Silver powder, mixed silver powder and conductive paste, and method for producing silver powder and mixed silver powder
By optimizing silver powder particle orientation and mechanical properties, the silver powders and pastes achieve reduced electrode wiring resistance and improved printability, addressing the challenge of forming fine lines with low resistance and high conductivity.
Patent Information
- Application Number
- PCT/JP2024/018223
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional silver powders and pastes struggle to reduce the resistance of electrode wiring to 15 μm or less while maintaining printability and conductivity, especially when forming fine lines, due to limitations in particle orientation and aspect ratio.
The development of silver powders with a high percentage of (111) plane-oriented particles and controlled KAM values, combined with mechanical strain and specific surface area optimization, to create a conductive paste that enhances electrode wiring conductivity and printability.
The resulting silver powders and pastes achieve reduced electrode wiring resistance and improved printability, enabling the formation of fine lines with lower resistance and increased conductivity.
Smart Images

Figure JP2024018223_21112024_PF_FP_ABST
Abstract
Description
Silver powder, mixed silver powder, conductive paste, and method for producing silver powder and mixed silver powder
[0001] The present invention relates to a silver powder, a mixed silver powder, a conductive paste, and a method for producing the silver powder and the mixed silver powder.
[0002] Conductive pastes containing a mixture of spherical silver powder and flat flake silver powder as a filler and a resin component are used in applications such as forming electrode circuits in solar cells, filling via holes, and as adhesives for mounting components.
[0003] Patent Document 1 describes a silver paste comprising silver powder as a filler, a resin component, and an organic solvent, in which the silver powder is a mixed silver powder obtained by mixing microspherical silver powder having an average primary particle size of 0.6 μm or less and ultrathin plate-like silver powder having an average primary particle thickness of 50 nm or less.
[0004] Patent Document 2 describes silver particles that are flake-shaped, have a single crystal structure, and have the largest plane of the lattice plane (111).
[0005] JP 2005-285673 A JP 2019-173120 A
[0006] Conventionally, the line width of electrode wiring has been about 25 μm, but there is a demand for the line width to be narrowed to 15 μm or less. When forming thin wires using conductive paste, there is a demand for printing to be possible without wire breakage, and for the resistance of the electrode wiring to be further reduced.
[0007] Therefore, the present invention aims to obtain silver powder and mixed powders that can achieve even lower resistance in electrode wiring when fine lines are printed, as well as conductive pastes using the same, and provides a method for producing such silver powder.
[0008] As a result of intensive research into achieving the above-mentioned object, the inventors have completed the present invention, which is summarized as follows:
[0009] (1) A silver powder containing silver particles whose main upper surface region is a (111) plane or a plane close to a (111) plane in an amount of 20% or more but less than 95% of all particles, and wherein the KAM value of the silver particles is 0.4 or more and 1.0 or less.
[0010] (2) The silver powder according to (1), wherein the aspect ratio, calculated by dividing the volume-based median diameter by the laser diffraction method by the average thickness of the cross-section of the silver particles, is 1.2 or more and less than 4.0.
[0011] (3) The silver powder according to (1) or (2), wherein the average thickness of the silver particles measured in cross section is 310 nm or more.
[0012] (4) A method for producing silver powder, comprising applying mechanical energy to highly crystalline silver powder in which 30% or more of the total particles contain silver particles whose main region on the upper surface is a (111) plane or a plane close to a (111) plane, and the KAM value of the silver particles is less than 0.4, to impart strain to the silver particles until the KAM value of the silver particles becomes 0.4 or more and 1.0 or less.
[0013] (5) A method for producing silver powder according to (4), in which an amino acid is added to a silver chelate complex solution to prepare a solution, and then an ascorbic acid-based reducing agent is added to obtain the highly crystalline silver powder.
[0014] (6) A method for producing silver powder according to (4) or (5), wherein the silver powder after the strain is imparted has an aspect ratio of 1.2 or more and less than 4.0, calculated by dividing the volume-based median diameter by a laser diffraction method by the average thickness of the cross-section of the silver particles.
[0015] (7) A method for producing silver powder according to any one of (4) to (6), wherein the highly crystalline silver powder has an average thickness of 310 nm or more when measured in cross section, and the silver powder after being subjected to the strain has an average thickness of 310 nm or more when measured in cross section.
[0016] (8) A method for producing a mixed silver powder, which comprises mixing the silver powder according to any one of (1) to (3) with fine silver powder having a larger specific surface area than the silver powder.
[0017] (9) A method for producing a mixed silver powder according to (8), in which the silver powders according to any one of (1) to (3) are mixed so that the mixing ratio is 10 wt % to 90 wt %.
[0018] (10) A mixed silver powder containing at least silver particles whose upper surface main region is a (111) plane or a plane close to a (111) plane, and whose KAM value is 0.4 or more and 1.0 or less.
[0019] (11) The specific surface area after mixing is 0.20 m 2 / g or more 1.50m 2 / g or less.
[0020] (12) A conductive paste containing the silver powder according to any one of (1) to (3), a resin component, and a solvent.
[0021] (13) A conductive paste containing the mixed silver powder according to (10) or (11), a resin component, and a solvent.
[0022] According to the present invention, it is possible to obtain silver powder and mixed powder that can achieve low resistance of electrode wiring when fine lines are printed, and further, a conductive paste using the same.
[0023] 1 is a diagram illustrating a surface close to the (111) plane in the present invention. It is a diagram showing an SEM image of silver particles of a silver powder according to Example 1, in which the main region of the upper surface of the silver particle is the (111) plane or a surface close to the (111) plane, together with an IPF map and a KAM map obtained by EBSD measurement of the upper surface of the silver particle. It is a diagram showing an SEM image of silver particles of a silver powder according to Example 2, in which the main region of the upper surface of the silver particle is the (111) plane or a surface close to the (111) plane, together with an IPF map and a KAM map obtained by EBSD measurement of the upper surface of the silver particle. It is a diagram showing an SEM image of silver particles of a silver powder according to Example 3, in which the main region of the upper surface of the silver particle is the (111) plane or a surface close to the (111) plane, together with an IPF map and a KAM map obtained by EBSD measurement of the upper surface of the silver particle. 1 is a diagram showing an SEM image of silver particles of Comparative Example 1, in which the main region of the upper surface of the silver particle is the (111) plane, together with an IPF map and a KAM map obtained by EBSD measurement of the upper surface of the silver particle. 2 is a diagram showing an SEM image of silver particles of Comparative Example 2, in which the main region of the upper surface of the silver particle is the (111) plane or a plane close to the (111) plane, together with an IPF map and a KAM map obtained by EBSD measurement of the upper surface of the silver particle. 3 is an SEM image of silver particles of Comparative Example 3, together with an IPF map and a KAM map obtained by EBSD measurement of the upper surface of the silver particle. 4 is an SEM image of Example 1 at 2000x magnification. 5 is an SEM image of Comparative Example 3 at 2000x magnification.
[0024] Before describing the embodiments of the silver powder according to the present invention, the terms used in this specification will be explained.
[0025] <Plane Orientation> The plane orientation of the silver powder according to the present invention is identified by mapping based on a color sample of a stereo triangular diagram with the (111), (001), and (101) planes as vertices in an orientation distribution (IPF map) measured by electron backscatter diffraction (EBSD). In this measurement, a crystalline sample on a stage in a SEM chamber is tilted significantly so that the stage tilt (Tilt) is 60° to 70°, and an electron beam is irradiated onto the sample at a specified angle of incidence. The diffracted electrons reflected by the sample are captured by the EBSD camera to obtain a Kikuchi pattern. An orientation distribution (IPF map) for the upper surface of the silver particles is then created. In the examples, an EBSD analyzer (OIM Analysis 6.2 manufactured by TSL Solutions Co., Ltd.) was used to perform measurements in a measurement range of 60 μm × 180 μm with a step size of 0.30 μm. SEM observation was performed under conditions of an acceleration voltage of 15 kV, a magnification of 1500x, and a tilt of 70°. Measurement points with low reliability, where the reliability index (CI value) was 0.2 or less, were excluded, and an orientation distribution (Inverse Pole Figure (IPF)) map was created and evaluated. Since an electron beam irradiated to a location other than the top surface of the silver particle fails to obtain sufficient diffracted electrons or results in a low reliability index, measurement points that are not on the top surface of the silver particle can be excluded by setting the reliability index. Therefore, the region for which the IPF map is created is defined as the top surface of the silver particle in the present invention.
[0026] <Faces Close to the (111) Face> In an IPF map measured by EBSD, each point on the map is mapped based on a stereo triangular color sample graph, with the vertices representing the (111), (001), and (101) faces. A schematic diagram of the color sample of this mapping is shown in Figure 1. In practice, each point on the IPF map and color sample graph is distinguished by RGB color; for example, the (111) face is RGB = (0,0,255) (color name: blue), the (001) face is RGB = (255,0,0) (color name: red), and the (101) face is RGB = (0,255,0) (color name: green). In the CSS color code of Figure 1, area A (the area with a color close to blue) surrounded by straight lines at RGB = (0,0,255), RGB = (0,85,255), RGB = (85,85,255), and RGB = (85,0,255) is treated as the "surface close to the (111) plane" in this specification. When the main region of the upper surface of a silver particle in an IPF map observed during actual observation of the silver particle is represented by a color corresponding to area A in this color sample graph, the surface of the silver particle can be considered as the "surface close to the (111) plane." Furthermore, the "main region" refers to 60% or more of the area colored in this IPF map. In this specification, the percentage is determined by evaluating 15 or more silver particles observed on the IPF map. That is, when 60% or more of the upper surface of a silver particle observed on an IPF map is a surface close to the (111) plane, the silver particle is said to be a silver particle in which the main region of the upper surface of the silver particle is a (111) plane or a surface close to the (111) plane.
[0027] <KAM Value> The KAM value of a silver particle is determined by increasing the observation magnification so that each silver particle, as confirmed in the above-mentioned IPF map, has a main region on its top surface that is a (111) plane or a plane close to the (111) plane, enlarging the observation so that the field of view includes one silver particle, creating a strain distribution (KAM map) measured by SEM-EBSD for the top surface of the silver particle, and calculating the average value of the strain histogram on the top surface of the silver particle. The strain distribution (Kernel Average Misorientation (KAM)) value of the top surface portion of the silver particle is evaluated for each of 10 or more of the above-mentioned silver particles observed on the IPF map. The KAM value according to the present invention is the average value of the KAM values on the top surfaces of 10 or more silver particles (silver particles whose main region on their top surfaces is a (111) plane or a plane close to the (111) plane). In the examples, the conditions for EBSD analysis were a measurement range of 6 μm × 18 μm, a step size of 40 nm, and SEM observation conditions were a magnification of 15,000 times, but the same conditions for IPF map observation were used to create an orientation distribution (Inverse Pole Figure (IPF)) map of the upper surface of the corresponding silver particle, and then a KAM map was obtained.
[0028] <Median Diameter> The volume-based median diameter of the silver powder according to the present invention, measured by the laser diffraction method, is determined from the particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer. In this embodiment, the following description will be given using a Microtrac particle size distribution analyzer MT-3300EXII (hereinafter simply referred to as the particle size distribution analyzer) manufactured by Microtrac-Bell Corporation as the laser diffraction / scattering particle size distribution analyzer. The particle size distribution of the silver powder may be measured by dispersing the silver powder in a predetermined dispersion medium, i.e., by wet measurement. In the examples, 0.1 g of silver powder was added to 40 mL of isopropyl alcohol as the dispersion medium and dispersed for 2 minutes using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho Co., Ltd., US-150T; 19.5 kHz, tip diameter 18 mm), to prepare a dispersion. This dispersion was then subjected to the particle size distribution analyzer to measure the particle size distribution of the silver powder.
[0029] In this specification, the volume-based median diameter is also referred to as the cumulative 50% diameter or D50. The cumulative 50% diameter is the diameter at which the cumulative particle amount from the smaller particle diameter side in the particle size distribution is 50% on a volume basis. Similarly, the cumulative 10% diameter is the diameter at which the cumulative particle amount from the smaller particle diameter side in the particle size distribution is 10% on a volume basis. The cumulative 90% diameter is the diameter at which the cumulative particle amount from the smaller particle diameter side in the particle size distribution is 90% on a volume basis. Hereinafter, the volume-based cumulative 10% diameter, cumulative 50% diameter, and cumulative 90% diameter may be referred to as D10, D50, and D90, respectively.
[0030] <Average Thickness> The average thickness in cross-sectional measurements of silver particles in the silver powder according to the present invention refers to the average value of thicknesses determined based on SEM images of the cross sections of the silver particles. In the examples, SEM images for understanding the cross-sectional shape of the silver particles were obtained by polishing resin-solidified silver powder with a cross-section polisher, ArBlade 5000 (manufactured by Hitachi High-Technologies Corporation), to expose the cross section, and then observing the cross section of the silver particle under an SEM at 5000x magnification. The thickness of the silver particles refers to the short side of a rectangle with the smallest area surrounding each particle image in the SEM image of the silver particle cross section. The average thickness refers to the average value of the short side measured when 20 or more silver particles are imaged in the thickness measurement.
[0031] <Aspect Ratio> In addition, for the silver powder according to the present invention, the aspect ratio is the value obtained by dividing the volume-based median diameter by the laser diffraction method by the average thickness of the silver particles measured in cross section, and is referred to as "the aspect ratio obtained by dividing the volume-based median diameter by the laser diffraction method by the average thickness of the silver particles measured in cross section."
[0032] <Specific Surface Area> The specific surface area (SSA) of the silver powder according to the present invention is measured using the BET method. In the examples, values measured using a Macsorb HM-model 1210 manufactured by Mountech Co., Ltd. were used.
[0033] The silver powder according to this embodiment will be described in detail below. In this embodiment, the silver powder refers to a powder formed as an aggregate of silver particles (hereinafter simply referred to as silver powder).
[0034] (Silver Powder) The silver powder according to this embodiment contains silver particles whose upper surface predominant region is a (111) plane or a plane close to the (111) plane in SEM-EBSD measurement, accounting for 20% or more but less than 95% of the total particles, and the KAM value of the silver particles is 0.4 or more but 1.0 or less. A conductive paste using these silver particles can achieve low resistance of electrode wiring when fine-line printed.
[0035] In the silver powder according to the present invention, preferably 30% or more, and more preferably 40% or more, of all silver particles have a (111) plane or a plane close to the (111) plane as the main region of their upper surfaces in SEM-EBSD measurement. Even if the silver powder is composed only of planes close to the (111) plane, it is still more preferable that less than 70% of all silver particles have a (111) plane or a plane close to the (111) plane as the main region of their upper surfaces. The content of "silver particles having a (111) plane or a plane close to the (111) plane as the main region of their upper surfaces" in the silver powder is the percentage of silver particles observed to have a (111) plane or a plane close to the (111) plane as the main region of their upper surfaces in an IPF map (mapping based on a color sample graph) of an EBSD measurement in which the silver particles are dispersed and arranged so as to minimize overlapping, relative to the total number of particles observed. Hereinafter, this number percentage will also be referred to as the IPF value.
[0036] Furthermore, the average KAM value obtained by evaluating 10 or more silver particles in which the main region of the upper surface of the silver particle is a (111) plane or a plane close to the (111) plane in SEM-EBSD measurement is 0.4 to 1.0, and preferably 0.5 or more. The silver particles of the present invention have distortion compared to silver particles whose crystals have grown to have a (111) plane, and by having distortion with a KAM value in the range of 0.4 to 1.0, further lower resistance of the electrode wiring can be obtained.
[0037] Furthermore, the silver powder according to the present invention preferably has an average thickness of 310 nm or more when measured through cross sections of the silver particles, and an aspect ratio, calculated by dividing the volume-based median diameter by the average thickness using a laser diffraction method, of 1.2 or more and less than 4.0. When the aspect ratio is in the range of 1.2 or more and less than 4.0, fine line printability is improved compared to flat silver particles having an aspect ratio of 4.0 or more. When the thickness is less than 310 nm, it is difficult to form a dense fired film, and the conductivity of the fired film is likely to decrease. Furthermore, the paste viscosity increases when the paste is formed, which may result in a decrease in paste printability. Furthermore, a large average thickness makes it easier to impart strain that results in the above-mentioned KAM value when "mechanical energy is applied" during the manufacturing process described below. The average thickness is more preferably 400 nm or more, and even more preferably 500 nm or more. Furthermore, it is preferably 3000 nm or less. When it exceeds 3000 nm, fine line printing may become difficult. The aspect ratio is more preferably 1.5 or more, and even more preferably 1.8 or more, and more preferably 3.8 or less, and even more preferably 3.6 or less.
[0038] Silver particles in which the main region of the upper surface of the silver particles in SEM-EBSD measurement is a (111) plane or a plane close to the (111) plane also preferably have a particle shape of approximately polygonal plates or approximately polygonal prisms derived from the face-centered cubic crystal structure of silver. That is, the upper surface of the silver particles is preferably the polygonal upper surface of an approximately polygonal plate, or the polygonal upper surface of an approximately polygonal prism. Furthermore, particle shapes with rounded corners are also preferred, and the approximately polygonal plates or approximately polygonal prisms may have rounded corners as long as a portion of the upper surface (bottom) or side surface is observed to be considered a polygonal plate or a polygonal prism.
[0039] The specific surface area of the silver powder according to the present invention is 0.10 m 2 / g or more 1.00m 2 The lower limit of the specific surface area is preferably 0.15 m / g or less. 2 / g or more is more preferable, and 0.20m 2 The upper limit of the specific surface area is preferably 0.90 m / g or more.2 / g or less is more preferable, and 0.80m 2 It is more preferable that the content is 1 / g or less.
[0040] (Method for producing mixed silver powder) It is also preferable to obtain a mixed silver powder by mixing the silver powder of the present invention with a fine silver powder having a larger specific surface area than the silver powder of the present invention. By mixing the silver powder of the present invention with the fine silver powder, the silver filling rate in the paste can be increased when a conductive paste is formed, thereby further reducing the resistance of the electrode wiring. The proportion of the silver powder of the present invention in the mixed silver powder is preferably 10 wt% to 90 wt%. It is also preferable to mix the silver powder of the present invention at 20 wt% or more, and preferably at 30 wt% or more. It is more preferable to mix the silver powder of the present invention at 80 wt% or less, and even more preferable to mix at 70 wt% or less. The fine silver powder having a larger specific surface area than the silver powder of the present invention can be a silver powder having an IPF value of zero, and it is preferable that the average aspect ratio (long side / short side) of the circumscribed rectangle with the smallest area is less than 1.5. Furthermore, it is more preferable that the average Heywood diameter of a fine silver powder having a larger specific surface area than the silver powder according to the present invention is smaller than the average thickness of the silver particles according to the present invention in cross-sectional measurement, and it is even more preferable that the average Heywood diameter of the fine silver powder is less than 500 nm. The average aspect ratio and average Heywood diameter of the fine silver powder are determined by measuring the long side / short side of the circumscribed rectangle that has the smallest area and the Heywood diameter of a total of 400 or more silver particles using image analysis particle size distribution measurement software (Mac-View, manufactured by Mountech Co., Ltd.) on an SEM image.
[0041] (Mixed Silver Powder) The mixed silver powder according to the present invention contains at least silver particles whose upper surface predominant region is a (111) plane or a plane close to the (111) plane, and the KAM value of the silver particles is 0.4 or more and 1.0 or less. Regardless of the mixing ratio with fine silver powder whose IPF value is zero, if the mixed silver powder contains the silver powder according to the present invention, the IPF map will show silver particles whose upper surface predominant region is a (111) plane or a plane close to the (111) plane. The specific surface area of the mixed silver powder is 0.20 m 2 / g or more 1.50m 2 / g or less, and 2 / g or more 1.20m 2 / g or less is more preferable, and 0.35m 2 / g or more 1.10m 2 A more preferable range suitable for a conductive paste that can be printed with fine lines is a specific surface area of 0.40 m / g or less. 2 / g or more 0.80m 2 / g or less, and most preferably the specific surface area is 0.60 m 2 / g or more 0.75m 2 / g or less.
[0042] Furthermore, in the above-mentioned mixed silver powder, the ratio of the number of silver particles whose upper surface predominantly consists of a (111) plane or a plane close to the (111) plane to the total number of particles (IPF value) measured by SEM-EBSD is difficult to measure because the number of particles per unit weight of the fine silver powder is large. However, for example, in an IPF map containing the silver particles of the present invention within the field of view, the ratio is preferably 0.1% or more, and more preferably 1% or more. On the other hand, the mixed silver powder preferably contains the silver particles at 90% or less of the total particles, more preferably 80% or less, and even more preferably 70% or less. This is because if the proportion of the silver particles is too high, there will be fewer starting points for necking due to polycrystalline particles during electrode formation by heat treatment.
[0043] (Conductive Paste) The conductive paste according to the present invention contains the above-mentioned mixed silver powder, a resin component, and a solvent. The solvent, binder, etc. can be appropriately selected depending on the mode of use.
[0044] (Method for producing silver powder)
[0045] In explaining the method for producing silver powder according to the present invention, a silver powder containing 30% or more silver particles whose upper surface has a main region formed by a (111) plane or a surface close to the (111) plane and having a KAM value of less than 0.4 is referred to as a highly crystalline silver powder. The method for producing silver powder according to the present invention is characterized in that mechanical energy is applied to highly crystalline silver powder containing 30% or more silver particles whose upper surface has a main region formed by a (111) plane or a surface close to the (111) plane, thereby imparting strain to the silver particles until the KAM value of the silver particles reaches 0.4 or more and 1.0 or less. The highly crystalline silver powder preferably has an average thickness of 310 nm or more as measured through cross-section. Furthermore, the silver particles in the silver powder obtained by applying mechanical energy preferably have an average thickness of 310 nm or more as measured through cross-section, and the average aspect ratio is preferably 1.2 or more and less than 4.0. In the highly crystalline silver powder, in silver particles in which the main region of the upper surface of the silver particle is a (111) plane or a plane close to the (111) plane, it is more preferable that the thickness in the direction perpendicular to the (111) plane or a plane close to the (111) plane is 310 nm or more.
[0046] Specific embodiments of a manufacturing method suitable for manufacturing the silver powder according to this embodiment will be described below. Note that the manufacturing method of silver powder described below is one example for realizing the manufacturing of the silver powder according to this embodiment, and the silver powder according to this embodiment is not limited to the silver powder manufactured by the manufacturing method described below.
[0047] First, it is preferable to prepare a silver aqueous solution as a raw material. This silver aqueous solution may be any solution containing silver ions, such as a silver nitrate aqueous solution. The silver aqueous solution may also be a silver aqueous solution containing silver sulfate, silver cyanide, or silver acetate.
[0048] The pH of this silver aqueous solution can be adjusted, followed by temperature adjustment. The pH is preferably 1.0 or higher and 5.0 or lower, and more preferably 1.5 or higher and 3.0 or lower. For example, concentrated nitric acid can be used for the adjustment. The silver particle size can be adjusted by adjusting the pH. The temperature of the silver aqueous solution is preferably 10°C or higher and 35°C or lower, and more preferably 17°C or higher and 30°C or lower. Within this temperature range, silver particles can be recovered by reduction. Furthermore, by adjusting the temperature, the silver particle size can be optimized.
[0049] Next, a chelating compound is preferably mixed as a complexing agent to complex the silver ions in the silver aqueous solution to form a silver chelate complex solution. Examples of chelating compounds include an EDTA-4Na aqueous solution, as well as ethylenediamine, glycine, citric acid, malic acid, succinic acid, alkenylsuccinic acid, and DMSA. Furthermore, it is preferable to add an amino acid as an additive to assist complexation when mixing the chelating compound. For example, an L(+)-arginine aqueous solution can be used, as well as L-alanine, L-asparagine, L-glutamine, L-phenylalanine, L-glutamic acid, L-glutamine, L-aspartic acid, L-glycine, and L-tryptophan. Adding an amino acid increases the thickness of the silver particles, resulting in a highly crystalline silver powder with an average thickness of 310 nm or more.
[0050] A reducing agent is then added to the resulting silver chelate complex solution to produce and precipitate highly crystalline silver powder. It is also preferable to simultaneously add a surface treatment agent to improve dispersibility during precipitation of the highly crystalline silver powder. Known reducing agents can be used as the reducing agent, but it is preferable to use an L-ascorbic acid aqueous solution, a sodium L-ascorbate aqueous solution, an isoascorbic acid aqueous solution, or the like, because they are capable of reduction even in the acidic pH range and allow for easy control of particle size and aspect ratio. Furthermore, fatty acids or salts thereof can be used as surface treatment agents, such as stearic acid emulsion, oleic acid, hardened castor fatty acid, palmitic acid, myristic acid, lauric acid, capric acid, ricinoleic acid, linoleic acid, and linolenic acid.
[0051] Any method and raw materials can be used to produce the above-mentioned highly crystalline silver powder, but it is particularly preferable to add an amino acid to a silver chelate complex solution to prepare the solution, and then add an ascorbic acid-based reducing agent, as this causes the highly crystalline silver powder to grow thickly and is well dispersed, making it easy to process mechanically.
[0052] Furthermore, the highly crystalline silver powder in the slurry (suspension) obtained by the wet reaction can be recovered as a dry powder by subjecting it to solid-liquid separation by filtration or the like, followed by washing and drying.
[0053] The slurry may be filtered using a Nutsche filter or the like, and filtration, water washing, and drying may be performed in this order. In the water washing, the electrical conductivity of the washing solution is measured, and the water washing is preferably repeated until the electrical conductivity becomes 2.0 mS / m or less, more preferably 1.0 mS / m or less.
[0054] The washed highly crystalline silver powder is preferably thoroughly dehydrated and then dried. Drying can be performed using a dryer such as a forced circulation atmospheric dryer, a vacuum dryer, or an airflow dryer. The drying temperature is preferably 100°C or less, and more preferably 80°C or less. Temperatures above 100°C are not preferred because they may cause the silver particles in the silver powder to aggregate and sinter. The drying time can be set at any time depending on the temperature, but is preferably 5 hours or more.
[0055] Here, mechanical energy is applied to the dried highly crystalline silver powder to distort the silver particles in the silver powder until the KAM value reaches 0.4 or more and 1.0 or less. The highly crystalline silver powder preferably has an average thickness of 310 nm or more.
[0056] In the present invention, "applying mechanical energy" refers to applying a physical force to the silver powder, such as shear force due to the rotation of an agitator blade or collision force between silver particles, primarily mechanical energy. As the apparatus, it is preferable to use an electric mill such as a sample mill with a high-speed rotating agitator blade or an airflow mill. Furthermore, in the present invention, "imparting strain" refers to slightly distorting the crystal planes of single-crystal particles in the highly crystalline silver powder. Slightly distorting the crystal planes activates the particles without significantly impairing in-plane conductivity, promoting necking during heat treatment for electrode formation, which is advantageous for reducing the resistance of the electrode wiring. Furthermore, it is also preferable that sharp corners originating from the crystal planes of the generated highly crystalline silver powder be removed as a result of "imparting strain," since this reduces the risk of clogging during printing. Note that even if mechanical energy is applied to the silver powder, as in Comparative Example 2 described below, if only agglomerations are loosened and the energy applied to the silver powder is small, the KAM value will not be 0.4 to 1.0. In order to impart strain until the KAM value is 0.4 or more and 1.0 or less, it is necessary to apply sufficient mechanical energy.
[0057] The conductive paste using the silver particles thus obtained can achieve low resistance of electrode wiring when fine lines are printed.
[0058] Examples of silver powder, conductive paste, and methods for producing silver powder will be described below.
[0059] Example 1 3,000 g of a silver nitrate aqueous solution containing 170 g of silver was prepared, and 45.4 g of 67.5 wt % concentrated nitric acid was added to adjust the pH, followed by adjusting the temperature to 25°C. While stirring this solution, 0.43 g of a 4.3 wt % EDTA-4Na aqueous solution (Chilest OD-50) and 10.7 g of a 5 wt % L(+)-arginine aqueous solution were added to obtain a silver complex aqueous solution. Subsequently, 1,500 g of a 10 wt % L-ascorbic acid aqueous solution was added to this silver complex aqueous solution, and the stirring was stopped and the solution was allowed to stand for 4 minutes and 30 seconds to reduce the silver complex aqueous solution. Stirring was resumed, and 2.03 g of a commercially available stearic acid emulsion (Cellosol 920 manufactured by Chukyo Yushi Co., Ltd., containing 82% water) was added to obtain a slurry containing silver particles.
[0060] Next, this slurry was filtered, washed with water until the electrical conductivity of the solution after passing the water was 0.5 mS / m or less, and then vacuum dried at 73° C. for 10 hours to obtain a highly crystalline silver powder.
[0061] As a treatment for imparting strain, 50 g of each sample was placed in a sample mill (SK-10 model, manufactured by Kyoritsu Riko Co., Ltd.) and subjected to strain imparting treatment at the maximum rotation speed for 60 seconds, thereby obtaining silver powder as an aggregate of silver particles according to Example 1.
[0062] The mixed silver powder used to obtain the conductive paste has an SSA of approximately 0.6 m 2 / g to 0.75m 2 The silver powder of Example 1 and fine silver powder (AG-2-1C agent added, manufactured by DOWA Hitec) were mixed in a weight ratio of 1:1 so that the silver powder had a specific surface area of 1.00 m / g. The IPF value of the AG-2-1C agent added was zero, and the volume-based median diameter (D50) was 0.80 μm. 2 The external shapes of a total of 400 or more silver particles were measured for each SEM image of the AG-2-1C agent-added silver particles using image analysis particle size distribution measurement software (Mac-View, manufactured by Mountech Co., Ltd.), and the particles were found to be spherical silver powder with an average aspect ratio of 1.3 and an average Heywood diameter of 0.34 μm.
[0063] Example 2 Silver powder according to Example 2 was obtained in the same manner as in Example 1, except that the amount of nitric acid was changed to 30.2 g.
[0064] The mixed silver powder used to obtain the conductive paste has an SSA of approximately 0.6 m 2 / g to 0.75m 2 The silver powder of Example 2 and AG-2-1C agent added manufactured by Dowa Hitec were mixed in a weight ratio of 1:1 so as to obtain a coating weight of 10 ...
[0065] Example 3 Silver powder according to Example 2 was obtained in the same manner as in Example 1, except that the amount of nitric acid was changed to 15.1 g.
[0066] The mixed silver powder used to obtain the conductive paste has an SSA of approximately 0.6 m 2 / g to 0.75m 2 The silver powder of Example 3 and AG-2-1C agent added manufactured by Dowa Hitec were mixed in a weight ratio of 1:1 so as to obtain a coating weight of 10 ...
[0067] Comparative Example 1 Silver powder according to Comparative Example 1 was obtained in the same manner as in Example 1, except that no strain-imparting treatment was carried out. The silver powder according to Comparative Example 1 is the above-mentioned highly crystalline silver powder.
[0068] The mixed silver powder used to obtain the conductive paste has an SSA of approximately 0.6 m 2 / g to 0.75m 2 The silver powder of Comparative Example 1 and AG-2-1C agent added manufactured by Dowa Hitec were mixed in a weight ratio of 1:1 so as to obtain a coating weight of 1 / g.
[0069] Comparative Example 2 Silver powder according to Comparative Example 2 was obtained in the same manner as in Example 1, except that the apparatus used for the distortion imparting treatment was changed to a coffee mill (ECG62 manufactured by Melitta).
[0070] The mixed silver powder used to obtain the conductive paste has an SSA of approximately 0.6 m 2 / g to 0.75m 2The silver powder of Comparative Example 2 and AG-2-1C agent added manufactured by Dowa Hitec were mixed in a weight ratio of 6:4 so as to obtain a coating weight of 1000g / g.
[0071] Comparative Example 3 FA-S-20 silver powder manufactured by Dowa Hitec was prepared. This silver powder was prepared by mixing approximately spherical silver powder with a lubricant and then flattening the powder using a vibration mill.
[0072] The silver powder mixture for obtaining the conductive paste was prepared by mixing the silver powder of Comparative Example 3 with AG-2-1C agent added (manufactured by Dowa Hitec) in a weight ratio of 7:3, since the SSA of the silver powder of Comparative Example 3 was larger than that of the other silver powders (Examples 1 to 3 and Comparative Examples 1 and 2), so that the SSA when mixed would be closer to the SSA of the other silver powders after mixing.
[0073] Table 1 shows an outline of the production conditions of the silver powders according to the above examples and comparative examples.
[0074]
[0075] (Silver Powder Evaluation) The silver powder was evaluated as described below.
[0076] First, the specific surface area of the silver powder was measured using a Macsorb HM-model 1210 manufactured by Mountech Co., Ltd. When measuring the specific surface area, a He—N 2 After degassing by passing a mixed gas (30% nitrogen) through the tube, the value measured by the BET single-point method was used.
[0077] The particle size distribution of the silver powder was measured using a laser diffraction particle size analyzer (Microtrac Particle Size Distribution Analyzer MT-3300EXII manufactured by Microtrac-Bell Corporation). Immediately before measurement, 0.3 g of silver powder was added to 40 mL of isopropyl alcohol and dispersed for 5 minutes using an ultrasonic cleaner with an output of 45 W. The particle size distribution of the silver particles in the dispersion was then measured. The median diameter (cumulative 50% particle diameter, so-called D50) was a volume-based value. The above specific surface area and particle size distribution were also measured for the mixed silver powder.
[0078] Next, cross-sectional observation of the silver particles in the silver powder was performed. First, 4 g of each silver powder was added to a mixture of 0.7 g of Specifix Resin and 0.1 g of Specifix-20 Curing Agent as a curing agent, and the mixture was gently mixed with a spatula. The mixture was then degassed for 30 minutes in a desiccator under reduced pressure and mixed again with a spatula. The paste was placed in a mold and left at room temperature overnight to harden the resin. The resin-hardened silver powder was polished with a cross-section polisher ArBlade 5000 (Hitachi High-Tech Corporation) to expose the cross-section, and then SEM images were taken with an FE-SEM IT-800SHL (JEOL Ltd.). The thickness was calculated as the short side of the rectangle that surrounded each particle image with the smallest area.
[0079] Next, the silver particles were placed on a stage covered with a conductive adhesive sheet so that they did not overlap, and an EBSE-SEM was used to perform SEM observation of the silver particles in the silver powder and to create IPF and KAM maps. Figures 2 to 7 show SEM images of silver particles in Examples 1 to 3 and Comparative Examples 1 to 3, each of which has a (111) plane or a plane close to the (111) plane as the main region on the upper surface of the silver particle, observed at 15,000x magnification, along with IPF and KAM maps obtained by EBSD measurement of the upper surface of the silver particle. The SEM image is labeled A, the IPF map is labeled B, and the KAM map is labeled C. Figures 8 and 9 show SEM images at 2,000x magnification showing the particle shapes of Example 1 and Comparative Example 3, respectively.
[0080] As described above, the plane orientation of the silver powder according to the present invention was measured using an electron backscatter diffraction (EBSD) analyzer (OIM Analysis 6.2 manufactured by TSL Solutions Co., Ltd.) with a step size of 0.30 μm in a measurement range of 60 μm × 180 μm. SEM observation was performed under conditions of an acceleration voltage of 15 kV, a magnification of 1500x, and a tilt of 70°. An orientation distribution map (Inverse Pole Figure (IPF)) of the upper surface of the silver particles was created by excluding measurement points with low reliability, where the reliability index (CI value) was 0.2 or less. All silver particles (at least 15 or more) on the IPF map were evaluated, and the percentage (%) of silver particles whose main upper surface region was a (111) plane or a plane close to the (111) plane was evaluated and used as the IPF value. In the silver particles of Comparative Example 3, as shown in the IPF map (symbol B) of Figure 7 , numerous small regions exhibiting various plane orientations were observed in the IPF map of the top surface of the silver particles (considered to be polycrystalline particles), even at a magnification of 1500x. However, not a single silver particle was observed in which the main region on the top surface of the silver particle was a (111) plane or a plane close to the (111) plane, and therefore the IPF value was set to zero.
[0081] Further measurements were performed by focusing on 10 or more "silver particles whose main region on the upper surface of the silver particle is a (111) plane or a plane close to the (111) plane" observed on the IPF map at 1500x magnification, and increasing the magnification so that each silver particle was within the field of view. An orientation distribution (Inverse Pole Figure (IPF)) map of the silver particles was created using the same measurement method as above, except that the EBSD analyzer conditions were a measurement range of 6 μm × 18 μm, a step size of 40 nm, and SEM observation conditions were a magnification of 15,000x. Here, a strain distribution (Kernel Average Misorientation (KAM)) was obtained using only the upper surface portions of the 10 or more silver particles, and the KAM value was evaluated. The average KAM value was calculated from the KAM values of the upper surfaces of the 10 or more silver particles. In Comparative Example 3, IPF and KAM maps were obtained for polycrystalline particles using the same measurement method, and the average KAM value was calculated. The results are shown in Table 2 below.
[0082] (Evaluation of Conductive Paste) The properties of the conductive paste were evaluated as follows.
[0083] First, the conductive paste was prepared by mixing 93% by mass of the mixed silver powder obtained in the examples and comparative examples, 3.8% by mass of epoxy resin (ADEKA EP4901E), 1.0% by mass of (Mitsubishi Chemical jER1009), 0.2% by mass of curing agent (Wako Pure Chemical Industries, Ltd. boron trifluoride monoethylamine complex), and 2.3% by mass of solvent (BCA: butyl carbitol acetate) at 1200 rpm for 30 seconds using a propellerless rotary and revolving stirring and degassing device (EME Corporation VMX-N360). The mixture was then kneaded using a three-roll mill (EXAKT 80S) with a roll gap of 100 μm to 20 μm to obtain a conductive paste.
[0084] The conductive paste obtained by the above procedure was used to print a line pattern with a line width of 17 μm and a length of 150 mm using a screen printer (MT-320T manufactured by Microtec Corporation) to form a conductive paste film. The obtained film was heat-cured at 200°C for 30 minutes using an air circulation dryer to form a conductive film. The line resistance value of each conductive film was measured using a digital multimeter (R6551 manufactured by ADVANTEST Corporation).
[0085] The evaluation results of the silver powder, mixed silver powder, and conductive paste thereof are shown in Table 2.
[0086]
[0087] It was confirmed that the conductive paste using the silver powder obtained according to the present invention had a reduced line resistance compared to the comparative example.
[0088] The silver powder according to this embodiment is suitable for use as a conductive filler for conductive paste. The conductive paste using the silver powder according to this embodiment can be used to form a conductive pattern or an electrode on a substrate. The conductive paste using the silver powder according to this embodiment can be printed on a substrate by, for example, screen printing, offset printing, photolithography, or the like, to form a conductive film such as a conductive pattern or an electrode (hereinafter, sometimes simply referred to as a conductive film).
[0089] According to the present invention, it is possible to obtain silver powder and mixed powder that can achieve low resistance of electrode wiring when line-printed, and further to obtain a conductive paste using the same.
Claims
1. A silver powder in which 20% or more but less than 95% of the total particles are silver particles in which the main region of the upper surface of the silver particle is a (111) plane or a plane close to a (111) plane, and the KAM value of the silver particles is 0.4 or more and 1.0 or less.
2. The silver powder according to claim 1, in which the aspect ratio, calculated by dividing the volume-based median diameter by a laser diffraction method by the average thickness of the cross-section of the silver particles, is 1.2 or more and less than 4.
0.
3. The silver powder according to claim 1 or 2, wherein the average thickness of the cross-section of the silver particles is 310 nm or more.
4. A method for producing silver powder, comprising applying mechanical energy to highly crystalline silver powder in which 30% or more of the total particles contain silver particles whose main region on the upper surface of the silver particles is a (111) plane or a plane close to a (111) plane, and in which the KAM value of the silver particles is less than 0.4, to impart distortion to the silver particles until the KAM value of the silver particles becomes 0.4 or more and 1.0 or less.
5. A method for producing silver powder as described in claim 4, in which an amino acid is added to a silver chelate complex solution to prepare a solution, and then an ascorbic acid-based reducing agent is added to obtain the highly crystalline silver powder.
6. A method for producing silver powder as described in claim 4, wherein the silver powder after the strain is imparted has an aspect ratio of 1.2 or more and less than 4.0, calculated by dividing the volume-based median diameter by a laser diffraction method by the average thickness measured in cross-section of the silver particles.
7. A method for producing silver powder as described in claim 4, wherein the highly crystalline silver powder has an average thickness of 310 nm or more when measured in cross section, and the silver powder after the strain is imparted has an average thickness of 310 nm or more when measured in cross section.
8. A method for producing a mixed silver powder, comprising mixing the silver powder according to claim 1 with fine silver powder having a larger specific surface area than said silver powder.
9. A method for producing a mixed silver powder according to claim 8, comprising mixing the silver powder according to claim 1 in a proportion of 10 wt % to 90 wt % of the mixed silver powder.
10. A mixed silver powder containing at least silver particles in which the main region of the upper surface of the silver particle is a (111) plane or a plane close to a (111) plane, and the KAM value of the silver particles is 0.4 or more and 1.0 or less.
11. The specific surface area after mixing is 0.20 m 2 / g or more 1.50m 2The mixed silver powder according to claim 10, wherein the silver content is 1 / g or less.
12. A conductive paste comprising the silver powder according to claim 1, a resin component, and a solvent.
13. A conductive paste comprising the mixed silver powder according to claim 10, a resin component, and a solvent.
Citation Information
Patent Citations
Silver paste and electronic element
JP2018055883A
Silver paste, joined body, and method for manufacturing joined body
JP2019087396A
Silver powder
JP2022186757A