Aluminum-zinc-silicon-magnesium-plated steel sheet
Optimizing the magnesium content in the plating film of aluminum-zinc-silicon-magnesium plated steel sheets to 0.7-0.98% addresses corrosion resistance and appearance degradation issues, ensuring effective corrosion protection and stability during environmental exposure.
Patent Information
- Application Number
- PCT/JP2023/019178
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
Aluminum-zinc-silicon-magnesium plated steel sheets face issues with corrosion resistance deterioration and appearance degradation when exposed to natural environments, particularly during processing.
The composition of the plating film is optimized with a magnesium content between 0.7% and 0.98% by mass, along with 50-60% aluminum and 1.1-2.0% silicon, to enhance corrosion resistance and maintain appearance integrity.
This composition significantly reduces corrosion loss and crack width standard deviation, maintaining corrosion resistance and appearance quality even after repeated cyclic corrosion tests.
Smart Images

Figure JP2023019178_28112024_PF_FP_ABST
Abstract
Description
Aluminum-zinc-silicon-magnesium coated steel sheet
[0001] The present invention relates to an aluminum-zinc-silicon-magnesium plated steel sheet.
[0002] Patent Document 1 discloses an iron product having a coating. The coating contains aluminum, silicon, and zinc. The mass % of aluminum in the coating is 25 mass % to 70 mass %. The mass % of silicon in the coating is 0.5 mass % or more. According to the invention disclosed in Patent Document 1, an iron product having a coating with excellent ductility, excellent adhesion, and excellent corrosion resistance is provided.
[0003] Patent Document 2 discloses an aluminum-zinc-silicon-magnesium-based plated steel sheet. The plating film of this aluminum-zinc-silicon-magnesium-based plated steel sheet contains 45% by mass to 65% by mass of aluminum, 1.0% by mass to 4.0% by mass or less of silicon, and 1.0% by mass to 10.0% by mass of magnesium. The remainder of the plating film consists of zinc and unavoidable impurities. The Mg in this plating film 2 Si and MgZn 2 The diffraction intensity of Mg measured by X-ray diffraction satisfies the following relationship (1): 2 Si(111) / MgZn 2 (100)≦2.0 (1) where Mg 2 Si(111):Mg 2 Diffraction intensity of Si (111) plane (plane spacing d = 0.3668 nm) MgZn 2 (100): MgZn 2 The diffraction intensity of the (100) plane (plane spacing d=0.4510 nm) of the sample is: According to the invention disclosed in Patent Document 2, stable and excellent corrosion resistance can be achieved.
[0004] Japanese Patent Publication No. 46-7161 Japanese Patent Application Laid-Open No. 2022-73969
[0005] There is room for further improvement in corrosion resistance in the coating of the iron product disclosed in Patent Document 1. The aluminum-zinc-silicon-magnesium plated steel sheet disclosed in Patent Document 2 has superior corrosion resistance compared to the iron product disclosed in Patent Document 1.
[0006] However, the aluminum-zinc-silicon-magnesium-based plated steel sheet disclosed in Patent Document 2 has room for further improvement in terms of suppressing deterioration of appearance when initially exposed to the natural environment and the effect of processing on corrosion resistance. The present invention aims to solve these problems. Its object is to provide an aluminum-zinc-silicon-magnesium-based plated steel sheet that is suppressed in terms of suppressing deterioration of appearance when initially exposed to the natural environment and suppressing a decrease in corrosion resistance when processed.
[0007] As a result of extensive research into the above-mentioned problems, the present inventors discovered that when the mass percent of magnesium contained in the plating film satisfies certain requirements, the initial deterioration of appearance after exposure to the natural environment can be suppressed, and the decrease in corrosion resistance after processing can be suppressed, leading to the completion of the present invention.
[0008] In order to solve the above-mentioned problems, according to one aspect of the present invention, an aluminum-zinc-silicon-magnesium-based plated steel sheet comprises a base steel sheet and a plating film. The plating film contains zinc, 50% by mass or more and 60% by mass or less of aluminum, 1.1% by mass or more and 2.0% by mass or less of silicon, and magnesium. The sum of the mass percent of zinc, the mass percent of aluminum, the mass percent of silicon, and the mass percent of magnesium contained in the plating film is less than 100% by mass. The mass percent of magnesium in the plating film is 0.7% by mass or more and 0.98% by mass or less.
[0009] Furthermore, it is desirable that the mass % of magnesium in the above-mentioned plating film is 0.7 mass % or more and 0.81 mass % or less.
[0010] According to the present invention, deterioration of the appearance when exposed to the natural environment is suppressed initially, and deterioration of corrosion resistance when processed is suppressed.
[0011] FIG. 1 is a diagram showing the configuration of an aluminum-zinc-silicon-magnesium-based plated steel sheet according to an embodiment of the present invention. FIG. 2 is a conceptual diagram showing the configuration of continuous hot-dip galvanizing equipment according to examples and comparative examples of the present invention. FIG. 3 is a diagram showing data on the composition, corrosion loss, and cracks of plated films according to examples and comparative examples of the present invention. FIG. 4 is a diagram showing the effect of the magnesium concentration of plated films on the corrosion loss at the time point when 60 cycles of cyclic corrosion testing have been repeated according to examples and comparative examples of the present invention. FIG. 5 is a diagram showing the surface of samples up to 240 cycles of cyclic corrosion testing according to examples and comparative examples of the present invention. FIG. 6 is a diagram showing the surface of samples at the time point when 156 cycles of cyclic corrosion testing have been repeated according to examples and comparative examples of the present invention. FIG. 7 is a diagram showing the surface of samples at the time point when 540 cycles of cyclic corrosion testing have been repeated according to examples and comparative examples of the present invention.
[0012] Hereinafter, an embodiment of the present invention will be described.
[0013] <Description of the Structure of the Aluminum-Zinc-Silicon-Magnesium-Based Plated Steel Sheet> Fig. 1 is a schematic diagram of a cross section of an aluminum-zinc-silicon-magnesium-based plated steel sheet 10 according to this embodiment. The aluminum-zinc-silicon-magnesium-based plated steel sheet 10 according to this embodiment comprises a substrate steel sheet 20 and a plating coating 22. The substrate steel sheet 20 according to this embodiment is the same as a well-known steel sheet, and therefore a detailed description thereof will not be repeated. The plating coating 22 according to this embodiment is formed on the surface of the substrate steel sheet 20.
[0014] <Description of Components of Plated Coating> The plated coating 22 according to this embodiment contains aluminum, zinc, silicon, and magnesium.
[0015] In this embodiment, the mass % of aluminum contained in the plating film 22 is 50 mass % or more and 60 mass % or less. As long as it is within this range, the specific mass % of aluminum contained in the plating film 22 according to this embodiment is not particularly limited. However, it is particularly desirable that the mass % of aluminum be close to 55 mass %. Therefore, it is desirable that the mass % of aluminum be within a range of, for example, 54 mass % or more and 59 mass % or less.
[0016] In this embodiment, the mass % of silicon contained in the plating film 22 is 1.1 mass % or more and 2.0 mass % or less. As long as it is within this range, the specific mass % of silicon contained in the plating film 22 according to this embodiment is not particularly limited. However, it is desirable that the mass % of silicon be a value within a predetermined range, for example, 0.022 to 0.029 times the mass % of aluminum contained in the plating film 22.
[0017] The mass % of magnesium contained in the plating film 22 according to this embodiment is 0.7 mass % or more and 0.98 mass % or less. The specific mass % of magnesium contained in the plating film 22 according to this embodiment is not particularly limited as long as it is 0.7 mass % or more and 0.98 mass % or less. However, the mass % of magnesium is preferably 0.7 mass % or more and 0.81 mass % or less.
[0018] The total of the mass percent of aluminum, the mass percent of zinc, the mass percent of silicon, and the mass percent of magnesium contained in the plating film 22 according to this embodiment is less than 100 mass percent. As long as this requirement is met, the specific mass percent of zinc contained in the plating film 22 according to this embodiment is not particularly limited. Furthermore, the plating film 22 according to this embodiment may contain optional components in addition to aluminum, zinc, silicon, and magnesium. However, it is desirable that the optional components be limited to unavoidable impurities.
[0019] <Description of Manufacturing Method> The manufacturing method of the aluminum-zinc-silicon-magnesium-based plated steel sheet according to the present invention is similar to the manufacturing method of well-known aluminum-zinc-silicon-magnesium-based plated steel sheet, and therefore, detailed description thereof will not be repeated here.
[0020] <Explanation of Examples> Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0021] (Description of Continuous Hot-Dip Galvanizing Equipment) In this example and comparative example, aluminum-zinc-silicon-magnesium-plated steel sheets are produced using well-known continuous hot-dip galvanizing equipment. FIG. 2 is a conceptual diagram showing the configuration of the continuous hot-dip galvanizing equipment. The continuous hot-dip galvanizing equipment includes a plating pot 40, a metal roll 42, a gas wiping nozzle 44, a forced-air cooling system 46, and a steel sheet transport device (not shown). The plating pot 40 contains molten metal for plating. When the substrate steel sheet 20 is immersed in the molten metal, the molten metal adheres to the substrate steel sheet 20. The metal roll 42 is contained within the plating pot 40. When the plating pot 40 contains the molten metal, the metal roll 42 is submerged in the molten metal. The metal roll 42 changes the traveling direction of the substrate steel sheet 20 immersed in the molten metal. The gas wiping nozzle 44 sprays gas onto the substrate steel sheet 20 as it is pulled out of the molten metal. This removes excess molten metal adhering to the substrate steel sheet 20. The forced air cooling equipment 46 air-cools the substrate steel sheet 20 from which excess molten metal has been removed by the gas wiping nozzle 44. This solidifies the molten metal remaining on the surface of the substrate steel sheet 20. The solidified molten metal becomes the plating coating 22. The steel sheet transport device transports the substrate steel sheet 20 so that it is immersed in the molten metal in the plating pot 40, and then pulled up and passes through the gas wiping nozzle 44 and the forced air cooling equipment 46.
[0022] Example 1 (Preparation of Molten Metal) To prepare the molten metal for use in a plating bath, an operator placed aluminum bare metal, silicon bare metal, magnesium bare metal, and molten zinc in a plating pot 40. At this time, the mass % of aluminum in the metal placed in the plating pot 40 was 55 mass %. The mass % of silicon in the metal placed in the plating pot 40 was 1.6 mass %. The mass % of magnesium in the metal placed in the plating pot 40 was 0.7 mass %. The mass % of zinc in the metal placed in the plating pot 40 was 42.7 mass %. Once the aluminum, silicon, and magnesium had dissolved in the zinc, the operator adjusted the temperature of the molten metal in the plating pot 40 to 600 degrees Celsius (873.15 Kelvin).
[0023] (Preparation of the base steel sheet) To prepare the base steel sheet 20, an operator sprayed cooling gas onto the base steel sheet 20, which had been heated to 700°C (973.15 Kelvin). The thickness of the base steel sheet 20 was 0.5 mm. As a result, the temperature of the base steel sheet 20 became 500°C (773.15 Kelvin).
[0024] (Coating Bath) To form a plating film 22 on the surface of the substrate steel sheet 20, the steel sheet transport device of the continuous hot-dip plating equipment described above placed the substrate steel sheet 20 prepared as described above into the coating pot 40 containing the molten metal prepared as described above. As a result, the molten metal adhered to the surface of the substrate steel sheet 20. Once the molten metal adhered to the surface of the substrate steel sheet 20, the steel sheet transport device lifted the substrate steel sheet 20 from the coating pot 40 and passed it through a gas wiping nozzle 44 and forced air cooling equipment 46. The gas wiping nozzle 44 sprayed gas onto the substrate steel sheet 20, thereby removing excess molten metal from the surface of the substrate steel sheet 20. The forced air cooling equipment 46 air-cooled the substrate steel sheet 20 from which the excess molten metal had been removed by the gas spraying. As a result of this air cooling, the molten metal adhering to the substrate steel sheet 20 solidified. As the molten metal solidifies, the alloy that was the molten metal becomes the plating film 22 on the substrate steel sheet 20. The substrate steel sheet 20 with the plating film 22 formed on its surface is the aluminum-zinc-silicon-magnesium-based plated steel sheet 10 according to this example.
[0025] (Cyclic Corrosion Test) An operator cut out a test specimen (dimensions: length 150 mm × width 70 mm × thickness 0.5 mm) from the aluminum-zinc-silicon-magnesium-plated steel sheet 10 according to this example. The operator coated the side and back surfaces of the test specimen with paint. This prevented the side and back surfaces of the test specimen from corroding when saltwater was sprayed onto the front surface of the test specimen. Once the side and back surfaces of the test specimen were coated with paint, the operator measured the mass of the test specimen. This mass is referred to as the "mass before test." After measuring the mass before test, the operator performed a cyclic corrosion test on the test specimen in accordance with Japan Automotive Engineering Society (JASO) M609. That is, the following cycle was repeated up to 600 times. The cycle consisted of spraying saltwater on the test specimen for two hours, drying the saltwater-sprayed test specimen for four hours, and then placing the dried test specimen in a humid environment for two hours. The specific details of this test are well known, so a detailed description thereof will not be repeated here. The test specimen used for the cyclic corrosion test was a CCT-1L manufactured by Suga Testing Instruments Co., Ltd. After the cyclic corrosion test was completed, the operator immersed the test specimen in a nitric acid aqueous solution (concentration: 15% by mass) for 30 seconds. This removed corrosion products from the test specimen. The operator then dried the test specimen after removing it from the nitric acid aqueous solution. The operator measured the mass of the dried test specimen. This mass is referred to as the "post-test mass." After measuring the post-test mass, the operator calculated the difference between the pre-test mass and the post-test mass. After calculating this difference, the operator divided this difference by the area of the front surface (the exposed surface without paint) of the test specimen (150 mm x 70 mm = 10,500 square millimeters = 0.0105 square meters). The value obtained by this division was the corrosion loss amount for this example. The corrosion loss amount was 7.11 grams / square meter.
[0026] (Crack Width Measurement) An operator cut out a test specimen (20 mm length × 20 mm width × 0.5 mm thickness) from the aluminum-zinc-silicon-magnesium-plated steel sheet 10 according to this example. The operator bent the test specimen using well-known pliers and a vice. The operator bent the test specimen so that the inner diameter of the recessed portion formed by the bending was twice the plate thickness of the test specimen. After the test specimen was bent, the operator attached the bent portion to a scanning electron microscope (model number: JSM-7001F) manufactured by JEOL Ltd., and measured the crack width at the bent portion. The crack width was measured according to the following procedure. First, the operator drew a line 1 mm long in actual size at a location on the test specimen that corresponded to an area of 3 mm length × 2 mm width in actual size on the image obtained by the scanning electron microscope. In the following description, this line will be referred to as the "calibration line." The calibration lines were drawn so as to extend perpendicular to the ridge direction in the bending process described above. Five calibration lines were drawn at each location corresponding to an area of 3 mm length x 2 mm width in actual size. After the five calibration lines were drawn, the operator measured the number of cracks intersecting the calibration lines and the width of each crack at the location where the calibration line intersected the test line. The number of cracks and crack widths were similarly measured at four other locations on the test piece. This resulted in the number of cracks and crack widths being measured at five locations on one test piece. Consequently, the number of cracks and crack widths were measured for 25 calibration lines. In this example, the total number of cracks at those five locations was 130. After measuring the number of cracks and crack widths, the operator calculated the standard deviation of the crack widths. In this example, the standard deviation of the crack widths was 12.8.
[0027] Example 2 (Preparation of Molten Metal) The aluminum-zinc-silicon-magnesium based plating molten metal according to this example was prepared in the same manner as in Example 1. Therefore, the detailed description thereof will not be repeated here.
[0028] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this example is the same as in Example 1. Therefore, the detailed description thereof will not be repeated here.
[0029] (Plating Bath) The plating bath according to this example is the same as that in Example 1. Therefore, detailed description thereof will not be repeated here.
[0030] (Crack Width Measurement) No crack width measurement was performed for this example.
[0031] (Cyclic Corrosion Test) The specific procedure for the cyclic corrosion test according to this example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated here. The corrosion loss in this example was 7.66 grams / m².
[0032] Example 3 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this example was the same as that of Example 1, except for the following points: the mass % of zinc in the metal placed in the plating pot 40 was 42.62 mass %, and the mass % of magnesium in the metal placed in the plating pot 40 was 0.78 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this example will not be repeated.
[0033] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this example is the same as in Example 1. Therefore, the detailed description thereof will not be repeated here.
[0034] (Plating Bath) The plating bath according to this example is the same as that in Example 1. Therefore, detailed description thereof will not be repeated here.
[0035] (Crack Width Measurement) No crack width measurement was performed for this example.
[0036] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this example was 7.78 g / m².
[0037] Example 4 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this example was the same as that of Example 1, except for the following points: the mass % of zinc in the metal placed in the plating pot 40 was 42.59 mass %, and the mass % of magnesium in the metal placed in the plating pot 40 was 0.81 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this example will not be repeated.
[0038] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this example is the same as in Example 1. Therefore, the detailed description thereof will not be repeated here.
[0039] (Plating Bath) The plating bath according to this example is the same as that in Example 1. Therefore, detailed description thereof will not be repeated here.
[0040] (Crack Width Measurement) No crack width measurement was performed for this example.
[0041] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this example was 7.83 g / m².
[0042] Example 5 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this example was the same as that of Example 1, except for the following points: the mass % of zinc in the metal placed in the plating pot 40 was 42.42 mass %, and the mass % of magnesium in the metal placed in the plating pot 40 was 0.98 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this example will not be repeated.
[0043] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this example is the same as in Example 1. Therefore, the detailed description thereof will not be repeated here.
[0044] (Plating Bath) The plating bath according to this example is the same as that in Example 1. Therefore, detailed description thereof will not be repeated here.
[0045] (Crack Width Measurement) The specific procedure for measuring crack width in this example was the same as in Example 1. Therefore, a detailed description thereof will not be repeated. In this example, the total number of cracks in five locations on the test piece was 139. The standard deviation of the crack width was 12.7. (Cyclic Corrosion Test) The specific procedure for the cyclic corrosion test in this example was the same as in Example 1. Therefore, a detailed description thereof will not be repeated. The corrosion loss in this example was 10.46 grams / m².
[0046] Comparative Example 1 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc in the metal placed in the plating pot 40 was 43.4 mass %, and the mass % of magnesium in the metal placed in the plating pot 40 was 0 mass %, i.e., no magnesium was contained. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0047] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0048] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0049] (Crack Width Measurement) The specific procedure for measuring the crack width in this comparative example was the same as in Example 1. Therefore, the detailed description thereof will not be repeated. In this comparative example, the total number of cracks in the five locations on the test piece was 134. The standard deviation of the crack width was 10.9.
[0050] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 13.98 g / m².
[0051] Comparative Example 2 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc in the metal placed in the plating pot 40 was 43.1 mass %, and the mass % of magnesium in the metal placed in the plating pot 40 was 0.3 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0052] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0053] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0054] (Crack Width Measurement) No crack width measurement was performed for this comparative example.
[0055] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 6.43 grams / m².
[0056] Comparative Example 3 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.95 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 0.45 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0057] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0058] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0059] (Crack Width Measurement) No crack width measurement was performed for this comparative example.
[0060] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 6.33 grams / m².
[0061] Comparative Example 4 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.85 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 0.55 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0062] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0063] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0064] (Crack Width Measurement) No crack width measurement was performed for this comparative example.
[0065] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 8.33 g / m².
[0066] Comparative Example 5 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.28 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 1.12 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0067] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0068] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0069] (Crack Width Measurement) The specific procedure for measuring the crack width in this comparative example was the same as in Example 1. Therefore, the detailed description thereof will not be repeated. In this comparative example, the total number of cracks in the five locations on the test piece was 141. The standard deviation of the crack width was 17.3.
[0070] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss amount in this comparative example was 10.49 g / m².
[0071] Comparative Example 6 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.22 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 1.18 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0072] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0073] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0074] (Crack Width Measurement) No crack width measurement was performed for this comparative example.
[0075] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 13.43 g / m².
[0076] Comparative Example 7 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.15 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 1.25 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0077] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0078] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0079] (Crack Width Measurement) No crack width measurement was performed for this comparative example.
[0080] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 12.52 grams / m².
[0081] Comparative Example 8 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.11 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 1.29 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0082] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0083] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0084] (Crack Width Measurement) No crack width measurement was performed for this comparative example.
[0085] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 13.47 g / m².
[0086] Comparative Example 9 (Preparation of Molten Metal) The preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example was the same as that of Example 1, except for the following points: the mass % of zinc relative to the metal placed in the plating pot 40 was 42.03 mass %, and the mass % of magnesium relative to the metal placed in the plating pot 40 was 1.37 mass %. Therefore, except for these points, the description of the preparation of the aluminum-zinc-silicon-magnesium-based coating molten metal according to this comparative example will not be repeated.
[0087] (Preparation of Base Steel Sheet) The preparation of the base steel sheet 20 according to this comparative example was the same as in Example 1. Therefore, detailed description thereof will not be repeated here.
[0088] (Plating Bath) The plating bath used in this comparative example is the same as that used in Example 1. Therefore, detailed description thereof will not be repeated here.
[0089] (Crack Width Measurement) The specific procedure for measuring the crack width in this comparative example was the same as in Example 1. Therefore, the detailed description thereof will not be repeated. In this comparative example, the total number of cracks in the five locations on the test piece was 128. The standard deviation of the crack width was 17.7.
[0090] (Cyclic Corrosion Test) The specific procedure of the cyclic corrosion test according to this comparative example was the same as that of Example 1. Therefore, the detailed description thereof will not be repeated. The corrosion loss in this comparative example was 11.17 g / m².
[0091] <Explanation of Effects> FIG. 3 is a diagram showing data on the composition, corrosion loss, and cracking of the plating film according to the examples and comparative examples. FIG. 4 is a diagram showing the effect of the magnesium concentration of the plating film 22 according to the examples and comparative examples on the corrosion loss after 60 cycles of cyclic corrosion testing. FIG. 5 is a diagram showing the surface of a sample after 240 cycles of cyclic corrosion testing according to the examples and comparative examples. FIG. 6 is a diagram showing the surface of a sample after 156 cycles of cyclic corrosion testing according to the examples and comparative examples. FIG. 7 is a diagram showing the surface of a sample after 540 cycles of cyclic corrosion testing according to the examples and comparative examples. FIG. 8 is a diagram showing the effect of the magnesium concentration of the plating film 22 according to the examples and comparative examples on the standard deviation of crack width. The effects of the aluminum-zinc-silicon-magnesium-based plated steel sheet according to the present examples will be described below with reference to FIGS. 3 to 8.
[0092] 3 and 4, when the magnesium concentration in the plating film 22 is 0.3 mass% or more and 1.12 mass% or less, the corrosion loss amount at the time when the cyclic corrosion test has been repeated 60 cycles is significantly reduced. When the magnesium concentration is 0.7 mass% or more and less than 0.98 mass%, the corrosion loss amount at the time when the cyclic corrosion test has been repeated 60 cycles is significantly reduced compared to when the magnesium concentration is 0.55 mass% or 0.98 mass%.
[0093] Furthermore, as is clear from Figures 5 and 6, in Examples 4 and 5, the increase in white spots on the sample surface due to repeated cyclic corrosion tests was suppressed up to approximately 156 cycles. That is, when the magnesium concentration in the plating film 22 was 0.98% by mass or less, the increase in white spots on the sample surface was suppressed up to approximately 156 cycles of the cyclic corrosion test. The white spots on the sample surface are corrosion products of the plating layer. Therefore, this indicates that when the magnesium concentration in the plating film 22 is 0.98% by mass or less, deterioration of the appearance at the beginning of exposure to the natural environment is suppressed.
[0094] Next, as is clear from Figure 7, after 540 cycles of the cyclic corrosion test, only Example 4 (the magnesium concentration in the plated film 22 was 0.81 mass%) showed no corrosion of the substrate steel sheet 20. At this point, both Example 5 (the magnesium concentration in the plated film 22 was 0.98 mass%) and Comparative Example 5 (the magnesium concentration in the plated film 22 was 1.12 mass%) showed corrosion of the substrate steel sheet 20. From these facts, it is clear that when the magnesium concentration in the plated film 22 is less than 0.98 mass%, corrosion resistance is high in the case of long-term use.
[0095] 8, when the magnesium concentration of the plating film 22 is 0.7 mass % or more and 0.98 mass % or less, the standard deviation of the crack width is particularly small compared to when the magnesium concentration exceeds 0.98 mass %. When the magnesium concentration of the plating film 22 exceeds 0.98 mass %, the standard deviation of the crack width increases.
[0096] The small standard deviation of the crack widths described above means that in samples in which the magnesium concentration of the plating coating 22 was 0.7 mass % or more and 0.98 mass % or less, many cracks with relatively uniform widths occurred when the sample was bent. In a situation in which both large and small cracks occurred, there was a high risk that the substrate steel sheet 20 would be exposed in the former cracks. In a situation in which many cracks with relatively uniform widths occurred, there was a low risk that the substrate steel sheet 20 would be exposed in those many cracks. A lower risk of the substrate steel sheet 20 being exposed improves corrosion resistance. As a result, there was also a lower risk that corrosion resistance would be reduced when the sample was bent.
[0097] The embodiments disclosed herein are examples in all respects, and the scope of the present invention is not limited to the above-described embodiments, and various design changes may be made without departing from the spirit of the present invention.
[0098] REFERENCE SIGNS LIST 10...Aluminum-zinc-silicon-magnesium-based plated steel sheet 20...Base steel sheet 22...Plating film 40...Plating pot 42...Metal roll 44...Gas wiping nozzle 46...Forced air cooling equipment
Claims
1. An aluminum-zinc-silicon-magnesium-based plated steel sheet comprising a base steel sheet and a plating film, the plating film containing zinc, 50% by mass or more and 60% by mass or less of aluminum, 1.1% by mass or more and 2.0% by mass or less of silicon, and magnesium, wherein the sum of the mass percentages of the zinc, the mass percentages of the aluminum, the mass percentages of the silicon and the mass percentages of the magnesium is less than 100% by mass, and the mass percentage of the magnesium in the plating film is 0.7% by mass or more and 0.98% by mass or less.
2. The aluminum-zinc-silicon-magnesium plated steel sheet according to claim 1, characterized in that the mass percentage of magnesium in the plating film is 0.7 mass% or more and 0.81 mass% or less.
Citation Information
Patent Citations
Hot dipping aluminum silicon zinc yttrium magnesium plating solution and hot dipping technology thereof
CN107587096A
HOT DIP Al BASED PLATED STEEL SHEET HAVING EXCELLENT CORROSION RESISTANCE, AND PRODUCTION METHOD THEREFOR
JP2004244655A
Zn-Al ALLOY HOT-DIP PLATED STEEL SHEET SUPERIOR IN CORROSION RESISTANCE AND WORKABILITY, AND PRODUCTION METHOD THEREFOR
JP2007284718A
Coated plated steel material
WO2013027837A1
Surface-treated steel sheet
WO2018179397A1