Rare earth magnet
The rare earth magnet with a multilayered hydrogen barrier coating addresses the issue of hydrogen embrittlement by preventing hydrogen permeation, ensuring durability and performance in high-pressure hydrogen environments, thus enhancing hydrogen liquefaction efficiency.
Patent Information
- Application Number
- PCT/JP2024/003280
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-02-01
- Publication Date
- 2024-11-21
AI Technical Summary
Rare earth magnets used in hydrogen liquefaction processes are prone to hydrogen embrittlement due to hydrogen permeation through cracks or pinholes in their coatings, leading to performance deterioration in high-pressure hydrogen environments.
A rare earth magnet with a multilayered film coating covering its entire outer surface, comprising two or more layers of hydrogen barrier materials such as ceramics, metals, or alloys, which effectively inhibits hydrogen gas permeation and prevents contact between hydrogen and the magnet body.
The multilayered film coating significantly enhances the durability of rare earth magnets in hydrogen environments, preventing hydrogen embrittlement and maintaining performance over extended periods, thereby improving the efficiency of hydrogen liquefaction processes.
Smart Images

Figure JP2024003280_21112024_PF_FP_ABST
Abstract
Description
rare earth magnets
[0001] The present disclosure relates to rare earth magnets.
[0002] In recent years, various technologies for efficiently liquefying hydrogen gas have been developed with the aim of utilizing hydrogen as a promising clean energy source. For example, power recovery expansion turbines have been considered for the hydrogen liquefaction process. Power recovery expansion turbines have a mechanism for cooling hydrogen gas by adiabatic expansion and recovering the power generated in this process by driving a generator to generate electricity.
[0003] The power recovery expansion turbine used in the hydrogen liquefaction process is installed in a hydrogen environment. The generator that makes up the power recovery expansion turbine contains rare earth magnets. Rare earth magnets typically pulverize in a hydrogen environment due to hydrogen embrittlement. There is a need to develop rare earth magnets that are durable in a hydrogen environment.
[0004] Non-Patent Document 1 (E. Serra et al., "Hydrogen Permeation Measurements on Alumina," Journal of American Ceramic Society (2004)) discloses ceramics as a material with hydrogen barrier properties. Non-Patent Document 2 (Tsukahara Sonoko, "Metallic Materials and Hydrogen as Viewed as Ultra-High Vacuum Materials," Applied Physics (2000)) describes research into TiN coating of metal parts to suppress hydrogen release from the metal parts in order to improve the degree of vacuum in vacuum equipment.
[0005] Patent Document 1 (JP 2007-116171 A) discloses a method for preventing hydrogen embrittlement of rare earth sintered magnets, in which a metal oxide layer and / or a metal nitride layer is formed on the surface of the rare earth sintered magnet directly or via a metal plating layer. Patent Document 2 (JP 2012-204517 A) discloses a rare earth magnet comprising a magnet body and a protective layer. The magnet body has a surface region containing a specific element such as Si. The protective layer has a first layer containing a metal such as Al or an alloy containing the metal, and a second layer containing nitride.
[0006] Patent Document 3 (JP 2020-102552 A) discloses an RFeB-based sintered magnet. This magnet comprises a sintered body containing rare earth elements and a protective layer of Ni plating covering the surface. The sintered body contains grain boundaries where Cu is present with a concentration gradient that decreases from the surface to the interior.
[0007] JP 2007-116171 A JP 2012-204517 A JP 2020-102552 A
[0008] E. Serra et. al., "Hydrogen Permeation Measurements on Alumina", Journal of American Ceramic Society (2004) Sonoko Tsukahara, "Metallic Materials and Hydrogen as Ultra-High Vacuum Materials", Applied Physics (2000)
[0009] Ceramics have traditionally been known as brittle materials. Therefore, the ceramic coatings proposed in Patent Documents 1 and 2 may develop minute cracks during their manufacture. Patent Document 3 states that the formation of minute pinholes is unavoidable even in metal coatings produced by plating. Hydrogen gas can pass through cracks or pinholes formed in the coating. If cracks or pinholes penetrate the coating, the hydrogen gas that passes through the coating will come into contact with the magnet body. As a result, hydrogen embrittlement occurs in rare earth magnets, and the magnet may not be able to maintain its specified performance.
[0010] In particular, expansion turbines used in hydrogen liquefaction processes are placed in a high-pressure hydrogen environment for long periods of time. If the rare earth magnets disclosed in Patent Documents 1 to 3 are exposed to a hydrogen environment of several MPa for long periods of time, there is concern that their performance will deteriorate due to hydrogen embrittlement. No rare earth magnets have yet been proposed that have excellent hydrogen barrier properties and can be used for long periods of time in a high-pressure hydrogen environment.
[0011] An object of the present disclosure is to provide a rare earth magnet that has excellent durability in a hydrogen environment.
[0012] The rare earth magnet according to the present disclosure comprises a body and a multilayer coating covering the entire outer surface of the body. The body is made of a ferromagnetic material containing a rare earth element. The coating has two or more layers.
[0013] The rare earth magnet according to the present disclosure is provided with a coating that has excellent hydrogen barrier properties. By providing this coating, contact between hydrogen gas and the magnet body can be avoided for long periods of time in high-pressure hydrogen environments. This rare earth magnet has excellent durability in hydrogen environments. A generator including this rare earth magnet can be applied to a power recovery expansion turbine in a hydrogen liquefaction process. Power recovery by this power recovery expansion turbine is expected to improve the production efficiency of liquefied hydrogen.
[0014] Fig. 1 is a cross-sectional view of a rare earth magnet according to an embodiment of the present disclosure. Fig. 2 is a conceptual diagram for explaining the rare earth magnet of the present disclosure. Fig. 3 is a cross-sectional view of the rare earth magnet of Example 1. Fig. 4 is a conceptual diagram for explaining a method for manufacturing the rare earth magnet of Fig. 3. Fig. 5 is a scanning electron microscope image of the cross sections of Example 1 and Comparative Example 2.
[0015] Hereinafter, the present disclosure will be described in detail based on preferred embodiments, with appropriate reference to the drawings. The present disclosure is not limited to the following embodiments, and additions, deletions, and modifications are possible within the scope of the present disclosure. In addition, unless otherwise specified in the present specification, "X to Y" means "X or more and Y or less."
[0016] [Rare Earth Magnet] The rare earth magnet according to the present disclosure comprises a main body and a coating with a multilayer structure. In the present disclosure, the coating has two or more layers. The coating covers the entire outer surface of the main body. The main body is made of a ferromagnetic material containing a rare earth element. In other words, the "main body" is a rare earth magnet without a coating, or a rare earth magnet before the coating is formed.
[0017] When this rare earth magnet is placed in a hydrogen environment, the two or more layers of coating prevent hydrogen gas from passing through. By covering the entire outer surface of the body with two or more layers of coating, contact between hydrogen gas and the body is avoided, preventing deterioration due to hydrogen embrittlement. This rare earth magnet has excellent durability in a hydrogen environment.
[0018] FIG. 1 shows a cross-sectional view of a rare earth magnet 20 according to one embodiment of the present disclosure. This rare earth magnet 20 comprises a main body 24 and a coating 30. The main body 24 is made of a ferromagnetic material containing a rare earth element. This coating 30 has a two-layer structure consisting of a first layer 26 and a second layer 28, and covers the entire outer surface of the main body 24. In other words, the main body 24 is shielded from the outside air by the coating 30 consisting of the first layer 26 and the second layer 28. In this rare earth magnet 20, the outer surface of the main body 24 is not exposed to the outside air.
[0019] 2A and 2B are partially enlarged cross-sectional views (conceptual diagrams) illustrating the manufacturing process of the rare earth magnet 20 of FIG. 1. The configuration and effects of the present disclosure will be explained below using FIG. 2.
[0020] 2(2A) shows a main body 24 and a portion of a first layer 26 that covers the outer surface of the main body 24. As shown in the figure, the first layer 26 contains a plurality of minute cracks 14. It is believed that the cracks 14 in the first layer 26 are generated during the formation of the first layer 26. The cracks 14 may penetrate the first layer 26.
[0021] 2(2B) shows the main body 24, a first layer 26 that covers the outer surface of the main body 24, and a portion of the second layer 28 that covers the outer surface of the first layer 26. As shown in the figure, the second layer 28 also contains a plurality of minute cracks 14. It is believed that the cracks 14 in the second layer 28 are generated during the formation of the second layer 28. The cracks 14 may penetrate the second layer 28.
[0022] In this specification, the term "crack" refers to a defect or void present in the coating immediately after the coating is formed, and there are no particular limitations on the shape of the crack. The presence of cracks in the coating can be confirmed by observation with an optical microscope or an electron microscope.
[0023] As shown in Figure 2 (2B), in this rare earth magnet 20, no cracks 14 in the second layer 28 are located directly below cracks 14 in the first layer 26. In other words, this rare earth magnet 20 does not contain cracks 14 that penetrate the coating 30 from its outer surface toward the main body 24. With this rare earth magnet 20, hydrogen gas that passes through cracks 14 in the first layer 26 is blocked by the second layer 28. With this rare earth magnet 20, contact between the main body 24 and hydrogen gas can be prevented in a hydrogen environment. With this rare earth magnet 20, morphological changes and performance degradation due to hydrogen embrittlement are suppressed even when the magnet is left in a hydrogen environment for an extended period of time.
[0024] With conventionally known film-forming methods and conditions, it is difficult to completely avoid the formation of cracks 14 during film formation. However, the size (surface area) of the first layer 26 and the second layer 28 is typically sufficiently large compared to the size of cracks 14 that form during film formation. Therefore, the probability that a crack 14 in the second layer 28 will be located directly above a crack 14 in the first layer 26 is sufficiently small. With this rare earth magnet 20, the probability that a crack 14 will form that penetrates the coating 30 from its surface toward the main body 24 is low. With this rare earth magnet 20, even if multiple microcracks 14 form during the formation of the first layer 26 or the second layer 28, hydrogen gas can be prevented from permeating the coating 30 and coming into contact with the main body 24. This rare earth magnet maintains its performance for a long period of time in a hydrogen environment.
[0025] [Main Body] The main body may be made of a ferromagnetic material containing a rare earth element, and there are no particular limitations on its shape, size, etc. An appropriate form can be selected and used depending on the application.
[0026] Rare earth elements refer to the lanthanoid group, from lanthanum (atomic number 57) to lutetium (atomic number 71), scandium (atomic number 21), and yttrium (atomic number 39). Intermetallic compounds of these rare earth elements with iron, cobalt, and other iron group elements are known as ferromagnetic materials. Representative examples include neodymium-iron-boron magnets (Nd 2 Fe 14 B, also called "neodymium magnets"), samarium-cobalt magnets (SmCo 5or Sm 2 Co 17 , also called "samarium-cobalt magnets"), praseodymium magnets (PrCo 5 High-performance, low-cost neodymium magnets can be suitably used.
[0027] [Coating] As mentioned above, the coating of the rare earth magnet of the present disclosure has a multi-layer structure. From the viewpoint of effectively blocking the passage of hydrogen gas in a hydrogen environment, the number of layers constituting the coating is at least two, and may be three or more, four or more, five or more, six or more, or 20 or less.
[0028] The number of layers constituting the coating may vary in some areas as long as the effects of the present disclosure are achieved. In other words, in some areas of the outer surface of the body, the number of layers constituting the coating may be 3 or more, 4 or more, 5 or more, 6 or more, or 20 or less. For example, in one embodiment of the present disclosure, the number of layers constituting the coating may be at least 2 over the entire area of the outer surface of the body, and the number of layers constituting the coating may be 3 or more over some areas of the outer surface of the body. In another embodiment, the number of layers constituting the coating may be at least 2 over the entire area of the outer surface of the body, and the number of layers constituting the coating may be 3 or more over some areas of the outer surface of the body, and the number of layers constituting the coating may be 4 or more over other areas of the outer surface of the body.
[0029] The thickness of the coating is not particularly limited as long as the effects of the present disclosure are obtained. Similarly, the thickness of each layer constituting the coating is not particularly limited. For example, the thickness of each layer constituting the coating may be 1 nm or more, 2 nm or more, 3 nm or more, or 5 nm or more, and may be 10 μm or less, 9 μm or less, or 8 μm or less. The average thickness of the entire coating may be 2 nm or more, 3 nm or more, 5 nm or more, or 20 μm or less, or 18 μm or less. The rare earth magnet may have a coating of the same thickness over the entire outer surface of the main body, or a coating of different thicknesses over some areas of the outer surface of the main body. The thickness of the coating and the thickness of each layer constituting the coating can be determined by observation with an optical microscope or an electron microscope.
[0030] The material of the coating may be any material having hydrogen barrier properties, such as ceramics, metals, and alloys. Examples of metals used as the coating material include aluminum (Al), chromium (Cr), titanium (Ti), and zinc (Zn). Two or more metals may be used in combination.
[0031] As the alloy, a titanium alloy (Ti alloy) is preferred, and a titanium alloy with a titanium content of 60% by mass or more is more preferred. The titanium content of the titanium alloy may be 70% by mass or more, 80% by mass or more, or 90% by mass or more. As long as the effects of the present disclosure are obtained, the titanium alloy may contain other elements that are intentionally added or may contain other elements as unavoidable impurities. Examples of other elements contained in the titanium alloy include nickel (Ni), aluminum (Al), V (vanadium), Mo (molybdenum), iron (Fe), palladium (Pd), platinum (Pt), tin (Sn), niobium (Nb), zinc (Zn), and chromium (Cr). Two or more types of alloys may be used in combination.
[0032] In this specification, the term "ceramics" refers to inorganic compounds such as oxides, carbides, nitrides, borides, and fluorides of metal and nonmetal elements, as well as composite compounds thereof. Metal elements constituting ceramics include aluminum (Al), chromium (Cr), erbium (Er), titanium (Ti), tungsten (W), zirconium (Zr), iron (Fe), zinc (Zn), magnesium (Mg), calcium (Ca), niobium (Nb), lead (Pb), lanthanum (La), cerium (Ce), gallium (Ga), hafnium (Hf), neodymium (Nd), manganese (Mn), tantalum (Ta), antimony (Sb), strontium (Sr), tin (Sn), nickel (Ni), and yttrium (Y). Non-metal elements constituting ceramics include silicon (Si), boron (B), and the like.
[0033] The ceramics used as the coating material are Al 2 O 3 , Cr 2 O 3 , Er 2 O 3 , SiO 2 , ZrO 2 , TiO 2 , ZrSiO 4 , MgO, Al 2 O 3 TiO 2 Oxide ceramics such as BN, TiN, TiAlN, SiN, WN, CrWN, CrN, Cr 2 N, AlCrN, ZrN, TaN, AlN, Si 3 N 4 , HfN, NbN and other nitride ceramics, TiC, SiC, ZrC, TaC, HfC, Cr 3 C 2 Carbide ceramics such as CaF 2 , Y.F. 3 , Y 2 O 3 Examples of the ceramic include fluoride ceramics such as F. Two or more ceramics may be used in combination. A ceramic may be used in combination with the above-mentioned metal or alloy.
[0034] The material of the coating may be one or more selected from the group consisting of oxide ceramics, nitride ceramics, carbide ceramics, metals and alloys. 2 O 3 , Cr 2 O 3 , Er 2 O 3 , SiO 2 , BN, TiN, TiAlN, SiN, WN, CrWN, CrN, Cr 2 The material may be one or more selected from the group consisting of N, AlCrN, ZrN, TiC, Al, Cr, Zn, Ti, and a Ti alloy. Furthermore, the materials of the two or more layers constituting the coating may be the same or different, as long as the effects of the present disclosure can be obtained.
[0035] The method for coating the outer surface of the main body with a coating is not particularly limited, and known methods such as physical vapor deposition (PVD), chemical vapor deposition (CVD), and thermal spraying can be appropriately selected and used. Examples of physical vapor deposition (PVD) include vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition (CVD) include thermal CVD, plasma CVD, and photo CVD. Examples of thermal spraying include flame spraying, high-velocity flame spraying, detonation spraying, electric spraying, and cold spray. Depending on the materials of the coating and the main body, electrolytic or electroless plating methods may also be used.
[0036] Below, as an example, a method for forming a film using a sputtering device will be described. The sputtering device is equipped with a vacuum chamber. A workpiece and a target are placed in the vacuum chamber, and a small amount of inert gas (e.g., argon gas) is introduced. The inert gas is converted into plasma and collides with the target. This collision causes components of the target to be ejected at the molecular level, which then adhere and deposit on the workpiece placed opposite the target. This adhesion and deposition forms a layer made of the components of the target on the surface of the workpiece. Note that, in the present disclosure, regardless of the manufacturing method, it is sufficient that the film is formed to cover the entire outer surface of the body, and the device and conditions can be selected according to the materials of the body and the film.
[0037] 4A-4F show an example of a method for manufacturing a rare earth magnet according to the present disclosure. In (4A)-(4F), the top-to-bottom direction of the page is the vertical direction, and the left-to-right direction of the page is the horizontal direction. In (4A)-(4F), reference numeral 16 denotes a holder for holding the workpiece in the vacuum chamber of the sputtering device.
[0038] As shown in FIG. 4 (4A), in this manufacturing method, first, a main body 4 made of a ferromagnetic material containing a rare earth element is prepared and placed on a holder 16. A target is disposed in a vacuum chamber facing the main body 4. The target contains the constituent components of the coating described above. The target material may be, for example, one or more selected from the group consisting of oxide ceramics, nitride ceramics, carbide ceramics, metals, and alloys. Sputtering is performed using this target to form a first layer 6 that coats the outer surface of the main body 4 and constitutes the coating 40 (4B). Subsequently, sputtering is performed using the same target or a target of a different material to form a second layer 8 that coats the outer surface of the first layer 6 and constitutes the coating 40 (4C).
[0039] 4B and 4C, the first layer 6 and the second layer 8 are formed in the area where the main body 4 is not in contact with the holding portion 16, and are not formed in the area where the main body 4 is in contact with the holding portion 16. In other words, the outer surface of the main body 4 is composed of an area covered with the two-layer coating 40 consisting of the first layer 6 and the second layer 8, and an area not covered with the coating 40.
[0040] Next, the main body 4 including the first layer 6 and the second layer 8 is turned upside down and placed on the holder 16 so that the area not covered with the coating 40 faces up (4D). Note that in other embodiments, it is not necessary to turn the main body 4 upside down, and it is sufficient to change the position where it comes into contact with the holder 16 and move it so that the area not covered with the coating 40 is exposed.
[0041] After the body 4 including the first layer 6 and the second layer 8 is turned upside down, sputtering is performed using the same target or a target of a different material to form a third layer 10 that coats the outer surface of the second layer 8 and a portion of the outer surface of the body 4 and constitutes the coating 40 (4E). Subsequently, sputtering is performed using the same target or a target of a different material to form a fourth layer 12 that coats the outer surface of the third layer 10 and constitutes the coating 40 (4F).
[0042] 4E and 4F, the third layer 10 and the fourth layer 12 are formed in the region where the second layer 8 is not in contact with the retaining portion 16, and are not formed in the region where the second layer 8 is in contact with the retaining portion 16. According to this manufacturing method, the regions of the main body 4 that are not covered with the first layer 6 and the second layer 8 are covered with the third layer 10 and the fourth layer 12. As a result, the entire outer surface of the main body 4 is covered with two or more layers of the coating 40. In other words, the outer surface of the main body 4 is composed of a region covered with the four-layer coating 40 consisting of the first layer 6, the second layer 8, the third layer 10, and the fourth layer 12, and a region covered with the two-layer coating 40 consisting of the third layer 10 and the fourth layer 12.
[0043] The method for manufacturing a rare earth magnet in this embodiment includes placing the main body 4 on the holder 16 (4A), sputtering to form the first layer 6 and the second layer 8 on the outer surface of the main body 4 (excluding the area in contact with the holder 16) ((4B) and (4C)), moving the main body 4 coated with the first layer 6 and the second layer 8 so that the outer surface of the second layer 8 contacts the holder 16 (4D), and sputtering to form the third layer 10 and the fourth layer 12 on the outer surface of the second layer 8 (excluding the area in contact with the holder 16) ((4E) and (4F)). A cross-sectional view of a rare earth magnet 2 obtained by this manufacturing method is shown in Figure 3.
[0044] 3, the rare earth magnet 2 comprises a main body 4 made of a ferromagnetic material containing rare earth elements, and a coating 40 with a multilayer structure (two or four layers) that covers the entire outer surface of the main body 4. The coating 40 includes a first layer 6, a second layer 8, a third layer 10, and a fourth layer 12, each made of a material with hydrogen gas barrier properties. The first layer 6, the second layer 8, the third layer 10, and the fourth layer 12 each inhibit the permeation of hydrogen gas.
[0045] The first layer 6, second layer 8, third layer 10, and fourth layer 12 may each contain multiple fine cracks generated during sputtering. These cracks may penetrate each layer of the coating 40. However, as mentioned above, the probability that cracks in each layer will penetrate all of the layers that make up the coating 40 is considered to be quite small. In this rare earth magnet 2, hydrogen gas that passes through cracks in the outermost fourth layer 12 is blocked by the third layer 10 inside and does not reach the main body 4. In this rare earth magnet 2, the coating 40 has a multilayer structure of two or more layers, which effectively prevents hydrogen gas from passing through. This rare earth magnet 2 has high hydrogen barrier properties.
[0046] The hydrogen barrier performance of the rare earth magnet of the present disclosure can be confirmed by a hydrogen exposure test, described below. In this test, a rare earth magnet equipped with a multilayer coating is exposed to high-pressure (e.g., 1 MPa to 100 MPa) hydrogen gas, and morphological changes are observed after a long period of time (e.g., 1,000 hours or more). The rare earth magnet of the present disclosure shows no change in appearance even after 1,000 hours of exposure to 4 MPa hydrogen gas at room temperature. This result indicates that the coating prevents contact between the hydrogen gas and the magnet body, preventing hydrogen embrittlement of the magnet body. Instead of observing the morphology after hydrogen exposure, the hydrogen barrier performance of the rare earth magnet may also be evaluated by measuring magnetic properties such as coercivity.
[0047] As such, the rare earth magnet disclosed herein has excellent durability in a hydrogen environment. Even when placed in a hydrogen environment for a long period of time, hydrogen gas does not reach the magnet's body, preventing morphological changes due to hydrogen embrittlement. A generator using this rare earth magnet can be used for a long period of time in a high-pressure hydrogen environment. Applying an expansion turbine including this generator to a power recovery expansion turbine in a hydrogen liquefaction process improves the efficiency of hydrogen liquefaction.
[0048] The effects of the present disclosure will be clarified below by examples, but the present disclosure should not be interpreted as being limited based on the description of these examples.
[0049] [Example 1] A rare earth magnet of Example 1 was manufactured according to the manufacturing process shown in Figure 4. Specifically, a neodymium magnet (4) was first prepared as the main body. This neodymium magnet (4) was placed in the holder (16) of a sputtering device, and Cr 2 By sputtering N, a first layer (6) having a thickness of 2 to 3 μm was obtained. It was visually confirmed that the first layer (6) was formed on the entire surface of the main body except for the contact area between the main body (4) and the holding part (16). Subsequently, Cr 2 A second layer (8) having a thickness of 2 to 3 μm was obtained by sputtering N. It was visually confirmed that the second layer (8) was formed on the entire surface except for the contact area between the main body (4) and the holding part (16).
[0050] Next, the body (4) on which the first layer (6) and the second layer (8) were formed was removed from the sputtering device and placed again on the holder (16) at a position where the area on which the first layer (6) and the second layer (8) were formed was in contact with the holder (16). Thereafter, Cr was deposited on the body (4) in the same manner as the first layer (6) and the second layer (8). 2N was sputtered to form a third layer (10) and a fourth layer (12), each 2 to 3 μm thick, to obtain the rare earth magnet of Example 1 equipped with a coating (40). A conceptual diagram of a cross section of this rare earth magnet (2) is shown in FIG. 3. A scanning electron microscope (SEM) image of the cross section of this rare earth magnet (2) is shown in FIG. 5. The photograph shown in the "Contrast Enhancement" column in FIG. 5 is an image of raw data processed to clearly show cracks. As shown in FIG. 5, in Example 1, cracks were visible near the main body, but they did not reach the surface of the coating, and it was confirmed that no cracks penetrated the coating.
[0051] [Example 2] Cr 2 A rare earth magnet of Example 2 was obtained in the same manner as in Example 1, except that N was replaced with Ti (pure titanium).
[0052] Comparative Example 1 The neodymium magnet prepared in Example 1 was prepared as is as Comparative Example 1. The rare earth magnet of Comparative Example 1 was not provided with a coating.
[0053] Comparative Example 2 The entire surface of the neodymium magnet prepared in Example 1 was covered with one layer of Cr. 2 The rare earth magnet of Comparative Example 2 was obtained by coating the magnet with a N coating. A scanning electron microscope (SEM) image of the cross section of the rare earth magnet of Comparative Example 2 is shown in Figure 5. The photograph shown in the "Contrast Enhancement" column in Figure 5 was obtained by image processing of raw data to clearly show cracks. As shown in Figure 5, it was confirmed that the rare earth magnet of Comparative Example 2 contained cracks that penetrated the coating.
[0054] [Hydrogen Exposure Test] The rare earth magnets of the Examples and Comparative Examples were evaluated for durability in a hydrogen environment. Specifically, each rare earth magnet was stored in a hydrogen gas environment (4 MPa pressure, room temperature) for 1,000 hours, and then its appearance was observed with the naked eye. In Comparative Example 1, which had no coating, and Comparative Example 2, which had a single coating, damage was observed and the magnets were pulverized within 168 hours. In contrast, the rare earth magnets of Examples 1 and 2, in which the entire surface of the magnet body was covered with at least two layers of coating, showed no change in appearance even after 1,000 hours of storage, indicating their long-term usability in a hydrogen gas environment.
[0055]
[0056] Disclosed Items Each of the following items discloses a preferred embodiment.
[0057] [Item 1] A rare earth magnet comprising a main body and a multilayer coating covering the entire outer surface of the main body, wherein the main body is made of a ferromagnetic material containing a rare earth element, and the coating has two or more layers.
[0058] [Item 2] A rare earth magnet according to item 1, wherein the number of layers forming the coating in a partial region of the outer surface of the main body is three or more.
[0059] [Item 3] A rare earth magnet according to item 1, wherein the number of layers forming the coating in a partial region of the outer surface of the main body is four or more.
[0060] [Item 4] The rare earth magnet according to any one of Items 1 to 3, wherein the material of the coating is one or more selected from the group consisting of oxide ceramics, nitride ceramics, carbide ceramics, metals, and alloys.
[0061] [Item 5] The material of the coating is Al 2 O 3 , Cr 2 O 3 , Er 2 O 3 , SiO 2 , BN, TiN, TiAlN, SiN, WN, CrWN, CrN, Cr 2 5. The rare earth magnet according to any one of items 1 to 4, wherein the rare earth magnet is one or more selected from the group consisting of N, AlCrN, ZrN, TiC, Al, Cr, Zn, Ti, and Ti alloys.
[0062] [Item 6] The rare earth magnet according to Item 5, wherein the Ti alloy has a Ti content of 60 mass % or more.
[0063] [Item 7] A rare earth magnet according to any one of items 1 to 6, wherein the thickness of each layer constituting the coating is 1 nm or more and 10 μm or less.
[0064] [Item 8] The rare earth magnet according to any one of Items 1 to 7, wherein the coating includes layers made of different materials.
[0065] [Item 9] A rare earth magnet according to any one of items 1 to 8, which does not contain cracks that penetrate the coating from its outer surface toward the main body.
[0066] The rare earth magnets described above can be used in a variety of applications that require durability in a hydrogen environment.
[0067] 2, 20... Rare earth magnet 4, 24... Main body 6, 26... First layer 8, 28... Second layer 10... Third layer 12... Fourth layer 30, 40... Coating 14... Crack 16... Holding portion
Claims
1. A rare earth magnet comprising a body and a multi-layer coating covering the entire outer surface of the body, the body being made of a ferromagnetic material containing rare earth elements, and the coating having two or more layers.
2. A rare earth magnet as set forth in claim 1, wherein the number of layers constituting the coating in a partial area of the outer surface of the body is three or more.
3. A rare earth magnet as set forth in claim 1, wherein the number of layers constituting the coating in a partial area of the outer surface of the body is four or more.
4. The rare earth magnet according to claim 1, wherein the material of said coating is one or more selected from the group consisting of oxide ceramics, nitride ceramics, carbide ceramics, metals and alloys.
5. The material of the above coating is Al 2 O 3 , Cr 2 O 3 , Er 2 O 3 , SiO 2 , BN, TiN, TiAlN, SiN, WN, CrWN, CrN, Cr 2 2. The rare earth magnet according to claim 1, wherein the metal is one or more selected from the group consisting of N, AlCrN, ZrN, TiC, Al, Cr, Zn, Ti, and Ti alloys.
6. The rare earth magnet according to claim 5, wherein the Ti alloy has a Ti content of 60 mass % or more.
7. The rare earth magnet according to claim 1, wherein the thickness of each layer constituting said coating is from 1 nm to 10 μm.
8. The rare earth magnet of claim 1, wherein said coating comprises layers of different materials.
9. A rare earth magnet as defined in claim 1, which is free of cracks extending through said coating from its outer surface toward said body.
Citation Information
Patent Citations
Rare earth magnet manufacturing method
JP2005210095A
Rare earth magnet and method for producing same
WO2007077809A1