Nonwoven fabric, method for producing same, laminated nonwoven fabric, and sanitary material
The development of a nonwoven fabric with specific propylene and isotactic pentad fractions, and molecular orientation parameters, addresses the challenge of achieving mechanical properties and flexibility in polypropylene-based sanitary materials, resulting in a fabric suitable for disposable diapers.
Patent Information
- Application Number
- PCT/JP2024/016196
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-21
AI Technical Summary
Existing nonwoven fabrics made from polypropylene resin for sanitary materials face challenges in achieving both excellent mechanical properties and flexibility, with previous technologies failing to provide sufficient strength and adhesion while maintaining flexibility.
A nonwoven fabric composed of composite fibers with a propylene fraction of 98.5-100%, isotactic pentad fraction of 90-100%, and specific molecular orientation parameters, along with a melting point of 130-155°C, is developed, utilizing a metallocene-catalyzed polypropylene resin to enhance fiber strength and adhesion.
The resulting nonwoven fabric exhibits both excellent mechanical properties and flexibility, making it suitable for sanitary materials like disposable diaper backsheets, with improved thermal bonding and texture.
Smart Images

Figure JP2024016196_21112024_PF_FP_ABST
Abstract
Description
Nonwoven fabric, its manufacturing method, laminated nonwoven fabric, and sanitary material
[0001] The present invention relates to a nonwoven fabric, a method for producing the same, a laminated nonwoven fabric, and a sanitary material.
[0002] Spunbond nonwoven fabrics made of polyolefin resins, particularly nonwoven fabrics made of polypropylene resins, are low cost and have excellent processability and flexibility, and are therefore widely used primarily for sanitary material applications.
[0003] In recent years, in order to reduce the amount of petroleum-derived polymers used in sanitary material applications, there has been a demand for a reduction in the basis weight of nonwoven fabrics made from polypropylene-based resins, which are used in sanitary material applications, while at the same time, there is a demand for the fabrics to exhibit the same mechanical properties and flexibility as current products, even when the basis weight is reduced.
[0004] As a nonwoven fabric that combines mechanical properties and flexibility, for example, Patent Document 1 proposes a nonwoven fabric containing thermally adhesive fibers in which a fiber-forming resin containing an ethylene-propylene copolymer is exposed on at least a portion of the fiber surface, the fiber-forming resin containing an ethylene-propylene copolymer having an ethylene content within a specific range and having a certain amount of eluted components at 40°C, a certain proportion of ethylene components in the eluted components, and a certain weight-average molecular weight of the eluted components, as measured by temperature-rising elution fractionation. This invention also discloses that the nonwoven fabric has excellent low-temperature adhesiveness and is soft and not sticky to the touch.
[0005] Patent Document 2 proposes a nonwoven fabric made of fibers containing polypropylene that has an isotactic pentad fraction, a syndiotactic pentad fraction, heterogeneous bonds, a weight average molecular weight, and a polydispersity index (Mw / Mn) within specific ranges and that is confirmed to have no terminal double bonds.The invention also describes that the nonwoven fabric has excellent flexibility and strength.
[0006] Patent Document 3 proposes a thermally adhesive conjugate fiber having a core component of crystalline polypropylene and a sheath component of polyolefin having a lower melting point than the core component, and wherein the ratio of the weight average molecular weight of the core component to the weight average molecular weight of the sheath component (core component Mw / sheath component Mw) is equal to or less than a certain level. This invention also describes that a nonwoven fabric made from this fiber has high puncture strength.
[0007] Patent Document 4 proposes a fiber assembly made of thermally adhesive fibers having a first core component made of highly crystalline polypropylene with a wide molecular weight distribution and a small amount of low molecular weight components, and a second sheath component made of a resin with a melting point lower than that of the first component. This invention also describes that the fiber assembly has extremely small thermal shrinkage during thermal bonding and can be easily processed into a nonwoven fabric with good texture.
[0008] Patent Document 5 proposes a nonwoven fabric for use as a recessed portion of a mechanical fastener, which is made of constituent fibers including heat-fusible conjugate fibers having a core / sheath structure in which the sheath component has a lower melting point, the melting points of the core component and the sheath component being within a specific range, and the fusion point strength and content of the heat-fusible conjugate fibers being above a certain level. According to this invention, it is stated that this nonwoven fabric has excellent fusion point strength, peel strength, and fuzz resistance.
[0009] Patent Document 6 proposes a nonwoven fabric in which the crystallite size of the polyolefin fiber and the bending stiffness of the nonwoven fabric are within a certain range. It is also described that this nonwoven fabric has high processability while maintaining excellent flexibility.
[0010] Patent Document 7 proposes a spunbond nonwoven fabric containing a polypropylene resin having a crystallization temperature, molecular weight distribution (Mw / Mn), and melt flow rate within specific ranges, and describes that this invention provides a spunbond nonwoven fabric with good water resistance and tensile strength.
[0011] JP 2003-171825 A, International Publication No. 1998 / 23799, JP 2007-107143 A, JP 5-9809 A, JP 2002-233404 A, JP 2012-21260 A, JP 2018-168509 A
[0012] The technology proposed in Patent Document 1 allows for thermal bonding at low temperatures and produces a flexible nonwoven fabric, but the strength of the individual fibers is insufficient, and as a result, there is a problem in that it is not possible to produce a nonwoven fabric that exhibits sufficient mechanical properties.
[0013] The technology proposed in Patent Document 2 makes it possible to obtain a nonwoven fabric that takes advantage of the inherent lightness and flexibility of polypropylene fibers and has improved heat resistance, but there are still issues with the mechanical properties of the nonwoven fabric.
[0014] Although the technique proposed in Patent Document 3 can produce a nonwoven fabric having a certain level of puncture strength, there are still problems with the mechanical properties of the nonwoven fabric.
[0015] Although the technique proposed in Patent Document 4 can produce a nonwoven fabric with good texture, there are still problems with the mechanical properties of the nonwoven fabric.
[0016] In the technology proposed in Patent Document 5, the constituent fibers are sheath-core composite fibers, and thus a nonwoven fabric having excellent strength at the fusion points can be obtained. However, the strength of the fibers alone is insufficient, and as a result, there is a problem in that a nonwoven fabric exhibiting sufficient mechanical properties cannot be obtained.
[0017] The technology proposed in Patent Document 6 suppresses molecular movement by using a large crystallite size, and produces a processable nonwoven fabric while maintaining flexibility to a certain extent. However, there are still issues with the mechanical properties of the nonwoven fabric.
[0018] Although the technique proposed in Patent Document 7 can produce a nonwoven fabric having a certain tensile strength, there are still problems with the mechanical properties of the nonwoven fabric.
[0019] Therefore, an object of the present invention is to provide a nonwoven fabric that combines excellent flexibility and mechanical properties, a method for producing the same, a laminated nonwoven fabric, and a sanitary material.
[0020] As a result of further investigations, the present inventors have found that in order for a nonwoven fabric to exhibit excellent mechanical properties, it is important that the constituent fibers exhibit excellent mechanical properties and that the fibers are sufficiently bonded to each other at the fused portions. However, it was found that simply using composite fibers as the fibers constituting the nonwoven fabric in order to achieve sufficient bonding would result in insufficient fiber strength and would make it impossible to obtain a nonwoven fabric with excellent mechanical properties. Therefore, as a result of further intensive investigations, it was found that a nonwoven fabric with excellent mechanical properties can be obtained by using composite fibers having a propylene fraction and an isotactic pentad fraction of at least a certain level and a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S The difference between C -O S ) is within a specific range, and further, the melting point of the nonwoven fabric is within a specific range, the nonwoven fabric has both excellent mechanical properties and flexibility, and the present invention has been completed based on this finding.
[0021] The present invention aims to solve the above problems, and provides the following inventions.
[0022] [1] A nonwoven fabric made of conjugated fibers containing a polypropylene-based resin as a main component, wherein the conjugated fibers have a propylene fraction of 98.5% or more and 100.0% or less, an isotactic pentad fraction of 90.0% or more and 100.0% or less, and a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S The difference between C -O S ) is 0.2 or more and 4.0 or less, and the melting point of the nonwoven fabric is 130°C or more and 155°C or less.
[0023] [2] The nonwoven fabric according to [1], wherein the heat of crystalline fusion of the nonwoven fabric is 82 J / g or more and 120 J / g or less.
[0024] [3] A molecular orientation parameter O in the fiber axis direction at the center of the fiber C The nonwoven fabric according to [1] or [2], wherein the tensile strength is 5.0 or more and 10.0 or less.
[0025] [4] The nonwoven fabric according to any one of [1] to [3], wherein the nonwoven fabric is a spunbonded nonwoven fabric.
[0026] [5] The nonwoven fabric according to any one of [1] to [4], wherein the nonwoven fabric has fused portions and non-fused portions, the fused portions have a crystallite size of (040) plane in wide-angle X-ray diffraction of 10.0 nm or more and 13.5 nm or less, and the non-fused portions have a crystallite size of (110) plane in wide-angle X-ray diffraction of 5.0 nm or more and 10.0 nm or less.
[0027] [6] A method for producing a nonwoven fabric according to any one of [1] to [5] above, comprising the steps of: melt-extruding, through a conjugate spinneret, polypropylene-based resin A which has a propylene fraction of 98.5% to 100.0% and which has been polymerized using a metallocene catalyst; and polypropylene-based resin B which has a propylene fraction of 98.5% to 100.0% and which has a melt flow rate higher than that of polypropylene-based resin A by 6 g / 10 min to 200 g / 10 min, and which has been polymerized using a metallocene catalyst; and pulling and stretching the spun polypropylene-based resin A and polypropylene-based resin B to form islands-in-sea composite fibers having island components made of polypropylene-based resin A and a sea component made of polypropylene-based resin B; depositing the islands-in-sea composite fibers to form a fiber web made of the islands-in-sea composite fibers; and thermally bonding the fiber web.
[0028] [7] The method for producing a nonwoven fabric according to [6], wherein the polypropylene resin A has a melt flow rate of 10 g / 10 min or more and 90 g / 10 min or less.
[0029] [8] The method for producing a nonwoven fabric according to [6] or [7], wherein the polypropylene-based resin A and / or the polypropylene-based resin B has an isotactic pentad fraction of 90.0% or more and 100.0% or less.
[0030] [9] The method for producing a nonwoven fabric according to any one of [6] to [8], wherein the number of islands in the islands-in-sea type composite fiber is 1 or more and 10 or less.
[0031]
[10] The method for producing a nonwoven fabric according to any one of [6] to [9], wherein the polypropylene resin A has a polydispersity (Mw / Mn) of 1.5 or more and 3.5 or less in molecular weight measurement.
[0032]
[11] A sanitary material using the nonwoven fabric according to any one of [1] to [5] above.
[0033]
[12] A laminated nonwoven fabric having a layer of the nonwoven fabric according to any one of [1] to [5] above and a fiber layer different from the layer of the nonwoven fabric.
[0034]
[13] A sanitary material using the laminated nonwoven fabric according to
[12] above.
[0035] The present invention provides a nonwoven fabric that combines excellent flexibility and mechanical properties, a method for producing the same, a laminated nonwoven fabric, and a sanitary material. Due to its properties, the nonwoven fabric of the present invention is suitable for use in sanitary materials, particularly in backsheets for disposable diapers.
[0036] FIG. 1 is a diagram illustrating the measurement points for the crystallite size of the (040) plane in the fused portion of the nonwoven fabric of the present invention in wide-angle X-ray diffraction, and the crystallite size of the (110) plane in the non-fused portion in wide-angle X-ray diffraction.
[0037] The nonwoven fabric of the present invention is a nonwoven fabric composed of conjugated fibers containing a polypropylene-based resin as a main component, and the conjugated fibers have a propylene fraction of 98.5% or more and 100.0% or less, an isotactic pentad fraction of 90.0% or more and 100.0% or less, and a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S The difference between C -O S ) is 0.2 or more and 4.0 or less, and the melting point of the nonwoven fabric is 130°C or more and 155°C or less.
[0038] The nonwoven fabric of the present invention will be described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the present invention, and various modifications are possible within the scope of the present invention.
[0039] [Polypropylene-based resin] The nonwoven fabric of the present invention is composed of conjugated fibers containing a polypropylene-based resin as a main component. By using a polypropylene-based resin, a low-cost nonwoven fabric with excellent flexibility can be obtained.
[0040] The polypropylene resin used in the present invention may be a propylene homopolymer, a copolymer of propylene and ethylene, or a copolymer of propylene and various α-olefins, etc. Here, α-olefin refers to a hydrocarbon having a double bond at the α-position, such as 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, or 4-methyl-1-pentene.
[0041] The polypropylene resin used in the present invention preferably has a propylene fraction of 98.5% or more and 100.0% or less. When the propylene fraction of the polypropylene resin is preferably 98.5% or more, more preferably 98.8% or more, and even more preferably 99.0% or more, the tensile strength of the composite fiber is increased, resulting in a nonwoven fabric with excellent mechanical properties. Furthermore, the upper limit of the propylene fraction of the polypropylene resin that can be achieved in the present invention is 100.0%.
[0042] The propylene fraction (%) of the polypropylene resin referred to here is a value measured and calculated by the following procedure: (1) Weigh the polypropylene resin that is the raw material for the composite fiber, and 4 (orthodichlorobenzene in which hydrogen has been replaced with deuterium) is added to a sample concentration of 8 mass / v%, and the mixture is heated to 135°C. (2) The obtained solution is analyzed using a nuclear magnetic resonance apparatus (for example, "ECZ-600" manufactured by JEOL RESONANCE). 13C-NMR measurement is performed, and the peak area due to propylene units and the peak areas due to ethylene units and α-olefin units are calculated from the NMR spectrum. (3) Sum A of the peak areas due to propylene units, ethylene units, and α-olefin units AP Peak area A due to propylene units PP The ratio (A PP / A AP (4) Measurements are taken three times for each level, and the arithmetic mean value is rounded to one decimal place to calculate the propylene fraction (%) of the polypropylene resin.
[0043] The propylene fraction of the polypropylene-based resin used in the present invention can be controlled, for example, by the composition of the raw material monomers. Specifically, the propylene fraction of the polypropylene-based resin can be increased by increasing the propylene ratio of the raw material monomers used in polymerization of the polypropylene-based resin.
[0044] The polypropylene resin used in the present invention preferably has an isotactic pentad fraction of 90.0% or more and 100.0% or less. When the isotactic pentad fraction of the polypropylene resin is preferably 90.0% or more, more preferably 92.0% or more, and even more preferably 94.0% or more, the heat of crystalline fusion increases when the polypropylene resin is made into fibers, resulting in high tensile strength of the composite fiber and a nonwoven fabric with excellent mechanical properties. Furthermore, the upper limit of the isotactic pentad fraction of the polypropylene resin that can be achieved in the present invention is 100.0%.
[0045] The isotactic pentad fraction (%) of the polypropylene resin referred to here is a value measured and calculated by the following procedure: (1) Weigh the polypropylene resin that is the raw material for the composite fiber, and add o-dichlorobenzene-d 4 (orthodichlorobenzene in which hydrogen has been replaced with deuterium) is added to a sample concentration of 8 mass / v%, and the mixture is heated to 135°C. (2) The obtained solution is analyzed using a nuclear magnetic resonance apparatus (for example, "ECZ-600" manufactured by JEOL RESONANCE). 13(3) Based on the method described in "Zambelli et al., Macromolecules, Vol. 8, p. 687 (1975)", the peaks in the obtained NMR spectrum derived from methyl groups are assigned, and the sum of the intensities of all peaks derived from methyl groups, S AP The peak intensity S due to the mesopentad sequence MP The ratio (S MP / S AP (4) Measurements are carried out three times for each level, and the arithmetic mean value is rounded off to one decimal place to calculate the isotactic pentad fraction (%) of the polypropylene resin.
[0046] The isotactic pentad fraction of the polypropylene resin used in the present invention can be controlled, for example, by a polymerization catalyst. To increase the isotactic pentad fraction of the polypropylene resin, a conventionally known Ziegler-Natta catalyst or a metallocene catalyst having a cyclopentadienyl skeleton is usually used as a polymerization catalyst. However, since the polypropylene resin produced with a Ziegler-Natta catalyst has a high melting point (160°C to 170°C), it is preferable to use a metallocene catalyst having a cyclopentadienyl skeleton.
[0047] The polypropylene resin used in the present invention preferably has a melt flow rate (MFR) of 10 g / 10 min or more and 1000 g / 10 min or less. By setting the MFR of the polypropylene resin to preferably 10 g / 10 min or more, more preferably 15 g / 10 min or more, and even more preferably 20 g / 10 min or more, the stability during spinning is improved, resulting in a nonwoven fabric with a uniform texture. Furthermore, by setting the MFR of the polypropylene resin to preferably 1000 g / 10 min or less, more preferably 500 g / 10 min or less, and even more preferably 300 g / 10 min or less, the tensile strength of the composite fiber is increased and the bonded joints are less likely to break, resulting in a nonwoven fabric with excellent mechanical properties.
[0048] The MFR (g / 10 min) of a polypropylene-based resin referred to here is a value measured and calculated according to the following procedure in accordance with ASTM D1238 (Method A). This standard stipulates that polypropylene-based resins be measured under a load of 2.16 kg and at a temperature of 230°C. (1) 20 g of the polypropylene-based resin used as the raw material for the composite fiber is sampled. (2) The sampled polypropylene-based resin is placed in a melt flow rate measuring device (e.g., the "MELT INDEXER F-F01" manufactured by Toyo Seiki Seisakusho Co., Ltd.) heated to 230°C, and measurement is performed under conditions of a load of 2.16 kg and a temperature of 230°C. (3) Five measurements are performed per level, and the arithmetic mean value is rounded to the nearest tenth to calculate the MFR (g / 10 min) of the polypropylene-based resin.
[0049] The MFR of the polypropylene resin used in the present invention can be controlled, for example, by the molecular weight and polydispersity (Mw / Mn) of the polypropylene resin. Specifically, the MFR of the polypropylene resin can be reduced by increasing the molecular weight and decreasing the polydispersity (Mw / Mn) of the polypropylene resin.
[0050] The polypropylene resin used in the present invention preferably has a polydispersity (Mw / Mn) of 1.5 or more and 3.5 or less. When the polydispersity (Mw / Mn) of the polypropylene resin is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, the molecular orientation is not excessively high, resulting in a nonwoven fabric with excellent flexibility. Furthermore, when the polydispersity (Mw / Mn) is preferably 3.5 or less, more preferably 3.2 or less, and even more preferably 3.0 or less, the molecular orientation parameter of the resulting composite fiber is high even at the same spinning speed, resulting in high composite fiber strength and a nonwoven fabric with excellent mechanical properties.
[0051] The polydispersity (Mw / Mn) of the polypropylene-based resin referred to here is a value measured and calculated by the following procedure. (1) 5 mg of polypropylene-based resin, which is the raw material for the composite fiber, is collected. (2) 5 mL of 1,2,4-trichlorobenzene is added to the collected 5 mg of polypropylene-based resin, and the mixture is heated at 165°C for 20 minutes to dissolve the polypropylene-based resin, thereby obtaining a polypropylene-based resin solution. (3) The obtained polypropylene-based resin solution is filtered using a PTFE filter (e.g., "T010A (pore size: 0.45 μm)" manufactured by Advantec Toyo Co., Ltd.) to prepare a sample solution. (4) The prepared sample solution is loaded into a high-temperature GPC apparatus (e.g., "PL-220" manufactured by Polymer Laboratories, etc.), and measurement is performed at a column temperature of 145°C. The weight-average molecular weight Mw, number-average molecular weight Mn, and polydispersity (Mw / Mn) are calculated by analyzing the GPC discharge curve. (5) Measurements are carried out three times for each level, and the arithmetic mean value is rounded off to one decimal place to calculate the polydispersity (Mw / Mn) of the polypropylene resin.
[0052] The polydispersity (Mw / Mn) of the polypropylene resin used in the present invention can be controlled, for example, by a polymerization catalyst. Specifically, the polydispersity (Mw / Mn) of the polypropylene resin can be reduced by using a metallocene catalyst.
[0053] The polypropylene-based resin used in the present invention can be blended with other component resins as long as the effects of the present invention are not impaired. In other words, as long as the effects of the present invention are not impaired, the polypropylene-based resin according to the present invention may be a resin obtained by blending at least one resin selected from a propylene homopolymer, a copolymer of propylene and ethylene, and a copolymer of propylene and the above-mentioned α-olefin with the other component resin. Examples of the other component resin include polyolefin-based resins such as polyethylene and poly-4-methyl-1-pentene, which have a melting point close to that of polypropylene (note that, as in the example of the above-mentioned "polypropylene-based resin," "polyolefin-based resin" refers to a resin in which the molar fraction of the polyolefin unit in the repeating units is 80 mol % or more and 100 mol % or less. Unless otherwise specified, the same applies to "...-based resin"). In addition, polyester-based resins with a melting point close to that of polypropylene and polyamide-based resins with a melting point close to that of polypropylene are preferred from the viewpoint of imparting flexibility. Suitable low-crystalline polyolefin resins include, for example, ethylene-propylene copolymers and low stereoregular polypropylenes (polypropylenes with an isotactic pentad fraction of 0.60 or less). In this case, the upper limit of the mass ratio of the other component resins is preferably 20% by mass or less, more preferably 10% by mass or less, in order to fully exhibit the properties of the polypropylene resin.
[0054] To the polypropylene-based resin used in the present invention, additives such as commonly used antioxidants, weathering stabilizers, light resistance stabilizers, heat resistance stabilizers, antistatic agents, antistatic aids, spinning agents, antiblocking agents, lubricants including polyethylene wax, crystal nucleating agents, and pigments, or other polymers may be added as needed, in order to further enhance the effects of the present invention or to impart other properties, within a range that does not impair the effects of the present invention.
[0055] The polypropylene resin used in the present invention preferably contains 0.01% by mass or more of a fatty acid amide compound in order to improve slipperiness and flexibility. By making the content of the fatty acid amide compound preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, the fatty acid amide compound acts as a lubricant on the fiber surface, resulting in a nonwoven fabric with excellent tactile feel. Furthermore, the upper limit of the content of the fatty acid amide compound in the present invention is not particularly limited, but is preferably 5.0% by mass or less from the viewpoints of cost and productivity.
[0056] [Conjugated Fiber] The nonwoven fabric of the present invention is a conjugated fiber having a propylene fraction of 98.5% or more and 100.0% or less, an isotactic pentad fraction of 90.0% or more and 100.0% or less, and a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S The difference between C -O S ) is 0.2 or more and 4.0 or less. By using such conjugate fibers, the fibers have high molecular orientation and excellent adhesive strength at the fused portions, resulting in a nonwoven fabric with excellent mechanical properties.
[0057] The composite fiber according to the present invention is a fiber obtained by conjugating two or more types of resins. The composite form is not particularly limited as long as it does not impair the effects of the present invention, and may be an islands-in-sea type in which the sea component and the sheath component are made of different resins, or it is also possible to use two or more blended resins for the sea component and / or the island component. In the present invention, a composite fiber generally called a sheath-core composite fiber is considered to be one form of islands-in-sea composite fiber having one island component. In other words, this islands-in-sea type composite fiber having one island component includes concentric sheath-core composite fibers and eccentric sheath-core composite fibers.
[0058] The composite fiber according to the present invention preferably has 1 or more and 10 or less island component parts. By having the number of island component parts preferably 10 or less, more preferably 6 or less, and even more preferably 4 or less, the tensile strength of the composite fiber is increased, resulting in a nonwoven fabric with excellent mechanical properties. When the number of island component parts is 2 or more, at least one island should be arranged at least in the central portion. Furthermore, by having the number of island component parts preferably 1 or more, the composite fiber becomes more flexible, resulting in a nonwoven fabric with excellent flexibility.
[0059] The conjugated fiber according to the present invention has a propylene fraction of 98.5% or more and 100.0% or less. A propylene fraction of 98.5% or more, preferably 98.8% or more, and more preferably 99.0% or more increases the tensile strength of the conjugated fiber, resulting in a nonwoven fabric with excellent mechanical properties. The upper limit of the propylene fraction of the conjugated fiber that can be achieved in the present invention is 100.0%.
[0060] The propylene fraction (%) of the composite fiber referred to here is a value measured and calculated by the following procedure: (1) The composite fiber in the non-bonded portion taken from the nonwoven fabric is weighed, and the weight is measured using orthodichlorobenzene-d 4 (orthodichlorobenzene in which hydrogen has been replaced with deuterium) is added to a sample concentration of 8 mass / v%, and the mixture is heated to 135°C. (2) The obtained solution is analyzed using a nuclear magnetic resonance apparatus (for example, "ECZ-600" manufactured by JEOL RESONANCE). 13 C-NMR measurement is performed, and the peak area due to propylene units and the peak areas due to ethylene units and α-olefin units are calculated from the NMR spectrum. (3) Sum A of the peak areas due to propylene units, ethylene units, and α-olefin units AF Peak area A due to propylene units PF The ratio (A PF / A AF (4) For each level, measure three times by changing the sampling location of the composite fiber, and calculate the arithmetic mean value, rounded to one decimal place, as the propylene fraction (%) of the composite fiber.
[0061] The propylene fraction of the composite fiber according to the present invention can be controlled by, for example, the propylene fraction of the polypropylene-based resin. Specifically, the propylene fraction of the composite fiber can be increased by increasing the propylene fraction of the polypropylene-based resin.
[0062] The conjugated fiber according to the present invention has an isotactic pentad fraction of 90.0% or more and 100.0% or less. When the isotactic pentad fraction is 90.0% or more, preferably 92.0% or more, and more preferably 94.0% or more, the tensile strength of the conjugated fiber is increased, resulting in a nonwoven fabric with excellent mechanical properties. Furthermore, the upper limit of the isotactic pentad fraction of the conjugated fiber that can be achieved in the present invention is 100.0%.
[0063] The isotactic pentad fraction (%) of the composite fiber referred to here is a value measured and calculated by the following procedure: (1) The composite fiber in the non-bonded portion taken from the nonwoven fabric was weighed, and the weight was measured using o-dichlorobenzene-d 4 (orthodichlorobenzene in which hydrogen has been replaced with deuterium) is added to a sample concentration of 8 mass / v%, and the mixture is heated to 135°C. (2) The obtained solution is analyzed using a nuclear magnetic resonance apparatus (for example, "ECZ-600" manufactured by JEOL RESONANCE). 13 (3) Based on the method described in "Zambelli et al., Macromolecules, Vol. 8, p. 687 (1975)", the peaks in the obtained NMR spectrum derived from methyl groups are assigned, and the sum of the intensities of all peaks derived from methyl groups, S AF The peak intensity S due to the mesopentad sequence MF The ratio (S MF / S AF (4) For each level, measurements are taken three times at different sampling locations of the composite fiber, and the arithmetic mean value is rounded to one decimal place to calculate the isotactic pentad fraction (%) of the composite fiber.
[0064] The isotactic pentad fraction of the conjugated fiber according to the present invention can be controlled by, for example, the isotactic pentad fraction of the polypropylene-based resin. Specifically, the isotactic pentad fraction of the conjugated fiber can be increased by increasing the isotactic pentad fraction of the polypropylene-based resin.
[0065] The composite fiber according to the present invention has a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S The difference between C -O S ) is 0.2 or more and 4.0 or less. C -O S When O is 0.2 or more, preferably 0.5 or more, and more preferably 0.8 or more, the fiber surfaces soften while maintaining the orientation of the central portions of the fibers during thermal bonding, and the fibers bond together, making the bonded portions less likely to break, resulting in a nonwoven fabric with excellent mechanical properties. C -O S When the ratio is 4.0 or less, preferably 3.5 or less, the process stability during spinning is improved, and the molecular orientation at the center of the fiber does not become excessively high, resulting in a nonwoven fabric with uniform texture and excellent flexibility.
[0066] Here, the molecular orientation parameter O in the fiber axis direction at the center of the fiber C , the molecular orientation parameter O in the fiber axis direction at the fiber surface S , the difference between them O C -O Sis a value measured and calculated by the following procedure: (1) Composite fibers in non-bonded portions are sampled from a nonwoven fabric. (2) The sampled composite fibers are cut with a razor at a cutting angle of approximately 4° relative to the fiber axis direction to expose the longitudinal fiber cross section, and then the fibers are set in a Raman spectrometer (for example, the RAMANOR T64000 manufactured by Horiba, Ltd.), and a laser is irradiated onto the longitudinal fiber cross section from a direction perpendicular to the fiber axis to perform microscopic Raman measurement. (3) Measurement is performed under conditions where the polarization direction is parallel to the fiber axis direction, and polarized Raman spectra are obtained for the fiber center (for sea-island composite fibers, the midpoint of an island component fiber in the fiber diameter direction if the composite fiber has one or more island components at the midpoint; or the midpoint of the island component fiber in the fiber diameter direction if the composite fiber does not have an island at the midpoint of the composite fiber diameter direction) and the fiber surface (0.5 μm inward from the side surface of the fiber in the fiber diameter direction). (4) CH 2 810 cm assigned to the coupling mode of bending vibration and C-C stretching vibration -1 The Raman band intensity near I 810 And CH 2 840 cm attributed to bending vibration mode -1 The Raman band intensity of I 840 Then, the molecular orientation parameter is calculated using the following formula: Molecular orientation parameter = I 810 / I 840 (5) For each level, measurements were taken three times at both the fiber center and the fiber surface by changing the sampling location of the composite fiber. The arithmetic mean value of the molecular orientation parameter in the fiber axis direction at the fiber center was rounded to one decimal place to obtain the molecular orientation parameter O in the fiber axis direction at the fiber center. C The arithmetic mean value of the molecular orientation parameters in the fiber axis direction at the fiber surface portion is rounded to one decimal place to obtain the molecular orientation parameter O in the fiber axis direction at the fiber surface portion. S (6) Molecular orientation parameter O in the fiber axis direction at the center of the fiber C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S From the value of O C -O S Calculate.
[0067] In addition, the O of the composite fiber according to the present inventionC -O S For example, the O-type composite fiber can be controlled by adjusting the difference in polymer properties, particularly the difference in MFR, between the island and sea components when the composite fiber is made into an islands-in-sea composite fiber. Specifically, by using a polypropylene resin for the sea component having a higher MFR than the polypropylene resin for the island components, the O-type composite fiber can be controlled by adjusting the difference in polymer properties, particularly the difference in MFR, between the island and sea components. C -O S can be made larger.
[0068] The composite fiber according to the present invention has a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C The molecular orientation parameter O in the fiber axis direction at the center of the fiber is preferably 5.0 or more and 10.0 or less. C is preferably 5.0 or more, more preferably 5.3 or more, and even more preferably 5.5 or more, the molecular orientation of the composite fibers is high and the tensile strength is high, resulting in a nonwoven fabric with excellent mechanical properties. C By making the ratio preferably 10.0 or less, more preferably 9.5 or less, the molecular orientation at the center of the fiber is not excessively high, and the composite fiber becomes soft, resulting in a nonwoven fabric with excellent flexibility.
[0069] The cross-sectional shape of the conjugated fiber according to the present invention may be a round cross-section, a flat cross-section, or an irregular cross-section such as a Y-shape or a C-shape. Of these, a round cross-section is preferred, as this eliminates the difficulty in bending that is inherent in structures such as a flat cross-section or an irregular cross-section, and allows for the production of a nonwoven fabric with excellent flexibility.
[0070] The conjugated fiber according to the present invention preferably has an average single fiber diameter of 5.0 μm or more and 20.0 μm or less. By making the average single fiber diameter preferably 5.0 μm or more, more preferably 8.0 μm or more, and even more preferably 10.0 μm or more, yarn breakage during spinning can be suppressed, resulting in a nonwoven fabric with fewer defects. Furthermore, by making the average single fiber diameter preferably 20.0 μm or less, more preferably 17.0 μm or less, the nonwoven fabric will have excellent texture, uniform texture, and excellent mechanical properties.
[0071] The average single fiber diameter (μm) of the composite fiber referred to here is a value measured and calculated by the following procedure: (1) A 5 mm × 5 mm test piece is taken from a nonwoven fabric. (2) On the surface of the nonwoven fabric, composite fibers present at a position at least 10% away from the bonded joint relative to the distance between adjacent bonded joints are embedded in an embedding agent such as epoxy resin, and the fibers are cut with a razor in a direction perpendicular to the fiber axis to expose the fiber cross section. An image is then taken with a scanning electron microscope (e.g., "SU1510" manufactured by Hitachi High-Technologies Corporation) at a magnification that allows observation of 10 or more fibers. (3) Using the taken image, the area A formed by the cross-sectional contour of the single fiber is calculated using image analysis software (e.g., "WinROOF2015" manufactured by Mitani Shoji Co., Ltd.). F Measure the area of 10 pieces and calculate the area A F (4) For each level, measurements are taken 10 times by changing the sampling location of the test piece, and the arithmetic mean value of 100 pieces in total is rounded to one decimal place to calculate the average single fiber diameter (μm).
[0072] The average single filament diameter of the conjugated fiber according to the present invention can be controlled, for example, by the spinning temperature, single-hole throughput, spinning speed, etc., which will be described later. Specifically, the average single filament diameter of the conjugated fiber can be reduced by increasing the spinning temperature, decreasing the single-hole throughput, or increasing the spinning speed.
[0073] The tensile strength of the composite fiber according to the present invention is preferably 1.2 cN / dtex or more and 5.0 cN / dtex or less. When the lower limit of the tensile strength of the composite fiber is 1.2 cN / dtex or more, a nonwoven fabric having excellent mechanical properties is obtained. On the other hand, when the upper limit of the tensile strength of the composite fiber is 5.0 cN / dtex or less, a nonwoven fabric having excellent flexibility is obtained.
[0074] The tensile strength of the composite fiber in the present invention is determined by the following procedure, in accordance with JIS L1015:2010, "8.7 Tensile Strength and Elongation (ISO Method)." (1) The density of the composite fiber is measured by the following procedures (1-1) to (1-3). (1-1) Water and ethanol are mixed in a room controlled at 15°C. The mass fraction of ethanol is set to 40% to 70%, and 31 levels of aqueous ethanol solutions with different concentrations at 1% intervals are prepared. (1-2) Ninety-three 5 mm x 5 mm test pieces are randomly cut from a portion of a nonwoven fabric, excluding the widthwise edges, after ultrasonic cleaning to remove impurities. (1-3) The cut test pieces are immersed in aqueous ethanol solutions, taking care not to trap air bubbles, and left for at least 6 hours. (1-4) Among the ethanol solutions in which the test pieces did not sink to the bottom, the mass fraction X of the ethanol solution with the lowest ethanol mass fraction is measured. E The operation of obtaining the mass fraction (unitless) of the composite fiber is carried out three times, and the density is calculated from the arithmetic mean value of the mass fraction of the obtained aqueous ethanol solution using the following formula. 3 ) = -0.000005 x X E 2 -0.0017 x X E+1.0153 (2) Six composite fibers constituting a nonwoven fabric and located at a distance of 10% or more from the fused portion relative to the distance between adjacent fused portions are randomly selected. Each composite fiber is selected so that its fiber length is 50 mm or more. If the fiber length of the selected composite fiber is less than 50 mm, another composite fiber is selected at random so that all six composite fibers are 50 mm or more. (3) The selected composite fibers are cut in half to obtain 12 composite fibers. Six of the 12 composite fibers are used as samples for (4) and (5) below, and the remaining six are used as samples for (6) to (8). (4) The composite fibers are embedded in an embedding agent such as epoxy resin, and an image of the fiber cross section perpendicular to the fiber axis is taken using a microscope (e.g., a scanning electron microscope "SU1510" manufactured by Hitachi High-Technologies Corporation) at a magnification that allows observation of 10 or more composite fibers. (5) Composite fibers randomly extracted from each captured image are analyzed using image analysis software to measure the area of the fiber cross section, and the single fiber diameter (circle-equivalent diameter, μm) of the composite fiber calculated in terms of a perfect circle is determined. This, along with the density calculated in (1), is used to calculate the net fineness (dtex) based on the following formula, and the result is rounded to two decimal places: Net fineness (dtex) = π × (single fiber diameter of composite fiber (cm) / 2) 2 ×Density (g / cm 3 ) x 1,000,000 (cm) (6) Each composite fiber with a spatial distance of 20 mm is loosely stretched along the dividing line, and both ends are attached to a piece of paper with adhesive, and six samples are prepared, each consisting of a section. (7) The sample from (6) is attached to the grips of a tensile tester (for example, the "RTC1210A" manufactured by A&D Co., Ltd.), and pulled at a grip spacing of 20 mm and a pulling speed of 20 mm / min, and the load (cN) at which the sample breaks is measured. (8) The load obtained in (7) is divided by the net fineness (dtex) obtained in (5) to calculate the tensile strength (cN / dtex), and the average tensile strength (cN / dtex) calculated for each sample is calculated and rounded to one decimal place.
[0075] In order to make the tensile strength of the conjugate fiber according to the present invention fall within the above range, for example, a polypropylene-based resin polymerized using a metallocene catalyst may be used.
[0076] [Nonwoven Fabric] The nonwoven fabric of the present invention contains the conjugated fiber and has a melting point of 130° C. or more and 155° C. or less. By producing such a nonwoven fabric, the nonwoven fabric can have both excellent flexibility and mechanical properties.
[0077] The nonwoven fabric of the present invention may be a long-fiber nonwoven fabric such as a spunbonded nonwoven fabric or a meltblown nonwoven fabric, or a short-fiber nonwoven fabric such as a needle-punched nonwoven fabric or a paper-made nonwoven fabric. Of these, a spunbonded nonwoven fabric is preferred because it is easy to achieve a low basis weight and easily achieves both excellent flexibility and mechanical properties.
[0078] The nonwoven fabric of the present invention may be a single-layer nonwoven fabric consisting of only a layer of nonwoven fabric described below, or may be a nonwoven fabric consisting of multiple layers of the same type of nonwoven fabric. However, if the nonwoven fabric of the present invention has a fiber layer of a type different from the layer of the nonwoven fabric of the present invention, for example, if the nonwoven fabric of the present invention is a spunbond nonwoven fabric, a layer of meltblown nonwoven fabric, a layer of papermaking nonwoven fabric, or a layer of woven fabric or knitted fabric, it is considered to be a laminated nonwoven fabric described below.
[0079] The nonwoven fabric of the present invention has a melting point of 130° C. or higher and 155° C. or lower. A melting point of 130° C. or higher, preferably 135° C. or higher, and more preferably 138° C. or higher provides heat resistance sufficient for practical use and improves the dimensional stability of the nonwoven fabric, resulting in a nonwoven fabric with excellent flexibility. Furthermore, a melting point of 155° C. or lower, preferably 150° C. or lower, facilitates thermal bonding, resulting in a nonwoven fabric with excellent mechanical properties.
[0080] The melting point (°C) of the nonwoven fabric referred to here is a value measured and calculated by the following procedure. (1) A 2.0 mg test piece is taken from the nonwoven fabric and placed in a differential scanning calorimeter (e.g., a "DSC Q2000" manufactured by TA Instruments). (2) Differential scanning calorimetry (1st DSC) is performed under nitrogen at a heating rate of 16°C / min and a measurement temperature range of 50°C to 230°C, followed by rapid cooling at a heating rate of 100°C / min, followed by differential scanning calorimetry (2nd DSC) again under nitrogen at a heating rate of 16°C / min and a measurement temperature range of 50°C to 230°C. (3) The peak top temperature (°C) of the largest endothermic peak in the DSC curve of the 2nd DSC is calculated. (4) For each level, measurements are taken three times by changing the location of the test piece, and the melting point (°C) is calculated by rounding off the arithmetic mean value to the nearest whole number.
[0081] The melting point of the nonwoven fabric of the present invention can be controlled by, for example, the polymerization catalyst or the propylene fraction of the composite fiber. Specifically, the melting point of the nonwoven fabric can be lowered by using a metallocene catalyst as the polymerization catalyst or by lowering the propylene fraction of the composite fiber.
[0082] The nonwoven fabric of the present invention preferably has a heat of crystalline fusion of 82 J / g or more and 120 J / g or less. By having a heat of crystalline fusion of 82 J / g or more, preferably 85 J / g or more, and more preferably 88 J / g or more, the crystallinity of the nonwoven fabric can be appropriately increased, resulting in a nonwoven fabric with excellent mechanical properties. Furthermore, by having a heat of crystalline fusion of 120 J / g or less, more preferably 110 J / g or less, the crystallinity of the nonwoven fabric does not become excessively high, resulting in a nonwoven fabric with excellent flexibility.
[0083] The heat of crystalline fusion (J / g) of the nonwoven fabric referred to here is a value measured and calculated by the following procedure. (1) A 2.0 mg test piece is taken from the nonwoven fabric and placed in a differential scanning calorimeter (e.g., a "Q2000" manufactured by TA Instruments). (2) Differential scanning calorimetry (1st DSC) is performed under nitrogen at a heating rate of 16°C / min and a measurement temperature range of 50°C to 230°C, followed by rapid cooling at a heating rate of 100°C / min, followed by differential scanning calorimetry (2nd DSC) again under nitrogen at a heating rate of 16°C / min and a measurement temperature range of 50°C to 230°C. (3) The endothermic heat (J / g) of the largest endothermic peak in the DSC curve of the 2nd DSC is calculated. (4) For each level, measurements are taken three times by changing the location of the test piece, and the arithmetic mean value is rounded to the first decimal place to calculate the heat of crystalline fusion (J / g).
[0084] The heat of crystalline fusion of the nonwoven fabric of the present invention can be controlled, for example, by the propylene fraction of the composite fiber. Specifically, the heat of crystalline fusion of the nonwoven fabric can be increased by increasing the propylene fraction of the composite fiber.
[0085] The nonwoven fabric of the present invention has fused portions and non-fused portions. In the present invention, a fused portion refers to a location where the composite fibers are fused together after being compressed in the cross-sectional direction of the nonwoven fabric, for example, to such an extent that the cross-sectional shape of the composite fibers is deformed to a degree that differs from the shape of the remaining portions, and the composite fibers are melted to the point where they become lumpy or film-like. Specifically, in the case of thermal bonding using an uneven roll (embossing roll) and a flat roll, the fused portion refers to the portion where the convex portions of the embossing roll contact the nonwoven fabric. Meanwhile, a non-fused portion refers to a portion other than the fused portion.
[0086] In the nonwoven fabric of the present invention, the fused portions preferably have a crystallite size of (040) plane of 10.0 nm or more and 13.5 nm or less in wide-angle X-ray diffraction, and the unfused portions preferably have a crystallite size of (110) plane of 5.0 nm or more and 10.0 nm or less in wide-angle X-ray diffraction. By simultaneously satisfying these two requirements, the nonwoven fabric has excellent mechanical properties due to high fiber strength and high adhesive strength at the fused portions.
[0087] As described above, the nonwoven fabric of the present invention preferably has a crystallite size of 10.0 nm or more and 13.5 nm or less in wide-angle X-ray diffraction of the (040) plane of the fused portion. By setting the lower limit of the crystallite size of the (040) plane of the fused portion to preferably 10.0 nm or more, more preferably 11.0 nm or more, the crystallite size is sufficiently large, resulting in a nonwoven fabric with better mechanical properties. On the other hand, by setting the upper limit of the crystallite size of the (040) plane of the fused portion to preferably 13.5 nm or less, more preferably 13.0 nm or less, the nonwoven fabric has better flexibility.
[0088] Next, in the nonwoven fabric of the present invention, the crystallite size of the (110) plane of the non-fused portion is 5.0 nm or more and 10.0 nm or less in wide-angle X-ray diffraction. The lower limit of the crystallite size of the (110) plane of the non-fused portion is 5.0 nm or more, preferably 6.0 nm or more, and more preferably 8.0 nm or more, resulting in a nonwoven fabric with sufficient crystallite size and better mechanical properties. On the other hand, the upper limit of the crystallite size of the (110) plane of the non-fused portion is 10.0 nm or less, preferably 9.5 nm or less, resulting in a uniform crystallite size and a nonwoven fabric with excellent mechanical properties. That is, the crystallite size of the (110) plane of the non-fused portion is 5.0 nm or more and 10.0 nm or less, resulting in a sufficient crystallite size and a uniform crystallite size, resulting in a nonwoven fabric with excellent mechanical properties.
[0089] In the present invention, the crystallite sizes of the (040) plane in the fused portions of the nonwoven fabric and the (110) plane in the nonfused portions of the nonwoven fabric can be controlled by the catalyst and melt flow rate used when polymerizing the polypropylene resin. The larger the melt flow rate, the smaller the crystallite sizes of the (040) plane in the fused portions of the nonwoven fabric and the (110) plane in the nonfused portions of the nonwoven fabric.
[0090] In the present invention, the crystallite size of the (040) plane in wide-angle X-ray diffraction of the fused portion and the crystallite size of the (110) plane in wide-angle X-ray diffraction of the non-fused portion refer to values measured and calculated by the following methods. (1) A 5 cm x 5 cm test piece is randomly taken from a portion of the nonwoven fabric excluding a 10 cm portion from the widthwise end, which portion has both a fused portion and a non-fused portion. The locations used for measuring the fused portion and the non-fused portion are determined according to the following (1-1) and (1-2). (1-1) For measuring the fused portion of the nonwoven fabric, a location (13) in the fused portion near the center of the test piece is used, which is at a distance of 50% or less of the radius of the inscribed circle (12) of the fused portion (11) of the test piece (1) from the center of the inscribed circle (12), as shown in FIG. 1 . (1-2) To measure the non-fused portion of the nonwoven fabric, a location in the non-fused portion near the center of the test piece that is at least 10% away from the fused portion relative to the distance between adjacent fused portions is used. (2) To measure the non-fused portion, 20 fibers present in the location determined in (1-2) are grouped together so that their fiber axes are aligned in the same direction. (3) For the sample from the location determined in (1-1) (the fused portion sample) and the sample grouped in (2) (the non-fused portion sample), wide-angle X-ray diffraction measurements are performed using an X-ray diffractometer (e.g., a Bruker AXS "D8 DISCOVER μHR Hybrid"). Here, the fused portion sample is irradiated with X-rays from the thickness direction of the nonwoven fabric, and the non-fused portion sample is irradiated with X-rays from the fiber diameter direction. (4) An X-ray diffraction profile is obtained by measuring the sample of the fused portion and averaging the entire circumference of the peak corresponding to the (040) plane, and by measuring the sample of the non-fused portion and averaging the sector in the equatorial direction of the peak corresponding to the (110) plane. (5) The crystallite size of each is calculated by the half-width β of the peak. e The crystallite size L (nm) is calculated from the following formula (Scherrer's formula) using (°): e 2 -β 0 2 ) 0.5 × cos θ) where λ is the incident X-ray wavelength, β 0 represents the corrected value of the half-width, and θ represents the Bragg angle (°) of the peak top.
[0091] In addition, in order to make the crystallite size of the (040) plane in the wide-angle X-ray diffraction of the fused portion and the crystallite size of the (110) plane in the wide-angle X-ray diffraction of the unfused portion fall within the above-mentioned ranges, for example, a polypropylene-based resin using a metallocene catalyst as a polymerization catalyst can be used.
[0092] The melt flow rate of the nonwoven fabric of the present invention is preferably 20 g / 10 min or more and 100 g / 10 min or less. By setting the melt flow rate of the nonwoven fabric within this range, it is easy to control the crystallite size of the (040) plane of the fused portion of the nonwoven fabric and the (110) plane of the nonwoven fabric in the nonfused portion of the nonwoven fabric within the above range. When the lower limit of the melt flow rate of the nonwoven fabric is preferably 20 g / 10 min or more, more preferably 30 g / 10 min or more, the nonwoven fabric has excellent flexibility. Furthermore, when the upper limit of the melt flow rate of the nonwoven fabric is preferably 100 g / 10 min or less, more preferably 60 g / 10 min or less, the nonwoven fabric has sufficient strength for practical use.
[0093] The melt flow rate of the nonwoven fabric in the present invention refers to the arithmetic mean value of values obtained by taking five 5 g test pieces from a portion of the nonwoven fabric excluding 10 cm from each end in the width direction, and measuring the taken test pieces under conditions of a load of 2160 g and a temperature of 230° C. in accordance with ASTM D1238 (Method A). For the measurement, for example, a melt indexer "F-F01" manufactured by Toyo Seiki Seisakusho, Ltd. can be used.
[0094] The melt flow rate of the nonwoven fabric can be controlled by the weight average molecular weight of the polypropylene resin. The higher the weight average molecular weight of the polypropylene resin, the lower the melt flow rate.
[0095] The nonwoven fabric of the present invention has a basis weight of 5 g / m 2 More than 100g / m 2 The basis weight is preferably 5 g / m or less. 2 More preferably, 7 g / m 2 By satisfying the above conditions, the nonwoven fabric has a uniform texture and excellent mechanical properties. 2or less, more preferably 50 g / m 2 The nonwoven fabric has excellent flexibility when it satisfies the following conditions.
[0096] Here, the basis weight of the nonwoven fabric (g / m 2 ) is a value measured and calculated by the following procedure in accordance with "6.2 Mass per unit area (ISO method)" of JIS L1913:2010 "General nonwoven fabric testing methods." (1) A 20 cm x 25 cm test piece is taken from the nonwoven fabric. However, if a 20 cm x 25 cm test piece cannot be taken, a test piece with a total area of 500 cm is taken. 2 (2) For the test pieces taken, measure the mass (g) under standard conditions and calculate the area of 1 m 2 Mass per unit (g / m 2 (3) For each level, measurements are taken three times by changing the location of the test piece, and the arithmetic mean value is rounded to the nearest whole number to convert it into basis weight (g / m 2 ) is calculated as follows.
[0097] The basis weight of the nonwoven fabric of the present invention can be controlled, for example, by the single-hole discharge rate and conveying speed during spinning, which will be described later. Specifically, the basis weight of the nonwoven fabric can be reduced by decreasing the single-hole discharge rate and increasing the conveying speed.
[0098] The nonwoven fabric of the present invention has a tensile strength per unit area of 1.40 (N / 25 mm) / (g / m 2 ) or more 3.00 (N / 25mm) / (g / m 2 The tensile strength per unit area is preferably 1.40 (N / 25 mm) / (g / m 2 ) or more, more preferably 1.50 (N / 25mm) / (g / m 2 ) or more, more preferably 1.55 (N / 25mm) / (g / m 2 ) or more, the nonwoven fabric has excellent mechanical properties. In addition, the tensile strength per unit area is preferably 3.00 (N / 25 mm) / (g / m 2 ) or less, more preferably 2.80 (N / 25mm) / (g / m 2 ) or less, the nonwoven fabric will have excellent flexibility.
[0099] Here, the tensile strength per unit area of the nonwoven fabric ((N / 25 mm) / (g / m 2 )) is a value measured and calculated by the following procedure in accordance with "6.3 Tensile Strength and Elongation (ISO Method)" of JIS L1913:2010 "General Nonwoven Fabric Testing Methods." (1) 25 mm x 40 mm test pieces are taken from the nonwoven fabric in both the machine direction (longitudinal direction) and the transverse direction (width direction) of the nonwoven fabric. (2) The long side direction (40 mm) of the taken test piece is set as the tensile direction, and the test piece is set in a tensile tester (such as the "RTC-1210A" manufactured by A&D Co., Ltd.) with a grip spacing of 20 mm. (3) A tensile test is carried out at a pulling speed of 20 mm / min, and the maximum point load (N / 25 mm) is measured. (4) For each level, measure five times in both the longitudinal and transverse directions by changing the sampling location of the test piece. The arithmetic mean value of the ten measurements, rounded to three decimal places, is taken as the average maximum point load (N / 25mm). The tensile strength per unit area ((N / 25mm) / (g / m)) is calculated using the following formula. 2 )) is calculated. 2 )) = Maximum point load (N / 25mm) / basis weight (g / m 2 ).
[0100] The tensile strength per unit area of the nonwoven fabric of the present invention can be determined by, for example, the propylene fraction and isotactic pentad fraction of the polypropylene resin, MFR, and the molecular orientation parameter difference (O C -O S ) and the molecular orientation parameter O in the fiber axis direction at the center of the fiber. C The nonwoven fabric can be controlled by the melting point and heat of crystalline fusion of the nonwoven fabric, and / or the spinning speed and heat bonding conditions (bonding rate, temperature, linear pressure, etc.) during spinning, which will be described later. Specifically, the propylene fraction and isotactic pentad fraction of the polypropylene resin can be increased, the MFR can be decreased, or the molecular orientation parameter difference (O C -O S ) and the molecular orientation parameter O in the fiber axis direction at the center of the fiber. CThe tensile strength per unit area of the nonwoven fabric can be increased by increasing the tensile strength per unit area of the nonwoven fabric, increasing the melting point or heat of crystalline fusion of the nonwoven fabric, increasing the spinning speed during spinning, or increasing the bonding rate, temperature, and linear pressure during thermal bonding.
[0101] The nonwoven fabric of the present invention preferably has a bending resistance of 10 mm or more and 50 mm or less. A bending resistance of preferably 10 mm or more, more preferably 20 mm or more, results in a nonwoven fabric with appropriate rigidity and excellent handleability. Furthermore, a bending resistance of preferably 50 mm or less, more preferably 45 mm or less, results in a nonwoven fabric with excellent flexibility.
[0102] The bending resistance (mm) of the nonwoven fabric referred to here is a value obtained by measuring three times in each of the machine direction (longitudinal direction of the nonwoven fabric) and the cross direction (width direction of the nonwoven fabric) of the nonwoven fabric in accordance with "6.7 Bending resistance (JIS method and ISO method)" "6.7.3 41.5° cantilever method" of JIS L1913:2010 "Testing methods for general nonwoven fabrics," and then rounding off the arithmetic mean value (mm) of all values in the machine direction and the cross direction to one decimal place.
[0103] The bending resistance of the nonwoven fabric of the present invention can be determined by, for example, the cross-sectional shape of the composite fiber and the molecular orientation parameter O in the fiber axis direction at the center of the fiber. C The heat of crystalline fusion and the basis weight of the nonwoven fabric can be controlled by the heat of fusion and the basis weight of the nonwoven fabric, and / or the thermal bonding conditions (bonding rate, temperature, linear pressure, etc.) described later. Specifically, when the cross section of the composite fiber is a round cross section, the molecular orientation parameter O in the fiber axis direction at the center of the fiber can be controlled by the heat of fusion and the basis weight of the nonwoven fabric. C The bending resistance of the nonwoven fabric can be reduced by reducing the heat of crystal fusion of the nonwoven fabric, reducing the basis weight, and reducing the bonding rate, temperature, and linear pressure during thermal bonding.
[0104] [Method for producing nonwoven fabric] Next, a method for producing the nonwoven fabric of the present invention will be described. The method for producing the nonwoven fabric of the present invention preferably includes the steps of melt-extruding, through a conjugate spinneret, polypropylene-based resin A polymerized with a metallocene catalyst and having a propylene fraction of 98.5% to 100.0%, and polypropylene-based resin B polymerized with a metallocene catalyst and having a propylene fraction of 98.5% to 100.0%, which has a melt flow rate higher than that of polypropylene-based resin A by 6 g / 10 min to 200 g / 10 min, and the spun polypropylene-based resin A and the polypropylene-based resin B, to form islands-in-sea composite fibers having island components and polypropylene-based resin B as a sea component, stacking the islands-in-sea composite fibers to form a fiber web composed of the islands-in-sea composite fibers, and thermally bonding the fiber web. This production method makes it possible to consistently produce nonwoven fabrics that exhibit both excellent flexibility and mechanical properties. Each step of the above preferred embodiment will now be described in further detail.
[0105] (a) Step of forming islands-in-sea composite fibers First, in this step, the following are melt-extruded from a composite spinneret: polypropylene resin A polymerized with a metallocene catalyst and having a propylene fraction of 98.5% to 100.0%, and polypropylene resin B polymerized with a metallocene catalyst and having a propylene fraction of 98.5% to 100.0%, and having a melt flow rate higher than that of polypropylene resin A by 6 g / 10 min to 200 g / 10 min. By doing so, a nonwoven fabric with excellent mechanical properties can be obtained.
[0106] (a-1) Polypropylene Resin A In the method for producing a nonwoven fabric of the present invention, the polypropylene resin A to be used in the island component fibers is preferably a polypropylene resin produced using a metallocene catalyst as a polymerization catalyst. When the polypropylene resin A is a polypropylene resin produced using a metallocene catalyst, the process stability during spinning is improved compared to polypropylene resins produced using a Ziegler-Natta catalyst, and the molecular orientation parameter O of the island component fibers containing the polypropylene resin A is reduced. C Since it is possible to increase the viscosity and lower the melting point, it is possible to obtain a nonwoven fabric with a highly uniform texture and excellent mechanical properties and flexibility.
[0107] Specific examples of the metallocene catalyst include ethylene bisindenyl zirconium dichloride, ethylene bis(tetrahydroindenyl)zirconium dichloride, dimethylsilylene bis(dimethylcyclopentadienyl)zirconium dichloride, dimethylsilylene bis(trimethylcyclopentadienyl)zirconium dichloride, dimethylsilylene bis(indenyl)zirconium dichloride, dimethylsilylene bis(2-methylindenyl)zirconium dichloride, dimethylsilylene bis(2-methyl-4-isopropylindenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(9-fluorenyl)zirconium dichloride, cyclohexylidene(cyclopentadienyl)(9-fluorenyl)zirconium dichloride, and the like. cyclopentadienyl)(9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(9-fluorenyl)zirconium dichloride, methylphenylmethylene(cyclopentadienyl)(9-fluorenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, cyclohexylidene(cyclopentadienyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, methylphenylmethylene(cyclopentadienyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, and the like. Among these, it is preferable to use a metallocene catalyst having a cyclopentadienyl skeleton in the present invention, since it is possible to increase the isotactic pentad fraction of the polypropylene-based resin.
[0108] In addition to aluminoxane, examples of the co-catalyst that can be used include dimethylanilinium tetrakis(pentafluorophenyl)borate, and also triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis(pentafluorophenyl)aluminate, magnesium chloride, alumina, and tris(pentafluorophenyl)boron.
[0109] In the nonwoven fabric manufacturing method of the present invention, the polypropylene-based resin A used in the island component preferably has a propylene fraction of 98.5% or more and 100.0% or less. By ensuring that the propylene fraction of polypropylene-based resin A is preferably 98.5% or more, more preferably 98.8% or more, and even more preferably 99.0% or more, the spinning process stability is improved and the heat of crystalline fusion of the resulting nonwoven fabric is increased, resulting in a nonwoven fabric with highly uniform texture and excellent mechanical properties. The upper limit of the propylene fraction of polypropylene-based resin A that can be achieved in the present invention is 100.0%.
[0110] In the nonwoven fabric manufacturing method of the present invention, the polypropylene resin A contained in the island component preferably has an isotactic pentad fraction of 90.0% or more and 100.0% or less. When the isotactic pentad fraction of the polypropylene resin A is preferably 90.0% or more, more preferably 92.0% or more, and even more preferably 94.0% or more, the heat of crystalline fusion of the resulting nonwoven fabric is increased, resulting in a nonwoven fabric with excellent mechanical properties. Furthermore, the upper limit of the isotactic pentad fraction of the polypropylene resin A that can be achieved in the present invention is 100.0%.
[0111] In the method for producing a nonwoven fabric of the present invention, the polypropylene-based resin A used in the island component fibers preferably has a polydispersity (Mw / Mn) of 1.5 or more and 3.5 or less. When the polydispersity (Mw / Mn) of the polypropylene-based resin A is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, the spinning stress of the island component fibers does not become excessively high, thereby suppressing yarn breakage and enabling the production of a nonwoven fabric with fewer defects. Furthermore, when the polydispersity (Mw / Mn) is preferably 3.5 or less, more preferably 3.2 or less, and even more preferably 3.0 or less, the molecular orientation parameter of the island component fibers in the islands-in-sea type composite fibers obtained at the same spinning speed becomes high, thereby increasing the strength of the composite fibers and enabling the production of a nonwoven fabric with excellent mechanical properties.
[0112] In the method for producing a nonwoven fabric of the present invention, the polypropylene resin A preferably has a melt flow rate of 10 g / 10 min or more and 90 g / 10 min or less. By setting the lower limit of the melt flow rate range to preferably 10 g / 10 min or more, more preferably 25 g / 10 min or more, stable spinning is possible even with a thin fiber diameter, and a nonwoven fabric with excellent texture and uniform texture can be obtained. On the other hand, by setting the upper limit of the melt flow rate range to preferably 90 g / 10 min or less, more preferably 80 g / 10 min or less, and even more preferably 60 g / 10 min or less, a decrease in the single yarn strength of the islands-in-sea type composite fiber can be suppressed, and the mechanical properties of the nonwoven fabric can be improved.
[0113] The melt flow rate of the polypropylene resin in the present invention refers to a value measured in accordance with ASTM D1238 (Method A) under conditions of a load of 2160 g and a temperature of 230° C., similar to the method for measuring the melt flow rate of a nonwoven fabric. For the measurement, for example, a melt indexer "F-F01" manufactured by Toyo Seiki Seisakusho, Ltd. can be used.
[0114] The melt flow rate of the polypropylene resin can be controlled by the weight average molecular weight of the polypropylene resin. The higher the weight average molecular weight of the polypropylene resin, the smaller the melt flow rate.
[0115] (a-2) Polypropylene Resin B In the method for producing a nonwoven fabric of the present invention, the polypropylene resin B contained in the sea component is preferably a polypropylene resin produced using a metallocene catalyst as a polymerization catalyst. When the polypropylene resin B is a polypropylene resin produced using a metallocene catalyst, the process stability during spinning is improved and the melting point can be lowered compared to polypropylene resins produced using a Ziegler-Natta catalyst, and therefore a nonwoven fabric with highly uniform texture and excellent flexibility can be obtained.
[0116] In the method for producing a nonwoven fabric of the present invention, the polypropylene-based resin B contained in the sea component preferably has a propylene fraction of 98.5% or more and 100.0% or less. By making the propylene fraction of the polypropylene-based resin B preferably 98.5% or more, more preferably 98.8% or more, and even more preferably 99.0% or more, the process stability during spinning is improved and the heat of crystalline fusion of the resulting nonwoven fabric is increased, resulting in a nonwoven fabric with highly uniform texture and excellent mechanical properties. Furthermore, the upper limit of the propylene fraction of the polypropylene-based resin B that can be achieved in the present invention is 100.0%.
[0117] In the method for producing a nonwoven fabric of the present invention, the polypropylene-based resin B contained in the sea component preferably has an isotactic pentad fraction of 90.0% or more and 100.0% or less. When the isotactic pentad fraction of the polypropylene-based resin B is preferably 90.0% or more, more preferably 92.0% or more, and even more preferably 94.0% or more, the heat of crystalline fusion of the resulting nonwoven fabric is increased, thereby enabling the production of a nonwoven fabric with excellent mechanical properties. Furthermore, the upper limit of the isotactic pentad fraction of the polypropylene-based resin B that can be achieved in the present invention is 100.0%.
[0118] In the method for producing a nonwoven fabric of the present invention, the melt flow rate MFR of the polypropylene resin B is B and the melt flow rate MFR of the polypropylene resin A A Melt flow rate difference (MFR B -MFR A It is preferable that the melt flow rate difference (MFR) is 6 g / 10 min or more and 200 g / 10 min or less. B -MFR A ) is preferably 6 g / 10 min or more, more preferably 10 g / 10 min or more, and further preferably 15 g / 10 min or more, so that the spinning stress is concentrated on the island component where the polypropylene-based resin A is arranged, and the molecular orientation parameter difference (O C -O S ) is large, it is possible to obtain a nonwoven fabric with excellent mechanical properties. B -MFRA ) is preferably 200 g / 10 min or less, more preferably 150 g / 10 min or less, and further preferably 100 g / 10 min or less, so that the spinning stress is not excessively concentrated on the island component having the polypropylene-based resin A, and the process stability during spinning is improved, so that a nonwoven fabric with a uniform texture can be obtained.
[0119] In the nonwoven fabric manufacturing method of the present invention, the polypropylene-based resin B preferably has a melt flow rate of 30 g / 10 min or more and 290 g / 10 min or less while satisfying the above relationship. By setting the lower limit of this melt flow rate range to preferably 30 g / 10 min or more, more preferably 45 g / 10 min or more, it is possible to stably spin even thin fibers, and to obtain a nonwoven fabric that is excellent in texture and uniform in texture. On the other hand, by setting the upper limit of this melt flow rate range to preferably 290 g / 10 min or less, more preferably 280 g / 10 min or less, and even more preferably 250 g / 10 min or less, it is possible to suppress a decrease in the single yarn strength of the islands-in-sea type composite fiber and to obtain a nonwoven fabric with excellent mechanical properties.
[0120] (a-3) Melt extrusion from a conjugate spinneret In the method for producing the nonwoven fabric of the present invention, the islands-in-sea type conjugate fiber can be obtained by melt spinning using an extruder such as a pressure melter, single-screw extruder, or twin-screw extruder. Polypropylene resin A and polypropylene resin B, which are separately melted and extruded, are passed through pipes, metered by a metering device such as a gear pump, passed through a filter to remove foreign matter, and then introduced to the spinneret. At this time, the temperature from the resin pipe to the spinneret (spinning temperature) is preferably 180°C or higher and 280°C or lower. By keeping the spinning temperature within the above range, a stable melt state can be achieved, resulting in excellent spinning stability.
[0121] It is preferred that the polypropylene-based resin A and the polypropylene-based resin B introduced into the spinneret join together at the top of the spinneret to form a cross section of an islands-in-sea type composite fiber in which the polypropylene-based resin A is arranged as island components and the polypropylene-based resin B is arranged as a sea component.
[0122] The spinneret used for extrusion preferably has a nozzle hole diameter D of 0.1 mm or more and 0.6 mm or less, and furthermore, L / D, defined as the quotient obtained by dividing the land length L of the nozzle hole (the length of the straight tube portion having the same diameter as the nozzle hole) by the hole diameter D, is preferably 1 or more and 10 or less.
[0123] In the present invention, the mass ratio of polypropylene-based resin A as the island component to polypropylene-based resin B as the sea component is preferably 10% by mass or more and 70% by mass or less, where the mass ratio of polypropylene-based resin B to the total of both is 10% by mass or more and more preferably 20% by mass or more. By setting the mass ratio of polypropylene-based resin B as preferably 10% by mass or more, more preferably 20% by mass or more, excellent thermal adhesiveness can be obtained, and therefore a nonwoven fabric having excellent mechanical properties can be obtained. On the other hand, by setting the mass ratio of polypropylene-based resin B as preferably 70% by mass or less, more preferably 50% by mass or less, the islands-in-sea type composite fiber has excellent single yarn strength, and therefore a nonwoven fabric having excellent mechanical properties can be obtained.
[0124] In the present invention, the number of islands in the islands-in-sea type composite fiber is preferably 1 or more and 10 or less. When the lower limit of the number of islands is preferably 1 or more, a nonwoven fabric having excellent single yarn strength of the composite fiber can be obtained. On the other hand, when the upper limit of the number of islands is preferably 10 or less, a nonwoven fabric having excellent thermal adhesiveness can be obtained.
[0125] (a-4) Drawing and Stretching of Polypropylene Resin It is preferable to form islands-in-sea type composite fibers in which the polypropylene resin A is the island component and the polypropylene resin B is the sea component by drawing and stretching the polypropylene resin A and the polypropylene resin B extruded (spun) from the spinneret holes.
[0126] The islands-in-sea type composite fiber spun from the spinneret is then cooled. Examples of methods for cooling the spun islands-in-sea type composite fiber include a method of forcibly blowing cold air onto the yarn, a method of allowing the yarn to cool naturally at the ambient temperature around the yarn, and the like, or a combination of these methods can be used.
[0127] The composite fiber is cooled and solidified by being blown with cooling air (air). The temperature of the cooling air can be determined in consideration of the balance with the cooling air speed from the viewpoint of cooling efficiency, but is preferably 30°C or less. By setting the upper limit of the cooling air temperature to preferably 30°C or less, more preferably 20°C or less, and even more preferably 15°C or less, the cooling efficiency of the islands-in-sea type composite fiber can be increased, and spinnability can be improved. Furthermore, the lower limit of the cooling air temperature is preferably 0°C or more from the viewpoint of the cooling cost of the air and from the viewpoint of preventing adhesion of moisture to the fibers due to cooling.
[0128] The cooling air is preferably blown in a direction substantially perpendicular to the islands-in-sea type composite fibers discharged from the spinneret (when the fibers run vertically, the direction refers to a direction parallel to the ground). In this case, the speed of the cooling air is preferably 10 m / min or more from the viewpoint of cooling efficiency and uniformity of fineness, and is preferably 100 m / min or less from the viewpoint of spinning stability.
[0129] Furthermore, it is preferable to start cooling at a distance of 0 mm or more and 300 mm or less downstream from the nozzle hole of the spinneret. By setting the lower limit of the distance from the spinneret to the start of cooling to preferably 0 mm or more, more preferably 5 mm, it is possible to stabilize discharge without causing a decrease in the spinneret surface temperature. Furthermore, by setting the upper limit of the distance from the spinneret to preferably 300 mm or less, more preferably 100 mm or less, it is possible to stabilize the thinning behavior of the islands-in-sea type composite fiber and improve spinnability.
[0130] Next, the cooled and solidified filaments are drawn. If a spunbonding method is used, the cooled and solidified filaments are not wound up but are drawn by compressed air ejected from an ejector installed below the spinneret. The islands-in-sea type composite fiber entering the ejector is accelerated by the accelerating air flow, and the spinning speed, which is the running speed of the islands-in-sea type composite fiber, reaches a speed close to the air flow speed.
[0131] The accelerating air flow can be achieved by sealing the area where the cooling air is blown and gradually reducing the cross-sectional area of the sealed area toward the downstream of the spinning line, thereby accelerating the air flow rate. However, in order to obtain high cooling efficiency and air flow rate, it is preferable to not seal the area where the cooling air is blown and to use an ejector.
[0132] In the spunbonding method, various shapes of spinneret and ejector can be used, such as round and rectangular shapes. Among them, it is preferable to use a combination of a rectangular spinneret and a rectangular ejector, from the viewpoints that the amount of compressed air used is relatively small and fusion and abrasion between the yarns are unlikely to occur.
[0133] In this case, the distance from the spinneret to the ejector inlet is preferably 400 mm or more and 3000 mm or less. By making the distance from the spinneret to the ejector inlet preferably 400 mm or more, the islands-in-sea type composite fiber enters the ejector after being cooled and solidified, thereby obtaining excellent spinning stability. Furthermore, by making the distance from the spinneret to the ejector inlet preferably 3000 mm or less, the spinning stress does not become excessively high, thereby suppressing yarn breakage and allowing for the production of a nonwoven fabric with few defects.
[0134] The spinning speed is preferably 2.0 km / min or more and 6.0 km / min or less. By setting the spinning speed to preferably 2.0 km / min or more, more preferably 2.3 km / min or more, the molecular orientation parameter O along the fiber axis at the center of the fiber can be reduced. C Since the average single fiber diameter is increased and the average single fiber diameter is reduced, a nonwoven fabric excellent in mechanical properties and flexibility can be obtained. Furthermore, by setting the spinning speed to preferably 6.0 km / min or less, it is possible to suppress yarn breakage during spinning and to improve spinning stability.
[0135] The spinning speed referred to here is a value measured and calculated by the following procedure: (1) The average single fiber diameter W (μm) of the islands-in-sea type composite fiber, and the density ρ (g / cm 3) is the value measured by the above procedure. (2) The polypropylene resin discharged from the spinneret is collected for 1 minute and weighed, and the value obtained is the discharge rate (g / min). This operation is carried out three times, and the arithmetic mean value is divided by the number of spinneret holes to obtain the single-hole discharge rate Q (g / min). (3) The value obtained by rounding to one decimal place is calculated as the spinning speed using the following formula: Spinning speed (km / min) = Q × 1000 / ((W / 2) 2 ×π×ρ) (wherein Q represents the single-hole output rate (g / min), W represents the average single fiber diameter (μm), and ρ represents the density (g / cm 3 ) represents.
[0136] (b) Step of forming a fiber web The islands-in-sea type composite fibers obtained in the above step are deposited to form a fiber web composed of the islands-in-sea type composite fibers. Specifically, the islands-in-sea type composite fibers are spread by passing through a spreading part where the surrounding air flow speed is reduced, and then landed on a net conveyer which sucks air from the back side, and collected as a fiber web.
[0137] The collected fiber web is preferably transported at a transport speed of 5 m / min to 1200 m / min. Another preferred embodiment is to temporarily bond the collected fiber web by contacting one side of the web with a hot flat roll on a net. This prevents the surface layer of the fiber web from turning over or being blown away while being transported on the net, thereby preventing deterioration of the formation, and improves transportability from the time the yarn is collected to the time it is thermally bonded.
[0138] In the nonwoven fabric manufacturing method of the present invention, the method for forming the fiber web can be selected from known manufacturing methods such as the meltblowing method and the staple fiber carding method in addition to the spunbonding method described above. However, the spunbonding method is preferred because of its excellent productivity. The spunbonding method not only has excellent productivity and mechanical strength, but also suppresses the fuzzing and fiber shedding that are common in staple fiber nonwoven fabrics. Furthermore, by laminating multiple layers of collected spunbonded nonwoven fiber webs or thermally bonded spunbonded nonwoven fabrics (both of which are referred to as S) with SS, SSS, and SSSS, productivity and uniformity of texture are improved.
[0139] (c) Step of thermally bonding the fiber web In this step, the fiber web obtained in (b) above is thermally bonded. The thermal bonding method is not particularly limited, and examples include a method of thermally fusing the fiber web using various rolls, such as a heat embossing roll, each of which has an engraving (concave or recessed portion) on the surface of a pair of upper and lower rolls; a heat embossing roll consisting of a combination of one roll with a flat (smooth) surface and the other with an engraving (concave or recessed portion) on the surface of a roll; and a heat calender roll consisting of a combination of upper and lower flat (smooth) rolls; a method of thermally fusing the fiber web using ultrasonic vibrations from a horn; and a method of passing hot air through the nonwoven fiber web to soften or melt the surfaces of the islands-in-sea composite fibers and thermally fusing the fiber intersections. Among these, it is preferable to use a heat embossing roll, each of which has an engraving (concave or recessed portion) on the surface of a pair of upper and lower rolls; or a heat embossing roll consisting of a combination of one roll with a flat (smooth) surface and the other with an engraving (concave or recessed portion) on the surface of a roll. This not only increases productivity but also provides bonded portions that improve the strength of the nonwoven fabric and non-bonded portions that improve the texture and feel.
[0140] The adhesion rate during thermal bonding is preferably 5% or more and 30% or less. By setting the adhesion rate to preferably 5% or more, more preferably 10% or more, a nonwoven fabric with excellent mechanical properties can be obtained. Furthermore, by setting the adhesion rate to preferably 30% or less, more preferably 20% or less, a nonwoven fabric with excellent flexibility can be obtained.
[0141] Here, the term "bonding rate" refers to the area ratio of the bonded portion to the entire nonwoven fabric. Specifically, when thermal bonding is performed using a pair of uneven rolls, the term refers to the area ratio of the portion of the nonwoven fabric where the convex portions of the upper roll and the convex portions of the lower roll overlap and contact the nonwoven fiber web (bonded portion). When thermal bonding is performed using an uneven roll and a flat roll, the term refers to the area ratio of the portion of the uneven roll where the convex portions of the uneven roll contact the nonwoven fiber web (bonded portion) to the entire nonwoven fabric. When ultrasonic bonding is performed, the term refers to the area ratio of the portion of the nonwoven fabric that is thermally bonded by ultrasonic processing (bonded portion).
[0142] The shape of the bonded portions formed by the hot embossing roll or ultrasonic bonding is not particularly limited, but for example, a circle, ellipse, square, rectangle, parallelogram, rhombus, regular hexagon, or regular octagon can be used. Furthermore, it is preferable that the bonded portions are uniformly spaced at regular intervals in both the longitudinal direction (machine direction) and the width direction of the nonwoven fabric. This reduces the variation in strength of the nonwoven fabric.
[0143] Furthermore, the surface temperature of the hot embossing roll during thermal bonding is preferably 100° C. or higher and 150° C. or lower. By setting the surface temperature of the hot embossing roll to preferably 100° C. or higher, more preferably 110° C. or higher, moderate thermal bonding can be achieved, resulting in a nonwoven fabric with excellent mechanical properties. Furthermore, by setting the surface temperature of the hot embossing roll to preferably 150° C. or lower, more preferably 145° C. or lower, excessive thermal bonding can be suppressed, resulting in a nonwoven fabric with excellent flexibility.
[0144] The linear pressure of the hot embossing roll during thermal bonding is preferably 50 N / cm or more and 500 N / cm or less. By setting the linear pressure of the hot embossing roll to preferably 50 N / cm or more, more preferably 100 N / cm or more, and even more preferably 150 N / cm or more, sufficient thermal bonding can be achieved, resulting in a nonwoven fabric with excellent mechanical properties. Furthermore, by setting the linear pressure of the hot embossing roll to preferably 500 N / cm or less, more preferably 400 N / cm or less, and even more preferably 300 N / cm or less, excessive thermal bonding can be suppressed, resulting in a nonwoven fabric with excellent flexibility.
[0145] Furthermore, in order to adjust the thickness of the nonwoven fabric, after the thermal bonding by the above-mentioned thermal embossing roll, thermocompression bonding can be further performed by a thermal calender roll consisting of a pair of upper and lower flat rolls. The pair of upper and lower flat rolls refers to metal rolls or elastic rolls with smooth surfaces, and a pair of metal rolls or a pair of metal rolls and elastic rolls can be used.
[0146] Here, the elastic roll refers to a roll made of a material that has greater elasticity than a metal roll. Examples of elastic rolls include so-called paper rolls made of paper, cotton, aramid paper, etc., and resin rolls made of urethane resin, epoxy resin, silicone resin, polyester resin, hard rubber, and mixtures of these.
[0147] (d) Other post-processing steps The nonwoven fabric of the present invention can be post-processed to the extent that the effects of the present invention are not impaired. Of course, in the present invention, the nonwoven fabric obtained by performing this post-processing step is also considered to be the nonwoven fabric of the present invention. Examples of post-processing include physical processing such as drilling and rubbing, and chemical processing such as hydrophilization and charging.
[0148] [Laminated Nonwoven Fabric] The nonwoven fabric of the present invention can be used as is, but it is also preferable to form a laminated nonwoven fabric having a layer of the nonwoven fabric and a fiber layer or film layer of a type different from that of the nonwoven fabric layer.
[0149] Here, the term "a fiber layer of a type different from the layer of the nonwoven fabric" as used herein refers to, for example, when the nonwoven fabric is a spunbond nonwoven fabric, a meltblown nonwoven fabric layer formed by a meltblowing method, a staple fiber nonwoven fabric layer formed by a papermaking method, or a woven or knitted fabric layer made of long fibers or spun yarns.
[0150] The laminated nonwoven fabric according to the present invention has a lamination structure in which at least one layer of the nonwoven fabric of the present invention is laminated. By laminating at least one layer of the nonwoven fabric, the nonwoven fabric acts as a reinforcing material, resulting in a laminated nonwoven fabric with excellent mechanical properties.
[0151] Furthermore, the method for producing the laminated nonwoven fabric according to the present invention is not particularly limited, but examples include a method in which the nonwoven fabric of the present invention is overlaid on a fiber layer or film layer of a type different from that of the nonwoven fabric layer without bonding, or a method in which part or all of the layers are integrated using an adhesive or thermal bonding processing.
[0152] Of course, the laminated nonwoven fabric of the present invention can also be post-processed in the same manner as the nonwoven fabric described above, provided that the effects of the present invention are not impaired. In the present invention, the laminated nonwoven fabric obtained by this post-processing step is also considered to be the laminated nonwoven fabric of the present invention.
[0153] The resin constituting the structure other than the nonwoven fabric of the present invention is not particularly limited, but is preferably a polypropylene-based resin because it is easy to bond.
[0154] [Hygiene Material] The hygienic material of the present invention is made using the nonwoven fabric or the laminated nonwoven fabric described above. More specifically, it comprises at least a portion of the nonwoven fabric or the laminated nonwoven fabric described above. The nonwoven fabric or the laminated nonwoven fabric described above has excellent flexibility and texture, a uniform texture, and sufficient strength for practical use, resulting in a hygienic material that is comfortable to wear. The hygienic material referred to here refers to primarily disposable items used for health-related purposes, such as medical care and nursing. Examples of the hygienic material of the present invention include disposable diapers, sanitary napkins, gauze, bandages, masks, gloves, adhesive bandages, and the like, and also includes components thereof, such as the top sheet, back sheet, and side gathers of disposable diapers. In particular, the hygienic material is preferably used for the back sheet of disposable diapers, which require high strength and flexibility.
[0155] Next, the nonwoven fabric of the present invention will be described in more detail based on examples, although the present invention is not limited to these examples.
[0156] [Measurement and Evaluation Methods] The property values in the examples were determined by the following methods. Unless otherwise specified, measurements were carried out according to the methods described above.
[0157] A. Propylene Fraction, Isotactic Pentad Fraction Measurements were carried out as described above using a nuclear magnetic resonance apparatus "ECZ-600" manufactured by JEOL RESONANCE under the following conditions. Measurement method: single 13 C pulse with inverse gated 1 H decoupling Observation kernel: 13 C Observation frequency: 150.9 MHz Chemical shift reference: orthodichlorobenzene-d 4 (133.0ppm) - Measurement temperature: 135°C.
[0158] B. Melt Flow Rate (MFR A , MFR B、 MFR B -MFR AThe melt flow rate was measured as described above using a "MELT INDEXER F-F01" manufactured by Toyo Seiki Seisakusho Co., Ltd. as the melt flow rate measuring device.
[0159] C. Weight-average molecular weight (Mw) and polydispersity (Mw / Mn) Measurements were carried out as described above using a "PL-220" manufactured by Polymer Laboratories as a high-temperature GPC apparatus under the following conditions: Standard sample: monodisperse polystyrene manufactured by Tosoh Corporation, dibenzyl manufactured by Tokyo Chemical Industry Co., Ltd. Injection volume: 0.200 mL Flow rate: 1.0 mL / min Guard column: Shodex HT-G manufactured by Showa Denko K.K. Column: Shodex HT-806M (2 columns) manufactured by Showa Denko K.K. Detector: differential refractive index detector RI.
[0160] D. Average Single Fiber Diameter and Spinning Speed Measurements were carried out as described above using a scanning electron microscope "SU1510" manufactured by Hitachi High-Technologies Corporation and image analysis software "WinROOF2015" manufactured by Mitani Shoji Co., Ltd. The spinning speed (km / min) was calculated from the obtained average single fiber diameter, the density measured by the above-mentioned method, and the single-hole output rate according to the above-mentioned formula.
[0161] E. Molecular orientation parameter (O C , O S , O C -O S The Raman spectrometer used was a "RAMANOR T64000" manufactured by Horiba Ltd., and measurements were carried out as described above under the following conditions: Measurement mode: Microscopic Raman Beam diameter: 1 μm Light source: Ar + Laser / 514.4 nm; Laser power: 100 mW; Diffraction grating: Single 1800 gr / mm; Slit: 100 μm; Detector: CCD (1024×256).
[0162] F. Tensile Strength of Composite Fiber The tensile strength (cN / dtex) of the composite fiber was measured and calculated by the above-mentioned method using a tensile tester "RTC1210A" manufactured by A&D Co., Ltd.
[0163] G. Melting Point and Heat of Crystal Fusion Measurements were carried out as described above using a differential scanning calorimeter "DSC Q2000" manufactured by TA Instruments.
[0164] H. Crystallite Size of the (040) Plane of the Fused Portion of the Nonwoven Fabric and the (110) Plane of the Nonfused Portion of the Nonwoven Fabric The crystallite sizes (nm) of the (040) plane of the fused portion of the nonwoven fabric and the (110) plane of the nonfused portion of the nonwoven fabric were measured and calculated by the method described above using a wide-angle X-ray diffraction measurement device, "D8 DISCOVER μHR Hybrid" manufactured by Bruker AXS.
[0165] I. Basis Weight Measurement was carried out as described above in accordance with "6.2 Mass per unit area" of JIS L1913:2010 "Test methods for general nonwoven fabrics."
[0166] J. Tensile strength per unit area A tensile tester "RTC-1210A" manufactured by A&D Co., Ltd. was used, and measurements were carried out as described above in accordance with "6.3 Tensile strength and elongation (ISO method)" of JIS L1913:2010 "General nonwoven fabric testing methods."
[0167] K. Bending Resistance Measurement was carried out as described above in accordance with "6.7.3 41.5° Cantilever Method" in "6.7 Bending Resistance (JIS Method and ISO Method)" of JIS L1913:2010 "Testing Methods for General Nonwoven Fabrics."
[0168] [Polypropylene Resin] The polypropylene resins used in the examples of the present invention are as follows.
[0169] [Polypropylene Resin A1] This is a propylene homopolymer obtained using a metallocene catalyst (denoted as "M" in Tables 1 to 4). This polypropylene resin A1 has a propylene fraction of 100.0%, an MFR of 30 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.4.
[0170] [Polypropylene Resin A2] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin A2 has a propylene fraction of 100.0%, an MFR of 36 g / 10 min, an isotactic pentad fraction of 91.0%, and a polydispersity (Mw / Mn) of 2.9.
[0171] [Polypropylene Resin A3] This is a propylene homopolymer obtained using a Ziegler-Natta catalyst (denoted as "ZN" in Tables 1 to 4). This polypropylene resin A3 has a propylene fraction of 100.0%, an MFR of 35 g / 10 min, an isotactic pentad fraction of 95.0%, and a polydispersity (Mw / Mn) of 3.7.
[0172] [Polypropylene Resin A4] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin A4 has a propylene fraction of 100.0%, an MFR of 36 g / 10 min, an isotactic pentad fraction of 93.0%, and a polydispersity (Mw / Mn) of 2.6.
[0173] [Polypropylene Resin A5] This is a propylene homopolymer obtained using a Ziegler-Natta catalyst. This polypropylene resin A5 has a propylene fraction of 100.0%, an MFR of 36 g / 10 min, an isotactic pentad fraction of 95.0%, and a polydispersity (Mw / Mn) of 3.4.
[0174] [Polypropylene Resin A6] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin A6 has a propylene fraction of 100.0%, an MFR of 150 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.1.
[0175] [Polypropylene Resin A7] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin A6 has a propylene fraction of 100.0%, an MFR of 9 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.8.
[0176] [Polypropylene Resin B1] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin B1 has a propylene fraction of 100.0%, an MFR of 60 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.0.
[0177] [Polypropylene Resin B2] This is an ethylene-propylene copolymer obtained using a metallocene catalyst. This polypropylene resin B2 has a propylene fraction of 98.5%, an MFR of 60 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.6.
[0178] [Polypropylene Resin B3] This is an ethylene-propylene copolymer obtained using a metallocene catalyst. This polypropylene resin B3 has a propylene fraction of 90.0%, an MFR of 60 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.0.
[0179] [Polypropylene Resin B4] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin B4 has a propylene fraction of 100.0%, an MFR of 50 g / 10 min, an isotactic pentad fraction of 60.0%, and a polydispersity (Mw / Mn) of 2.0.
[0180] [Polypropylene Resin B5] This is a propylene homopolymer obtained using a Ziegler-Natta catalyst. This polypropylene resin B5 has a propylene fraction of 100.0%, an MFR of 60 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 3.5.
[0181] [Polypropylene Resin B6] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin B6 has a propylene fraction of 100.0%, an MFR of 230 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.1.
[0182] [Polypropylene Resin B7] This is an ethylene-propylene copolymer obtained using a metallocene catalyst. This polypropylene resin B7 has a propylene fraction of 93.0%, an MFR of 50 g / 10 min, an isotactic pentad fraction of 45.0%, and a polydispersity (Mw / Mn) of 2.1.
[0183] [Polypropylene Resin B8] This is a propylene homopolymer obtained using a Ziegler-Natta catalyst. This polypropylene resin B8 has a propylene fraction of 100.0%, an MFR of 60 g / 10 min, an isotactic pentad fraction of 95.0%, and a polydispersity (Mw / Mn) of 4.0.
[0184] [Polypropylene Resin B9] This is a propylene homopolymer obtained using a metallocene catalyst. This polypropylene resin B9 has a propylene fraction of 100.0%, an MFR of 30 g / 10 min, an isotactic pentad fraction of 94.0%, and a polydispersity (Mw / Mn) of 2.4.
[0185] Example 1 (a) Fiber Forming Step The following polypropylene-based resins were used: Polypropylene-based resin A: Polypropylene-based resin A1 Polypropylene-based resin B: Polypropylene-based resin B1 Each of the polypropylene-based resins A and B was melt-extruded using a single-screw extruder and metered using a gear pump to be supplied to a spinneret such that polypropylene-based resin A constituted the island component and polypropylene-based resin B constituted the sea component. The mass ratio of polypropylene-based resin A to polypropylene-based resin B was adjusted to polypropylene-based resin A:polypropylene-based resin B = 70:30. The spinneret temperature was set to 230°C, and the polypropylene-based resin was extruded from a spinneret hole having a hole diameter D of 0.3 mm and a hole depth L of 0.6 mm at a single-hole throughput rate of 0.40 g / min. The spinneret used had a straight inlet hole located directly above the spinneret hole, and a tapered connection between the inlet hole and the spinneret hole. The number of island components (the number of islands when formed into a composite fiber) of the polypropylene-based resin A1 was 1.
[0186] The extruded fibrous resin was cooled and solidified by blowing cooling air at a temperature of 10°C and a speed of 60 m / min from the outside, and then pulled by the air flow using a rectangular ejector to obtain fibers. In this case, cooling was started 20 mm downstream from the nozzle hole of the composite spinneret, and the distance from the spinneret to the ejector inlet was 550 mm.
[0187] (b) Step of forming a fiber web Subsequently, the fibers obtained above were spread by passing through a spreading section where the surrounding air flow velocity was reduced, and then the fibers were landed on a net conveyer where air was sucked from the back side, to obtain a fiber web made of composite fibers. Thereafter, the collected fiber web was transported at a speed of 8 m / min.
[0188] (c) Step of bonding the obtained fiber web Subsequently, the fiber web made of the composite fiber obtained as described above was thermally bonded at a temperature of 125°C using a pair of upper and lower thermal embossing rolls consisting of a metal embossing roll with an upper roll engraved with a polka dot pattern and an adhesive area ratio of 11% and a metal flat roll as a lower roll, to obtain a nonwoven fabric. The evaluation results of the obtained nonwoven fabric are shown in Table 1.
[0189] [Examples 2 and 3] Nonwoven fabrics were obtained in the same manner as in Example 1, except that in the (a) fiber-forming step, the mass ratio of polypropylene-based resin A to polypropylene-based resin B was changed from polypropylene-based resin A:polypropylene-based resin B = 70:30 to polypropylene-based resin A:polypropylene-based resin B = 80:20 in Example 2 and polypropylene-based resin A:polypropylene-based resin B = 50:50 in Example 3. The evaluation results of the obtained nonwoven fabrics are shown in Table 1.
[0190] [Examples 4 and 5] (a) In the step of forming fibers, the spinning speed was 2.5 km / min, but was changed to 4.4 km / min in Example 4 and 3.8 km / min in Example 5, to obtain nonwoven fabrics in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabrics are shown in Table 1.
[0191] [Comparative Example 1] (a) Fiber Forming Step For the polypropylene-based resin, the polypropylene-based resin A1 was melt-extruded using a single-screw extruder and metered using a gear pump while being supplied to a spinneret. The temperature of the spinneret was 230°C, and the polypropylene-based resin was extruded from a spinneret hole having a hole diameter D of 0.3 mm and a hole depth L of 0.6 mm at a single-hole output rate of 0.40 g / min. The spinneret used had a straight inlet hole located directly above the spinneret hole, and a tapered connection between the inlet hole and the spinneret hole.
[0192] The extruded fibrous resin was cooled and solidified by blowing cooling air at a temperature of 10°C and a speed of 60 m / min from the outside, and then pulled by an air flow using a rectangular ejector to obtain fibers. In this case, cooling was started 20 mm downstream from the nozzle hole of the composite spinneret, and the distance from the spinneret to the ejector inlet was 550 mm.
[0193] (b) Step of forming a fiber web Subsequently, the fibers obtained above were spread by passing through a spreading section where the surrounding air flow velocity was reduced, and then landed on a net conveyer where air was sucked from the back side, to obtain a fiber web composed of single component fibers. Thereafter, the collected fiber web was transported at a speed of 8 m / min.
[0194] (c) Step of bonding the obtained fiber web Subsequently, the fiber web made of the monocomponent fiber obtained as described above was thermally bonded at a temperature of 125°C using a pair of upper and lower thermal embossing rolls consisting of a metal embossing roll with an upper roll engraved with a polka dot pattern and an adhesive area ratio of 11% and a metal flat roll as a lower roll, to obtain a nonwoven fabric. The evaluation results of the obtained nonwoven fabric are shown in Table 1.
[0195]
[0196] [Example 6, Comparative Example 2] (a) In the step of forming fibers, nonwoven fabrics were obtained in the same manner as in Example 1, except that polypropylene-based resin B was changed from polypropylene-based resin B1 to polypropylene-based resin B2 in Example 6 and polypropylene-based resin B3 in Comparative Example 2. The evaluation results of the obtained nonwoven fabrics are shown in Table 2.
[0197] [Example 7] A nonwoven fabric was obtained in the same manner as in Example 1, except that in the (a) fiber-forming step, polypropylene-based resin A was changed from polypropylene-based resin A1 to polypropylene-based resin A2. The evaluation results of the obtained nonwoven fabric are shown in Table 2.
[0198] [Comparative Example 3] A nonwoven fabric was obtained in the same manner as in Example 1, except that in the (a) fiber-forming step, polypropylene-based resin B was changed from polypropylene-based resin B1 to polypropylene-based resin B4. The evaluation results of the obtained nonwoven fabric are shown in Table 2.
[0199] [Comparative Example 4] A nonwoven fabric was obtained in the same manner as in Example 1, except that in the (a) fiber-forming step, polypropylene-based resin A was changed from polypropylene-based resin A1 to polypropylene-based resin A3, and polypropylene-based resin B was changed from polypropylene-based resin B1 to polypropylene-based resin B5. The evaluation results of the obtained nonwoven fabric are shown in Table 2.
[0200] [Example 8] A nonwoven fabric was obtained in the same manner as in Example 1, except that in the (a) fiber-forming step, polypropylene-based resin B was changed from polypropylene-based resin B1 to polypropylene-based resin B6. The evaluation results of the obtained nonwoven fabric are shown in Table 2.
[0201]
[0202] [Example 9] A nonwoven fabric was obtained in the same manner as in Example 1, except that in the (a) fiber-forming step, the mass ratio of polypropylene-based resin A to polypropylene-based resin B was changed from polypropylene-based resin A:polypropylene-based resin B = 70:30 to polypropylene-based resin A:polypropylene-based resin B = 60:40. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0203] [Example 10] A nonwoven fabric was obtained in the same manner as in Example 8, except that (a) in the step of forming fibers, the spinning speed was changed from 2.5 km / min to 3.0 km / min, and (c) in the step of adhesively processing the obtained fiber web, the temperature of the embossing roll was changed from 125°C to 120°C. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0204] [Example 11] A nonwoven fabric was obtained in the same manner as in Example 1, except that (a) in the step of forming fibers, polypropylene-based resin A4 was used instead of polypropylene-based resin A1, the spinning speed was changed from 2.5 km / min to 2.0 km / min, and (c) in the step of adhesively processing the obtained fiber web, the temperature of the embossing roll was changed from 125°C to 135°C. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0205] [Example 12] A nonwoven fabric was obtained in the same manner as in Example 10, except that in the (a) fiber-forming step, the single-hole output rate was changed from 0.40 g / min to 0.80 g / min and the spinning speed was changed from 3.0 km / min to 2.5 km / min. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0206] [Comparative Example 5] A nonwoven fabric was obtained in the same manner as in Example 1, except that (a) in the step of forming fibers, polypropylene-based resin B7 was used instead of polypropylene-based resin B1, and (c) in the step of adhesively processing the obtained fiber web, the temperature of the embossing roll was changed from 125°C to 110°C. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0207] [Comparative Example 6] A nonwoven fabric was obtained in the same manner as in Example 1, except that (a) in the step of forming fibers, polypropylene-based resin A5 was used instead of polypropylene-based resin A1, the spinning speed was changed from 2.5 km / min to 2.1 km / min, and (c) in the step of adhesively processing the obtained fiber web, the temperature of the embossing roll was changed from 125°C to 140°C. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0208]
[0209] [Comparative Example 7] A nonwoven fabric was obtained in the same manner as in Comparative Example 1, except that (a) in the step of forming fibers, the spinning speed was changed from 2.5 km / min to 3.1 km / min, and further, (c) in the step of adhesively processing the obtained fiber web, the temperature of the embossing roll was changed from 125°C to 135°C. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0210] [Comparative Example 8] (a) In the step of forming fibers, polypropylene-based resin A6 was used instead of polypropylene-based resin A1, polypropylene-based resin B6 was used instead of polypropylene-based resin B1, and the spinning speed was changed from 2.5 km / min to 3.0 km / min, except that a nonwoven fabric was obtained in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0211] [Comparative Example 9] (a) In the step of forming fibers, polypropylene-based resin A5 was used instead of polypropylene-based resin A1, polypropylene-based resin B8 was used instead of polypropylene-based resin B1, and the spinning speed was changed from 2.5 km / min to 2.0 km / min, except that a nonwoven fabric was obtained in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0212] [Comparative Example 10] (a) An attempt was made to obtain a nonwoven fabric by the same method as in Example 1, except that in the fiber-forming step, polypropylene-based resin A7 was used instead of polypropylene-based resin A1, and polypropylene-based resin B9 was used instead of polypropylene-based resin B1. However, because the melt flow rates of the polypropylene-based resins used were low, it was not possible to obtain composite fibers and nonwoven fabrics.
[0213]
[0214] The nonwoven fabrics of Examples 1 to 12 have a propylene fraction of 98.5% or more and 100.0% or less, an isotactic pentad fraction of 90.0% or more and 100.0% or less, and C -O S The nonwoven fabric was made of composite fibers with a melting point of 130° C. or higher and 155° C. or lower, which indicates that the nonwoven fabric was excellent in flexibility and mechanical properties.
[0215] On the other hand, the nonwoven fabrics of Comparative Examples 1, 7, and 8 were O C -O S The nonwoven fabrics of Comparative Examples 2 and 5 had low propylene fractions, and therefore both had poor tensile strength per unit area. The nonwoven fabric of Comparative Example 3 had a low isotactic pentad fraction, and the nonwoven fabrics of Comparative Examples 4, 6, and 9 had high melting points, and therefore also had poor tensile strength per unit area. Furthermore, a nonwoven fabric could not be obtained in Comparative Example 10.
[0216] 1: Test piece 11: Welded part 12: Inscribed circle of fused part 13: Point at a distance of 50% or less of the radius of the inscribed circle from the center of the inscribed circle of the fused part
Claims
1. A nonwoven fabric made of composite fibers mainly composed of polypropylene resin, the composite fibers having a propylene fraction of 98.5% or more and 100.0% or less, an isotactic pentad fraction of 90.0% or more and 100.0% or less, and a molecular orientation parameter O in the fiber axis direction at the center of the fiber. C and the molecular orientation parameter O in the fiber axis direction at the fiber surface. S Difference with (O C -O S ) is 0.2 or more and 4.0 or less, and the melting point of the nonwoven fabric is 130°C or more and 155°C or less.
2. The nonwoven fabric according to claim 1, wherein the heat of crystalline fusion of the nonwoven fabric is 82 J / g or more and 120 J / g or less.
3. Molecular orientation parameter O in the fiber axis direction at the center of the fiber C The nonwoven fabric according to claim 1 or 2, wherein the linear modulus is 5.0 or more and 10.0 or less.
4. The nonwoven fabric according to claim 1 or 2, wherein the nonwoven fabric is a spunbonded nonwoven fabric.
5. The nonwoven fabric according to claim 1 or 2, having fused portions and non-fused portions, wherein the fused portions have a crystallite size of (040) plane in wide-angle X-ray diffraction of 10.0 nm or more and 13.5 nm or less, and the non-fused portions have a crystallite size of (110) plane in wide-angle X-ray diffraction of 5.0 nm or more and 10.0 nm or less.
6. A method for producing a nonwoven fabric as claimed in claim 1, comprising the steps of: melt-extruding, from a composite spinneret, polypropylene-based resin A which has been polymerized by a metallocene catalyst and has a propylene fraction of 98.5% or more and 100.0% or less; and polypropylene-based resin B which has a melt flow rate higher than that of polypropylene-based resin A by 6 g / 10 min to 200 g / 10 min and which has been polymerized by a metallocene catalyst and has a propylene fraction of 98.5% or more and 100.0% or less; and pulling and stretching the spun polypropylene-based resin A and polypropylene-based resin B to form islands-in-sea type composite fibers having island components as said polypropylene-based resin A and a sea component as said polypropylene-based resin B; stacking the islands-in-sea type composite fibers to form a fiber web composed of the islands-in-sea type composite fibers; and thermally bonding the fiber web.
7. The method for producing a nonwoven fabric according to claim 6, wherein the polypropylene resin A has a melt flow rate of 10 g / 10 min or more and 90 g / 10 min or less.
8. The method for producing a nonwoven fabric according to claim 6 or 7, wherein the isotactic pentad fraction of the polypropylene-based resin A and / or the polypropylene-based resin B is 90.0% or more and 100.0% or less.
9. The method for producing a nonwoven fabric according to claim 6 or 7, wherein the number of islands in the islands-in-the-sea type composite fiber is 1 or more and 10 or less.
10. The method for producing a nonwoven fabric according to claim 6 or 7, wherein the polydispersity (Mw / Mn) of the polypropylene resin A in molecular weight measurement is 1.5 or more and 3.5 or less.
11. A sanitary material comprising the nonwoven fabric according to claim 1 or 2.
12. A laminated nonwoven fabric comprising a layer of the nonwoven fabric according to claim 1 or 2 and a fiber layer different from the layer of the nonwoven fabric.
13. A sanitary material comprising the laminated nonwoven fabric according to claim 12.
Citation Information
Patent Citations
Hot-melt conjugate and fiber aggregate
JP1993009809A
Polypropylene yarn
JP1993321019A
Polyolefin fibers and nonwoven fabric produced using the same
WO1997040216A1
Rubber-fiber composite, rubber-resin composite and pneumatic tire in which same is used
WO2017030121A1
Spunbond nonwoven fabric, laminate nonwoven fabric, manufacturing method of these and sanitary material
WO2022196527A1