Low-volatility, high-thermal-conductivity and single-component addition-type thermal conductive cement and preparation method therefor

By using a combination of mesoporous alumina and nanocopper particles in thermal conductivity, combining silica layer and inhibitors of unsaturated functional groups, the problem of volatility and short storage time of thermal conductivity is solved, and high thermal conductivity and long Time storage stability.

WO2024239423A1PCT designated stage expired Publication Date: 2024-11-28GOLOHO POLYMER (JIANGXI) CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/104393
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-06-30
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing thermal conductivity slurry has the problem of volatile oil discharge, and the storage time of reactive thermal conductivity slurry is short, which limits its application range.

Method used

Mesoporous alumina is used as the thermal filler, and nanocopper particles are loaded on its surface, and nanocopper particles are coated through a silica layer to improve thermal conductivity. At the same time, inhibitors of unsaturated functional groups are grafted on the surface of the thermal filler to prevent inhibition. The agent precipitates and extends storage stability.

Benefits of technology

It effectively improves the thermal conductivity and storage stability of thermal fillers, reduces the reaction activity of thermally conductive paste, extends the storage time at room temperature, and improves the mechanical properties and leveling after curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023104393_28112024_PF_FP_ABST
    Figure CN2023104393_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of heat transfer, and in particular relates to a low-volatility, high-thermal-conductivity and single-component addition-type thermal conductive cement and a preparation method therefor. The thermal conductive cement is prepared from, in parts by weight, the following raw materials: 100 parts of a vinyl-terminated polydimethylsiloxane, 700-1000 parts of a thermal conductive filler, 0-5 parts of fumed silica, 1-10 parts of a hydrogen-containing silicone oil, and 0.2-2 parts of a catalyst. The main body of the thermal conductive filler is mesoporous alumina; at least part of the surface of the mesoporous alumina is loaded with nano-copper particles, and at least part of the surface of the mesoporous alumina and nano-copper particles is coated with a silicon dioxide layer; and the surface of the silicon dioxide layer is grafted with an inhibitor containing an unsaturated functional group. By means of the preparation method of the present invention, the inhibitor containing an unsaturated functional group is grafted and introduced into the thermal conductive filler, such that the catalytic activity of a platinum catalyst at normal temperature can be effectively inhibited, thereby effectively reducing the reaction activity of the thermal conductive cement, and improving the normal-temperature storage performance thereof.
Need to check novelty before this filing date? Find Prior Art

Description

A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive mortar and its preparation method Technical Field

[0001] The present invention relates to the field of heat transfer technology, in particular to a low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive mortar and a preparation method thereof. Background Art

[0002] Thermally conductive silicone materials are typically made by adding various thermally conductive fillers to a silicone polymer carrier. Commonly used fillers include aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide. Thermally conductive silicone gaskets are cured, have minimal deformation, and are not reusable. Thermal grease, a mixture of oil and powder, does not cure. Long-term use at high temperatures can cause the silicone oil to precipitate, resulting in a dry, powdery material that is unusable. Thermal paste offers excellent thermal conductivity and heat transfer properties. It forms a clay-like consistency, is non-flowing and non-volatile, and is resistant to high and low temperatures. It is easy to use and is placed between electronic components and heat sinks, ensuring close contact and reducing thermal resistance, rapidly lowering the temperature of electronic devices and extending their lifespan and reliability.

[0003] Patent CN106398226A discloses a thermally conductive silicone gel and its preparation method, using vinyl-terminated polydimethylsiloxane or vinyl polymethylvinylsiloxane, with 100 parts of base polymer; 0.1-10 parts of cross-linking agent; 500-1800 parts of filler; and 0.1-15 parts of silane coupling agent. However, the use of low-molecular-weight vinyl-terminated polydimethylsiloxane or vinyl polymethylvinylsiloxane in high-temperature environments for long periods of time cannot solve the problem of low-molecular-weight precipitation.

[0004] Patents CN104497575A and CN111019357A both disclose a highly thermally conductive silicone paste. Its raw materials consist of silicone oil, a thermally conductive powder filler, a plasticizer, a powder surface treatment agent, a crosslinker, a high-temperature-resistant colorant, and a platinum catalyst. These thermally conductive gels are manufactured using a catalyst to crosslink the vinyl silicone oil and crosslinking agent, ultimately producing the thermally conductive silicone paste. However, these pre-processed thermally conductive gels generally suffer from poor toughness, hardness, and extrudability, directly impacting customer experience.

[0005] Patent CN111171571A discloses a highly elastic thermally conductive gel formed by a reaction of α,ω alkoxy-terminated polydimethylsiloxane with dimethyldimethoxysilane, dimethyldiethoxysilane, diphenyldimethoxysilane or diphenyldiethoxysilane. However, this patent cannot solve the problems of overall solidification and oil precipitation.

[0006] Patent CN113024164A relates to a single-component, high-flow, high-thermal-conductivity gel. This patent employs nano-fumed silica to adsorb a platinum catalyst, which is then wrapped with a polymer resin to ultimately achieve long-term stability at room temperature. The patent simply states that a storage-stable thermally conductive gel can be prepared according to the method in the patent, but does not provide a detailed discussion.

[0007] Currently, the thermal conductive gels on the market are mainly non-reactive types, which are prepared by cross-linking vinyl polysiloxane and hydrogen-containing polysiloxane under the catalysis of platinum catalyst. The biggest problem is that cross-linking has been formed during the preparation process, resulting in poor extrusion and limited use.

[0008] There are few reports on reactive thermally conductive gels on the market. They are mainly made by mixing vinyl polysiloxane, hydrogen-containing polysiloxane, thermally conductive fillers, acetylene alcohol inhibitors, and platinum catalysts. They are heated and cured into thermally conductive gels when used. Their main problem is that they have a short storage time at room temperature and must be stored for a long time in a frozen state, which makes them inconvenient to use and limits their scope of application. Summary of the Invention

[0009] Therefore, the purpose of the present invention is to provide a low-volatile, high-thermal-conductivity single-component addition-type thermal conductive paste and a preparation method thereof to overcome the above problems.

[0010] To achieve the above-mentioned purpose, the present invention is implemented through the following technical solutions:

[0011] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive mortar, comprising the following raw materials in proportion by weight: 100 parts of vinyl-terminated polydimethylsiloxane, 700-1000 parts of thermally conductive filler, 0-5 parts of fumed silica, 1-10 parts of hydrogenated silicone oil, and 0.2-2 parts of a catalyst;

[0012] The main body of the thermal conductive filler is mesoporous alumina;

[0013] At least a portion of the surface of the mesoporous alumina is loaded with nano copper particles

[0014] At least a portion of the surface of the mesoporous alumina and the nano-copper particles is coated with a silicon dioxide layer;

[0015] An inhibitor containing an unsaturated functional group is grafted onto the surface of the silicon dioxide layer.

[0016] Compared with the prior art, the low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive in the present invention has made certain modifications and improvements to the thermal conductive filler filled inside, thereby effectively improving the thermal conductivity of the thermal conductive filler and effectively extending the storage stability of the thermal conductive adhesive.

[0017] This application has made the following improvements to the thermal conductivity of thermally conductive fillers:

[0018] In the prior art, the thermal conductive fillers used to improve the thermal conductivity of silicone potting compounds are mainly selected from metal oxides and metal nitrides. Aluminum oxide is the most widely used in organic potting compounds because it has a higher thermal conductivity coefficient among metal oxides, is cheap, and has excellent insulation properties. However, the thermal conductivity coefficient of aluminum oxide is still only maintained at 30 W·m -1 ·K -1 Compared with metal materials and carbon materials, its thermal conductivity is still relatively low. Therefore, in order to improve the thermal conductivity of organic potting glue, the amount of aluminum oxide added can only be further increased. However, the large amount of thermal conductive material added will cause other properties of organic potting glue (leveling and mechanical properties) to decline to varying degrees, which seriously affects its own use.

[0019] The thermal conductive filler provided in this application is also based on alumina material, but a certain amount of nano-copper particles are loaded on the surface of the alumina. Therefore, compared with alumina, the thermal conductivity of metallic copper can be as high as 398 W·m -1 ·K -1 Therefore, the addition of nano copper particles can effectively improve the thermal conductivity of the overall thermal conductive filler to a certain extent.

[0020] However, conventional alumina fillers (such as spherical alumina) have a relatively smooth surface, which makes it easy for the nano-copper particles to fall off the alumina surface during loading, making it difficult for the nano-copper particles to adhere. Therefore, in this application, mesoporous silica is used to increase the contact area between the nano-copper particles and the alumina surface, thereby allowing the nano-copper particles to better adhere to the alumina surface. Actual tests have shown that thermally conductive fillers containing mesoporous alumina have significantly better thermal conductivity than thermally conductive fillers containing traditional spherical alumina.

[0021] While the addition of nano-copper particles can effectively improve the thermal conductivity of thermally conductive fillers, the applicant has discovered that, despite a low nano-copper content, they significantly increase the conductivity of the overall potting compound, hindering its application in the electronics industry. Therefore, the present invention coats at least a portion of the surface of the mesoporous alumina and nano-copper particles with a layer of silicon dioxide. Silicon dioxide has a lower resistivity than alumina, so the silicon dioxide coating of both surfaces shields the conductivity of the nano-copper particles and prevents oxidation by oxygen, thereby reducing their thermal conductivity.

[0022] In order to extend the storage stability of thermal conductive paste by using thermal conductive fillers, the present application has made the following improvements:

[0023] In order to improve the stability of single-component addition-type thermal conductive paste in the existing technology, a certain amount of inhibitors (such as substances containing S or P elements, unsaturated compounds, etc.) are usually added to the thermal conductive paste. These substances are usually small molecular substances. These small molecule inhibitors often migrate, precipitate and volatilize during storage, thereby weakening the inhibitory effect on the various components in the paste, thereby significantly reducing its storage stability. In the present application, inhibitors containing unsaturated functional groups are grafted onto the surface of the silica layer covering the surface of the mesoporous alumina and nano-copper particles, thereby effectively preventing the precipitation problem of these inhibitors, and further preventing the reaction of vinyl-terminated polydimethylsiloxane with hydrogen-containing silicone oil at room temperature. This process can be destroyed and reversed at high temperatures, so that the platinum metal catalyst can still catalyze the reaction between vinyl-terminated polydimethylsiloxane and hydrogen-containing silicone oil at high temperatures. Moreover, since the inhibitors contain unsaturated functional groups, these unsaturated functional groups can also react with hydrogen-containing silicone oil, so that the various components in the entire thermal conductive putty form a cross-linked network, further improving the mechanical properties of the putty after curing.

[0024] Therefore, in summary, this application combines alumina, nano-copper particles, and silica to produce a thermally conductive material with higher thermal conductivity and lower electrical conductivity. This effectively reduces the amount of thermally conductive filler used in silicone sealants, effectively improving the sealant's leveling and mechanical properties. Furthermore, this specially modified thermally conductive filler can effectively enhance the room-temperature storage performance of the thermally conductive adhesive.

[0025] Preferably, the preparation method of the thermally conductive filler is as follows:

[0026] (1) reacting alumina with an etching solution to obtain spherical mesoporous alumina;

[0027] (2) placing mesoporous alumina in a solution containing a copper precursor and a silicon dioxide precursor with silicon hydrogen and silicon alkoxy groups, uniformly dispersing the solution, and then adding an acidic reducing agent to reduce the copper precursor to obtain nano-copper particles, and hydrolyzing the silicon dioxide precursor to form polysiloxane, thereby coating the mesoporous alumina and the nano-copper particles, and obtaining mesoporous alumina loaded with nano-copper particles and polysiloxane;

[0028] (3) The mesoporous alumina loaded with nano-copper particles and polysiloxane is subjected to a condensation reaction with an alcohol inhibitor containing an unsaturated group to obtain the thermal conductive filler.

[0029] During the preparation process, the thermally conductive filler of the present invention is first etched on aluminum oxide using an etching solution. The etching solution can be an acid solution or an alkaline solution, both of which have a good etching effect on aluminum oxide. This allows the filler to react on the surface of the aluminum oxide, thereby forming a mesoporous structure on the surface.

[0030] Subsequently, the mesoporous alumina is placed in a solution containing a copper precursor and a silicon dioxide precursor with silicon hydrogen and silicon alkoxy groups. After being evenly dispersed, an acidic reducing agent is added. The copper precursor is reduced under the action of the acidic reducing agent to form nano-copper particles. Part of these nano-copper particles are embedded in the pores on the surface of the mesoporous alumina, and part is free in the solution. Since the formed nano-copper particles can coordinate with the silicon dioxide precursor with alkoxy groups, the nano-copper particles are coated. At the same time, since the silicon dioxide precursor contains alkoxy groups, it will undergo a hydrolysis reaction under acidic conditions, thereby forming a cross-linked polysiloxane structure after hydrolysis, and wrapping the alumina and nano-copper particles together, so that the alumina can achieve effective loading of the nano-copper particles.

[0031] Preferably, the silicon dioxide precursor containing silicon hydrogen and silicon alkoxy groups in step (2) is any one of trimethoxysilane, methyldimethoxysilane, triethoxysilane and methyldiethoxysilane.

[0032] Preferably, the alcohol inhibitor containing an unsaturated group in step (3) is any one of acetylene cyclohexanol, acetylene alcohol, propynol, butynol, methylbutynol, tert-butyl cyclohexanol, phenylbutynol, 3,5-dimethyl-1-hexyne-3-ol, 3,6-dimethyl-1-heptyne-3-3,7,11-trimethyldodecyne-3-ol.

[0033] Preferably, the viscosity of the vinyl-terminated polydimethylsiloxane is 100-10000 mPa.s.

[0034] Preferably, the fumed silica is fumed silica treated with hexamethyldisilazane, with a specific surface area of ​​100 to 600 m 2 / g.

[0035] Preferably, the hydrogen-containing silicone oil is a mixture of one or more hydrogen-containing silicone oils having a hydrogen content between 0.1% and 0.75%.

[0036] Preferably, the catalyst is a Custer catalyst, and its effective platinum content is 3000-8000 ppm.

[0037] In a second aspect, the present invention further provides a method for preparing the low-stress, low-volatility, high-thermal-conductivity single-component addition-type thermal conductive paste as described above, comprising the following steps:

[0038] (S.1) vinyl-terminated polydimethylsiloxane, thermal conductive filler, and fumed silica are mixed and stirred to obtain a base material;

[0039] (S.2) Add hydrogenated silicone oil and catalyst into a mixer containing the above-mentioned base material, stir evenly, and obtain a low-stress, high-thermal-conductivity, heat-curable thermal conductive gel.

[0040] Preferably, in step (S.1), the mixing and stirring temperature is 120-170°C, the vacuum degree is <-0.095 MPa, and the mixture is dehydrated for 120-240 minutes and then cooled to room temperature;

[0041] In the step (S.2), the vacuum degree is less than -0.095 MPa, and the stirring is carried out at a rotation speed of 10-20 Hz for 60-180 min.

[0042] Therefore, the present invention has the following beneficial effects:

[0043] (1) The present invention can effectively inhibit the catalytic activity of the platinum catalyst at room temperature by grafting an inhibitor containing unsaturated functional groups into the thermal conductive filler, thereby effectively reducing the reaction activity of the thermal conductive mortar and improving its storage performance at room temperature;

[0044] (2) This application effectively improves the thermal conductivity of the thermally conductive filler without affecting the electrical conductivity by introducing nano-copper particles and silica coatings into the thermally conductive filler;

[0045] (3) This application can significantly reduce the viscosity of the system, slow down the oil-powder separation, and improve the anti-settling effect of the system. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] FIG1 is an electron microscope photograph of the thermal conductive filler A1 of the present invention. Implementation Method

[0047] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only a portion of the embodiments of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0048]

Preparation of thermal conductive filler

[0049] Thermal conductive filler A1: Its preparation method is as follows:

[0050] (1) Immersing the spherical alumina in a 0.005 mol / L sodium hydroxide solution at room temperature for 15 min, allowing the spherical alumina to react with the sodium hydroxide for 30 min, and then filtering and washing to obtain spherical mesoporous alumina;

[0051] (2) 500 g of mesoporous alumina was placed in a solution containing 2 L of 30 g of copper sulfate pentahydrate and 24.5 g (0.2 mol) of trimethoxysilane, and the mixture was evenly dispersed to form a suspension. 40 g of citric acid was then added and continued to be stirred and dispersed. The mixture was then heated to 75 ° C and stirred for 2 h to reduce the copper sulfate to obtain nano-copper particles and hydrolyze the trimethoxysilane to form polysiloxane to coat the mesoporous alumina and the nano-copper particles. The mixture was filtered and dried at 80 ° C for 5 h to obtain mesoporous alumina loaded with nano-copper particles and polysiloxane.

[0052] (3) The obtained mesoporous alumina loaded with nano-copper particles and polysiloxane was placed in 1 L of toluene solution, and then 0.01 g of tri(pentafluorophenyl)borane was added thereto. After mixing evenly, 6.2 g (0.05 mol) of acetylene cyclohexanol was added dropwise thereto. The mixture was stirred at room temperature for 2 h, and then filtered and dried to obtain the thermal conductive filler A1, an electron microscope photograph of which is shown in FIG1 .

[0053] Thermal conductive filler A2: Its preparation method is as follows:

[0054] (1) Immersing the spherical alumina in a 0.005 mol / L sodium hydroxide solution at room temperature for 15 min, allowing the spherical alumina to react with the sodium hydroxide for 30 min, and then filtering and washing to obtain spherical mesoporous alumina;

[0055] (2) 500 g of mesoporous alumina was placed in a 2 L solution containing 35 g of copper chloride and 24.5 g (0.2 mol) of trimethoxysilane, and dispersed evenly to form a suspension. 30 g of ascorbic acid was then added and stirred and dispersed. The mixture was then heated to 60 ° C and stirred for 4 h to reduce the copper chloride to obtain nano-copper particles and hydrolyze the trimethoxysilane to form polysiloxane to coat the mesoporous alumina and the nano-copper particles. The mixture was filtered and dried at 85 ° C for 5 h to obtain mesoporous alumina loaded with nano-copper particles and polysiloxane.

[0056] (3) The obtained mesoporous alumina loaded with nano-copper particles and polysiloxane was placed in 1 L of toluene solution, and then 0.01 g of tri(pentafluorophenyl)borane was added thereto. After mixing evenly, 4.2 g (0.05 mol) of methylbutynol was added dropwise thereto. The mixture was stirred at room temperature for 2 h, and then filtered and dried to obtain the thermal conductive filler A2.

[0057] Thermal conductive filler A3: Its preparation method is as follows:

[0058] (1) Immersing the spherical alumina in a 0.005 mol / L sodium hydroxide solution at room temperature for 15 min, allowing the spherical alumina to react with the sodium hydroxide for 30 min, and then filtering and washing to obtain spherical mesoporous alumina;

[0059] (2) 500 g of mesoporous alumina was placed in a solution containing 2 L of 24.5 g (0.2 mol) of trimethoxysilane and dispersed uniformly to form a suspension. 30 g of ascorbic acid was then added and the mixture was stirred and dispersed. The mixture was then heated to 60 ° C and stirred for 4 h to allow the trimethoxysilane to hydrolyze to form polysiloxane, thereby coating the mesoporous alumina. The mixture was filtered and dried at 85 ° C for 5 h to obtain mesoporous alumina coated with polysiloxane.

[0060] (3) The obtained mesoporous alumina coated with polysiloxane was placed in 1 L of toluene solution, and then 0.01 g of tri(pentafluorophenyl)borane was added thereto. After mixing evenly, 4.2 g (0.05 mol) of methylbutynol was added dropwise thereto. The mixture was stirred at room temperature for 2 h, and then filtered and dried to obtain the thermal conductive filler A3.

[0061] Example 1

[0062] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0063] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 20.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0064] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0065] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0066] Example 2

[0067] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0068] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 700 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were added. 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0069] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0070] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0071] Example 3

[0072] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0073] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 1000 parts of thermal conductive filler A1 with a D50 of 20 μm, and hexamethyldisilazane were added to form a mixture with a specific surface area of ​​200 m 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0074] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0075] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0076] Example 4

[0077] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0078] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, thermal conductive filler A2 900 with a D50 of 20 μm, and hexamethyldisilazane were added to form a mixture with a specific surface area of ​​200 m 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0079] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0080] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0081] Example 5

[0082] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0083] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, and 900 parts of thermally conductive filler A1 with a D50 of 20 μm were added to a blender, and the mixture was dehydrated, blended, and kneaded at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and then cooled to obtain a base rubber.

[0084] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0085] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0086] Example 6

[0087] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0088] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 2 2 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0089] At room temperature, 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material, and stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 120 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0090] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0091] Example 7

[0092] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0093] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 2 5 parts of fumed silica (100g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0094] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0095] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0096] Example 8

[0097] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0098] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 2 0.5 parts of fumed silica (100g) was added into a blender, and the mixture was dehydrated, blended and kneaded at a temperature of 170°C and a vacuum degree of -0.095 MPa for 240 minutes, and then cooled to obtain a base rubber;

[0099] 1 part of dimethylmethylhydrogensiloxane with a hydrogen content of 0.75% was added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0100] 1.5 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 10 Hz for 60 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0101] Example 9

[0102] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0103] At 25°C, 100 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 120°C and a vacuum degree of -0.095 MPa for 120 minutes, and cooled to obtain a base rubber;

[0104] 10 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.1% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a speed of 15 Hz to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0105] At room temperature, 2 parts of 3000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material. The vacuum degree was -0.095 MPa and the rotation speed was 20 Hz. The mixture was stirred for 180 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive product.

[0106] Example 10

[0107] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0108] At 25°C, 100 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were added. 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0109] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred at a vacuum degree of -0.095 MPa and a speed of 20 Hz for 120 minutes to obtain a thermal conductive gel intermediate.

[0110] 1.5 parts of 5000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer containing the above base materials at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a rotation speed of 15 Hz for 60 minutes to obtain a finished thermal conductive gel.

[0111] Example 11

[0112] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0113] At 25°C, 100 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A1 with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were added. 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0114] 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material at room temperature, and stirred at a vacuum degree of -0.095 MPa and a speed of 20 Hz for 120 minutes to obtain a thermal conductive gel intermediate.

[0115] 1.5 parts of 5000 PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer containing the above base materials at room temperature. The mixture was stirred at a vacuum degree of -0.095 MPa and a rotation speed of 15 Hz for 60 minutes to obtain a finished thermal conductive gel.

[0116] Comparative Example 1

[0117] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0118] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of thermal conductive filler A3 with a D50 of 20 μm, and hexamethyldisilazane treated with a specific surface area of ​​200 m 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0119] At room temperature, 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% were added into a power vacuum planetary mixer containing the above base material, and stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 120 minutes to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive intermediate.

[0120] 1.5 parts of 3000PPM Custer platinum catalyst were mixed and added into a power vacuum planetary mixer filled with the above base material at room temperature, with a vacuum degree of -0.095Mpa and a rotation speed of 15hz for 60min to obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive mortar product.

[0121] Comparative Example 2

[0122] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0123] At 25°C, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 200 mPa.s, 50 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of alumina powder with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0124] At room temperature, 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% was added into a power vacuum planetary mixer containing the above base material, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a rotation speed of 15 Hz to obtain a thermal conductive gel intermediate.

[0125] 1 part of acetylene cyclohexanol and 1.5 parts of 3000 PPM Custer platinum catalyst were mixed at room temperature and added into a power vacuum planetary mixer filled with the above base materials. The mixture was stirred at a vacuum degree of -0.095 MPa and a rotation speed of 15 Hz for 60 minutes to obtain a finished thermal conductive gel.

[0126] Comparative Example 3

[0127] A low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive is prepared according to the following steps:

[0128] At 25°C, 100 parts of vinyl-terminated polydimethylsiloxane with a viscosity of 1000 mPa.s, 900 parts of alumina powder with a D50 of 20 μm, and a specific surface area of ​​200 m2 of hexamethyldisilazane-treated fruit were mixed. 2 0.5 parts of fumed silica (100g / g) were added into a blender, dehydrated and blended at 150°C and a vacuum degree of -0.095 MPa for 180 minutes, and cooled to obtain a base rubber;

[0129] At room temperature, 5 parts of dimethylmethylhydrogensiloxane with a hydrogen content of 0.18% was added into a power vacuum planetary mixer containing the above base material, and stirred for 120 minutes at a vacuum degree of -0.095 MPa and a rotation speed of 15 Hz to obtain a thermal conductive gel intermediate.

[0130] 2 parts of hydroxybutadiene, 1 part of dodecylene-3-ol, and 1.5 parts of 5000 PPM Custer platinum catalyst were mixed at room temperature and added into a power vacuum planetary mixer filled with the above base materials. The mixture was stirred at a vacuum degree of -0.095 MPa and a speed of 15 Hz for 60 minutes to obtain a finished thermal conductive gel.

[0131] Table 1: Component ratios of silicone potting compounds in Examples 1 to 5 and Comparative Example 1

[0132]

[0133] Note: The unit of each component in the above table is "part".

[0134] Performance test: The following performance tests were performed on the thermal conductive pastes prepared in Examples 1 to 10 and Comparative Examples 1 to 3 and the cured colloids. Specific test data are shown in Table 2.

[0135] Extrusion performance: Extrusion performance was tested in accordance with GB / T 14683-2017.

[0136] Storage time: The thermal conductive paste was stored at room temperature for 91 days to observe the change in its viscosity.

[0137] Curing time: Place the thermal conductive adhesive in a 100°C environment and measure its curing time.

[0138] Thermal conductivity: Thermal conductivity is tested in accordance with GB / T10297-2015.

[0139] Toughness / Hardness: Solidify the thermal conductive paste to obtain a colloid, cut the colloid into thin slices 2-3 mm thick, fold it in half, observe whether it can be broken, and test its Shore hardness.

[0140] Table 2

[0141]

[0142] As shown in Table 2, the preparation method described herein effectively suppresses the catalytic activity of the platinum catalyst at room temperature by grafting an inhibitor containing unsaturated functional groups into the thermally conductive filler. This effectively reduces the reactivity of the thermally conductive mortar and improves its room-temperature storage performance, which remains normal after 90 days of storage. Furthermore, the introduction of nano-copper particles and a silica layer into the thermally conductive filler effectively improves its thermal conductivity without affecting its electrical conductivity. Furthermore, it significantly reduces the viscosity of the system, slows oil-powder separation, and improves the system's anti-settling effect.

Claims

1. A low-volatile, high-thermal-conductivity, single-component, addition-type thermal conductive adhesive. It is characterized in that The invention is composed of the following raw materials in proportion by weight: 100 parts of vinyl-terminated polydimethylsiloxane, 700-1000 parts of thermal conductive filler, 0-5 parts of fumed silica, 1-10 parts of hydrogen-containing silicone oil, and 0.2-2 parts of catalyst; The main body of the thermal conductive filler is mesoporous alumina; At least a portion of the surface of the mesoporous alumina is loaded with nano copper particles At least a portion of the surface of the mesoporous aluminum oxide and the nano copper particles is coated with a silicon dioxide layer; An inhibitor containing an unsaturated functional group is grafted onto the surface of the silicon dioxide layer.

2. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to claim 1, It is characterized in that The preparation method of the thermal conductive filler is as follows: (1) reacting alumina with an etching solution to obtain spherical mesoporous alumina; (2) placing mesoporous alumina in a solution containing a copper precursor and a silicon dioxide precursor with silicon hydrogen and silicon alkoxy groups, and adding an acidic reducing agent after uniform dispersion, so that the copper precursor is reduced to obtain nano copper particles, and the silicon dioxide precursor is hydrolyzed to form polysiloxane, thereby coating the mesoporous alumina and the nano copper particles, and obtaining mesoporous alumina loaded with nano copper particles and polysiloxane; (3) A mesoporous alumina loaded with nano-copper particles and polysiloxane is subjected to a condensation reaction with an alcohol inhibitor containing an unsaturated group to obtain the thermal conductive filler.

3. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to claim 2, It is characterized in that In the step (2), the silicon dioxide precursor containing silicon hydrogen and silicon alkoxy groups is any one of trimethoxysilane, methyldimethoxysilane, triethoxysilane and methyldiethoxysilane.

4. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to claim 2 or 3, It is characterized in that The alcohol inhibitor containing an unsaturated group in step (3) is any one of acetylene cyclohexanol, acetylene alcohol, propynol, butynol, methyl butynol, phenyl butynol, 3,5-dimethyl-1-hexyne-3-ol, 3,6-dimethyl-1-heptyne-3-3,7,11-trimethyldodecyne-3-ol.

5. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to any one of claims 1 to 3, It is characterized in that The viscosity of the vinyl-terminated polydimethylsiloxane is 100-10000 mPa.s.

6. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to any one of claims 1 to 3, It is characterized in that The fumed silica is fumed silica treated with hexamethyldisilazane and has a specific surface area of ​​100 to 600 m 2 / g.

7. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to any one of claims 1 to 3, It is characterized in that The hydrogen-containing silicone oil is a mixture of one or more hydrogen-containing silicone oils with a hydrogen content between 0.1 and 0.75%.

8. The low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to any one of claims 1 to 3, It is characterized in that The catalyst is a Castel catalyst, and its effective platinum content is 3000-8000ppm.

9. The method for preparing the low-volatile, high-thermal-conductivity, single-component addition-type thermal conductive adhesive according to claims 1 to 8, characterized in that: The following steps are involved: (S.1) vinyl terminated polydimethylsiloxane, thermal conductive filler and fumed silica are mixed and stirred to obtain a base material; (S.2) Add hydrogen-containing silicone oil and catalyst into a mixer containing the above base material respectively, stir evenly, and obtain a low-volatile and high-thermal-conductivity single-component addition-type thermal conductive adhesive.

10. The method according to claim 9, It is characterized in that In the step (S.1), the mixing and stirring temperature is 120-170°C, the vacuum degree is ≤-0.095MPa, and the mixture is dehydrated for 120-240min and then cooled to room temperature; In the step (S.2), the vacuum degree is ≤-0.095 MPa, and the stirring is performed at a rotation speed of 10-20 Hz for 60-180 min.

Citation Information

Patent Citations

  • Preparation method and application of mesoporous aluminum oxide supported noble metal rhodium dehydrogenation catalyst

    CN113198467A

  • Mesoporous silica-coated nano-alumina-loaded nickel-molybdenum catalyst as well as preparation method and application thereof

    CN114682266A

  • Preparation method of heat-conducting filler and high-heat-conductivity reactive polyurethane hot melt adhesive composition

    CN114806486A

  • Methods of generating supported nanocatalysts and compositions thereof

    US20080206562A1

  • Method of manufacturing silica-coated metal nanoparticles

    US20100304006A1