Method of producing article, adhesive composition, and foamable adhesive sheet
By using differential scanning calorimetry to control the expansion of thermally expandable microcapsules within adhesive compositions, the method ensures that the foaming agent expands before the curing reaction, addressing the issue of decreased adhesive strength and enhancing the reliability of bonded members.
Patent Information
- Application Number
- PCT/JP2023/017855
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-21
AI Technical Summary
Adhesive compositions containing foaming agents often result in decreased adhesive strength, leading to inferior reliability and durability of bonded members due to improper heating conditions that do not align the foaming start temperature of the foaming agent with the curing start temperature of the adhesive layer.
A method involving a thermosetting resin and a thermally expandable microcapsule foaming agent, where differential scanning calorimetry is used to ensure the foaming agent expands before the curing reaction of the resin, maintaining adhesive layer thickness and enhancing strength by controlling the slopes in foaming rate-time and heat flow curves.
This approach improves adhesive strength and reliability by ensuring the foaming agent expands before the curing reaction, maintaining adhesive layer thickness and enhancing the bonding process.
Smart Images

Figure JP2023017855_21112024_PF_FP_ABST
Abstract
Description
Article manufacturing method, adhesive composition, and foamable adhesive sheet
[0001] The present disclosure relates to a method for producing an article, and an adhesive composition and a foamable adhesive sheet used therein.
[0002] Adhesives for bonding members together are used in a variety of fields, and many bonding methods are known.
[0003] In recent years, it has been proposed to use adhesive compositions containing a foaming agent (for example, Patent Documents 1 and 2).
[0004] Japanese Patent No. 6223477 Japanese Patent Application Laid-Open No. 2019-203062
[0005] Regarding the heating conditions for an adhesive composition containing a foaming agent, for example, Patent Document 1 discloses that when the thermal foaming temperature (foaming initiation temperature) of the foaming agent is T1 and the curing initiation temperature of the adhesive layer is T2, the relationship T1≦T2 is satisfied.
[0006] However, the inventors of the present disclosure have investigated heating conditions for adhesive compositions containing a foaming agent and found that even when the foaming initiation temperature of the foaming agent and the curing initiation temperature of the adhesive layer are in a predetermined relationship, the adhesive strength may decrease. When the adhesive strength decreases, there is a problem in that the reliability, durability, etc. of the members bonded with the adhesive composition containing a foaming agent are deteriorated.
[0007] The present disclosure has been made in view of the above-described circumstances, and a primary object of the present disclosure is to provide a method for producing an article that can improve adhesive strength, as well as an adhesive composition and a foamable adhesive sheet to be used therein.
[0008] One embodiment of the present disclosure is a method for manufacturing an article, the method including: a disposing step of disposing an adhesive composition containing a thermosetting resin and a foaming agent between a first member and a second member; and a bonding step of heating the adhesive composition to foam and cure it, thereby bonding the first member and the second member, wherein the foaming agent is a thermally expandable microcapsule, and when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera under the heating conditions in the bonding step, an expansion rate-time curve is obtained with time on the horizontal axis and the expansion rate of the foaming agent on the vertical axis, and the slope of a tangent line drawn at the apex of the peak on the long-term side of the curve is defined as A, and when differential scanning calorimetry is performed on the adhesive composition under the heating conditions in the bonding step, In a DSC curve, the horizontal axis represents time and the vertical axis represents heat flow, and the slope of the tangent drawn at the peak of the exothermic peak to the curve on the long-term side of the exothermic peak is B, where A<B; when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera, the time at the peak of the exothermic peak is T1 in an expansion rate-time curve, the horizontal axis represents time and the vertical axis represents the expansion rate of the foaming agent; and when differential scanning calorimetry is performed on a composition obtained by removing the foaming agent from the adhesive composition, the DSC curve, the horizontal axis represents time and the vertical axis represents heat flow, and the time at the peak of the exothermic peak is T2, the adhesive composition is heated in the bonding step so that T1<T2.
[0009] Another embodiment of the present disclosure provides an adhesive composition comprising a thermosetting resin and a foaming agent, wherein the foaming agent is a thermally expandable microcapsule; when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera under heating conditions of heating from room temperature to the maximum foaming temperature of the foaming agent over a period of 5 minutes and then maintaining the temperature at the maximum foaming temperature of the foaming agent, the resulting expansion rate-time curve has time on the horizontal axis and the expansion rate of the foaming agent on the vertical axis. The slope of the tangent line drawn at the apex of the peak to the curve on the long-term side of the peak is defined as C; and when differential scanning calorimetry is performed on the adhesive composition under the heating conditions, the resulting DSC curve has time on the horizontal axis and heat flow on the vertical axis. The slope of the tangent line drawn at the apex of the exothermic peak to the curve on the long-term side of the exothermic peak is defined as D, where C is less than D.
[0010] Another embodiment of the present disclosure provides a foamable adhesive sheet having an adhesive layer, wherein the adhesive layer contains the adhesive composition described above.
[0011] The method for manufacturing an article according to the present disclosure has the effect of being able to improve adhesive strength.
[0012] 1 is a process diagram illustrating a method for manufacturing an article according to the present disclosure. FIG. 1 is a schematic cross-sectional view illustrating a foamable adhesive sheet according to the present disclosure. FIG. 2 is a graph illustrating an expansion rate-time curve for a foaming agent. FIG. 3 is a graph illustrating a DSC curve for an adhesive composition. FIG. 4 is a graph illustrating an expansion rate-time curve for a foaming agent and a DSC curve for an adhesive composition. FIG. 5 is a graph illustrating an expansion rate-time curve for a foaming agent and a DSC curve for a composition obtained by omitting the foaming agent from the adhesive composition. FIG. 6 is a schematic cross-sectional view illustrating a foamable adhesive sheet according to the present disclosure. FIG. 7 is a schematic cross-sectional view illustrating a foamable adhesive sheet according to the present disclosure. FIG. 8 is a graph illustrating an expansion rate-time curve for a foaming agent and a DSC curve for the adhesive composition for the adhesive compositions of Production Examples 1 to 3. FIG. 9 is a graph illustrating an expansion rate-time curve for a foaming agent and a DSC curve for the adhesive composition for Adhesive Composition 1. FIG. 10 is a graph illustrating an expansion rate-time curve for a foaming agent and a DSC curve for the adhesive composition for Adhesive Composition 4. 1 is a graph showing the relationship between the heating temperature and the holding time at the heating temperature, and adhesive strength. 2 is a graph showing the relationship between the heating temperature and the holding time at the heating temperature, and cohesive failure rate.
[0013] Embodiments of the present disclosure will be described below with reference to the drawings and the like. However, the present disclosure can be implemented in many different forms, and should not be construed as being limited to the description of the embodiments exemplified below. Furthermore, to clarify the explanation, the drawings may schematically depict the width, thickness, shape, etc. of each part compared to the actual form, but these are merely examples and are not intended to limit the interpretation of the present disclosure. Furthermore, in this specification and each drawing, elements similar to those previously described with reference to the preceding drawings will be designated by the same reference numerals, and detailed descriptions may be omitted as appropriate.
[0014] In this specification, when describing a mode in which another component is placed on a certain component, the term "above" or "below" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween. Also, in this specification, when describing a mode in which another component is placed on the surface of a certain component, the term "on the surface side" or "on the surface" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween.
[0015] In this specification, the term "sheet" also includes a member called a "film." In addition, the term "film" also includes a member called a "sheet." In addition, the numerical ranges in this specification are ranges of average values.
[0016] The method for producing an article according to the present disclosure, as well as the adhesive composition and foamable adhesive sheet used therein, will be described in detail below.
[0017] A. Method for Manufacturing an Article The method for manufacturing an article according to the present disclosure is a method for manufacturing an article, comprising: a disposing step of disposing an adhesive composition containing a thermosetting resin and a foaming agent between a first member and a second member; and a bonding step of heating the adhesive composition to foam and cure it, thereby bonding the first member and the second member, wherein the foaming agent is a thermally expandable microcapsule, and when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera under the heating conditions in the bonding step, the horizontal axis represents time and the vertical axis represents the foaming rate of the foaming agent. In the expansion rate-time curve, the slope of the tangent drawn at the apex of the peak on the long-term side of the peak is defined as A, and the differential scanning calorimetry is performed on the adhesive composition under the heating conditions in the bonding step. In a DSC curve obtained by performing calorimetry, the horizontal axis represents time and the vertical axis represents heat flow, and the slope of the tangent drawn at the peak of the exothermic peak to the curve on the long-term side of the exothermic peak is B, where A<B; when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera, the horizontal axis represents time and the vertical axis represents the expansion ratio of the foaming agent, and the time at the peak of the peak is T1; and when differential scanning calorimetry is performed on a composition obtained by removing the foaming agent from the adhesive composition, the horizontal axis represents time and the vertical axis represents heat flow, and the time at the peak of the exothermic peak is T2, the adhesive composition is heated in the bonding step so that T1<T2.
[0018] A method for manufacturing an article according to the present disclosure will be described with reference to the drawings. FIGS. 1( a) and 1(b) are process diagrams illustrating an example of a method for manufacturing an article according to the present disclosure. FIGS. 1( a) and 1(b) also illustrate an example of a method for manufacturing an article using a foamable adhesive sheet as illustrated in FIG. 2. As shown in FIG. 2, a foamable adhesive sheet 10 has an adhesive layer 1 containing an adhesive composition that includes a thermosetting resin and a foaming agent. In this method for manufacturing an article, first, as shown in FIG. 1(a), the foamable adhesive sheet 10 is placed between a first member 20a and a second member 20b. Next, as shown in FIG. 1(b), the adhesive composition contained in the adhesive layer of the foamable adhesive sheet 10 is heated to foam and harden. After foaming and hardening, the first member 20a and the second member 20b are bonded (joined) by the adhesive sheet 11. This results in an article 100 in which the adhesive sheet 11 is placed between the first member 20a and the second member 20b.
[0019] In the present disclosure, the blowing agent is a thermally expandable microcapsule, which contains a thermally expandable agent such as hydrocarbon encapsulated within a resin shell. When the thermally expandable microcapsule is heated, the resin constituting the shell softens, and the pressure of the thermally expandable agent, such as hydrocarbon, increases, causing the microcapsule to expand. Because the shell thins as a result of the expansion, further heating causes the thermally expandable microcapsule to lose its thermally expandable agent, causing the microcapsule to shrink. Therefore, when differential scanning calorimetry is performed on the blowing agent using a differential scanning calorimeter equipped with a camera under the heating conditions of the bonding process, an expansion rate-time curve, such as that shown in FIG. 3, is obtained, with time on the horizontal axis and the expansion rate of the blowing agent on the vertical axis.
[0020] In the present disclosure, the adhesive composition contains a thermosetting resin. Therefore, when differential scanning calorimetry is performed on the adhesive composition under the heating conditions in the bonding step, an exothermic peak due to the curing reaction of the thermosetting resin is observed in the DSC curve, where the horizontal axis represents time and the vertical axis represents heat flow, as shown in Fig. 4, for example.
[0021] 5 is a graph superimposing an expansion rate-time curve, where the horizontal axis represents time and the vertical axis represents the expansion rate of the foaming agent, obtained by differential scanning calorimetry of a foaming agent using a differential scanning calorimeter equipped with a camera under the heating conditions of the bonding process, and a DSC curve, where the horizontal axis represents time and the vertical axis represents heat flow, obtained by differential scanning calorimetry of an adhesive composition under the heating conditions of the bonding process. As shown in FIG. 5, in the expansion rate-time curve 31 for the foaming agent, the slope of a tangent line L1 drawn at the apex of the peak to the curve on the long-time side of the peak is designated A. Furthermore, in the DSC curve 32 for the adhesive composition, the slope of a tangent line L2 drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak is designated B. In this case, A<B.
[0022] In the present disclosure, since A<B, the curing reaction of the thermosetting resin can proceed before the contraction of the foaming agent progresses, and the thermosetting resin can be sufficiently cured. Therefore, the thickness of the adhesive layer during foaming can be maintained, and the adhesive strength can be improved.
[0023] On the other hand, if A≧B, the foaming agent shrinks before the curing reaction of the thermosetting resin progresses, and as a result, the thickness of the adhesive layer cannot be maintained during foaming, which may result in a decrease in adhesive strength.
[0024] 6 is a graph superimposing an expansion rate-time curve, where the horizontal axis represents time and the vertical axis represents the expansion rate of the blowing agent, obtained by differential scanning calorimetry using a differential scanning calorimeter equipped with a camera, and a DSC curve, where the horizontal axis represents time and the vertical axis represents heat flow, obtained by differential scanning calorimetry of a composition obtained by removing the blowing agent from the adhesive composition. As shown in FIG. 6 , the time at the apex of the peak in the expansion rate-time curve 33 for the blowing agent is designated T1. Furthermore, the time at the apex of the exothermic peak in the DSC curve 34 for the adhesive composition obtained by removing the blowing agent is designated T2. In this case, in the bonding step, the adhesive composition is heated so that T1 < T2.
[0025] In the present disclosure, in the bonding step, the adhesive composition is heated so that T1 < T2, thereby promoting the expansion of the foaming agent before the curing reaction of the thermosetting resin proceeds, and the foaming agent can be sufficiently expanded, thereby increasing the thickness of the adhesive layer during foaming and improving the adhesive strength.
[0026] On the other hand, if T1≧T2, the curing reaction of the thermosetting resin proceeds before the expansion of the foaming agent proceeds, which inhibits the expansion of the foaming agent, reducing the thickness of the adhesive layer during foaming and potentially reducing the adhesive strength.
[0027] In this manner, in the present disclosure, the adhesive strength can be improved by heating the adhesive composition so that the adhesive composition satisfies A < B and the adhesive composition satisfies T1 < T2 in the bonding step, thereby improving the reliability, durability, etc. of the article obtained by the article manufacturing method of the present disclosure.
[0028] Each step of the method for manufacturing an article and the adhesive composition according to the present disclosure will be described below.
[0029] 1. Adhesive Composition The adhesive composition of the present disclosure contains a thermosetting resin and a foaming agent. The foaming agent is thermally expandable microcapsules.
[0030] (1) Properties In the adhesive composition of the present disclosure, differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera under the heating conditions in the bonding step described below. The resulting expansion rate-time curve has time on the horizontal axis and the foaming rate of the foaming agent on the vertical axis. The slope of the tangent line drawn at the apex of the peak to the curve on the long-term side of the peak is defined as A. Differential scanning calorimetry is performed on the adhesive composition under the heating conditions in the bonding step described below. The slope of the tangent line drawn at the apex of the exothermic peak to the curve on the long-term side of the exothermic peak is defined as B. A<B.
[0031] Differential scanning calorimetry (DSC) of the blowing agent is performed as follows: First, 0.16 mg to 0.17 mg of the blowing agent is weighed into a container. Next, using a differential scanning calorimeter equipped with a camera, the temperature is increased and maintained at a nitrogen gas flow rate of 20 ml / min under the heating conditions of the bonding process.
[0032] A differential scanning calorimeter equipped with a camera can measure thermal properties using the differential scanning calorimeter and also observe changes in the morphology, color, and other characteristics of a sample during differential scanning calorimetry. In a differential scanning calorimeter equipped with a camera, DSC data and image data are synchronized. Therefore, by performing differential scanning calorimetry on a blowing agent using a differential scanning calorimeter equipped with a camera, the foaming behavior of the blowing agent can be analyzed. Specifically, the area occupied by the blowing agent is first determined from the image data. In this case, as shown in FIG. 3, for example, the value of the area occupied by the blowing agent at time 0 among all the image data is considered to be the foaming ratio of the blowing agent at 0%, and the value at which the area occupied by the blowing agent is maximum is considered to be the foaming ratio of the blowing agent at 100%. The change in the foaming ratio of the blowing agent over time is shown as an expansion ratio-time curve, as shown in FIG. 3, for example. A suitable differential scanning calorimeter equipped with a camera is, for example, the "High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation.
[0033] When performing differential scanning calorimetry (DSC) on the foaming agent, the adhesive composition may be dissolved in a solvent to separate the foaming agent. The solvent is not particularly limited as long as it is capable of dissolving components other than the foaming agent contained in the adhesive composition, and is appropriately selected depending on the type of thermosetting resin contained in the adhesive composition, etc. For example, a solvent used in the adhesive composition can be used. Specifically, methyl ethyl ketone, ethyl acetate, toluene, etc. can be used.
[0034] In addition, in the foaming rate-time curve for the foaming agent, the tangent line drawn at the apex of the peak to the curve on the long-time side of the peak is determined by the following method. The apex of the peak is the point where the foaming rate of the foaming agent is 100%. Also, on the curve on the long-time side of the peak, the point where the foaming rate of the foaming agent is 70% is determined. Then, as shown in Figure 5, for example, the straight line connecting the apex of the peak (the point where the foaming rate of the foaming agent is 100%) and the point on the curve on the long-time side of the peak where the foaming rate of the foaming agent is 70% is defined as the tangent line L1 drawn at the apex of the peak to the curve on the long-time side of the peak.
[0035] The peak in the foaming ratio-time curve refers to the portion from when the curve leaves the baseline to when it returns to the baseline.
[0036] Differential scanning calorimetry (DSC) of the adhesive composition is performed as follows: First, 5.00 mg to 5.03 mg of the adhesive composition is weighed into a container. Next, using a differential scanning calorimeter, the temperature is increased and maintained at a nitrogen gas flow rate of 20 ml / min under the heating conditions for the bonding process.
[0037] When performing differential scanning calorimetry (DSC) on the adhesive composition, for example, if the adhesive composition contains a solvent, the solvent is evaporated before the differential scanning calorimetry is performed.
[0038] In addition, in the DSC curve for the adhesive composition, the tangent drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak is determined by the following method. First, the heat flow at the apex of the exothermic peak is determined. Furthermore, when the heat flow at the apex of the exothermic peak is set to 100%, the point on the curve on the long-time side of the exothermic peak where the heat flow is 70% is determined. Then, the line connecting the apex of the exothermic peak and the point on the curve on the long-time side of the exothermic peak where the heat flow is 70% is defined as the tangent drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak. For example, in Figure 5, when the heat flow hf1 at the apex of the exothermic peak is set to 100%, the heat flow hf2 is the point where it is 70% of the heat flow hf1. The line connecting the apex of the exothermic peak (the point indicating the heat flow hf1) and the point indicating the heat flow hf2 can be defined as the tangent L2 drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak.
[0039] The baseline of the DSC curve for the adhesive composition is set to 0.
[0040] The exothermic peak in a DSC curve refers to the portion of the curve from when it leaves the baseline until when it returns to the baseline.
[0041] The expansion rate-time curve for the foaming agent and the DSC curve for the adhesive composition are superimposed to form a single graph using the following method. First, since the horizontal axis represents time, the horizontal axis of the expansion rate-time curve for the foaming agent and the horizontal axis of the DSC curve for the adhesive composition are made to coincide. Furthermore, for the vertical axis, the position of the baseline in the expansion rate-time curve for the foaming agent is made to coincide with the position of the baseline in the DSC curve for the adhesive composition. In this case, the baseline of the expansion rate-time curve for the foaming agent is set to 0. As described above, the baseline of the DSC curve for the adhesive composition is also set to 0. Furthermore, for the vertical axis, the position of the apex of the peak in the expansion rate-time curve for the foaming agent (the point showing a 100% expansion rate of the foaming agent) is made to coincide with the position of the apex of the exothermic peak in the DSC curve for the adhesive composition. This results in a graph such as that shown in FIG. 5, for example.
[0042] Furthermore, when the adhesive composition contains multiple blowing agents, it is sufficient that A<B is satisfied for at least one of the blowing agents. In particular, it is preferable that A<B is satisfied for the blowing agent contained in the adhesive composition that is present in the greatest amount. It is particularly preferable that A<B is satisfied for all of the multiple blowing agents contained in the adhesive composition.
[0043] When there are multiple peaks in the expansion rate-time curve for a blowing agent, it is sufficient that A<B is satisfied for at least one of the peaks. When there are multiple peaks in the expansion rate-time curve, the adhesive composition usually contains multiple blowing agents. In particular, it is preferable that A<B is satisfied for all of the peaks.
[0044] Furthermore, when the DSC curve for the adhesive composition shows multiple exothermic peaks due to the curing reaction of the thermosetting resin, it is sufficient that A<B is satisfied for at least one of the exothermic peaks. When the DSC curve shows multiple exothermic peaks due to the curing reaction of the thermosetting resin, for example, the adhesive composition contains multiple thermosetting resins. In particular, it is preferable that A<B be satisfied for an exothermic peak with a small slope B among the multiple exothermic peaks due to the curing reaction of the thermosetting resin. It is particularly preferable that A<B be satisfied for all of the exothermic peaks.
[0045] In the adhesive composition, A<B. In particular, B is preferably much greater than A. When the slope B is large, the curing rate of the thermosetting resin increases. When the slope A is small, the shrinkage rate of the foaming agent decreases. Therefore, when B is much greater than A, the thermosetting resin can be sufficiently cured before the shrinkage of the foaming agent progresses, and the adhesive strength can be improved.
[0046] In the adhesive composition, the slope A can be controlled, for example, by adjusting the shell thickness of the thermally expandable microcapsules, which are the foaming agent. Specifically, the slope A tends to decrease when the shell thickness of the thermally expandable microcapsules is thick. On the other hand, the slope A tends to increase when the shell thickness of the thermally expandable microcapsules is thin.
[0047] Furthermore, in the case of an adhesive composition, the slope B can be controlled, for example, by adjusting the composition of the adhesive composition. For example, when the adhesive composition further contains a curing agent, the slope B tends to be larger. For example, when the adhesive composition further contains a curing agent and a curing catalyst, the slope B tends to be larger. For example, when the adhesive composition contains a polyfunctional thermosetting resin, the slope B tends to be larger.
[0048] Furthermore, in the expansion ratio-time curve for the blowing agent, the time from the apex of the peak (the point at which the expansion ratio of the blowing agent is 100%) until the contraction of the blowing agent stabilizes is, for example, 0.5 minutes or more and 60 minutes or less, and may be 1 minute or more and 45 minutes or less. If the time is too short, the slope A becomes large, and it is possible that A<B is not satisfied. If the time is too long, the expansion ratio of the blowing agent may decrease.
[0049] Furthermore, in the DSC curve for the adhesive composition, the time from the apex of the exothermic peak to the baseline is, for example, 0.1 minutes or more and 30 minutes or less, or alternatively 0.2 minutes or more and 10 minutes or less, or 0.3 minutes or more and 5 minutes or less. If this time is too long, the slope B becomes small, and it is possible that A<B is not satisfied. If this time is too short, it is possible that storage stability is reduced.
[0050] As described below, when a foamable adhesive sheet is used in the present disclosure and the foamable adhesive sheet has a first adhesive layer and a second adhesive layer, the adhesive composition contained in at least one of the first adhesive layer and the second adhesive layer only needs to contain a foaming agent. When only the adhesive composition contained in one of the first adhesive layer and the second adhesive layer contains a foaming agent, the adhesive composition containing the foaming agent only needs to satisfy the above-mentioned properties. When both the adhesive composition contained in the first adhesive layer and the adhesive composition contained in the second adhesive layer contain a foaming agent, the adhesive composition contained in at least one of the adhesive layers only needs to satisfy the above-mentioned properties. In particular, it is preferable that the adhesive compositions contained in both the first adhesive layer and the second adhesive layer satisfy the above-mentioned properties.
[0051] (2) Composition The adhesive composition according to the present disclosure contains a thermosetting resin and a foaming agent. The foaming agent is thermally expandable microcapsules.
[0052] (a) Foaming Agent The foaming agent is a thermally expandable microcapsule. As the foaming agent, a thermally expandable microcapsule that is generally used in adhesive compositions can be used.
[0053] The thermally expandable microcapsules preferably have a core made of a thermal expansion agent such as hydrocarbon and a shell made of a resin such as acrylonitrile copolymer.
[0054] The foaming agent may be used alone or in combination of two or more kinds.
[0055] The foaming initiation temperature of the foaming agent is preferably equal to or higher than the softening temperature of the thermosetting resin and equal to or lower than the activation temperature of the curing reaction of the thermosetting resin. The foaming initiation temperature of the foaming agent is, for example, 70°C or higher, and may be 100°C or higher. If the foaming initiation temperature is too low, foaming may start early, and foaming may occur in a state where the flexibility and fluidity of the resin component are low, making it difficult to produce uniform foam. On the other hand, the foaming initiation temperature of the foaming agent is, for example, 210°C or lower. If the foaming initiation temperature is too high, the resin component may deteriorate.
[0056] The softening temperature of the thermosetting resin can be measured using the ring and ball softening temperature test method specified in JIS K7234.
[0057] The average particle size of the foaming agent may be, for example, 10 μm or more, 13 μm or more, or 17 μm or more. The average particle size of the foaming agent is preferably equal to or less than the thickness of the adhesive layer, and may be, for example, 44 μm or less, 30 μm or less, or 24 μm or less.
[0058] The average particle size of the foaming agent is the particle size at 50% of the cumulative value in the particle size distribution determined by laser diffraction scattering. Furthermore, when measuring the average particle size of the foaming agent, the adhesive composition is dissolved in a solvent to separate the foaming agent. The solvent is not particularly limited as long as it is capable of dissolving components other than the foaming agent contained in the adhesive composition, and is appropriately selected depending on the type of thermosetting resin contained in the adhesive composition, etc. For example, a solvent used in the adhesive composition can be used. Specific examples that can be used include methyl ethyl ketone, ethyl acetate, toluene, etc.
[0059] The expansion ratio at the maximum expansion temperature of the blowing agent is, for example, 1.5 times or more, and may be 3 times or more, while the expansion ratio at the maximum expansion temperature of the blowing agent is, for example, 15 times or less, and may be 10 times or less.
[0060] The content of the foaming agent is, for example, 0.5 parts by mass or more, or may be 2 parts by mass or more, or 3 parts by mass or more, or 4 parts by mass or more, or may be 5 parts by mass or more, relative to 100 parts by mass of the resin component contained in the adhesive composition. On the other hand, the content of the foaming agent is, for example, 25 parts by mass or less, or may be 20 parts by mass or less, or may be 15 parts by mass or less, relative to 100 parts by mass of the resin component contained in the adhesive composition.
[0061] (b) Thermosetting Resin As the thermosetting resin, a thermosetting resin generally used in adhesive compositions can be used. The thermosetting resin can be applied even when the first member or the second member does not have transparency, such as when the first member or the second member is made of metal.
[0062] Examples of thermosetting resins include epoxy resins, acrylic resins, phenolic resins, unsaturated polyester resins, alkyd resins, urethane resins, and thermosetting polyimide resins.
[0063] Among these, epoxy resins are preferred. In this case, the adhesive composition preferably contains an epoxy resin, which is a thermosetting resin, a curing agent, and a foaming agent. In general, adhesive compositions containing epoxy resins are excellent in mechanical strength, heat resistance, insulating properties, chemical resistance, etc., and have little cure shrinkage, making them suitable for a wide range of applications.
[0064] The epoxy resin will be described below by way of example.
[0065] (Epoxy Resin) The epoxy resin in the present disclosure is a compound that has at least one epoxy group or glycidyl group and cures by a crosslinking polymerization reaction in combination with a curing agent. The epoxy resin also includes a monomer having at least one epoxy group or glycidyl group.
[0066] Examples of epoxy resins include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of epoxy resins include bisphenol-type epoxy resins such as bisphenol A-type epoxy resins and bisphenol F-type epoxy resins, novolac-type epoxy resins such as bisphenol A novolac-type epoxy resins and cresol novolac-type epoxy resins, and modified epoxy resins such as urethane-modified epoxy resins and rubber-modified epoxy resins. Other specific examples include biphenyl-type epoxy resins, stilbene-type epoxy resins, triphenolmethane-type epoxy resins, alkyl-modified triphenolmethane-type epoxy resins, triazine-nucleus-containing epoxy resins, dicyclopentadiene-modified phenol-type epoxy resins, naphthalene-type epoxy resins, glycol-type epoxy resins, and pentaerythritol-type epoxy resins. The epoxy resins may be one type or two or more types.
[0067] Bisphenol A epoxy resins can exist in a liquid state or a solid state at room temperature depending on the number of repeating units in the bisphenol skeleton. Bisphenol A epoxy resins having, for example, 2 to 10 bisphenol skeletons in the main chain are solid at room temperature. Bisphenol A epoxy resins are particularly preferred because they can improve heat resistance.
[0068] The epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.
[0069] (c) Acrylic Resin In the present disclosure, when the adhesive composition contains an epoxy resin as a thermosetting resin, it may further contain an acrylic resin compatible with the epoxy resin. The acrylic resin is a resin compatible with the epoxy resin. Because the acrylic resin is compatible with the epoxy resin, it is easy to improve the toughness of the adhesive layer. As a result, the adhesiveness after foaming and curing can be improved. Furthermore, it is believed that the acrylic resin acts as a compatibilizer for the foaming agent (e.g., a foaming agent whose shell is an acrylonitrile copolymer resin), uniformly dispersing and foaming, thereby improving the adhesiveness after foaming and curing. In addition, the flexibility of the acrylic resin can be exerted, improving adhesion to the substrate after foaming and curing and crack resistance after foaming and curing. Furthermore, the compatibility of the acrylic resin with the epoxy resin can maintain high surface hardness of the adhesive layer. On the other hand, if the acrylic resin is incompatible with the epoxy resin, a flexible portion is formed on the surface of the adhesive layer, making the interface with the first member and the second member less slippery, which may reduce workability.
[0070] The acrylic resin in the present disclosure is compatible with the epoxy resin. The compatibility of the acrylic resin with the epoxy resin can be confirmed, for example, by observing the cross section of an adhesive layer prepared using the adhesive composition with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to see if micron-sized islands are present. More specifically, the average particle size of the islands is preferably 1 μm or less. In particular, the average particle size of the islands may be 0.5 μm or less, or even 0.3 μm or less. A large number of samples is preferably used, for example, 100 or more. The area to be observed is a range of 100 μm × 100 μm, or, if the thickness of the adhesive layer is 100 μm or less, a range of the thickness × 100 μm.
[0071] The acrylic resin may have a polar group, such as an epoxy group, a hydroxyl group, a carboxyl group, a nitrile group, or an amide group.
[0072] The acrylic resin may be a homopolymer of an acrylic acid ester monomer, a mixed component containing two or more of the above homopolymers, or a copolymer of two or more acrylic acid ester monomers, a component containing one or more copolymers. The acrylic resin may also be a mixed component of the above homopolymer and the above copolymer. The "acrylic acid" acrylic acid ester monomer also includes the concept of methacrylic acid. Specifically, the acrylic resin may be a mixture of a methacrylate polymer and an acrylate polymer, or an acrylic acid ester polymer such as acrylate-acrylate, methacrylate-methacrylate, or methacrylate-acrylate. Of these, it is preferable that the acrylic resin contain a copolymer of two or more acrylic acid ester monomers (a (meth)acrylic acid ester copolymer).
[0073] Examples of the monomer component constituting the (meth)acrylic acid ester copolymer include the monomer components described in JP 2014-065889 A. The monomer component may have the polar group described above. Examples of the (meth)acrylic acid ester copolymer include an ethyl acrylate-butyl acrylate-acrylonitrile copolymer, an ethyl acrylate-acrylonitrile copolymer, and a butyl acrylate-acrylonitrile copolymer. Note that "acrylic acid" such as methyl acrylate and ethyl acrylate also includes "methacrylic acid" such as methyl methacrylate and ethyl methacrylate.
[0074] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an acrylic block copolymer such as a methacrylate-acrylate copolymer. Examples of (meth)acrylates constituting the acrylic block copolymer include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and benzidyl acrylate. In these examples, "acrylic acid" also includes "methacrylic acid."
[0075] Specific examples of methacrylate-acrylate copolymers include acrylic copolymers such as methyl methacrylate-butyl acrylate-methyl methacrylate (MMA-BA-MMA) copolymer, which also includes block copolymers of polymethyl methacrylate-polybutyl acrylate-polymethyl methacrylate (PMMA-PBA-PMMA).
[0076] The acrylic copolymer may have no polar groups, or may be a modified product in which the above-mentioned polar groups have been partially introduced. The modified product is highly compatible with epoxy resins, thereby further improving adhesion.
[0077] Among these, the acrylic resin is preferably a (meth)acrylic acid ester copolymer having a first polymer portion having a glass transition temperature (Tg) of 10° C. or lower and a second polymer portion having a glass transition temperature (Tg) of 20° C. or higher. Such a (meth)acrylic acid ester copolymer has a first polymer portion that forms a soft segment and a second polymer portion that forms a hard segment. By adding such a copolymer, the toughness of the adhesive layer after curing can be improved, thereby further increasing the adhesive strength.
[0078] The manifestation of the above-mentioned effect can be presumed as follows: By using an acrylic resin having both a soft segment and a hard segment, such as the above-mentioned (meth)acrylic acid ester copolymer, the hard segment contributes to heat resistance, and the soft segment contributes to toughness or flexibility, so that an adhesive layer having good heat resistance, toughness, and flexibility can be obtained.
[0079] At least one of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer has compatibility with epoxy resins. When the first polymer portion has compatibility with epoxy resins, flexibility can be increased. Furthermore, when the second polymer portion has compatibility with epoxy resins, cohesion and toughness can be increased.
[0080] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and particularly preferably an A-B-A block copolymer in which a compatible portion is polymer block A and an incompatible portion is polymer block B. Furthermore, it is preferably an A-B-A block copolymer in which a first polymer portion is an incompatible portion and a second polymer portion is a compatible portion, and in which the first polymer portion is polymer block B and the second polymer portion is polymer block A.
[0081] The (meth)acrylic acid ester copolymer may be a modified product in which the above-mentioned polar group is introduced into a part of the first polymer segment or the second polymer segment.
[0082] A specific example of the (meth)acrylic acid ester copolymer having the first polymer portion and the second polymer portion is the above-mentioned MMA-BA-MMA copolymer.
[0083] The content of the acrylic resin, based on 100 parts by mass of the resin components contained in the adhesive composition, may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more. If the content of the acrylic resin is too low, the adhesive properties after foaming and curing and the adhesion of the adhesive layer to the substrate may be reduced. On the other hand, the content of the acrylic resin, based on 100 parts by mass of the resin components contained in the adhesive composition, may be, for example, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less. If the content of the acrylic resin is too high, the film strength may be reduced.
[0084] (d) Curing Agent The adhesive composition of the present disclosure may further contain a curing agent.
[0085] When the adhesive composition contains an epoxy resin as the thermosetting resin, the curing agent may be any curing agent that is generally used in epoxy resin adhesives.
[0086] The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C can have a longer storage stability (pot life) than a curing agent that is liquid at 23°C. The curing agent may be a latent curing agent. The curing agent is usually a curing agent that undergoes a curing reaction by heat. One type of curing agent may be used alone, or two or more types may be used.
[0087] The reaction initiation temperature of the curing agent is, for example, 110°C or higher, and may be 130°C or higher. If the reaction initiation temperature is too low, the reaction will start early, and curing will occur with low flexibility and fluidity of the resin component, making it difficult to achieve uniform curing. On the other hand, the reaction initiation temperature of the curing agent is, for example, 200°C or lower. If the reaction initiation temperature is too high, the resin component may deteriorate. Note that when a highly heat-resistant resin such as a phenolic resin is used in addition to the epoxy resin, the resin component will deteriorate less, and the reaction initiation temperature of the curing agent may be, for example, 300°C or lower. The reaction initiation temperature of the curing agent can be determined by differential scanning calorimetry (DSC).
[0088] Specific examples of the curing agent include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.
[0089] Examples of imidazole-based curing agents include imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylic acid salts of imidazole compounds, and adducts with epoxy compounds. Furthermore, it is preferable that the imidazole-based curing agent has a hydroxyl group. Crystallization occurs due to hydrogen bonding between the hydroxy groups, so the reaction initiation temperature tends to be high.
[0090] Examples of phenolic curing agents include phenolic resins. Further examples of phenolic resins include resol-type phenolic resins and novolac-type phenolic resins. From the viewpoints of adhesion to the substrate after foaming and curing and crack resistance after foaming and curing, phenolic novolac resins having a Tg of 110°C or less are particularly preferred. Furthermore, phenolic curing agents and imidazole-type curing agents may be used in combination. In this case, it is preferable to use an imidazole-type curing agent as a curing catalyst.
[0091] Examples of amine-based curing agents include aliphatic amines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA); aromatic amines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS); alicyclic amines; and polyamidoamines. Furthermore, examples of amine-based curing agents that can be used include dicyandiamide-based curing agents such as dicyandiamide (DICY), organic acid dihydrazide-based curing agents, amine adduct-based curing agents, and ketimine-based curing agents.
[0092] Examples of acid anhydride curing agents include alicyclic acid anhydrides (liquid acid anhydrides) such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA); and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA).
[0093] The isocyanate curing agent may, for example, be a blocked isocyanate.
[0094] Examples of thiol-based curing agents include ester-bonded thiol compounds, aliphatic ether-bonded thiol compounds, and aromatic ether-bonded thiol compounds.
[0095] In particular, it is preferable to use a curing agent other than an imidazole-based curing agent in combination with an imidazole-based curing agent, and in this case, it is preferable to use the imidazole-based curing agent as a curing catalyst.
[0096] The content of the curing agent is, for example, 1 part by mass or more and 40 parts by mass or less, based on 100 parts by mass of the resin component contained in the adhesive composition. For example, when an imidazole-based curing agent is used as the main curing agent, the content of the curing agent is preferably, for example, 1 part by mass or more and 15 parts by mass or less, based on 100 parts by mass of the resin component contained in the adhesive composition. On the other hand, when a phenol-based curing agent is used as the main curing agent, the content of the curing agent is preferably, for example, 5 parts by mass or more and 40 parts by mass or less, based on 100 parts by mass of the resin component contained in the adhesive composition. Note that using an imidazole-based curing agent or a phenol-based curing agent as the main curing agent means that the mass proportion of the imidazole-based curing agent or the phenol-based curing agent is the highest in the curing agent.
[0097] (e) Other Components When the thermosetting resin is an epoxy resin, the adhesive composition of the present disclosure may contain only the above-mentioned epoxy resin and acrylic resin as resin components, or may further contain other resins, such as urethane resins.
[0098] The total proportion of the epoxy resin and the acrylic resin relative to the resin components contained in the adhesive composition is, for example, 70% by mass or more, or may be 80% by mass or more, or 90% by mass or more, or may be 100% by mass.
[0099] The content of the resin component contained in the adhesive composition is, for example, 60% by mass or more, or may be 70% by mass or more, or 80% by mass or more, or may be 90% by mass or more.
[0100] The adhesive composition may contain additives such as a silane coupling agent, a filler, an antioxidant, a light stabilizer, an ultraviolet absorber, a lubricant, a plasticizer, an antistatic agent, a crosslinking agent, and a colorant, as needed. Examples of the silane coupling agent include an epoxy-based silane coupling agent. Examples of the filler include inorganic fillers such as calcium carbonate, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, a molybdenum compound, and titanium dioxide. Examples of the antioxidant include a phenol-based antioxidant and a sulfur-based antioxidant.
[0101] The adhesive composition may or may not contain a solvent. In this specification, the term "solvent" is used in a broad sense to include not only a strict solvent (a solvent that dissolves a solute) but also a dispersion medium. The solvent contained in the adhesive composition is volatilized and removed when the adhesive composition is applied and dried to form an adhesive layer.
[0102] (3) Preparation Method The adhesive composition can be obtained by mixing the above-mentioned components and, if necessary, kneading and dispersing them. As a mixing and dispersing method, a general kneading disperser, such as a two-roll mill, a three-roll mill, a pebble mill, a tron mill, a Szegvari attritor, a high-speed impeller disperser, a high-speed stone mill, a high-speed impact mill, a desper, a high-speed mixer, a ribbon blender, a co-kneader, an intensive mixer, a tumbler, a blender, a desperzer, a homogenizer, or an ultrasonic disperser can be used.
[0103] 2. Placement Step The placement step in the present disclosure is a step of placing the adhesive composition between the first member and the second member.
[0104] When disposing the adhesive composition between the first and second members, for example, a foamable adhesive sheet having an adhesive layer containing the adhesive composition may be used, and the foamable adhesive sheet may be disposed between the first and second members. Alternatively, for example, a liquid adhesive composition may be used, and the liquid adhesive composition may be applied to at least one surface of the first and second members. Among these, it is preferable to use a foamable adhesive sheet and dispose the foamable adhesive sheet between the first and second members. The foamable adhesive sheet has excellent handleability and workability.
[0105] When a foamable adhesive sheet is used, the foamable adhesive sheet may, for example, have only an adhesive layer containing the adhesive composition, or may have a first adhesive layer containing the adhesive composition and a second adhesive layer containing the adhesive composition, or may have a first adhesive layer containing the adhesive composition, a substrate, and a second adhesive layer containing the adhesive composition, in that order.
[0106] The foamable adhesive sheet will be described later.
[0107] Furthermore, when a foamable adhesive sheet is used, the method for disposing the foamable adhesive sheet between the first and second members is appropriately selected depending on the types of the first and second members. Examples include a method of disposing a foamable adhesive sheet on one of the first and second members and disposing the other member on the side of the foamable adhesive sheet opposite the one member; a method of inserting a foamable adhesive sheet into the gap between the first and second members; a method of disposing a foamable adhesive sheet in a hole or groove in the first member, and then inserting a second member into the gap after disposing the foamable adhesive sheet in the hole or groove in the first member. Furthermore, for example, when the first member has a hole or groove and the second member is disposed in the hole or groove of the first member to be bonded, a method of attaching a foamable adhesive sheet to the second member and then disposing the second member with the foamable adhesive sheet attached in the hole or groove in the first member; a method of attaching a foamable adhesive sheet to the hole or groove in the first member and then disposing the second member in the hole or groove in the first member with the foamable adhesive sheet attached, and the like.
[0108] Furthermore, when a liquid adhesive composition is used, the method for disposing the liquid adhesive composition between the first and second members is appropriately selected depending on the types of the first and second members, etc. Examples include a method of applying the liquid adhesive composition to one of the first and second members and then disposing the other member on the coating of the liquid adhesive composition; a method of injecting the liquid adhesive composition into the gap between the first and second members; a method of applying the liquid adhesive composition to holes, grooves, etc. in the first member, and then inserting the second member into the gap after the liquid adhesive composition has been applied to the holes, grooves, etc. in the first member. Furthermore, for example, when the first member has holes or grooves and the second member is disposed in the holes or grooves of the first member to be bonded, a method of applying the liquid adhesive composition to the second member and then disposing the second member with the liquid adhesive composition applied in the holes or grooves of the first member; a method of applying the liquid adhesive composition to the holes or grooves of the first member and then disposing the second member in the holes or grooves of the first member with the liquid adhesive composition applied thereto, etc.
[0109] The method for applying the liquid adhesive composition is not particularly limited, and examples thereof include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.
[0110] 3. Bonding Step The bonding step in the present disclosure is a step of heating the adhesive composition to foam and cure it, thereby bonding the first member and the second member together.
[0111] In the present disclosure, when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera, the time at the top of the peak in the expansion rate-time curve is defined as T1, with the horizontal axis representing time and the vertical axis representing the expansion rate of the foaming agent. When differential scanning calorimetry is performed on the adhesive composition from which the foaming agent has been removed, the time at the top of the exothermic peak in the DSC curve is defined as T2, with the horizontal axis representing time and the vertical axis representing heat flow. In the bonding step, the adhesive composition is heated so that T1 < T2.
[0112] Here, differential scanning calorimetry (DSC) of the blowing agent is performed as follows: First, 0.16 mg to 0.17 mg of the blowing agent is weighed into a container. Next, using a differential scanning calorimeter equipped with a camera, the blowing agent is heated and maintained at a nitrogen gas flow rate of 20 ml / min at a predetermined heating rate, heating temperature, holding time, and heating rate.
[0113] Differential scanning calorimetry (DSC) of a composition obtained by removing the blowing agent from the adhesive composition is performed by the following method. First, 5.00 mg to 5.03 mg of the composition obtained by removing the blowing agent from the adhesive composition is weighed into a container. Next, using a differential scanning calorimeter, the temperature is increased and maintained at a nitrogen gas flow rate of 20 ml / min, and at a predetermined heating rate, heating temperature, holding time, and heating rate. Here, the heating conditions for the differential scanning calorimetry (DSC) of the blowing agent and the differential scanning calorimetry (DSC) of the adhesive composition obtained by removing the blowing agent are the same.
[0114] Furthermore, the expansion rate-time curve for the foaming agent and the DSC curve for the adhesive composition from which the foaming agent has been removed are superimposed into a single graph using the following method. Since the horizontal axis represents time, the horizontal axis of the expansion rate-time curve for the foaming agent and the horizontal axis of the DSC curve for the adhesive composition from which the foaming agent has been removed coincide. This results in a graph such as that shown in Figure 6, for example.
[0115] Furthermore, when the adhesive composition contains multiple blowing agents, it is sufficient that at least one of the blowing agents satisfies T1<T2. In particular, it is preferable that the blowing agent contained in the adhesive composition with the largest content satisfies T1<T2. It is particularly preferable that all of the multiple blowing agents contained in the adhesive composition satisfy T1<T2.
[0116] When there are multiple peaks in the expansion rate-time curve for a blowing agent, it is sufficient that T1<T2 is satisfied for at least one of the peaks. When there are multiple peaks in the expansion rate-time curve, the adhesive composition usually contains multiple blowing agents. In particular, it is preferable that T1<T2 is satisfied for all peaks.
[0117] Furthermore, when the adhesive composition contains a plurality of thermosetting resins, it is preferable that all of the plurality of thermosetting resins contained in the adhesive composition satisfy T1<T2.
[0118] In the case where a DSC curve for a composition obtained by removing the foaming agent from the adhesive composition shows multiple exothermic peaks due to the curing reaction of the thermosetting resin, it is preferable that T1 < T2 be satisfied for all of the exothermic peaks.
[0119] In the bonding step, the adhesive composition is heated so that T1<T2.
[0120] In the bonding process, for example, by adjusting the temperature rise time from room temperature to the heating temperature, it is possible to control the time T1 at the top of the peak in the expansion ratio-time curve for the foaming agent and the time T2 at the top of the exothermic peak in the DSC curve for a composition obtained by excluding the foaming agent from the adhesive composition. Specifically, when the temperature rise time from room temperature to the heating temperature is short, T1 tends to be shorter than T2. On the other hand, when the temperature rise time from room temperature to the heating temperature is long, T1 tends to be longer than T2.
[0121] Furthermore, the heating temperature in the bonding step is preferably within ±40°C of the maximum foaming temperature of the foaming agent, more preferably within ±30°C of the maximum foaming temperature of the foaming agent, and even more preferably within ±20°C of the maximum foaming temperature of the foaming agent. If the heating temperature is higher than the above range, even if the thermosetting resin is cured, the foaming agent may shrink, making it impossible to maintain the thickness of the adhesive layer at the time of foaming, and the adhesive strength may decrease. On the other hand, if the heating temperature is lower than the above range, the foaming agent may not expand sufficiently, and the adhesive strength may decrease. In this case, interfacial failure may be more likely to occur between the adhesive composition and the first or second member after foaming and curing.
[0122] The maximum foaming temperature of the foaming agent refers to the temperature at the top of the peak in the foaming rate-time curve, which is obtained by subjecting the foaming agent to differential scanning calorimetry using a differential scanning calorimeter equipped with a camera, with time on the horizontal axis and the foaming rate of the foaming agent on the vertical axis. In this case, the heating conditions in the differential scanning calorimetry can be, for example, a temperature rise rate of 31°C / min.
[0123] In the bonding process, the temperature rise time from room temperature to the heating temperature is, for example, 0.1 to 60 minutes, or 0.3 to 45 minutes, or 0.5 to 30 minutes. If the temperature rise time is too short, the temperature rise rate becomes too fast, which may cause overshoot and a large deviation from the target temperature. On the other hand, if the temperature rise time is too long, the relationship T1<T2 may not be satisfied.
[0124] In the bonding step, the holding time at the heating temperature is, for example, from 0.5 minutes to 240 minutes, or alternatively from 1 minute to 120 minutes, or from 2 minutes to 60 minutes. If the heating temperature is high and the holding time is long, even if the thermosetting resin is cured, the foaming agent may shrink, making it impossible to maintain the thickness of the adhesive layer at the time of foaming, and the adhesive strength may decrease.
[0125] 4. Foamable Adhesive Sheet The foamable adhesive sheet of the present disclosure has at least an adhesive layer containing the adhesive composition described above.
[0126] The foamable adhesive sheet may have only an adhesive layer, or may have a first adhesive layer and a second adhesive layer, or may have a first adhesive layer, a substrate, and a second adhesive layer in that order. When a substrate is disposed between the first adhesive layer and the second adhesive layer, the handleability and workability of the foamable adhesive sheet can be improved. On the other hand, when the foamable adhesive sheet does not have a substrate, the overall thickness of the foamable adhesive sheet can be reduced. Therefore, for example, the foamable adhesive sheet can be inserted into narrow gaps.
[0127] For example, the foamable adhesive sheet 10 shown in Fig. 2 has only the adhesive layer 1. Furthermore, for example, the foamable adhesive sheet 10 shown in Fig. 7 has a first adhesive layer 1a, a substrate 2, and a second adhesive layer 1b in this order.
[0128] (1) Adhesive Layer The adhesive layer contains the adhesive composition.
[0129] The thickness of the adhesive layer is not particularly limited, but is preferably equal to or greater than the average particle size of the foaming agent, for example, 10 μm or more, or 15 μm or more, or even 20 μm or more. If the adhesive layer is too thin, it may be difficult to obtain sufficient adhesion to the substrate and adhesion after foaming and curing. On the other hand, the thickness of the adhesive layer is, for example, 200 μm or less, or may be 150 μm or less, or may be 100 μm or less. If the adhesive layer is too thick, the surface quality may deteriorate.
[0130] Here, the thickness of the adhesive layer is a value measured from a cross section of the foamable adhesive sheet in the thickness direction as observed with a transmission electron microscope (TEM), a scanning electron microscope (SEM), or a scanning transmission electron microscope (STEM), and can be the average value of thicknesses measured at 10 randomly selected locations. The same method can be used to measure the thickness of other layers of the foamable adhesive sheet.
[0131] The adhesive layer may be a continuous layer or a discontinuous layer. Examples of discontinuous layers include stripes and dots. The surface of the adhesive layer may have an uneven shape such as an embossed shape.
[0132] The adhesive layer can be formed, for example, by applying the adhesive composition and removing the solvent. Examples of the application method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.
[0133] (2) Substrate The substrate preferably has insulating properties. The substrate is preferably in the form of a sheet. The substrate may have a single-layer structure or a multi-layer structure. The substrate may or may not have a porous structure inside.
[0134] Examples of the substrate include a resin substrate and a nonwoven fabric.
[0135] Examples of resins contained in the resin substrate include polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyester; polycarbonate; polyarylate; polyurethane; polyamide resins such as polyamide and polyetheramide; polyimide resins such as polyimide, polyetherimide, and polyamideimide; polysulfone resins such as polysulfone and polyethersulfone; polyetherketone resins such as polyetherketone and polyetheretherketone; polyphenylene sulfide (PPS); and modified polyphenylene oxide. The glass transition temperature of the resin is, for example, 80°C or higher, or may be 140°C or higher, or 200°C or higher. Furthermore, a liquid crystal polymer (LCP) may be used as the resin.
[0136] Examples of nonwoven fabrics include nonwoven fabrics containing fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers.
[0137] The substrate may be subjected to a surface treatment in order to enhance adhesion to the adhesive layer.
[0138] The average thickness of the substrate is not particularly limited and may be, for example, 2 μm or more, 5 μm or more, or 9 μm or more, and may be, for example, 200 μm or less, 100 μm or less, or 50 μm or less.
[0139] (3) Other Components The foamable adhesive sheet of the present disclosure may have other components, as needed, in addition to the adhesive layer and substrate described above.
[0140] (a) Intermediate Layer The foamable adhesive sheet of the present disclosure may have an intermediate layer between the substrate and the adhesive layer. The presence of the intermediate layer can improve the adhesion of the adhesive layer to the substrate. Furthermore, the presence of the intermediate layer can, for example, reduce stress at the bent portion when the foamable adhesive sheet is folded, or reduce stress at the cut portion when the foamable adhesive sheet is cut. As a result, lifting or peeling of the adhesive layer from the substrate can be suppressed when the foamable adhesive sheet is bent or cut.
[0141] For example, in the foamable adhesive sheet 10 shown in Fig. 8, a first intermediate layer 3a is disposed between the substrate 2 and the first adhesive layer 1a, and a second intermediate layer 3b is disposed between the substrate 2 and the second adhesive layer 1b. Although the foamable adhesive sheet 10 in Fig. 8 has both the first intermediate layer 3a and the second intermediate layer 3b, it may have only one of them.
[0142] The material contained in the intermediate layer is not particularly limited as long as it can increase the adhesion between the substrate and the adhesive layer and relieve stress, and is appropriately selected depending on the materials of the substrate and the adhesive layer, etc. Examples include polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, polymers obtained by copolymerizing at least two or more of these, crosslinked products thereof, and mixtures thereof.
[0143] The crosslinked product is a crosslinked product obtained by crosslinking the above-mentioned resin with a curing agent. Examples of the curing agent include an isocyanate-based curing agent. Furthermore, for example, when the reactive group / NCO equivalent is 1, it is preferable to add the isocyanate-based curing agent in a ratio of 0.5 mass % to 20 mass % relative to the resin.
[0144] In particular, the intermediate layer preferably contains a crosslinked resin. Note that a crosslinked resin is one that does not melt even at high temperatures. This improves adhesive strength at high temperatures, i.e., heat resistance.
[0145] The thickness of the intermediate layer is not particularly limited, but may be, for example, 0.1 μm or more, 0.5 μm or more, or 1 μm or more. If the intermediate layer is too thin, the effect of suppressing peeling of the adhesive layer from the substrate when the foamable adhesive sheet is bent or cut may not be sufficiently obtained. On the other hand, the thickness of the intermediate layer may be, for example, 4 μm or less, or 3.5 μm or less. Since the intermediate layer itself usually does not have high heat resistance, if the intermediate layer is too thick, heat resistance (adhesive strength at high temperatures) may be reduced.
[0146] The intermediate layer can be formed, for example, by applying a resin composition and removing the solvent. Examples of the application method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.
[0147] (4) Foamable Adhesive Sheet The thickness of the foamable adhesive sheet in the present disclosure is, for example, 10 μm or more, and may be 20 μm or more. On the other hand, the thickness of the foamable adhesive sheet is, for example, 1000 μm or less, and may be 200 μm or less.
[0148] (5) Manufacturing Method of Foamable Adhesive Sheet The manufacturing method of the foamable adhesive sheet in the present disclosure is not particularly limited. For example, when the foamable adhesive sheet does not have a substrate, a method can be used in which the adhesive composition is applied to one side of a separator and dried to form an adhesive layer, and then the separator is peeled off from the adhesive layer. Furthermore, when the foamable adhesive sheet has a first adhesive layer, a substrate, and a second adhesive layer in this order, a method can be used in which the adhesive composition is applied to both sides of the substrate and dried to form the first adhesive layer and the second adhesive layer. The first adhesive layer and the second adhesive layer can be formed sequentially or simultaneously. Another example is a method in which the adhesive composition is applied to one side of the substrate and dried to form the first adhesive layer, and the adhesive composition is applied to one side of the separator and dried to form the second adhesive layer, and then the second adhesive layer and the separator are laminated to the other side of the substrate.
[0149] 5. First Member and Second Member The first member and second member in the present disclosure are appropriately selected depending on the intended use of the article. The first member and second member are preferably members that require adhesion and insulation. For example, they may be components of electrical or electronic devices.
[0150] B. Adhesive Composition The adhesive composition according to the present disclosure is an adhesive composition containing a thermosetting resin and a foaming agent, wherein the foaming agent is a thermally expandable microcapsule. Differential scanning calorimetry was performed on the foaming agent using a differential scanning calorimeter equipped with a camera, under heating conditions in which the temperature was raised from room temperature to the maximum foaming temperature of the foaming agent over a period of 5 minutes and the temperature was maintained at the maximum foaming temperature of the foaming agent. When differential scanning calorimetry was performed on the foaming agent under the heating conditions in which the temperature was raised from room temperature to the maximum foaming temperature of the foaming agent over a period of 5 minutes and the temperature was maintained at the maximum foaming temperature of the foaming agent, the resulting expansion rate-time curve had a horizontal axis representing time and a vertical axis representing the foaming rate of the foaming agent. The slope of the tangent line drawn at the apex of the peak to the curve on the long-term side of the peak was defined as C, and when differential scanning calorimetry was performed on the adhesive composition under the heating conditions in which the DSC curve had a horizontal axis representing time and a vertical axis representing heat flow, the slope of the tangent line drawn at the apex of the peak to the curve on the long-term side of the exothermic peak was defined as D, where C<D.
[0151] Here, differential scanning calorimetry (DSC) of the blowing agent is performed by the following method. First, 0.16 mg to 0.17 mg of the blowing agent is weighed into a container. Next, using a differential scanning calorimeter equipped with a camera, the temperature is raised and maintained under heating conditions of a nitrogen gas flow rate of 20 ml / min, the temperature is raised from room temperature to the maximum foaming temperature of the blowing agent in 5 minutes, and then maintained at the maximum foaming temperature of the blowing agent.
[0152] In the expansion rate-time curve for a foaming agent, the method for determining the tangent drawn at the apex of the peak on the curve on the long-time side of the peak is the same as that described above in "A. Method for manufacturing an article."
[0153] Differential scanning calorimetry (DSC) of the adhesive composition is performed as follows: First, 5.00 mg to 5.03 mg of the adhesive composition is weighed into a container. Next, using a differential scanning calorimeter, the temperature is increased and maintained under heating conditions of a nitrogen gas flow rate of 20 ml / min, from room temperature to the maximum foaming temperature of the foaming agent over 5 minutes, and then maintained at the maximum foaming temperature of the foaming agent.
[0154] In the DSC curve for the adhesive composition, the method for determining the tangent line drawn at the apex of the exothermic peak on the long-time side of the exothermic peak is the same as the method described above in "A. Method for manufacturing an article."
[0155] The method for overlaying the foaming rate-time curve for the foaming agent and the DSC curve for the adhesive composition to form a single graph is the same as the method described above in "A. Method for manufacturing an article."
[0156] Furthermore, when the adhesive composition contains multiple blowing agents, it is sufficient that C<D is satisfied for at least one of the blowing agents. In particular, it is preferable that C<D is satisfied for the blowing agent contained in the adhesive composition that is present in the greatest amount. It is particularly preferable that C<D is satisfied for all of the multiple blowing agents contained in the adhesive composition.
[0157] When there are multiple peaks in the expansion rate-time curve for a blowing agent, it is sufficient that C<D is satisfied for at least one of the peaks. When there are multiple peaks in the expansion rate-time curve, the adhesive composition usually contains multiple blowing agents. In particular, it is preferable that C<D is satisfied for all peaks.
[0158] Furthermore, when the DSC curve for the adhesive composition shows multiple exothermic peaks due to the curing reaction of the thermosetting resin, it is sufficient that C<D is satisfied for at least one of the exothermic peaks. When the DSC curve shows multiple exothermic peaks due to the curing reaction of the thermosetting resin, for example, the adhesive composition contains multiple thermosetting resins. In particular, it is preferable that C<D be satisfied for an exothermic peak with a small slope B among the multiple exothermic peaks due to the curing reaction of the thermosetting resin. It is particularly preferable that C<D be satisfied for all exothermic peaks.
[0159] In the adhesive composition, C<D. The relationship between C and D is the same as the relationship between A and B described above in "A. Method for manufacturing an article."
[0160] The method for controlling the inclination C is the same as the method for controlling the inclination A described above in "A. Method for manufacturing an article."
[0161] The method for controlling the inclination D is the same as the method for controlling the inclination B described above in "A. Method for manufacturing an article."
[0162] In addition, in the expansion rate-time curve for the foaming agent, the time from the apex of the peak (the point at which the expansion rate of the foaming agent is 100%) to when the contraction of the foaming agent stabilizes is the same as that described above in "A. Method for manufacturing an article."
[0163] Furthermore, in the DSC curve for the adhesive composition, the time from the peak of the exothermic peak to the baseline is the same as that described above in "A. Method for manufacturing an article."
[0164] The composition and preparation method of the adhesive composition are the same as those described above in "A. Method for manufacturing an article."
[0165] C. Foamable Adhesive Sheet The foamable adhesive sheet of the present disclosure is a foamable adhesive sheet having an adhesive layer, and the adhesive layer contains the adhesive composition described above.
[0166] The adhesive composition has been described above in the section "B. Adhesive Composition," so a description thereof will be omitted here.
[0167] The foamable adhesive sheet has been described above in the section "A. Article manufacturing method 4. Foamable adhesive sheet," so a detailed description thereof will be omitted here.
[0168] The foamable adhesive sheet of the present disclosure may have a separator.
[0169] The separator is not particularly limited as long as it can be peeled from the adhesive layer, and it can have a strength sufficient to protect the adhesive layer. Examples of such separators include release films and release papers. The separator may have a single-layer structure or a multi-layer structure.
[0170] An example of a separator having a single layer structure is a fluororesin film.
[0171] Further, examples of multilayer separators include laminates having a release layer on one or both sides of a substrate layer. Examples of substrate layers include resin films such as polypropylene, polyethylene, and polyethylene terephthalate, as well as paper such as fine paper, coated paper, and impregnated paper. The material for the release layer is not particularly limited as long as it has releasability, and examples include silicone compounds, organic compound-modified silicone compounds, fluorine compounds, aminoalkyd compounds, melamine compounds, acrylic compounds, polyester compounds, and long-chain alkyl compounds. These compounds can be emulsion-type, solvent-type, or solventless.
[0172] The uses of the foamable adhesive sheet of the present disclosure are not particularly limited, but the foamable adhesive sheet of the present disclosure is particularly suitable for use in the methods for manufacturing the above-mentioned articles.
[0173] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any configuration that is substantially identical to the technical idea described in the claims of the present disclosure and that provides similar effects is included within the technical scope of the present disclosure.
[0174] [Production Examples 1 to 3] First, adhesive compositions 1 to 3 were prepared with the compositions shown in Table 1 below. Details of each material listed in Table 1 are shown below. The units in Table 1 are "parts by mass."
[0175] Acrylic resin: PMMA-PBuA-PMMA (partially containing acrylamide groups), Tg: -20°C, 120°C, Mw: 150,000 Epoxy resin A: bisphenol A novolac type, solid at room temperature, softening temperature: 70°C, epoxy equivalent: 210 g / eq, Mw: 1300, melt viscosity at 150°C: 0.5 Pa s Epoxy resin B: BPA phenoxy type, solid at room temperature, softening temperature: 110°C, epoxy equivalent: 8000 g / eq, Mw: 50,000 Curing agent A: α-(hydroxy(or dihydroxy)phenylmethyl)-ω-hydropoly[biphenyl-4,4'-diylmethylene(hydroxy(or dihydroxy)phenylenemethylene)] Curing catalyst: 2-phenyl-4,5-dihydroxymethylimidazole, average particle size: 3 μm, melting point: 230°C, reaction start temperature 145°C to 155°C, active region 155°C to 173°C (Shikoku Chemicals Corporation, 2PHZ-PW) Foaming agent: thermally expandable microcapsules, average particle size 10 μm to 16 μm, expansion start temperature 123°C to 133°C, maximum expansion temperature 168°C to 178°C, core: hydrocarbon, shell: thermoplastic polymer Solvent: methyl ethyl ketone
[0176]
[0177] A release film (PET separator, manufactured by Nippa Corporation, PET50x1-J2, thickness 50 μm) was used. The adhesive composition was applied to the release-treated surface of the release film using an applicator so that the thickness after application was 45 μm. The composition was then dried in an oven at 100°C for 3 minutes to form an adhesive layer, yielding a foamable adhesive sheet.
[0178] [Evaluation 1] (1) Differential Scanning Calorimetry Measurement of Blowing Agent Differential scanning calorimetry was performed on the blowing agent using a differential scanning calorimeter equipped with a camera ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation) under the heating conditions of a temperature rise time from room temperature to 180°C: 5 minutes, and a holding time at 180°C: 15 minutes.
[0179] (2) Differential Scanning Calorimetry Measurement of Adhesive Composition Differential scanning calorimetry was performed on an adhesive layer containing the adhesive composition using a differential scanning calorimeter ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation) under heating conditions of a temperature rise time from room temperature to 180°C: 5 minutes, and a holding time at 180°C: 15 minutes.
[0180] (3) Relationship between Slope A and Slope B Using the method described above in "A. Article manufacturing method," graphs were created by overlaying the expansion rate-time curve for the foaming agent and the DSC curves for each of Adhesive Compositions 1 to 3. The graphs are shown in Figures 9(a) to 9(c). Furthermore, using the method described above in "A. Article manufacturing method," the slope A of the tangent line drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak in the expansion rate-time curve for the foaming agent was determined. Furthermore, using the method described above in "A. Article manufacturing method," the slope B of the tangent line drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak in the DSC curve for the adhesive layer containing the adhesive composition was determined.
[0181] (4) Adhesive Strength Two cold-rolled steel plates SPCC-SD (length 100 mm x width 25 mm x thickness 1.6 mm) were prepared. Spacers (Kapton tape) were placed on one of the steel plates at 15 mm intervals. The spacer thickness was 140 μm (the thickness of two sheets of Kapton tape P-221 manufactured by Nitto Denko Corporation). A foam adhesive sheet cut to 12.5 mm x 25 mm and with the release film peeled off was placed between the spacers, and the other steel plate was placed on top and secured with clips to obtain a test specimen. The test specimen was heated from room temperature to 180 ° C. in 5 minutes using an IR heater (handy heating furnace manufactured by Advance Riko Co., Ltd.), and then heated at 180 ° C. for 30 minutes to cure the foam adhesive sheet. The shear strength (adhesive strength) of the heated test piece was measured using Tensilon RTF1350 (manufactured by A&D Co., Ltd.) in accordance with JIS K6850 at a pulling rate of 10 mm / min and a temperature of 23°C.
[0182]
[0183] [Production Example 4] First, adhesive composition 4 having the following composition was prepared.
[0184] <Composition of Adhesive Composition 4> Acrylic resin (PMMA-PBuA-PMMA (partially containing acrylamide groups), Tg: -20°C, 120°C, Mw: 150,000): 40 parts by mass Epoxy resin C (bisphenol A type, liquid at room temperature, epoxy equivalent: 184 to 194 g / eq): 45 parts by mass Epoxy resin D (diaminodiphenylmethane type, highly viscous liquid, epoxy equivalent: 110 to 130 g / eq): 65 parts by mass Epoxy resin E (silicone-modified, epoxy equivalent: 1200 g / mol): 20 parts by mass Silane coupling agent (3-glycidoxypropyltrimethoxysilane): 2 parts by mass Curing agent B (phenol-formaldehyde polycondensate, softening point 80°C, hydroxyl equivalent 104 g / mol): 6 parts by mass Curing catalyst (2-phenyl-4,5-dihydroxymethylimidazole, average particle size: 3 μm, melting point: 230°C, reaction initiation temperature 145°C to 155°C, active region 155°C to 173°C (Shikoku Chemicals Corporation, 2PHZ-PW)): 10 parts by mass Foaming agent: thermally expandable microcapsules, average particle size 10 μm to 16 μm, expansion initiation temperature 123°C to 133°C, maximum expansion temperature 168°C to 178°C, core: hydrocarbon, shell: thermoplastic polymer: 20 parts by mass Solvent (methyl ethyl ketone): 114 parts by mass
[0185] Polyethylene naphthalate (PEN film, manufactured by Toyobo Film Solutions Co., Ltd., Teonex Q51, thickness 25 μm) was used as the substrate. The adhesive composition 1 used in Production Example 1 above was applied to one surface of the substrate using an applicator so that the thickness after application was 45 μm. The resultant was then dried in an oven at 100° C. for 3 minutes to form a first adhesive layer.
[0186] Next, a release film (PET separator, manufactured by Nippa Corporation, PET50x1-J2, thickness 50 μm) was used as a second separator, and the adhesive composition 4 was applied to the release-treated surface of the release film using an applicator so that the thickness after application was 45 μm. Thereafter, the resultant was dried in an oven at 100°C for 3 minutes to form a second adhesive layer.
[0187] Next, the surface of the laminate having the second separator and the second adhesive layer was laminated onto the surface of the laminate having the substrate and the first adhesive layer, thereby obtaining a foamable adhesive sheet in which the first adhesive layer, substrate, second adhesive layer, and second separator were arranged in this order.
[0188] [Evaluation 2] (1) Differential Scanning Calorimetry Measurement of the Blowing Agent Differential scanning calorimetry was performed on the blowing agent using a differential scanning calorimeter equipped with a camera ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation) under the heating conditions of a temperature rise time from room temperature to 180°C of 1 minute to 65 minutes and a holding time at 180°C of 30 minutes.
[0189] (2) Differential Scanning Calorimetry Measurement of Compositions Obtained by Removing the Foaming Agent from the Adhesive Compositions For adhesive compositions 1 and 4, compositions obtained by removing the foaming agent from each adhesive composition were subjected to differential scanning calorimetry measurement using a differential scanning calorimeter ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation) under heating conditions of a temperature rise time from room temperature to 180°C of 1 minute or more and 65 minutes or less, and a holding time at 180°C of 30 minutes.
[0190] (3) Relationship between Time T1 and Time T2 For each heating condition, a graph was created by superimposing the expansion rate-time curve for the foaming agent and the DSC curve for each adhesive composition from which the foaming agent was removed. Graphs for adhesive composition 1 where the temperature rise times were 5 minutes and 65 minutes are shown in Figures 10(a) and (b), respectively. Graphs for adhesive composition 4 where the temperature rise times were 5 minutes and 65 minutes are shown in Figures 10(a) and (b), respectively. Furthermore, the time T1 at the apex of the peak in the expansion rate-time curve for the foaming agent was determined. Furthermore, the time T2 at the apex of the exothermic peak was determined in the DSC curve for the adhesive composition from which the foaming agent was removed.
[0191] (4) Adhesive Strength Two cold-rolled steel plates SPCC-SD (length 100 mm × width 25 mm × thickness 1.6 mm) were prepared. Spacers (Kapton tape or fluorine tape) were placed on one of the steel plates at 15 mm intervals. The spacer thickness was approximately 370 μm (the thickness of two sheets of Kapton tape P-221 manufactured by Nitto Denko Corporation and one sheet of Fluororesin Adhesive Tape 8410 manufactured by Teraoka Seisakusho Co., Ltd.). A foam adhesive sheet cut to 12.5 mm × 25 mm and with the second separator peeled off was placed between the spacers, and the other steel plate was placed on top and secured with clips to obtain a test specimen. The test specimen was heated from room temperature to 180°C over a period of 1 minute to 65 minutes using an IR heater (handy heating furnace manufactured by Advance Riko Co., Ltd.), and then heated at 180°C for 30 minutes to cure the foam adhesive sheet. After heating, the shear strength (adhesion strength) of the test piece was measured using Tensilon RTF1350 (manufactured by A&D Co., Ltd.) in accordance with JIS K 6850. The pulling speed was 10 mm / min and the temperature was 23°C.
[0192]
[0193] From Tables 2 and 3, it was confirmed that the adhesive strength was improved when the adhesive composition was heated so that A<B and T1<T2 in the bonding step.
[0194] [Evaluation 3] (1) Maximum Foaming Temperature of Foaming Agent Differential scanning calorimetry was performed on the foaming agent at a temperature rise rate of 31°C / min using a differential scanning calorimeter equipped with a camera ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation). The temperature at the apex of the peak in the foaming ratio-time curve for the foaming agent was taken as the maximum foaming temperature. The maximum foaming temperature was 174.5°C.
[0195] (2) Differential Scanning Calorimetry Measurement of the Blowing Agent Differential scanning calorimetry was performed on the blowing agent using a differential scanning calorimeter equipped with a camera ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation) under the heating conditions of a temperature rise time from room temperature to the maximum foaming temperature (174.5°C): 5 minutes, and a holding time at the maximum foaming temperature (174.5°C): 15 minutes.
[0196] (3) Differential Scanning Calorimetry Measurement of Adhesive Compositions Differential scanning calorimetry was performed on the adhesive layers containing the adhesive compositions 1 to 3 used in Production Examples 1 to 3 using a differential scanning calorimeter ("High Sensitivity Differential Scanning Calorimeter DSC7000X" manufactured by Hitachi High-Tech Science Corporation) under the heating conditions of a temperature rise time from room temperature to the maximum foaming temperature (174.5°C): 5 minutes, and a holding time at the maximum foaming temperature (174.5°C): 15 minutes.
[0197] (4) Relationship between Slope C and Slope D Using the method described above in "A. Article Manufacturing Method," the expansion rate-time curve for the foaming agent and the DSC curve for each adhesive composition were superimposed to create a graph. Furthermore, using the method described above in "A. Article Manufacturing Method," the slope C of the tangent line drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak in the expansion rate-time curve for the foaming agent was determined. Furthermore, using the method described above in "A. Article Manufacturing Method," the slope D of the tangent line drawn at the apex of the exothermic peak to the curve on the long-time side of the exothermic peak in the DSC curve for the adhesive layer containing the adhesive composition was determined.
[0198] (5) Adhesion Strength Adhesion strength was measured in the same manner as described in Evaluation 1 above.
[0199] It was confirmed that when C<D, the adhesive strength improved.
[0200] [Evaluation 4] (1) Adhesive Strength The adhesive strength of the foamable adhesive sheet of Production Example 4 was measured using the same method as described in Evaluation 2 above. The foamable adhesive sheet was heated under the following heating conditions: temperature rise time from room temperature to the heating temperature: 15 minutes, heating temperature: 150°C or higher and 200°C or lower, and holding time at the heating temperature: 0 minutes or higher and 120 minutes or lower. The results are shown in Figure 12.
[0201] After measuring the adhesive strength, the cohesive failure rate was calculated. The cohesive failure rate is the ratio of the area of the cohesive failure portion to the total adhesive area. The results are shown in Figure 13.
[0202] 12 and 13 suggest that there is a preferred range for the heating temperature.
[0203] REFERENCE SIGNS LIST 1 adhesive layer 1a first adhesive layer 1b second adhesive layer 2 substrate 10 foamable adhesive sheet 11 foamed and cured adhesive sheet 20a first member 20b second member 100 article
Claims
1. A method for manufacturing an article, comprising: a disposing step of disposing an adhesive composition containing a thermosetting resin and a foaming agent between a first member and a second member; and a bonding step of heating the adhesive composition to foam and harden it, thereby bonding the first member and the second member, wherein the foaming agent is a thermally expandable microcapsule, and when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera under the heating conditions in the bonding step, the foaming agent is measured using a differential scanning calorimeter equipped with a camera under heating conditions in the bonding step. In the expansion rate vs. time curve, the horizontal axis is time and the vertical axis is the expansion rate of the foaming agent. The slope of the tangent line drawn at the apex of the peak to the curve on the long-term side of the peak is A, and when differential scanning calorimetry is performed on the adhesive composition under heating conditions in the bonding step, the DSC curve is measured using a DSC curve with the horizontal axis being time and the vertical axis being heat flow. The slope of the tangent line drawn at the apex of the exothermic peak to the curve on the long-term side of the exothermic peak is B, and A<B. a differential scanning calorimeter equipped with a camera is used to measure the foaming agent, and the expansion rate of the foaming agent is measured on the vertical axis, and the time at the apex of the peak in the expansion rate-time curve is taken as T1; and a composition obtained by removing the foaming agent from the adhesive composition is measured on the DSC curve with time on the horizontal axis and heat flow on the vertical axis, and the time at the apex of the exothermic peak is taken as T2. In the method for manufacturing an article, in the bonding step, the adhesive composition is heated such that T1<T2.
2. The method for manufacturing an article according to claim 1, wherein the heating temperature in the bonding step is within a range of ±20°C of the maximum foaming temperature of the foaming agent.
3. A method for manufacturing an article as described in claim 1 or claim 2, wherein in the placing step, a foamable adhesive sheet having an adhesive layer containing the adhesive composition is used, and the foamable adhesive sheet is placed between the first member and the second member.
4. An adhesive composition containing a thermosetting resin and a foaming agent, wherein the foaming agent is a thermally expandable microcapsule; when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera under heating conditions of heating from room temperature to the maximum foaming temperature of the foaming agent in 5 minutes and maintaining the temperature at the maximum foaming temperature of the foaming agent, the slope of a tangent drawn at the apex of the peak to the curve on the long-term side of the peak in an expansion rate-time curve with time on the horizontal axis and the expansion rate of the foaming agent on the vertical axis is C; when differential scanning calorimetry is performed on the adhesive composition under the heating conditions, the slope of a tangent drawn at the apex of the exothermic peak to the curve on the long-term side of the exothermic peak in a DSC curve with time on the horizontal axis and heat flow on the vertical axis is D, and C<D; when differential scanning calorimetry is performed on the foaming agent using a differential scanning calorimeter equipped with a camera, the time to the apex of the peak in an expansion rate-time curve with time on the horizontal axis and the expansion rate of the foaming agent on the vertical axis is T1; The adhesive composition is used by heating the adhesive composition such that T1 < T2, where T2 is the time to the apex of an exothermic peak in a DSC curve obtained by performing differential scanning calorimetry on a composition obtained by removing the foaming agent from the adhesive composition, the DSC curve having a horizontal axis representing time and a vertical axis representing heat flow.
5. A foamable adhesive sheet having an adhesive layer, wherein the adhesive layer contains the adhesive composition according to claim 4.
Citation Information
Patent Citations
Tacky adhesive layer and tacky adhesive sheet
JP2014065889A
Adhesive sheet
JP2019203062A
Adhesive sheet
JP6223477B2
Manufacturing method of expandable adhesive sheet and article
JP2021155495A
Article manufacturing method, adhesive composition, and foamable adhesive sheet
JP7280986B1