Catalyst and alkynylation method

By using metal doped support oxide catalyst modified with nitrogen-containing heterocyclic compounds in alkynol production, side reactions are suppressed and catalyst recycling is realized, the problems of frequent side reactions and difficult catalyst recovery in industrial production of alkynol are solved, and the problem of high-quality side reactions and high-quality catalyst recovery is improved. Yield and environmentally friendly.

WO2024239777A1PCT designated stage expired Publication Date: 2024-11-28SHANDONG NHU PHARMA +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082490
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-03-19
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

In the large-scale industrial production of existing alkynols, catalysts under alkaline conditions lead to frequent side reactions, low reaction yields, and difficult to recover catalysts. The use of ammonia solvents requires a large amount of refrigeration energy, resulting in high production costs and environmental protection problems.

Method used

The metal-doped support oxide catalyst modified with nitrogen-containing heterocyclic compounds is used to modify the catalyst surface by a modifier to inhibit side reactions, realize the recycling of the catalyst, and carry out acetylation reaction without using solvents.

Benefits of technology

It improves the yield and raw material utilization of alkynol, reduces solvent use, reduces production costs, simplifies post-treatment operations, and realizes stable recovery of catalysts and environmentally friendly production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082490_28112024_PF_FP_ABST
    Figure CN2024082490_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst for an alkynylation reaction and an alkynylation method. The catalyst comprises a modifier and a metal oxide system. The metal oxide system is a support oxide doped with a first metal element, and the modifier is present in at least part of the surface region of the metal oxide system. The alkynylation method comprises the step of reacting a carbonyl-containing compound with a terminal alkynyl-containing compound in the presence of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst and acetylation method Technical Field The present invention belongs to the field of fine chemicals, and in particular, relates to a catalyst for the acetylation reaction of a carbonyl compound, and further provides an acetylation method of a carbonyl compound using the catalyst. Background Art Alkynol is an important kind of fine chemical product, mainly used in the production of VE main intermediates, DV chrysanthemic acid (pyrethroid intermediates), vitamin A, vitamin K1, carotenoid intermediates, synthetic rubber monomers, linalool and other fragrances. Some methods have been provided for the preparation of alkynols. For example, Reference 1 and Reference 2 prepare a Grignard reagent containing an alkynyl group and react it with a carbonyl compound to obtain an alkynol; Reference 3 utilizes an elimination reaction of a halogen-containing unsaturated alcohol to remove hydrogen halide to obtain an alkynol. Furthermore, when alkynols are produced industrially, ketones or aldehydes are usually used as raw materials, acetylene gas is dissolved in liquid ammonia, and alkynols are synthesized with substrates under the action of alkaline catalysts. The general reaction formula is: Wherein, R1 and R2 are hydrogen or hydrocarbon groups. Reference 4 discloses that a carbonyl compound is reacted with acetylene in the presence of ammonia and an alkali metal hydroxide, and in the examples, the highest conversion rate is about 95% and the highest selectivity is about 99%. Reference 5 discloses that ketone and acetylene are used as raw materials, potassium isobutoxide is used as a catalyst, and the raw materials ketone, acetylene and the catalyst potassium isobutoxide are continuously fed into a reactor. This patent only uses potassium isobutoxide as a catalyst, and does not require the use of ammonia. However, the catalyst cost is high and is difficult to recover. Reference 6 discloses that ketone and acetylene are used as raw materials, flake potassium hydroxide is used as catalyst, and ether is used as catalyst. The method uses water as solvent and nonionic surfactant as solvent, removes water under azeotropic conditions, suspends KOH in the organic phase, cools to below 20°C, and then introduces ketone and acetylene under normal pressure for reaction. However, due to the low solubility of acetylene, this method has the problem of limiting the reaction rate, and it is difficult to separate the product. Reference 7 discloses a new process for synthesizing acetylene alcohol from acetylene and ketone compounds, wherein acetylene is mixed with solvent ammonia and compressed, and then ketone compounds and potassium hydroxide catalyst are added, the acetylation reaction is completed in a reactor, ammonium chloride is added to terminate the reaction, and then the crude acetylene alcohol product is obtained by pressurized degassing, atmospheric degassing, scraper evaporation, and deketone removal, and then the anhydrous acetylene alcohol product is obtained by membrane separation and water removal. However, this method uses strong base potassium hydroxide as a catalyst, and multiple side reactions will occur while the main reaction is in progress; ammonium chloride needs to be added to terminate the reaction, resulting in the generation of waste salt. Reference 8 discloses an acetylation method, using N,N-dimethylformamide as a solvent, using inorganic cyanides such as sodium cyanide and potassium cyanide as a side reaction inhibitor, and in the presence of a catalyst alcohol salt or amino salt, a saturated or unsaturated ketone or aldehyde compound undergoes an acetylation reaction to obtain a corresponding acetylenic alcohol compound. However, this method requires multiple extractions, and the required amount of water is 30-200% of the solvent mass. The operation is cumbersome, not only produces a lot of wastewater, but also the use of highly toxic cyanide brings safety risks to operators. Although various synthetic methods of alkynols have been explored to a certain extent in the prior art as described above, there is still room for further improvement. References: Reference 1: CN112375091A Reference 2: CN104744211A Reference 3: CN107032956A Reference 4: CN1675152A Reference 5: CN1769254A Reference 6: CN102476978A Reference 7: CN106117010A Reference 8: CN110467519B Summary of the invention Problem that the invention aims to solve As mentioned above, the current industrial large-scale production of alkynols is usually carried out by using a catalyst to catalyze the acetylation reaction of aldehydes or ketones under alkaline conditions. The reaction is essentially a nucleophilic addition reaction: the CH bond at the end of the alkyne breaks under base catalysis to form an acetylenic carbon anion, which acts as a nucleophilic reagent to attack the positively charged carbon atom in the carbonyl group (the carbonyl group is a polar functional group, and the electronegativity of the oxygen atom in the carbonyl group is greater than that of the carbon atom, so the oxygen has a negative charge and the carbon has a positive charge). However, under alkaline conditions, in addition to the above-mentioned main reaction, there are also a variety of side reactions, such as the further reaction of the alkynol to form an acetylenediol, and the thermal decomposition of the alkynol. In addition, the aldol condensation reaction of the raw material aldehyde or ketone under alkaline conditions itself is also prone to generate by-products, and the occurrence of these side reactions all leads to a low reaction yield. In addition, in current industrial practice, the alkaline catalysts used in large quantities are almost impossible to recover and reuse, which not only leads to high production costs, but also easily causes environmental problems. In addition, in order to use ammonia as a solvent, ammonia must first be liquefied, which requires very low temperatures and consumes considerable refrigeration energy, which has become a major burden on energy consumption. Therefore, in view of the above problems in the industrial production of alkynols in the art, the present invention primarily provides a reaction catalyst suitable for preparing alkynol compounds from carbonyl-containing compounds and alkynyl-containing compounds, wherein the catalyst is obtained by modifying a metal-doped carrier oxide with a nitrogen-containing heterocyclic compound. The catalyst of the present invention can inhibit the occurrence of side reactions and provide the catalyst with recyclability. Furthermore, the present invention also provides a method for preparing alkynols using the above catalyst, which method not only has an improved yield, but also can reduce or even avoid the use of solvents. Therefore, it is an efficient and environmentally friendly acetylation method, which is conducive to the industrialized large-scale production of alkynols and their downstream products. Solutions for solving problems Through long-term research by the inventors of the present invention, it is found that the above technical problems can be solved by implementing the following technical solutions: [1]. The present invention first provides a catalyst for preparing alkynols via the reaction of a carbonyl-containing compound with a terminal alkynyl-containing compound, wherein: The catalyst comprises a modifier and a metal oxide system, wherein the metal oxide system is a carrier oxide doped with a first metal element. in, The modifier includes a nitrogen-containing heterocyclic compound, The first metal element includes one or more of Pd, Ru, Pt, Nb, Bi, Cu and Co, preferably, a combination of two or more elements. Furthermore, the modifier is present in at least a portion of the surface region of the metal oxide system. [2] The catalyst according to [1], wherein the carbonyl-containing compound has a molecular formula represented by the following formula (I): Wherein, R1 and R2 are the same or different each time they appear, and are independently hydrogen or a monovalent organic group, or R1 and R2 can be connected to form a ring, provided that R1 and R2 are not hydrogen at the same time. [3] The catalyst according to [1] or [2], wherein the terminal acetylenic group-containing compound has the following molecular formula (II): Wherein, R3 is hydrogen or a monovalent organic group. [4] The catalyst according to any one of [1] to [3], wherein the nitrogen-containing heterocyclic compound is selected from one or more of pyridine, imidazole, pyrazole, quinoline and oxazoline compounds. [5] The catalyst according to any one of [1] to [4], wherein the content of the first metal element in the metal oxide system is 0.1 to 10% by mass of the mass of the doped support oxide. [6] The catalyst according to any one of [1] to [5], wherein in the catalyst, the molar ratio of the nitrogen-containing heterocyclic compound to the first metal element is 10 to 20:1. [7]. Furthermore, the present invention also provides a method for preparing alkynol, wherein the method comprises: In the presence of the catalyst according to any one of [1] to [6] above, using a carbonyl-containing compound A step of reacting with a terminal acetylenic group-containing compound. [8] The method according to [7], wherein the reaction is carried out with or without a solvent. [9] The method according to [7] or [8], wherein the reaction temperature is below 70°C and the reaction time is below 6 hours.

[0010] . The method according to any one of [7] to [9], wherein the catalyst is a newly prepared catalyst or a reused catalyst. Effects of the Invention In the present invention, through the implementation of the above technical solution, it has been found that the present invention can achieve the following technical effects: (1) The method for acetylation of carbonyl-containing compounds and the catalyst thereof provided by the present invention not only inhibit the further generation of acetylenic alcohols into acetylenediols, but also eliminate the thermal decomposition of acetylenic alcohol products and the self-condensation reaction of substrate aldehydes or ketones, thereby effectively improving the product yield and raw material utilization rate. (2) The acetylation method provided by the present invention has a simple reaction system and can be successfully carried out even without using a solvent. Therefore, after the reaction is completed, there is no need for extraction treatment to extract the product, nor is there any need to add salt to quench the reaction. The catalyst is easy to recover, and no waste water and waste salt are generated. It is green and environmentally friendly, and the post-processing operation is greatly simplified. (3) The heterogeneous metal-doped catalyst used in the present invention is easy to recycle and has stable catalyst performance, thereby achieving catalyst recycling, effectively reducing production costs, and helping to improve the competitiveness of acetylenic alcohols and their downstream products. BRIEF DESCRIPTION OF THE DRAWINGS FIG1 is a SEM photograph of the catalyst morphology of Example 17; FIG2 is a gas phase detection spectrum and results of the ethynylation reaction liquid in Example 24; FIG3 is a gas phase detection spectrum and results of the ethynylation reaction liquid in Example 43. DETAILED DESCRIPTION The following is a detailed description of the present invention. The following description of the technical features is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that: In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B. In this specification, the numerical range expressed using "above" or "below" means a numerical range including the number. In this specification, the word "may" includes both performing a certain process and not performing a certain process. In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used and there is no limitation on the use method. In this specification, the term "unsaturated structure" refers to a structure formed by a carbon-carbon double bond, unless otherwise specified. In the present specification, the term "hydrocarbon group" is used to refer to an organic structure formed by two elements of carbon and hydrogen, and it may be an aromatic or non-aromatic group. In the present specification, the use of "halogen" refers to fluorine, chlorine, bromine or iodine. Preferred are fluorine, chlorine or bromine, and more preferred are bromine and chlorine. In this specification, the unit names used are all international standard unit names, and unless otherwise stated, the "%" used indicates weight or mass percentage. In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner. The present invention mainly provides a catalyst suitable for preparing alkynols by acetylation reaction of carbonyl compounds. At the same time, the present invention also provides a synthesis method for preparing alkynols by using the catalyst. Furthermore, the present invention is mainly based on the following insights: The catalyst of the present invention comprises: a metal oxide system obtained by doping with a first metal element and a modifier existing in at least a part of the surface of the metal oxide system. It has been found that the basicity of the support oxide after doping with the first metal is significantly enhanced, which promotes the cleavage of the CH bond in the alkyne to form a carbon anion, which acts as a nucleophile to attack the substrate containing the carbonyl group (such as aldehyde or ketone), significantly improving the reaction speed and conversion rate. The substrate (aldehyde or ketone) is adsorbed on the active site on the catalyst surface, and the alkynol product is quickly separated after the reaction is completed, which improves the selectivity of the reaction. Moreover, the modifier on the catalyst also plays a role in modifying the catalyst. Although the mechanism of the modified catalyst is not completely clear, it is speculated that the modifier combined with the surface of the metal oxide system has a large steric hindrance, but due to its own electronic properties, it does not affect the catalytic alkalinity of the catalyst. At the same time, it can also prevent the alkynol as the product from continuing to adsorb on the catalyst surface to continue the nucleophilic addition reaction, thereby avoiding the production of acetylenic diol by-products and improving the yield of the reaction. The nitrogen atom in the nitrogen heterocycle has an electron-donating property and can chelate with the metal to form a stable metal complex; in addition, the nitrogen atom is easy to transfer electrons, which can realize the recycling of the catalyst. <First aspect> In a first aspect of the present invention, a catalyst suitable for the acetylation reaction of a carbonyl-containing compound with a terminal acetylenic compound is provided. The catalyst of the present invention is a heterogeneous catalyst for the acetylation reaction, and the catalyst comprises a metal oxide system and a modifier present in at least a part of the surface of the metal oxide system. (Carbonyl compounds) In principle, there are no particular limitations on the carbonyl-containing compound of the present invention as long as it is useful for producing alkynol. In some specific embodiments of the present invention, the carbonyl-containing compound of the present invention may have one or more carbonyl groups. Such carbonyl groups may exist in the form of aldehyde groups or ketone groups. In the case of having one carbonyl group, the corresponding alkynol may be obtained by reacting with an alkynyl group; in the case of having multiple carbonyl groups, the corresponding compound having multiple alkynol groups may also be obtained. Alternatively, according to actual needs, some carbonyl groups that do not need to undergo acetylation reaction may be protected, thereby The acetylation reaction is only carried out at a specific site, and the protection method is not particularly limited and can be carried out by a conventional method known in the art. In some specific embodiments of the present invention, the carbonyl-containing compound has a structure or molecular formula as shown in the following formula (I): Wherein, R1 and R2 are the same or different each time they appear, and are independently hydrogen or a monovalent organic group, or R1 and R2 can be connected to form a ring, provided that R1 and R2 are not hydrogen at the same time. In principle, there is no particular limitation on the monovalent organic group as long as it does not affect the acetylation reaction. In some specific embodiments, the monovalent organic group can be selected from a hydrocarbon group having 1 to 50 carbon atoms, preferably 1 to 40 carbon atoms, and more preferably 2 to 30 or 3 to 20 carbon atoms. For these monovalent groups, they can be saturated hydrocarbon groups or hydrocarbon groups with one or more unsaturated structures; in other specific embodiments, these hydrocarbon structures can have any straight chain, branched chain or cyclic structure, and these straight chain, branched chain or cyclic structures can also have any one or more saturated structures (such as aromatic structures, etc.). In some preferred embodiments, it can be a straight chain, branched chain or (partial) cyclic structure group formed by 1 to 15 or 2 to 10 carbon atoms, and have one or two unsaturated structures. In addition, as a monovalent group, the above-mentioned hydrocarbon group may further have an optional substituent, which is not limited and may be selected from a halogen group, a nitrogen-containing group, a sulfur-containing group, an oxygen-containing group (such as an alkoxy group), etc. In addition, for the above-mentioned hydrocarbon group, every two carbon atoms in its hydrocarbon chain may be separated by silicon, oxygen, sulfur atoms or groups centered thereon. Furthermore, in some preferred embodiments of the present invention, the compound of formula (I) can be selected from any one of the group including but not limited to formaldehyde, acetone, butanone, 6-methyl-5-heptene-2-one, 6-methyl-5-octen-2-one, 6-methyl-2-heptanone, geranyl acetone, tetrahydrogeranyl acetone, plant ketone and furfural. Furthermore, through the acetylation reaction described below in the present invention, the corresponding structures formed are (taking acetylene as an example): propargyl alcohol, 2-methyl-3-butyn-2-ol, 3-methyl-pentyn-3-ol, dehydrolinalool, dehydroethyllinalool, dihydrodehydrolinalool, furfuryl acetylene alcohol, dehydronerolidol, tetrahydrodehydronerolidol, dehydroisophytol, and their structural formulas are respectively: (Compounds containing terminal acetylenic groups) The terminal acetylenic group-containing compound of the present invention is mainly used to provide a nucleophilic attacking group for the acetylation reaction. Therefore, the present invention is not particularly limited as long as the compound can undergo acetylation reaction. In some specific embodiments, the terminal alkynyl group-containing compound has the following molecular formula (II): Wherein, R3 is hydrogen or a monovalent organic group. For the monovalent organic group, in principle, it can have the same selection range as the monovalent organic group described above. From the perspective of synthetic economy and downstream utilization of alkynol products, R3 is preferably a hydrogen atom or an alkyl group with 1 to 5 carbon atoms, and more preferably, R3 is a hydrogen atom. For the terminal acetylenic group-containing compound of the present invention, the purity in the acetylation reaction described below is preferably 99% or more to reduce the occurrence of side reactions. (Metal Oxide System) The metal oxide system of the present invention is mainly used to provide catalytic alkalinity to enhance the nucleophilic reaction ability of the terminal acetylenic group-containing compound. Specifically, the metal oxide system of the present invention can be obtained by doping a carrier oxide with a first metal element. For the first metal element, in some specific embodiments of the present invention, it can include one or more of Pd, Ru, Pt, Nb, Bi, Cu, and Co. Preferably, from the perspective of improving substrate conversion rate and selectivity, the first metal element includes a combination of two or more of the above elements. In principle, there are no special restrictions on the carrier oxide as long as it can provide sufficient alkalinity and reaction sites. In some specific embodiments, the carrier oxide can be an oxide of a metal (hereinafter referred to as the "second metal"). For the second metal, it can contain one of transition metals, main group metals, or a mixed metal thereof. In some specific embodiments of the present invention, the second metal may include the same metal element as the first metal element, or the second metal does not include the same metal element as the first metal element. Furthermore, when the second metal includes the same metal element as the first metal element, the surface of the same metal element in the metal oxide system The concentration is higher than that inside. Further, considering the efficiency, selectivity and yield of the acetylation reaction, the carrier oxide usable in the present invention can be selected from a mixture of one or more of CeO2, BaCeO3, CaFeO3, LaCoO3, LaNiO3, LaFeO3, and γ-Al2O3. The support oxide may have a granular shape having a porous surface, and such a support oxide may be self-produced or commercially available. In addition, the carrier oxide doped with the first metal element means that at least a portion of the first metal element is incorporated into the crystal lattice structure of the carrier oxide. (Modifier) The main function of the modifier of the present invention is to provide surface modification for the metal oxide system without affecting the catalytic basicity, so as to provide an effective steric hindrance effect. The modifier of the present invention may include a nitrogen-containing heterocyclic compound, wherein the nitrogen atom provides an effective electronic effect, and the ring structure provides an effective steric effect. There is no particular limitation on the nitrogen-containing heterocyclic compounds of the present invention as long as one nitrogen atom exists in a saturated or unsaturated ring structure. Preferably, these nitrogen-containing heterocyclic compounds can be selected from one or more of pyridine, imidazole, pyrazole, quinoline, and oxazoline compounds. Furthermore, the nitrogen-containing ligand may preferably be selected from one or more of the following nitrogen-containing heterocyclic compounds L1 to L10: For the compound of the above structure, other substituent groups may exist on the ring structure without limitation. For these substituent groups, preferably, they may be alkyl, cycloalkyl, aryl, etc. having 1 to 30 or 2 to 20 carbon atoms. Furthermore, there is no particular limitation on the combination of the modifier and the metal oxide system. The modifier can be applied to at least a portion of the surface of the metal oxide system by impregnation or coating. (catalyst) As described above, the catalyst of the present invention comprises the above-mentioned metal oxide system and a modifier present in at least a portion of the surface of the metal oxide system. For the metal oxide system obtained by doping with a first metal element, the content of the first metal element can be 0.1 to 10 mass % of the mass of the doped carrier oxide, preferably 0.5 to 9 mass %, and more preferably 1 to 8 mass %, for example, 1.5 mass %, 2 mass %, 2.5 mass %, 3 mass %, 3.5 mass %, 4 mass %, 4.5 mass %, 5 mass %, 5.5 mass %, 6 mass %, 6.5 mass %, 7 mass %, 7.5 mass %, etc. Furthermore, regarding the amount of the modifier, in the catalyst, the molar ratio of the nitrogen-containing heterocyclic compound to the first metal element is 10 to 20:1, preferably 12 to 18:1, and more preferably 13 to 16:1. <Second Aspect> In the second aspect of the present invention, a method for preparing the catalyst in the first aspect is provided, the method mainly comprising: i. a first metal element doping step; ii. Modifier loading step. (Step i) The first metal element is doped into the above-mentioned carrier oxide mainly by at least partially inserting the first metal into the lattice structure of the carrier oxide to improve the overall basicity. In some specific embodiments of the present invention, step i may be performed by calcining the first metal source and the support oxide. The first metal source may be various acid salts of the first metal or their hydrates, such as nitrates, hydrochlorides, sulfates, acetates, citrates, formates, ammonium salts and one or more of their hydrates. Preferably, from the perspective of operational convenience, these first metal sources are water-soluble metal salts. In some specific embodiments, the first metal source, carrier oxide and solvent (water or organic solvent, etc.) can be mixed to form a mixed system. Preferably, the system can be mixed at 100-160° C. for 2-6 hours so that the first metal source is adsorbed on the surface of the carrier oxide, and then taken out and calcined. In principle, there is no particular limitation on the calcination conditions. For example, the calcination may be performed at 400-600° C. under atmospheric conditions to obtain a catalyst precursor doped with the first metal element. (Step ii) In principle, there is no particular restriction on the loading method of the modifier. For example, in some specific embodiments, the catalyst precursor can be impregnated with a solution in which the modifier is dissolved or dispersed, or the surface of the catalyst precursor can be coated (such as sprayed) with a solution in which the modifier is dissolved or dispersed to obtain the catalyst of the present invention. In some preferred embodiments, the catalyst precursor can be immersed in a solution in which the modifier is dispersed or dissolved by dipping, preferably, it can be mixed at 100 to 160° C. for 2 to 6 hours. (Other auxiliary methods) There is no particular limitation on other auxiliary preparation methods other than the above two steps, such as washing, stirring, drying and the like, which can be appropriately performed with reference to various known methods in the art. There is no particular limitation on the organic solvents that may be used in the above steps, and examples thereof include alcohol solvents, aromatic solvents and the like. <Third Aspect> The third aspect of the present invention relates to a method for carrying out an acetylation reaction using the catalyst of the first aspect of the present invention. Specifically, the acetylation reaction method of the present invention comprises the step of reacting a carbonyl-containing compound with a terminal acetylenic group-containing compound in the presence of a catalyst. In some specific embodiments, the acetylation reaction of the present invention is carried out with or without a solvent. Therefore, compared with the conventional industrial process in the prior art that uses liquid ammonia as a necessary solvent, it is more economical and environmentally friendly. In addition, for the acetylation reaction, the solvents allowed in the present invention are not particularly limited as long as they are inert to the reaction in principle. In some specific embodiments, these solvents may include alcohol solvents, aromatic solvents (such as toluene, xylene), ether solvents, etc. Furthermore, the temperature of the acetylation reaction can be generally below 70°C, preferably 30 to 60°C, more preferably 40 to 55°C, and the time of the acetylation reaction is less than 6 hours, for example 2 to 4 hours. Hour. In some preferred embodiments, in the reaction system, the mass concentration of the catalyst is controlled to be below 9%, preferably 2-7%. In addition, considering that some terminal acetylenic group-containing compounds are in a gaseous state, the reaction can be carried out under a pressurized state, for example, the acetylation reaction can be carried out under the condition of 0.15-0.25 MPa. In the present invention, the acetylation reaction does not require the use of a catalytic inhibitor such as ammonium chloride to terminate the reaction, and in the absence of a solvent, after the acetylation reaction is completed, the final product can be directly separated. In this case, the solid catalyst can also be obtained while separating the final product. Therefore, for the acetylation reaction of the present invention, the catalyst used therein can be a fresh catalyst (unused) prepared by the preparation method of the second aspect of the present invention, or it can be a regenerated catalyst recovered from a completed acetylation reaction. Regarding the catalyst recovery method, in some specific embodiments, it can be: When the conversion rate of the reactant (containing carbonyl compound) is detected to be lower than the specified standard, such as 90% or 80%, the catalyst is defined as deactivated. After the catalyst is deactivated, it is taken out from the reaction system, cleaned, and placed in a vacuum drying oven at above 100°C for 4 to 6 hours for activation treatment to restore its activity. Furthermore, for the acetylation reaction of the present invention, when using the aforementioned catalyst of the present invention, for carbonyl-containing compounds, the reaction conversion rate can preferably be above 88%, preferably above 90%, more preferably above 95%, and the selectivity can be above 85%, preferably above 90%, more preferably above 92%. Example The embodiments of the present invention are described in detail below with reference to the examples. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially. Example 1 In 30 mL of deionized water, add 1.25 g of Pd(NO3)2·2H2 and 1.62 g of Bi(NO3)2·5H2O. Start stirring at 400r / min, add 10.0g of BaCeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 11.74g of ligand 4,4'-bipyridine (L1, MW: 156.18) and disperse it in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 4 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0% Pd-7.0% Bi / BaCeO3-L1. Example 2 In 30mL of deionized water, add 1.25g of Pd(NO3)2·2H2O and 1.16g of Bi(NO3)2·5H2O, start stirring at 400r / min, and after complete dissolution, add 10.0g of BaCeO3 carrier, raise the temperature to 80℃, continue stirring for 6 hours, remove water by reduced pressure rotary evaporation, obtain a solid and place it in a 100℃ vacuum drying oven, dry to constant weight; take it out and place it in a muffle furnace, calcine at 500℃ for 6 hours, take it out after cooling, and obtain a precursor. Take 19.03g of ligand L10 (MW: 253.11) and disperse it in 50mL of deionized water. After fully stirring and mixing, add the precursor, raise the temperature to 120℃, stir at 400r / min for 4 hours, remove water by reduced pressure rotary evaporation to obtain a solid, place it in a vacuum drying oven at 100℃, and dry it to constant weight to obtain the catalyst 5.0% Pd-5.0% Bi / BaCeO3-L10. Example 3 In 30mL deionized water, add 0.75g Pd(NO3)2·2H2O and 1.62g Bi(NO3)2·5H2O, start stirring at 400r / min, add 10.0g BaCeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 600℃ for 4 hours, take out after cooling, and obtain precursor. Take 11.42g ligand L10 and disperse it in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 4 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 3.0%Pd-7.0%Bi / BaCeO3-L10. Example 4 In 30mL deionized water, add 1.17g PdCl2 and stir at 400r / min until it is completely dissolved. Then add 1.43g of Nb2O5 and 10.0g of CaFeO3 carrier, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 20.55g of ligand 2,2'-bipyridine (L2, MW: 156.18) and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 4 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 7.0% Pd-5.0% Nb / CaFeO3-L2. Example 5 In 30mL of deionized water, add 1.29g of RuCl3·3H2O and 3.52g of Ce(NH4)2(NO3)6, start stirring at 400r / min, and after complete dissolution, add 10.0g of LaCoO3 carrier, raise the temperature to 100℃, continue stirring for 4 hours, remove water by reduced pressure rotary evaporation, obtain a solid and place it in a 100℃ vacuum drying oven, dry to constant weight; take it out and place it in a muffle furnace, calcine at 600℃ for 4 hours, take it out after cooling, and obtain a precursor. Take 8.38g of ligand 4-aminopyridine (L3, MW: 94.11) and disperse it in 30mL deionized water. After fully stirring and mixing, add the precursor, raise the temperature to 120℃, stir at 400r / min for 4 hours, remove water by reduced pressure rotary evaporation to obtain a solid, place it in a vacuum drying oven at 100℃, and dry it to constant weight to obtain the catalyst 5.0%Ru-9.0%Ce / LaCoO3-L3. Example 6 In 30mL deionized water, add 1.29g of RuCl3·3H2O and 1.62g of Bi(NO3)2·5H2O, start stirring at 400r / min, add 10.0g of LaFeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 600℃ for 5 hours, take out after cooling, and obtain precursor. Take 8.38g of ligand 4-aminopyridine (L3, MW: 94.11) and disperse in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 4 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0%Ru-7.0%Bi / LaFeO3-L3. Example 7 In 50 mL of deionized water, add 0.75 g of Pd(NO3)2·2H2O, 1.95 g of Ce(NH4)2(NO3)6, stir at 400r / min, add 10.0g BaCeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 600℃ for 5 hours, take out after cooling, and obtain precursor. Take 8.81g ligand 4,4'-bipyridine (L1) and disperse in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 5 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 3.0%Pd-5.0%Ce / BaCeO3-L1. Example 8 In 50mL deionized water, add 0.86g of PtCl4 and 3.14g of Cu(OAc)2·H2O, start stirring at 400r / min, add 10.0g of LaNiO3 carrier after complete dissolution, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 600℃ for 4 hours, take out after cooling, and obtain precursor. Take 4.26g of ligand 3-aminopyrazole (L4, MW: 83.09) and disperse in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min constant temperature for 4 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0%Pt-10.0%Cu / LaNiO3-L4. Example 9 In 50mL deionized water, add 0.50g PdCl2 and 2.96g Co(OAc)2·4H2O, start stirring at 400r / min, add 10.0g LaFeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 600℃ for 5 hours, take out after cooling, obtain precursor. Take 4.17g ligand 4-methylpyrazole (L5, MW: 82.11) and disperse in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 4 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, obtain catalyst 3.0%Pd-7.0%Co / LaFeO3-L5. Example 10 In 50 mL of deionized water, add 0.86 g of PtCl4 and 3.54 g of CuSO4·5H2O and start stirring. Stir at 400r / min, add 10.0g of CeO2 carrier after it is completely dissolved, heat to 120℃, continue stirring for 6 hours, remove moisture by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 4.43g of ligand 5-aminoquinoline (L6, MW: 144.17) and disperse in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min constant temperature for 6 hours, remove moisture by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0% Pt-9.0% Cu / CeO2-L6. Embodiment 11 In 50mL of deionized water, add 1.29g of RuCl3·3H2O and 1.62g of Bi(NO3)2·5H2O, start stirring at 400r / min, and after complete dissolution, add 10.0g of γ-Al2O3 carrier, raise the temperature to 120°C, continue stirring for 6 hours, remove water by reduced pressure rotary evaporation, obtain a solid and place it in a 100°C vacuum drying oven, dry to constant weight; take it out and place it in a muffle furnace, calcine at 500°C for 6 hours, take it out after cooling, and obtain a precursor. Take 22.82g of ligand 2,2'-biquinoline (L7, MW: 256.3) and disperse it in 30mL deionized water. After fully stirring and mixing, add the precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by reduced pressure rotary evaporation to obtain a solid, place it in a vacuum drying oven at 100℃, and dry it to constant weight to obtain the catalyst 5.0%Ru-7.0%Bi / γ-Al2O3-L7. Example 12 In 50mL of deionized water, add 0.86g of PtCl4 and 1.62g of Bi(NO3)2·5H2O, start stirring at 400r / min, and after complete dissolution, add 10.0g of BaCeO3 carrier, raise the temperature to 100℃, continue stirring for 6 hours, remove water by reduced pressure rotary evaporation, obtain a solid and place it in a 100℃ vacuum drying oven, dry to constant weight; take it out and place it in a muffle furnace, calcine at 500℃ for 6 hours, take it out after cooling, and obtain a precursor. Take 4.67g of ligand 4,4-dimethyloxazoline (L8, Mw: 101.15) and disperse it in 30mL deionized water. After fully stirring and mixing, add the precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by reduced pressure rotary evaporation to obtain a solid, place it in a vacuum drying oven at 100℃, and dry to constant weight to obtain the catalyst 5.0% Pt-7.0% Bi / BaCeO3-L8. Embodiment 13 In 50mL of deionized water, add 0.50g of PdCl2 and 1.96g of Ce(NH4)2(NO3)6, and turn on Stir at 400r / min, add 10.0g of LaFeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 4 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 12.85g of ligand L9 and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min constant temperature for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 3.0%Pd-5.0%Ce / LaFeO3-L9. Embodiment 14 In 50mL deionized water, add 0.25g of Pd(NO3)2·2H2O and 1.62g of Bi(NO3)2·5H2O, start stirring at 400r / min, add 10.0g of BaCeO3 carrier after complete dissolution, heat to 100℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 4.76g of ligand L10 and disperse it in 30mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 1.0%Pd-7.0%Bi / LaFeO3-L10. Embodiment 15 In 50mL deionized water, add 0.83g PdCl2 and 2.74g Ce(NH4)2(NO3)6, start stirring at 400r / min, add 10.0g LaCoO3 carrier after complete dissolution, heat to 160℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 8 hours, take out after cooling, and obtain precursor. Take 19.03g ligand L10 and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0%Pd-7.0%Ce / LaCoO3-L10. Example 16 In 50 mL of deionized water, add 0.75 g of Pd(NO3)2·2H2O, 1.62 g of Bi(NO3)2·5H2O, stir at 400r / min, add 10.0g BaCeO3 carrier after complete dissolution, heat to 160℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, obtain precursor. Take 12.85g ligand L10 and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, obtain catalyst 3.0%Pd-7.0%Bi / BaCeO3-L10. Embodiment 17 In 30mL deionized water, add 1.25g Pd(NO3)2·2H2O and 1.62g Bi(NO3)2·5H2O, start stirring at 400r / min, add 10.0g BaCeO3 carrier after complete dissolution, heat to 160℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 11.89g ligand L10 and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0%Pd-7.0%Bi / BaCeO3-L10. The SEM image of the catalyst morphology is shown in Figure 1. Embodiment 18 In 30mL deionized water, add 0.75g Bi(NO3)2·5H2O and 3.52g Ce(NH4)2(NO3)6, start stirring at 400r / min, add 10.0g BaCeO3 carrier after complete dissolution, heat to 140℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 16.95g ligand L10 and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 7.0%Bi-9.0%Ce / BaCeO3-L10. Embodiment 19 In 30 mL of deionized water, add 1.62 g of Bi(NO3)2·5H2O and 3.63 g of CoCl2·6H2O. Start stirring at 400r / min, add 10.0g of BaCeO3 carrier after complete dissolution, heat to 140℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in a 100℃ vacuum drying oven, dry to constant weight; take out and place in a muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain the precursor. Take 16.95g of ligand L10 and disperse it in 50mL deionized water, stir and mix thoroughly, add the precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in a 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 7.0%Bi-9.0%Co / BaCeO3-L10. Embodiment 20 In 30mL deionized water, add 1.26g of Pd(NO3)2·2H2O, start stirring at 400r / min, add 10.0g of BaCeO3 carrier after complete dissolution, heat to 140℃, continue stirring for 5 hours, remove water by vacuum rotary evaporation, obtain solid and place in 100℃ vacuum drying oven, dry to constant weight; take out and place in muffle furnace, calcine at 500℃ for 6 hours, take out after cooling, and obtain precursor. Take 23.79g of ligand L10 and disperse it in 50mL deionized water, stir and mix thoroughly, add precursor, heat to 120℃, stir at 400r / min for 6 hours, remove water by vacuum rotary evaporation, obtain solid, place in 100℃ vacuum drying oven, dry to constant weight, and obtain catalyst 5.0% Pd / BaCeO3-L10. Embodiment 21 In 30mL of deionized water, add 2.09g of Bi(NO3)2·5H2O and stir at 400r / min. After complete dissolution, add 10.0g of BaCeO3 carrier, raise the temperature to 140°C, continue stirring for 5 hours, remove water by reduced pressure rotary evaporation, obtain a solid and place it in a 100°C vacuum drying oven, dry to constant weight; take it out and place it in a muffle furnace, calcine at 500°C for 6 hours, take it out after cooling, and obtain a catalyst 9.0% Bi / BaCeO3. Embodiment 22 In an autoclave, add 50.0g acetone, 2.5g catalyst 5.0% Pd-7.0% Bi / BaCeO3-L1 (catalyst mass concentration is 5.0%), replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 40°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4.0 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography, and the acetone conversion rate is 98.61%, and the selectivity of 2-methyl-3-butyn-2-ol is 95.53%. The reaction solution was distilled under reduced pressure to recover unreacted raw materials to obtain 68.11 g of crude 2-methyl-3-butyn-2-ol with a calculated yield of 94.08%. Embodiment 23 In an autoclave, add 50.0g acetone, 1.5g catalyst 5.0% Pd-5.0% Bi / BaCeO3-L10 (catalyst mass concentration is 3.0%), replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 50°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4.0 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography, and the acetone conversion rate is 98.82%, and the selectivity of 2-methyl-3-butyn-2-ol is 96.71%. The reaction solution was distilled under reduced pressure to recover unreacted raw materials to obtain 69.09 g of crude 2-methyl-3-butyn-2-ol with a calculated yield of 95.43%. Embodiment 24 In an autoclave, 50.0g of acetone, 3.5g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration of 7.0%), and 50.0g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60°C, constant temperature reaction was maintained, and the acetylene pressure was maintained at 0.20MPa. The reaction was carried out for 4.5 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, the acetone conversion rate was 99.62%, the 2-methyl-3-butyn-2-ol selectivity was 99.53%, and the gas phase spectrum of the reaction liquid was shown in Figure 1. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 71.71 g of crude 2-methyl-3-butyn-2-ol with a calculated yield of 99.05%. Embodiment 25 In an autoclave, add 50.0g acetone, 2.5g catalyst 5.0% Pd-5.0% Bi / BaCeO3-L10 (catalyst mass concentration is 5.0%), 50.0g deionized water, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 60°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography, and the acetone conversion rate is 98.62%, and the selectivity of 2-methyl-3-butyn-2-ol is 93.28%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 66.27 g of crude 2-methyl-3-butyn-2-ol with a calculated yield of 91.53%. Embodiment 26 In an autoclave, add 70.0g butanone, 3.51g catalyst 3.0% Pd-5.0% Bi / BaCeO3-L10 (catalyst mass concentration is 5.0%), 70.0g ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 60°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is detected by gas chromatography, and the butanone conversion rate is 98.73%, and the selectivity of 3-methyl-pentyn-3-ol is 94.93%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 90.19 g of crude 3-methyl-pentyn-3-ol with a calculated yield of 94.67%. Embodiment 27 In an autoclave, 100.0g of 6-methyl-5-heptene-2-one, 7.0g of catalyst 7.0% Pd-5.0% Nb / CaFeO3-L2 (catalyst mass concentration of 7.0%), 100.0g of ethanol were added, nitrogen was replaced 3 times, acetylene was introduced for replacement 3 times, stirring was turned on, and the temperature was set to 50°C, constant temperature reaction was maintained, and the acetylene pressure was maintained at 0.20MPa. The reaction was carried out for 3 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the conversion rate of 6-methyl-5-heptene-2-one was 98.02%, and the selectivity of dehydrolinalool was 95.78%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 112.86 g of crude dehydrolinalool with a calculated yield of 93.56%. Embodiment 28 In an autoclave, add 100.0g of 6-methyl-5-octen-2-one, 5.0g of catalyst 5.0%Ru-9.0%Ce / LaCoO3-L3 (catalyst mass concentration is 5.0%), 100.0g of ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 50°C, constant temperature reaction, maintain acetylene pressure 0.20MPa. React for 4.5 hours, release the pressure, press out the reaction liquid to filter out the catalyst, and the reaction liquid is detected by gas chromatography. The conversion rate of 6-methyl-5-octen-2-one is 98.12%, and the selectivity of dehydroethyl linalool is 97.48%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 113.21 g of crude dehydroethyl linalool with a calculated yield of 95.48%. Embodiment 29 In the autoclave, add 100.0 g of 6-methyl-2-heptanone, 5.0 g of catalyst 5.0% Ru-9.0% Ce / LaCoO3-L3 (catalyst mass concentration is 5.0%), 100.0g ethanol, replaced with nitrogen 3 times, then replaced with acetylene 3 times, stirred, and set the temperature to 60°C, constant temperature reaction, and maintain the acetylene pressure at 0.20MPa. React for 4 hours, release the pressure, press out the reaction liquid and filter out the catalyst, the reaction liquid is detected by gas chromatography, the conversion rate of 6-methyl-2-heptanone is 98.30%, and the selectivity of dihydrodehydrolinalool is 97.63%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 115.26 g of crude dihydrodehydrolinalool with a calculated yield of 95.80%. Embodiment 30 In an autoclave, 100.0 g of furfural, 5.0 g of catalyst 5.0% Ru-7.0% Bi / LaFeO3-L3 (catalyst mass concentration of 5.0%), and 100.0 g of toluene were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 40° C., constant temperature reaction, and the acetylene pressure was maintained at 0.20 MPa. The reaction was carried out for 3.5 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the furfural conversion rate was 98.44%, and the furfuryl acetylene alcohol selectivity was 97.89%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 123.61 g of crude furfuryl acetylene alcohol with a calculated yield of 95.25%. Embodiment 31 In an autoclave, add 100.0g of geranylacetone, 7.0g of catalyst 3.0% Pd-5.0% Ce / BaCeO3-L1 (catalyst mass concentration is 7.0%), 100.0g of isopropanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 60°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is detected by gas chromatography, and the conversion rate of geranylacetone is 97.64%, and the selectivity of dehydrogenated nerolidol is 97.23%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 107.58 g of crude dehydrogenated nerolidol with a calculated yield of 94.87%. Embodiment 32 In an autoclave, 100.0 g of tetrahydrogeranylacetone, 7.0 g of a catalyst 5.0% Pt-10.0% Cu / LaNiO3-L4 (catalyst mass concentration of 7.0%), and 100.0 g of methanol were added. The reaction mixture was replaced with acetylene for 3 times, and then stirred and the temperature was set to 50°C for constant temperature reaction, with the acetylene pressure maintained at 0.20 MPa. The reaction mixture was reacted for 5.0 hours, and the pressure was released. The reaction liquid was pressed out and the catalyst was filtered out. The reaction liquid was tested by gas chromatography, and the conversion rate of geranyl acetone was 97.82%, and the selectivity of tetrahydrodehydronerolidol was 96.05%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 106.12 g of crude tetrahydrodehydronerolidol with a calculated yield of 93.81%. Embodiment 33 In an autoclave, 100.0g of plant ketone, 7.0g of catalyst 3.0% Pd-7.0% Co / LaFeO3-L5 (catalyst mass concentration of 7.0%), and 100.0g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60°C, constant temperature reaction, and the acetylene pressure was maintained at 0.20MPa. The reaction was carried out for 5.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the plant ketone conversion rate was 97.42%, and the dehydroisophytol selectivity was 97.35%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 103.90 g of crude dehydroisophytol with a calculated yield of 94.72%. Embodiment 34 In an autoclave, add 100.0g of acetone, 7.0g of catalyst 5.0% Pt-9.0% Cu / CeO2-L6 (catalyst mass concentration is 7.0%), 100.0g of ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 60°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 5.0 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is detected by gas chromatography, and the acetone conversion rate is 98.48%, and the selectivity of 2-methyl-3-butyn-2-ol is 96.01%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 68.31 g of crude 2-methyl-3-butyn-2-ol with a calculated yield of 94.26%. Embodiment 35 In an autoclave, add 100.0g of butanone, 7.0g of catalyst 5.0% Ru-7.0% Bi / γ-Al2O3-L7 (catalyst mass concentration is 7.0%), and 100.0g of ethanol. Replace with nitrogen 3 times, then introduce acetylene 3 times, start stirring, set the temperature to 40°C, and react at a constant temperature, maintaining the acetylene pressure at 0.20MPa. React for 5.0 hours, release the pressure, press out the reaction liquid, filter out the catalyst, and detect the reaction liquid by gas chromatography. The ketone conversion rate was 96.57%, and the selectivity of 3-methyl-pentyn-3-ol was 95.62%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 125.43 g of crude 3-methyl-pentyn-3-ol with a calculated yield of 92.16%. Embodiment 36 In an autoclave, 100.0 g of 6-methyl-5-heptene-2-one, 7.0 g of catalyst 5.0% Pt-7.0% Bi / BaCeO3-L8 (catalyst mass concentration of 7.0%), and 100.0 g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60° C., constant temperature reaction, and the acetylene pressure was maintained at 0.20 MPa. The reaction was carried out for 4.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the conversion rate of 6-methyl-5-heptene-2-one was 97.69%, and the selectivity of dehydrolinalool was 96.73%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 113.83 g of crude dehydrolinalool with a calculated yield of 94.36%. Embodiment 37 In an autoclave, 100.0 g of 6-methyl-5-octen-2-one, 9.0 g of catalyst 3.0% Pd-5.0% Ce / LaFeO3-L9 (catalyst mass concentration is 9.0%), 100.0 g of ethanol, nitrogen replacement 3 times, acetylene replacement 3 times, stirring, and setting the temperature to 60 ° C, constant temperature reaction, maintaining acetylene pressure 0.20 MPa. React for 3.0 hours, release the pressure, press out the reaction liquid to filter out the catalyst, the reaction liquid is detected by gas chromatography, 6-methyl-5-octen-2-one conversion rate 98.64%, dehydroethyl linalool selectivity 96.51%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 112.71 g of crude dehydroethyl linalool with a calculated yield of 95.06%. Embodiment 38 In an autoclave, add 100.0g of 6-methyl-2-heptanone, 7.0g of catalyst 1.0% Pd-7.0% Bi / LaFeO3-L10 (catalyst mass concentration is 7.0%), 100.0g of ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 50°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4.0 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography. The conversion rate of 6-methyl-5-octen-2-one is 95.31%, and the dihydrodehydrolinalool is 1.31%. Selectivity 96.34%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 110.36 g of crude dihydrodehydrolinalool with a calculated yield of 91.73%. Embodiment 39 In an autoclave, 100.0g of furfural, 5.0g of catalyst 5.0% Pd-7.0% Ce / LaCoO3-L10 (catalyst mass concentration of 5.0%), and 100.0g of ethanol were added, replaced with nitrogen 3 times, and then acetylene was introduced for replacement 3 times, stirring was turned on, and the temperature was set to 50°C, constant temperature reaction was maintained, and the acetylene pressure was maintained at 0.20MPa. The reaction was carried out for 6.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the furfural conversion rate was 99.31%, and the furfuryl acetylene alcohol selectivity was 98.29%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 126.53 g of crude furfuryl acetylene alcohol with a calculated yield of 97.50%. Embodiment 40 In an autoclave, add 100.0g of geranylacetone, 5.0g of catalyst 3.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration is 5.0%), 100.0g of ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 60°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 3.5 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography, and the conversion rate of geranylacetone is 99.52%, and the selectivity of dehydrogenated nerolidol is 98.37%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 110.69 g of crude dehydrogenated nerolidol with a calculated yield of 97.61%. Embodiment 41 In an autoclave, 100.0 g of 6-methyl-5-octen-2-one, 5.0 g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration of 5.0%), and 100.0 g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60° C., constant temperature reaction, and the acetylene pressure was maintained at 0.20 MPa. The reaction was carried out for 3.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the conversion rate of 6-methyl-5-octen-2-one was 99.72%, and the selectivity of dehydroethyl linalool was 98.58%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 116.48 g of crude dehydroethyl linalool with a calculated yield of 98.24%. Embodiment 42 In an autoclave, 100.0 g of 6-methyl-5-octen-2-one, 1.0 g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration of 1.0%), and 100.0 g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60° C., constant temperature reaction, and the acetylene pressure was maintained at 0.20 MPa. The reaction was carried out for 5.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the conversion rate of 6-methyl-5-octen-2-one was 89.49%, and the selectivity of dehydroethyl linalool was 97.61%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 103.43 g of crude dehydroethyl linalool with a calculated yield of 87.23%. Embodiment 43 In an autoclave, 100.0g of 6-methyl-5-heptene-2-one (content 98.5%), 5.0g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration of 5.0%), 100.0g of ethanol were added, nitrogen was used for replacement 3 times, acetylene was introduced for replacement 3 times, stirring was turned on, and the temperature was set to 60°C, constant temperature reaction was maintained, and the acetylene pressure was maintained at 0.20MPa. The reaction was carried out for 5.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography. The conversion rate of 6-methyl-5-heptene-2-one was 98.69%, the selectivity of dehydrolinalool was 97.74%, and the gas phase spectrum of the reaction liquid was shown in Figure 2. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials and raw materials to obtain 125.07 g of crude dehydrolinalool with a calculated yield of 96.37%. Embodiment 44 In an autoclave, add 50.0g of formaldehyde, 5.0g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration is 5.0%), 100.0g of ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 30°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 4.0 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography, and the formaldehyde conversion rate is 99.67%, and the propargyl alcohol selectivity is 98.38%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 91.41 g of crude propargyl alcohol. The calculated yield is 97.92%. Embodiment 45 In an autoclave, add 100.0g of tetrahydrogeranyl acetone, 10.0g of catalyst 7.0% Bi-9.0% Ce / BaCeO3-L10 (catalyst mass concentration is 10.0%), 100.0g of ethanol, replace with nitrogen 3 times, then introduce acetylene for replacement 3 times, start stirring, set the temperature to 40°C, react at a constant temperature, and maintain the acetylene pressure at 0.20MPa. React for 6.0 hours, release the pressure, press out the reaction liquid and filter out the catalyst. The reaction liquid is tested by gas chromatography, and the conversion rate of tetrahydrogeranyl acetone is 90.71%, and the selectivity of tetrahydrodehydronerolidol is 89.64%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 91.74 g of crude tetrahydrodehydronerolidol with a calculated yield of 81.10%. Embodiment 46 In an autoclave, 100.0g of plant ketone, 10.0g of catalyst 7.0% Bi-9.0% Co / BaCeO3-L10 (catalyst mass concentration of 10.0%), and 100.0g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60°C, constant temperature reaction, and the acetylene pressure was maintained at 0.20MPa. The reaction was carried out for 6.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, the plant ketone conversion rate was 91.52%, and the dehydroisophytol selectivity was 85.23%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 85.20 g of crude dehydroisophytol with a calculated yield of 77.67%. Embodiment 47 In an autoclave, 100.0 g of 6-methyl-5-octen-2-one, 10.0 g of catalyst 5.0% Pd / BaCeO3-L10 (catalyst mass concentration of 10.0%), and 100.0 g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60° C., constant temperature reaction, and the acetylene pressure was maintained at 0.20 MPa. The reaction was carried out for 6.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the conversion rate of 6-methyl-5-octen-2-one was 89.82%, and the selectivity of dehydroethyl linalool was 86.29%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 91.67 g of crude dehydroethyl linalool with a calculated yield of 77.31%. Comparative Example 1 In an autoclave, 100.0 g of 6-methyl-5-octen-2-one, 10.0 g of catalyst 9.0% Bi / BaCeO3 (catalyst mass concentration of 10.0%), and 100.0 g of ethanol were added, replaced with nitrogen 3 times, and then replaced with acetylene 3 times, stirring was turned on, and the temperature was set to 60° C., constant temperature reaction, and the acetylene pressure was maintained at 0.20 MPa. The reaction was carried out for 6.0 hours, the pressure was released, the reaction liquid was pressed out and the catalyst was filtered out, and the reaction liquid was detected by gas chromatography, and the conversion rate of 6-methyl-5-octen-2-one was 80.26%, and the selectivity of dehydroethyl linalool was 62.34%. The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials to obtain 58.72 g of crude dehydroethyl linalool with a calculated yield of 49.52%. The above examples and comparative examples are shown in Table 1: Table 1: Embodiment 48 The catalyst recovered in Example 43 was directly subjected to a catalyst application experiment, and the reaction conditions and operations were the same as in Example 43. The experimental results are shown in Table 2. Table 2: It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto. The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A catalyst for preparing alkynols via the reaction of a carbonyl-containing compound with a terminal alkynyl-containing compound, characterized in that: The catalyst comprises a modifier and a metal oxide system, wherein the metal oxide system is a carrier oxide doped with a first metal element. in, The modifier includes a nitrogen-containing heterocyclic compound, The first metal element includes one or more of Pd, Ru, Pt, Nb, Bi, Cu and Co, Furthermore, the modifier is present in at least a portion of the surface region of the metal oxide system.

2. The catalyst according to claim 1, characterized in that The carbonyl-containing compound has a molecular formula represented by the following formula (I): Wherein, R1 and R2 are the same or different each time they appear, and are independently hydrogen or a monovalent organic group, or R1 and R2 can be connected to form a ring, provided that R1 and R2 are not hydrogen at the same time.

3. The catalyst according to claim 1 or 2, characterized in that The terminal acetylenic group-containing compound has the following molecular formula (II): Wherein, R3 is hydrogen or a monovalent organic group.

4. The catalyst according to any one of claims 1 to 3, characterized in that The nitrogen-containing heterocyclic compound is selected from one or more of pyridine, imidazole, pyrazole, quinoline and oxazoline compounds.

5. The catalyst according to any one of claims 1 to 4, characterized in that In the metal oxide system, the content of the first metal element is 0.1 to 10% by mass of the doped carrier oxide.

6. The catalyst according to any one of claims 1 to 5, characterized in that In the catalyst, the molar ratio of the nitrogen-containing heterocyclic compound to the first metal element is 10 to 20:

1.

7. The catalyst according to any one of claims 1 to 6, characterized in that The first metal element includes two or more elements of Pd, Ru, Pt, Nb, Bi, Cu and Co.

8. A method for preparing alkynols, characterized in that: The method comprises: In the step of reacting a carbonyl-containing compound with a terminal acetylenic group-containing compound in the presence of the catalyst according to any one of claims 1 to 7, the reaction is carried out with or without a solvent.

9. The method according to claim 8, characterized in that The reaction temperature is below 70° C., and the reaction time is below 6 hours.

10. The method according to claim 8 or 9, characterized in that: The catalyst is a newly prepared catalyst or a reused catalyst.

Citation Information

Patent Citations

  • Ethynation method

    CN110467519A

  • Catalyst and ethynylation process

    CN116651451A

  • Method for producing orthoalkylated hydroxyaromatic compound

    JP2005029518A