extender is added to the reactants to increase the molecular chain length of the polyurethane acrylate oligomer.
[0033] In some embodiments of the present invention, the chain extender is selected from at least one of polyester diols, alkyl diols, and polyether diols, preferably polyether diols.
[0034] In some embodiments of the present invention, the polyurethane acrylate oligomer may be a single oligomer or a combination of multiple oligomers.
[0035] In some embodiments of the present invention, the diisocyanate is selected from toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), diphenylmethane diisocyanate (MDI), and hexamethylene diisocyanate (HDI) trimer.
[0036] In some embodiments of the present invention, the acrylate containing a hydroxyl group is selected from at least one of hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).
[0037] In some embodiments of the present invention, the epoxy acrylate oligomer is selected from the group consisting of bisphenol A epoxy resin and a photopolymerizable compound containing a carboxyl group.
[0038] The photopolymerizable compound containing a carboxyl group is a compound containing a carboxyl group at one end and a photoinitiable double bond at the other end.
[0039] In some embodiments of the present invention, the compound containing a carboxyl group at one end and a photoinitiable double bond at the other end is acrylic acid, methacrylic acid, or a compound obtained by the reaction of an acid anhydride and a hydroxy acrylate.
[0040] The acid anhydride is selected from at least one of succinic anhydride, maleic anhydride, phthalic anhydride and tetrahydrophthalic anhydride.
[0041] The hydroxy acrylate compound is selected from hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).
[0042] The photocurable reactive monomer includes at least one of a monofunctional photocurable reactive monomer and a multifunctional photocurable reactive monomer. In some embodiments of the present invention, the multifunctional photocurable reactive monomer is a difunctional photocurable reactive monomer and a trifunctional photocurable reactive monomer.
[0043] Monofunctional photocurable reactive monomers include 2-phenoxyethyl acrylate (PHEA), isobornyl acrylate (IBOA), isodecyl acrylate, isooctyl acrylate, polyethylene glycol o-phenylphenyl ether acrylate (OPPEA), nonylphenol polyoxyethylene ether acrylate, and N-vinyl caprolactam.
[0044] If a monofunctional photocurable monomer is added, the upper limit of the amount added is 36% (based on the weight of the photocurable composition). A further preferred upper limit is 20% (based on the weight of the photocurable composition). Excessive addition of monofunctional monomers will affect the curing speed and increase volatility.
[0045] Bifunctional photocurable monomers include 1,6-hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA), and dipropylene glycol diacrylate (DPGDA).
[0046] The trifunctional photocurable reactive monomer includes trimethylolpropane triacrylate (TMPTA).
[0047] The photoinitiator of the present invention comprises one or more compounds of the general formula I.
[0048] In some embodiments of the present invention, the photoinitiator preferably comprises at least one compound of Formula II.
[0049] In some embodiments of the present invention, the addition ratio of general formula I therein is 0.3-10% (for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%) based on the weight of the photocurable composition.
[0050] In some embodiments of the present invention, when no colorant is added, the addition ratio of general formula I therein is preferably 0.3-6% (for example, 0.5%, 1%, 2%, 3%, 4% or 5%) by weight of the photocurable composition. Excessive addition will cause a more obvious yellowing problem.
[0051] In some embodiments of the present invention, the photoinitiator further comprises one or more of the following substances: phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2-isopropylthioxanthone, 2,4-diethylthiazolone to increase the curing speed.
[0052] The auxiliary agent may be one or more of a silane coupling agent, a defoaming agent, a dispersant, a leveling agent, and an active amine co-initiator. The auxiliary agent does not include a colorant.
[0053] The silane coupling agent may include mercaptopropyltrimethoxysilane and 3-chloropropyltrimethoxysilane.
[0054] The defoaming agent may include a polyether-modified silicone defoaming agent and a non-silicone polymer defoaming agent.
[0055] The dispersant may include a copolymer solution having acidic groups, such as BYK110; an acrylic front-stage copolymer, such as EFKA4310.
[0056] The leveling agent may include a silicone leveling agent or an acrylate leveling agent.
[0057] Active amine co-initiators may include ethylenediamine and amine-modified acrylates, which can further optimize the surface curing effect.
[0058] In some embodiments of the present invention, the photocurable composition includes 0.01-10% (e.g., 0.01% to 5%, 0.05% to 10%, 0.1% to 10%, 0.1% to 5%, 0.5% to 10%, 0.5% to 5%, 1% to 5%, or a value within one of these ranges) of an adjuvant based on the weight of the photocurable composition. Specific examples may include 0.01%, 0.05%, 0.1%, 0.25%, 0.5%, 0.75%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range between any two of these values.
[0059] A colorant may be further added to the photocurable composition. The amount of the colorant added may be 0.1-8% based on the weight of the photocurable composition.
[0060] The colorant can be an organic or inorganic toner. Preferably, the toner color can include white, red, yellow, blue, green, purple, and black.
[0061] The type and amount of colorant added can be adjusted as appropriate according to coloring requirements.
[0062] The colorant is selected from at least one of titanium dioxide, permanent red, ruby 4B, benzidine yellow, phthalocyanine blue, phthalocyanine green, permanent violet and carbon black.
[0063] In some embodiments of the present invention, the colorant is selected from titanium dioxide and phthalocyanine blue.
[0064] After adding the colorant, since the absorption of radiation by the toner will affect the curing effect of the composition, the addition amount of the compound of formula I is further increased to 1-8 weight % (e.g., 2 weight %, 3 weight %, 4 weight %, 5 weight %, 6 weight % or 7 weight %) to ensure that a suitable degree of curing is achieved, and the volatility of such compositions can also be improved.
[0065] In some embodiments of the present invention, the light source wavelength range applicable to the photocurable composition is 200-450 nm.
[0066] The present invention also provides application of the photocurable composition as optical fiber coating or optical fiber coloring coating.
[0067] The application of optical fiber coating is selected from at least one of optical fiber inner coating, optical fiber outer coating, optical fiber ribbon coating, and optical fiber tight sleeve coating. DETAILED DESCRIPTION
[0068] The present invention will be described below with reference to specific embodiments. It should be noted that the following examples are illustrative of the present invention and are intended only to illustrate the present invention and are not intended to limit the present invention. Other combinations and various modifications within the scope of the present invention may be made without departing from the spirit or scope of the present invention.
[0069] In the present invention, unless otherwise specified, all ratios are by weight and all temperatures are in degrees Celsius.
[0070] Test method:
[0071] Volatile matter test method: Place a glass slide in an oven and dry it for 30 minutes. Then take it out of the oven and place it in a desiccator to cool to room temperature. The weight is recorded as M1. Apply the coating sample on the glass slide to form a coating film of appropriate thickness, and weigh the total weight of the glass slide + coating, recorded as M2. Place the glass slide in a container box with a high-purity quartz glass upper layer, pass nitrogen for 1 minute, exhaust the air in the container, and then place it under a UV light source for curing. The light source energy is set to 1500mJ / cm 2 The conveyor belt speed is set to 17m / min. After the curing is completed, nitrogen is passed for 1 minute to remove the volatile gas. The total weight of the glass slide + the cured coating is weighed and recorded as M3. At this time, the volatile matter of the sample = (M2-M3) / (M2-M1)*100%.
[0072] Curing degree test method: The surface of the sample after the volatile matter test can be scanned by infrared spectrometer, and the 1410cm -1 Integrate the absorption peak of the standard absorption peak (such as 1730cm -1 The AU sample is determined by the integrated ratio of the two absorption peaks (S1410 / S1730). Uncured coating samples are tested in the same manner, and the integrated ratio of the two absorption peaks (L1410 / L1730) is determined as the AU liquid. The degree of cure of the coating film can be calculated using the formula: ((AU liquid - AU sample) / AU liquid) * 100%. The degree of cure is used to indicate the cure speed; a higher degree of cure indicates a faster cure speed.
[0073] The specific selection of compounds in the embodiments of the present invention is as follows:
[0074] Photocurable oligomers
[0075] Oligomer 1: polyurethane acrylate oligomer, obtained by the direct end-capping reaction of hydroxypropyl methacrylate (HPMA) and toluene diisocyanate (TDI).
[0076] Oligomer 2: a polyether polyurethane acrylate oligomer obtained by reacting a 1000 molecular weight polyether diol with diphenylmethane diisocyanate (MDI) and then capping with hydroxyethyl methacrylate (HEMA).
[0077] Oligomer 3: Epoxy acrylate oligomer, selected from Sanmu SM6104 epoxy acrylate.
[0078] Oligomer 4: modified epoxy acrylate, obtained by reacting maleic anhydride with hydroxyethyl methacrylate (HEMA) and then reacting with bisphenol A epoxy resin.
[0079] Photoinitiator:
[0080] Photoinitiator 1: a compound of formula II, wherein R1 and R2 are each a para-substituted methyl group.
[0081] Photoinitiator 2: 1-Hydroxycyclohexylphenyl ketone
[0082] Photoinitiator 3: 2,4,6-trimethylbenzoyldiphenoxyphosphine (TPO)
[0083] Additives:
[0084] Active amine co-initiator: amine-modified acrylate, selected from Sartomer CN550
[0085] Table 1
[0086] Table 2
[0087] From Examples 1-12 and Comparative Examples 1-3 in Tables 1 and 2 above, it can be seen that the photocurable composition comprising the compound of Formula I provided by the present invention has a higher degree of curing and a smaller amount of volatilization during the curing process, and has good application prospects in the optical fiber manufacturing industry.
[0088] The above embodiments are only for illustrating the technical concept and features of the present invention. Its purpose is to enable people familiar with this technology to understand the content of the present invention and implement it. It cannot be used to limit the scope of protection of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A photocurable composition, comprising: A photocurable oligomer, a photocurable active monomer and a photoinitiator, wherein the photoinitiator comprises at least one compound as shown in the general formula I: wherein R1, R2, and R3 are the same or different and are independently selected from substituted or unsubstituted alkyl or alkoxy groups of 1 to 5 carbon atoms, wherein the substituents are selected from alkyl or alkoxy groups of 1 to 3 carbon atoms; n=1, 2 or 3.
2. The photocurable composition according to claim 1, characterized in that The photocurable composition comprises: based on the weight of the photocurable composition, 35-95 wt % of a photocurable oligomer, 1-50 wt % of a photocurable active monomer, and 1-15 wt % of a photoinitiator.
3. The photocurable composition according to claim 1, characterized in that: R1, R2 and R3 are each independently selected from methyl, ethyl, propyl or isopropyl.
4. The photocurable composition according to claim 1, characterized in that: The photocurable oligomer is selected from at least one of a polyurethane acrylate oligomer and an epoxy acrylate oligomer.
5. The photocurable composition according to claim 4, characterized in that: The polyurethane acrylate oligomer is one or more of a monofunctional polyurethane acrylate oligomer, a difunctional polyurethane acrylate oligomer or a trifunctional polyurethane acrylate oligomer.
6. The photocurable composition according to claim 4, characterized in that: The epoxy acrylate oligomer is one or more of a monofunctional epoxy acrylate oligomer, a difunctional epoxy acrylate oligomer or a trifunctional epoxy acrylate oligomer.
7. The photocurable composition according to claim 4, characterized in that: The polyurethane acrylate oligomer is obtained by reacting diisocyanate with acrylate containing hydroxyl group.
8. The photocurable composition according to claim 4, characterized in that: The epoxy acrylate oligomer is obtained by reacting bisphenol A epoxy resin with a photopolymerizable compound containing a carboxyl group.
9. The photocurable composition according to claim 1, characterized in that: The photoinitiator comprises one or more compounds of Formula I.
10. The photocurable composition according to claim 1, characterized in that: The photoinitiator also includes one or more of the following substances: phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2-isopropylthioxanthone, 2,4-diethylthiazolone.
11. The photocurable composition according to claim 1, characterized in that: The photocurable composition further includes an auxiliary agent.
12. The photocurable composition according to claim 1, characterized in that: The photocurable composition further includes a colorant.
13. Use of the photocurable composition according to any one of claims 1 to 11 as optical fiber coating or optical fiber coloring coating.
14. The use according to claim 13, wherein the optical fiber coating is selected from at least one of an optical fiber inner coating, an optical fiber outer coating, an optical fiber ribbon coating or an optical fiber tight sleeve coating.
Citation Information
Patent Citations
Method and device for removing coating solidifying volatile material in optical fibre drawing process
CN101549962A
Device for removing coating curing volatile matter in optical fiber drawing process
CN214654487U
UV-LED-curing optical fiber coating resin and preparing method and application thereof
CN106010144A
Synthesis method of epoxy modified high-functionality polyurethane acrylic resin, ultraviolet curing coating and preparation method
CN116813864A
Optical fiber coating composition, optical fiber and preparation method of optical fiber
CN117209168A