Dry film, integrated sealing sheet, light emitting electronic component, and method for manufacturing light emitting electronic component
The use of a three-layer dry film in light-emitting electronic component manufacturing addresses the challenges of etching and brightness uniformity by pressure-bonding without etching, ensuring consistent brightness and reduced costs.
Patent Information
- Application Number
- PCT/JP2024/017580
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for manufacturing light-emitting electronic components using mini LEDs and micro LEDs face challenges such as time-consuming etching processes, potential brightness reduction, and uneven brightness due to differences in tilt and height of light emitting elements, as well as issues with residual black adhesive layers affecting brightness.
A dry film with a three-layer structure comprising a low-elasticity black curable resin layer, a low-elasticity transparent curable resin layer, and a high-elasticity transparent curable resin layer is used, which is pressure-bonded to the substrate without etching, ensuring uniform filling and removal of the black resin layer without affecting brightness, even with varying element heights and tilts.
This approach eliminates the need for time-consuming etching, maintains brightness and blackness, and prevents residual black adhesive layers, thereby reducing production costs and energy consumption while ensuring consistent performance.
Smart Images

Figure JP2024017580_28112024_PF_FP_ABST
Abstract
Description
Dry film, integrated encapsulating sheet, light-emitting electronic component, and method for manufacturing light-emitting electronic component
[0001] The present invention relates to a dry film, an integrated encapsulant sheet, a light-emitting electronic component, and a method for manufacturing a light-emitting electronic component. This application claims priority based on Japanese Patent Application No. 2023-085636 filed on May 24, 2023, the contents of which are incorporated herein by reference.
[0002] In recent years, display technologies known as mini-LEDs and micro-LEDs, which use extremely small light-emitting diodes, have been attracting attention. Mini-LEDs and micro-LEDs can be used in two ways. One is a technology that allows for localized control of backlight brightness by configuring an LCD backlight using a large number of LEDs arranged on a substrate. The other is a system in which the R (red), G (green), and B (blue) that make up a pixel are emitted by LEDs of each color, and the high-purity colors emitted by the LEDs of each color reach the eye as they are.
[0003] Mini-LEDs and micro-LEDs use electronic components in which multiple light-emitting elements are arranged on a substrate. Such electronic components use a dry film to fill the spaces between the multiple light-emitting elements with a resin that prevents light diffusion (see Patent Document 1). The dry film is a resin film obtained by applying a curable resin composition to a protective film and drying it. This dry film is then pressed onto the surface of the substrate where the light-emitting elements are arranged, filling the spaces between the light-emitting elements, and then cured.
[0004] In Patent Document 1, a light-diffusion preventing resin is used as a dry film to prevent light diffusion between a plurality of light-emitting elements. When a dry film made of a light-diffusion preventing resin is pressure-bonded to the surface of a substrate on which light-emitting elements are arranged, a light-diffusion preventing resin layer is inevitably formed not only between the light-emitting elements but also on the light-emitting elements.
[0005] If the light diffusion preventing resin layer formed on the light emitting element is left as it is, not only will light diffusion between the light emitting elements occur, but light that should be emitted toward the viewer will also be blocked. Regarding this problem, Patent Document 1 describes a method in which, after the dry film is pressed and bonded, the resin on the light emitting element is removed by etching such as plasma treatment, and the exposed light emitting element is covered with a light-transmitting sealant.
[0006] In Patent Document 2, a dry film having a two-layer structure is used, consisting of a black adhesive layer that is equal to or lower than the height of the light-emitting element, and a transparent adhesive layer that has a higher melting point than the black adhesive layer. With this method, the transparent adhesive layer is melted later to wash away the black adhesive layer on the light-emitting element, and the black adhesive layer is pressed against the bottom of the substrate between the light-emitting elements, so that no black adhesive layer remains on the light-emitting element.
[0007] Patent Publication No. 2022-22562 Chinese Patent Application Publication No. 115084320
[0008] However, when etching such as plasma treatment is performed as in Patent Document 1, it takes a long time, which is a factor in increasing manufacturing costs. Furthermore, it is difficult to completely remove the resin on the light-emitting element by etching, which may result in a partial decrease in brightness and unevenness. Furthermore, in order to provide a sealant layer on the outermost surface, it is also necessary to laminate an additional sealant dry film.
[0009] Patent Document 2 states that the black adhesive layer on the light-emitting elements can be washed away by a transparent adhesive layer and pressed against the bottom of the substrate between the light-emitting elements, preventing the black adhesive layer from remaining on the light-emitting elements. However, when the light-emitting elements are mounted with solder, differences arise between the light-emitting elements in terms of the inclination and height, so the transparent adhesive layer cannot wash away the black adhesive layer evenly, and the black adhesive layer remains on some of the light-emitting elements, reducing brightness.
[0010] The present invention provides a dry film that can omit a time-consuming etching process such as plasma treatment and can suppress a decrease in brightness even if the inclination or height of each light-emitting element varies from one light-emitting element to another. Furthermore, the present invention provides an integrated encapsulating sheet, a light-emitting electronic component, and a method for manufacturing a light-emitting electronic component using the dry film.
[0011] In order to achieve the above-mentioned object, the present invention employs the following configurations. [1] A dry film to be pressure-bonded to a surface of a device-mounted substrate on which a plurality of light-emitting elements are arranged, the dry film comprising a low-elasticity black cured resin layer, a low-elasticity transparent cured resin layer, and a high-elasticity transparent cured resin layer, which are laminated in this order from the side that is to be placed in direct contact with the device-mounted substrate during the pressure-bonding. [2] The dry film according to [1], in which the storage modulus of the high-elasticity transparent cured resin layer is greater than the storage modulus of the low-elasticity transparent cured resin layer and the low-elasticity black cured resin layer at 100°C. [3] The dry film according to [1] or [2], in which the storage modulus of the low-elasticity transparent cured resin layer is greater than the storage modulus of the low-elasticity black cured resin layer at 100°C. [4] The storage modulus of the high-elasticity transparent cured resin layer is 1.0 x 10 at 100°C. 7 [5] The dry film according to any one of [1] to [3], wherein the storage modulus of the low-elasticity black curable resin layer is 1.0 × 10 Pa or less at 100°C. 5 [6] The dry film according to any one of [1] to [4], wherein the storage modulus of the low-elasticity transparent curable resin layer is 1.0 × 10 Pa or less at 100°C. 5 [7] The dry film according to any one of [1] to [5], wherein the storage modulus of the highly elastic transparent curable resin layer is 1.0 × 10 Pa or less at 150°C. 5The dry film according to any one of [1] to [6], wherein the low-elasticity black curable resin layer has a total light transmittance of 0 to 30%. [8] The dry film according to any one of [1] to [7], wherein the low-elasticity black curable resin layer has a total light transmittance of 0 to 30%. [9] The dry film according to any one of [1] to [8], wherein the low-elasticity transparent curable resin layer has a total light transmittance of 50% or more.
[10] The dry film according to any one of [1] to [9], wherein the high-elasticity transparent curable resin layer has a total light transmittance of 50% or more.
[11] The dry film according to any one of [1] to
[10] , wherein the high-elasticity transparent curable resin layer comprises a high-molecular-weight epoxy resin.
[12] The dry film according to
[11] , wherein the high-molecular-weight epoxy resin has a weight-average molecular weight of 10,000 to 100,000.
[13] The dry film according to
[11] or
[12] , wherein the high-elasticity transparent curable resin layer comprises a phenoxy-type epoxy resin as the high-molecular-weight epoxy resin.
[14] The dry film according to any one of
[11] to
[13] , wherein the blending amount of the high-molecular-weight epoxy resin relative to 100% by mass of the total resin solids content of the high-elasticity, transparent curable resin layer is 30 to 80% by mass.
[15] The dry film according to any one of [1] to
[14] , wherein the low-elasticity, black curable resin layer contains an elastomer.
[16] The dry film according to
[15] , wherein the elastomer is a modified elastomer.
[17] The dry film according to
[16] , wherein the modified elastomer is acid-modified acrylonitrile butadiene rubber.
[18] The dry film according to any one of [1] to
[17] , wherein the low-elasticity, black curable resin layer contains carbon black.
[19] An integrated encapsulating sheet comprising the dry film according to any one of [1] to
[18] , and an encapsulating film layer provided on the opposite side of the high-elasticity, transparent curable resin layer from the low-elasticity, transparent curable resin layer.
[20] The integrated sealing sheet according to
[19] , wherein the sealing film layer comprises a support film layer and a hard coat layer provided on the opposite side of the support film layer from the highly elastic transparent curable resin layer.
[21] A light-emitting electronic component comprising: a substrate with a plurality of light-emitting elements arranged on a substrate; and the dry film according to any one of [1] to
[18] pressure-bonded to the surface of the substrate with the light-emitting elements on which the plurality of light-emitting elements are arranged, wherein the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and a portion of the high-elasticity transparent curable resin layer are filled between the plurality of light-emitting elements, and the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer are cured.
[22] A light-emitting electronic component comprising: a substrate with a plurality of light-emitting elements arranged on a substrate; and the integrated encapsulating sheet according to
[19] or
[20] pressure-bonded to the surface of the substrate with the light-emitting elements on which the plurality of light-emitting elements are arranged, wherein the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and a portion of the high-elasticity transparent curable resin layer are filled between the plurality of light-emitting elements, and the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer are cured.
[23] A method for producing a light-emitting electronic component, comprising: placing the dry film according to any one of [1] to
[18] on a surface of a device-mounted substrate, in which a plurality of light-emitting elements are arranged on a substrate, so that the low-elasticity black curable resin layer is in contact with the dry film; thermocompression bonding is performed; and curing the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer by heating.
[24] A method for producing a light-emitting electronic component according to
[23] , wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is performed by heating at 100 to 160°C.
[25] A method for producing a light-emitting electronic component, comprising placing the integrated encapsulating sheet according to
[19] or
[20] on a surface of a device-mounted substrate, in which a plurality of light-emitting elements are arranged on a substrate, so that the low-elasticity black curable resin layer is in contact with the dry film; thermocompression bonding is performed; and curing the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer by heating.
[26] The method for producing a light-emitting electronic component according to
[25] , wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is performed by heating at 100 to 160°C.
[0012] According to the dry film or the integrated encapsulating sheet of the present invention, even if the inclination or height of each light-emitting element differs, a decrease in brightness can be suppressed without performing etching such as a plasma treatment, which takes a lot of time. Furthermore, according to the light-emitting electronic component and the method for manufacturing a light-emitting electronic component of the present invention, a light-emitting electronic component having sufficient brightness and blackness can be obtained without increasing production costs or energy consumption.
[0013] FIG. 1 is a schematic cross-sectional view of a dry film according to a first embodiment of the present invention. FIG. 2 is a schematic explanatory view of a method for manufacturing a light-emitting electronic component according to the first embodiment of the present invention. FIG. 3 is a schematic explanatory view of a method for manufacturing a light-emitting electronic component according to the first embodiment of the present invention. FIG. 4 is a schematic explanatory view of a method for manufacturing a light-emitting electronic component according to the first embodiment of the present invention. FIG. 5 is a schematic explanatory view of a method for manufacturing a light-emitting electronic component according to the first embodiment of the present invention. FIG. 6 is a schematic cross-sectional view of an integrated encapsulating sheet according to a second embodiment of the present invention. FIG. 7 is a schematic explanatory view of a method for manufacturing a light-emitting electronic component according to the second embodiment of the present invention. FIG. 8 is a schematic explanatory view of a method for manufacturing a light-emitting electronic component according to the second embodiment of the present invention.
[0014] In this specification and claims, the term "main component" refers to a component that accounts for 50% by mass or more of the total solid content of the entire composition. A numerical range expressed by "to" refers to a numerical range in which the numerical values before and after "to" are the lower and upper limits.
[0015] First Embodiment Dry Film A dry film 100 according to a first embodiment will be described with reference to Figures 1 and 2. As shown in Figure 1, the dry film 100 is basically configured by laminating a low-elasticity black curable resin layer 1, a low-elasticity transparent curable resin layer 2, and a high-elasticity transparent curable resin layer 3. For ease of handling, the dry film 100 of this embodiment may further have a protective film on the surface of either or both of the low-elasticity black curable resin layer 1 and the high-elasticity transparent curable resin layer 3.
[0016] 1 shows an example in which protective films are provided on the surfaces of both the low-elasticity black curable resin layer 1 and the high-elasticity transparent curable resin layer 3. Specifically, the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, the high-elasticity transparent curable resin layer 3, and the second protective film 7 are sequentially laminated on the first protective film 6.
[0017] As shown in Fig. 2, the dry film 100 is used to fill the spaces between a plurality of light-emitting elements (light-emitting element 12, light-emitting element 13, light-emitting element 14) of a device-mounted substrate 10, which has a substrate 11 on which the light-emitting elements are arranged. Details of the device-mounted substrate 10 will be described later. The dry film 100 is used such that the low-elasticity black curable resin layer 1 is in direct contact with the device-mounted substrate 10 during pressure bonding, as shown in Fig. 2. A specific method for obtaining a light-emitting electronic component by pressure bonding the dry film 100 to the device-mounted substrate 10 will be described later.
[0018] <Low-elasticity black curable resin layer> The low-elasticity black curable resin layer 1 is a layer that prevents light diffusion between light-emitting elements and improves the contrast of the display. It also serves to sufficiently fill the spaces between the multiple light-emitting elements arranged on the element-mounted substrate 10 in the thermocompression bonding step, preventing poor appearance due to expansion of unfilled voids in the thermal curing step and damage to the light-emitting elements due to external factors in subsequent steps.
[0019] [Total Light Transmittance] The low-elasticity black curable resin layer 1 has a low total light transmittance. The total light transmittance of the low-elasticity black curable resin layer 1 is measured in a cured state. The low-elasticity black curable resin layer 1 is prepared so that the total light transmittance in the cured state is 0 to 30%. The low-elasticity black curable resin layer 1 is preferably prepared so that the total light transmittance in the cured state is 0 to 20%, and more preferably 0 to 10%. When the total light transmittance of the low-elasticity black curable resin layer 1 in a cured state is equal to or less than the upper limit, light diffusion between light-emitting elements can be prevented.
[0020] The total light transmittance in this specification can be measured using a haze meter. The total light transmittance in the cured state can be adjusted mainly by the presence or absence of a pigment or dye such as carbon black, or by the amount of the pigment or dye added. It can also be adjusted by the thickness of the resin layer or the type of resin.
[0021] [Storage Modulus] The low-elasticity black curable resin layer 1 is in an uncured or semi-cured state before being pressure-bonded to the element-mounted substrate 10 and cured. The storage modulus of the low-elasticity black curable resin layer 1 before curing is lower at 100°C than the storage modulus of the high-elasticity transparent curable resin layer 3 before curing. Furthermore, it is preferably lower at 100°C than the storage modulus of the low-elasticity transparent curable resin layer 2 before curing.
[0022] The storage modulus of the low-elasticity black curable resin layer 1 before curing was 1.0 × 10 at 100°C. 5 Pa or less, and 2 Pa or more, 1.0×10 5 Pa or less, and 3 Pa or more, 5.0×10 4 It is more preferable that the viscosity is 0.05 Pa or less.
[0023] When the storage modulus at 100°C of the low-elasticity black curable resin layer 1 before curing is equal to or less than the preferred upper limit, sufficient fluidity is obtained when the layer is pressure-bonded to the element-mounted substrate 10, and the layer can conform to the unevenness of the element-mounted substrate 10 due to the plurality of light-emitting elements and sufficiently fill the spaces between the plurality of light-emitting elements. When the storage modulus at 100°C of the low-elasticity black curable resin layer 1 before curing is equal to or greater than the preferred lower limit, uneven pressure during thermocompression bonding can be prevented, and a uniform appearance can be maintained. Furthermore, resin leakage outside the desired range can be prevented, and the film thickness after compression bonding can be ensured.
[0024] [Curable Resin Composition] The low-elasticity black curable resin layer 1 is composed of a curable resin composition. Examples of the curable resin composition include a thermosetting resin composition containing at least one resin selected from an epoxy resin, an acrylic resin, a polyester resin, and a polyurethane resin, and a curing agent.
[0025] An epoxy resin composition is preferred because it can be cured at low temperatures and has excellent heat resistance and reliability. In this specification, the epoxy resin composition refers to a composition containing an epoxy resin as a main component, or a composition containing an epoxy resin and a curing agent as main components.
[0026] (Epoxy Resin) In this specification and claims, an epoxy resin is a compound having an epoxy group in the molecule. The epoxy resin used in the present invention is preferably one having two or more epoxy groups in one molecule. This is because a crosslinked structure is formed by reaction with a modified resin having a functional group reactive with the epoxy group, and high heat resistance can be achieved in the cured product. Furthermore, when an epoxy resin having two or more epoxy groups is used, the degree of crosslinking with a curing agent having a functional group reactive with the epoxy group is sufficient, and sufficient heat resistance can be achieved in the cured product.
[0027] Examples of epoxy resins having two or more epoxy groups in one molecule include bifunctional epoxy resins having two epoxy groups in the molecule, polyfunctional epoxy resins having three or more epoxy groups in the molecule, and high-molecular-weight epoxy resins having a weight-average molecular weight of 10,000 or more. These may also be hydrogenated epoxy resins.
[0028] In this specification and claims, high molecular weight epoxy resins are not classified as bifunctional or polyfunctional epoxy resins, but as phenoxy-type epoxy resins, regardless of the number of epoxy groups in the molecule. The weight-average molecular weight of an epoxy resin is the molecular weight in terms of polystyrene measured by gel permeation chromatography.
[0029] Examples of epoxy resins include bisphenol-based epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, or phenoxy type epoxy resins obtained by polymerizing these resins, and hydrogenated versions of these resins; novolac type epoxy resins such as phenol novolac epoxy resins, o-cresol novolac epoxy resins, bisphenol A novolac epoxy resins, xylene structure-containing novolac epoxy resins, and naphthol novolac type epoxy resins; glycidyl ester-based epoxy resins such as phthalic acid diglycidyl ester, isophthalic acid diglycidyl ester, terephthalic acid diglycidyl ester, p-hydroxybenzoic acid glycidyl ester, tetrahydrophthalic acid diglycidyl ester, succinic acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and trimellitic acid triglycidyl ester; ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and the like. glycidyl ether-based epoxy resins such as butyl diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenylglycidyl ether ethane, triphenylglycidyl ether ethane, sorbitol polyglycidyl ether, and polyglycerol polyglycidyl ether; glycidylamine-based epoxy resins such as triglycidyl isocyanurate and tetraglycidyldiaminodiphenylmethane; linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil; and special skeleton epoxy resins such as brominated bisphenol A-type epoxy resins, phosphorus-containing epoxy resins, fluorine-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene-type epoxy resins, tertiary butylcatechol-type epoxy resins, triphenylmethane-type epoxy resins, tetraphenylethane-type epoxy resins, biphenyl-type epoxy resins, and bisphenol S-type epoxy resins, but are not limited to these.
[0030] Examples of high molecular weight epoxy resins that can be used include phenoxy-type epoxy resins, epoxy-modified polybutadiene, copolymers of glycidyl methacrylate and methyl methacrylate, modified polymers obtained by epoxy-modifying other resins, etc. These epoxy resins may be used alone or in combination of two or more.
[0031] Among the above epoxy resins, from the viewpoint of increasing the crosslink density after curing, polyfunctional epoxy resins are preferred as the epoxy resin used in the low-elasticity black curable resin layer 1. Among polyfunctional epoxy resins, novolac-type epoxy resins are particularly preferred because they are epoxy resins that can be appropriately introduced with a flexible skeleton and whose flexibility and softening point can be adjusted, making the cured product less susceptible to brittle fracture, improving the performance stability of the cured product of the epoxy resin composition over long-term use, increasing the crosslink density, and improving heat resistance.
[0032] Specific examples of novolac-type epoxy resins include "YX7700" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", "HP-7200H", and "HP-7200L" manufactured by DIC Corporation.
[0033] The amount of polyfunctional epoxy resin in the low-elasticity black curable resin layer 1 is preferably 10 to 99% by mass, more preferably 40 to 95% by mass, and even more preferably 60 to 90% by mass, relative to 100% by mass of the total resin solids content of the low-elasticity black curable resin layer 1. When the amount is equal to or greater than the lower limit, the crosslinking density can be increased, thereby imparting chemical resistance and heat resistance. When the amount is equal to or less than the upper limit, the storage modulus during thermocompression bonding can be adjusted, and the fluidity of the low-elasticity black curable resin layer 1 can be ensured.
[0034] The low-elasticity black curable resin layer 1 preferably does not contain a high-molecular-weight epoxy resin, or if it does contain one, it preferably contains a smaller amount of the high-elasticity transparent curable resin layer 3. This makes it easier to ensure sufficient fluidity during thermocompression bonding.
[0035] The blending amount of the high-molecular-weight epoxy resin in the low-elasticity black curable resin layer 1 is preferably less than 50% by mass, more preferably less than 30% by mass, and even more preferably less than 10% by mass, relative to 100% by mass of the total resin solid content of the low-elasticity black curable resin layer 1.
[0036] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the low-elasticity black curable resin layer 1 preferably contains an epoxy resin having a softening point or melting point of 100° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the low-elasticity black curable resin layer 1 contains an epoxy resin having a softening point or melting point of 50 to 95° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.
[0037] The total amount of epoxy resin in the low-elasticity black curable resin layer 1 is preferably 10 to 100% by mass, more preferably 20 to 99% by mass, and even more preferably 35 to 95% by mass, relative to 100% by mass of the total resin solids content of the low-elasticity black curable resin layer 1. Within this range, the storage modulus can be controlled and appropriate fluidity during thermocompression bonding can be ensured. Furthermore, if the amount is equal to or greater than the lower limit, heat resistance after curing can be improved.
[0038] (Elastomer) The low-elasticity black curable resin layer 1 preferably contains an elastomer in addition to a resin such as an epoxy resin. By containing an elastomer, it becomes easier to control the storage modulus, i.e., the fluidity.
[0039] As the elastomer, a thermosetting elastomer, commonly called "rubber," is preferred because it provides excellent heat resistance. Examples of thermosetting elastomers include acrylonitrile butadiene rubber (NBR), which is a random copolymer of butadiene and acrylonitrile, acrylic rubber, styrene butadiene rubber, vinyl acetate resin, and silicone resin. Among these, NBR is preferred because it has good compatibility with epoxy resins, allows control of the fluidity of the low-elasticity black curable resin layer 1 at around 100°C, and provides good adhesion to the low-elasticity transparent curable resin layer 2 and the element-mounted substrate 10.
[0040] The weight-average molecular weight of the elastomer is preferably 100,000 to 1,000,000, more preferably 120,000 to 500,000, and even more preferably 150,000 to 300,000. When the weight-average molecular weight of the elastomer is within the above range, the storage modulus of the low-elasticity black curable resin layer 1 can be controlled, and fluidity during thermocompression bonding can be ensured. When the weight-average molecular weight of the elastomer is equal to or less than the above upper limit, compatibility with the epoxy resin is improved, and fluidity during thermal curing can be more effectively controlled.
[0041] In particular, when the low-elasticity black curable resin layer 1 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group reactive with an epoxy group. A modified elastomer having a functional group reactive with an epoxy group also functions as a curing agent for the epoxy resin. Furthermore, since it can react and bond with the epoxy resin, it improves heat resistance and reliability against thermal shock. Furthermore, the difference in polarity between the functional group reactive with the epoxy resin and the resin skeleton favorably affects dispersibility, resulting in good dispersibility when carbon black is incorporated into the low-elasticity black curable resin layer 1.
[0042] Examples of functional groups capable of reacting with an epoxy group include acid groups such as a carboxy group, a sulfo group, a nitro group, and a phosphate group, as well as acid anhydride groups thereof, a hydroxyl group, and an amino group. Among these, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long usable time.
[0043] That is, when the low-elasticity black curable resin layer 1 is composed of an epoxy resin composition, it preferably contains an acid-modified elastomer having an acid group or an acid anhydride group, more preferably an acid-modified elastomer having a carboxy group, and particularly preferably an acid-modified acrylonitrile butadiene rubber (acid-modified NBR) having a carboxy group.
[0044] The acid-modified NBR having a carboxy group is preferably a carboxylated acrylonitrile rubber into which acrylic acid, methacrylic acid, maleic anhydride, etc. have been introduced. Commercially available carboxylated acrylonitrile rubbers include Nipol (registered trademark) NX775 and Nipol 1072CGJ manufactured by Nippon Zeon Co., Ltd. Two or more modified elastomers having a functional group reactive with an epoxy group may be used in combination.
[0045] The amount of elastomer blended in the low-elasticity black curable resin layer 1 is preferably greater than the amount of elastomer blended in the high-elasticity transparent curable resin layer 3. This allows the storage modulus of the low-elasticity black curable resin layer 1 during thermocompression bonding to be adjusted to an appropriate range lower than that of the high-elasticity transparent curable resin layer 3, and also allows flow during thermal curing to be suppressed, when the low-elasticity black curable resin layer 1 contains a large amount of low-molecular-weight components such as polyfunctional epoxy. As a result, the low-elasticity black curable resin layer 1 can have sufficient fluidity during thermocompression bonding and can be prevented from flowing out during thermal curing.
[0046] The amount of elastomer in the low-elasticity black curable resin layer 1 is preferably 0.01 to 90% by mass, more preferably 1 to 80% by mass, and even more preferably 5 to 65% by mass, relative to 100% by mass of the total resin solids content of the low-elasticity black curable resin layer 1. Within this range, the storage modulus can be controlled, and appropriate fluidity during thermocompression bonding can be ensured. Furthermore, when the amount is equal to or greater than the lower limit, the dispersibility of carbon black is improved. Furthermore, film-forming properties are improved, and the film thickness distribution can be narrowed when the epoxy resin composition is applied to form a film.
[0047] (Curing Agent) When the low-elasticity black curable resin layer 1 is composed of an epoxy resin composition, it may contain a curing agent for epoxy resins other than the modified elastomer having a functional group reactive with an epoxy group. Examples of the other curing agent include known curing agents such as phenol-based curing agents, acid anhydride-based curing agents, and amine-based curing agents. Two or more of the other curing agents may be used in combination.
[0048] (Curing Catalyst) When the low-elasticity black curable resin layer 1 is composed of an epoxy resin composition, it may contain a curing catalyst that promotes the curing reaction of the epoxy resin. Examples of curing catalysts include imidazole-based, tertiary amine-based, and phosphorus compound-based curing catalysts. Among these, imidazole-based catalysts are preferred because they are compatible with epoxy resins and are less likely to cause yellowing. Among imidazole-based curing catalysts, those containing a cyanoethyl group are particularly preferred because they are easily soluble in epoxy resins.
[0049] The amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solids content of the low-elasticity black curable resin layer 1. Within the above range, curing can be sufficiently promoted, ensuring the usable life of the dry film 100. Two or more types of curing catalysts may be used in combination.
[0050] (Black pigment or black dye) The low-elasticity black curable resin layer 1 is colored black. For coloring, it preferably contains a black pigment or a black dye, more preferably contains a black pigment, and even more preferably contains carbon black. By being colored black, it is possible to prevent light diffusion between the multiple light-emitting elements of the element-mounted substrate 10.
[0051] The particle size of the carbon black is preferably 10 to 500 nm, more preferably 10 to 300 nm, and particularly preferably 10 to 100 nm. The particle size refers to the average particle size and can be determined using a measuring device based on dynamic light scattering. An example of a measuring device based on dynamic light scattering is the NanotracWave II UT151 manufactured by Microtrac Bell.
[0052] The pH of the carbon black according to ISO 787-9 is preferably 5 or less, more preferably 1 to 4.5, and even more preferably 2 to 4. When the pH of the carbon black is equal to or less than the preferred upper limit, good dispersibility can be obtained, and the blackness can be improved. When the pH of the carbon black is equal to or more than the preferred lower limit, the dispersion stability in the coating liquid for the low-elasticity black curable resin layer is improved, and the stability of sedimentation and blackness is increased.
[0053] As the carbon black, one or more types of known carbon black such as gas black, channel black, furnace black, thermal black, and lamp black can be used. Resin-coated carbon black may also be used. Furthermore, carbon nanofibers and carbon nanotubes may also be used.
[0054] Gas black, which is an acidic carbon, is preferred because it has a large amount of surface functional groups, is highly dispersible, and exhibits sufficient light diffusion preventing properties even when added in small amounts. Furthermore, when the low-elasticity black curable resin layer 1 contains a modified elastomer having functional groups reactive with epoxy resins, the dispersibility is further improved due to the interaction between the surface functional groups of the gas black and the functional groups of the modified elastomer having functional groups reactive with epoxy resins, thereby ensuring good light diffusion preventing properties and coating liquid stability.
[0055] The amount of carbon black is preferably 0.1 to 15 mass %, and more preferably 1.0 to 10 mass %, based on the total solid content of the low-elasticity black curable resin layer 1. When the amount of carbon black is equal to or greater than the above-mentioned lower limit, sufficient light-blocking properties are obtained. When the amount of carbon black is greater than the above-mentioned upper limit, the thixotropy of the low-elasticity black curable resin layer 1 increases, the fluidity during thermocompression bonding decreases, and the layer cannot be sufficiently filled between the multiple light-emitting elements of the element-mounted substrate 10.
[0056] (Other Components) The low-elasticity black curable resin layer 1 may contain an inorganic filler to improve flame retardancy and heat resistance and to adjust the refractive index. The low-elasticity black curable resin layer 1 may further contain, as necessary, a resin other than the epoxy resin and the elastomer, a thickener, a defoaming agent and / or a leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.
[0057] <Transparent Curable Resin Layer> The dry film 100 of this embodiment includes two transparent curable resin layers: a low-elasticity transparent curable resin layer 2 and a high-elasticity transparent curable resin layer 3. These two layers have high total light transmittance. The total light transmittance of each of the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3 is measured in a cured state.
[0058] <Low-elasticity transparent curable resin layer 2> The low-elasticity transparent curable resin layer 2 is a layer that is filled at least partially between the plurality of light-emitting elements while the low-elasticity black curable resin layer 1 is pressed between the plurality of light-emitting elements arranged on the element-mounted substrate 10 during the thermocompression bonding process.
[0059] [Total Light Transmittance] The low-elasticity, transparent, curable resin layer 2 is preferably prepared so that the total light transmittance in the cured state is 50% or more, more preferably 50 to 95%, and even more preferably 80 to 90%. When the total light transmittance in the cured state of the low-elasticity, transparent, curable resin layer 2 is equal to or greater than the lower limit, even if the low-elasticity, transparent, curable resin layer 2 in the cured state remains on the light-emitting element, light is not prevented from reaching the viewer.
[0060] [Storage Modulus] The low-elasticity, transparent, curable resin layer 2 is in an uncured or semi-cured state before being pressure-bonded to the element-mounted substrate 10 and cured. The storage modulus of the low-elasticity, transparent, curable resin layer 2 before curing at 100°C is smaller than that of the high-elasticity, transparent, curable resin layer 3 before curing. Furthermore, the storage modulus at 100°C is preferably equal to or larger than that of the low-elasticity, black curable resin layer 1 before curing.
[0061] The storage modulus of the low-elasticity transparent curable resin layer 2 before curing is 1.0×10 5Pa or less, and 3 ~1.0 x 10 5 Pa, and preferably 5.0 × 10 3 ~1.0 x 10 5 Pa is more preferable.
[0062] When the storage modulus at 100°C of the low-elasticity transparent curable resin layer 2 before curing is equal to or less than the preferred upper limit, sufficient fluidity is obtained when the layer is pressed against the element-mounted substrate 10, and the layer can conform to the unevenness of the element-mounted substrate 10 caused by the plurality of light-emitting elements and sufficiently fill the spaces between the plurality of light-emitting elements together with the low-elasticity black curable resin layer 1.
[0063] If the storage modulus of the low-elasticity, transparent curable resin layer 2 at 100°C before curing exceeds the preferred upper limit, the fluidity of the low-elasticity, transparent curable resin layer 2 will be insufficient, making it difficult to sufficiently fill the spaces between the plurality of light-emitting elements. Furthermore, it will be difficult to sufficiently press the low-elasticity, black curable resin layer 1 into the spaces between the plurality of light-emitting elements. The storage modulus of the low-elasticity, transparent curable resin layer 2 at 100°C before curing is preferably 0.8 to 1000 times, and more preferably 1 to 100 times, the storage modulus of the low-elasticity, black curable resin layer 1 before curing.
[0064] [Curable Resin Composition] The low-elasticity transparent curable resin layer 2 is composed of a curable resin composition. As with the low-elasticity black curable resin layer 1, the curable resin composition may be a thermosetting resin composition containing at least one resin selected from epoxy resins, acrylic resins, polyester resins, and polyurethane resins, and a curing agent. Among these, an epoxy resin composition is preferred because it can be cured at low temperatures and has excellent heat resistance and reliability.
[0065] (Epoxy Resin) Examples of epoxy resins used in the low-elasticity, transparent curable resin layer 2 include the same types as those used in the low-elasticity, black curable resin layer 1. Among the above-mentioned epoxy resins, the epoxy resin used in the low-elasticity, transparent curable resin layer 2 is preferably a multifunctional epoxy resin, since it can increase the crosslink density after curing and has an appropriate molecular weight, making it easy to adjust the elastic modulus.
[0066] When the low-elasticity, transparent curable resin layer 2 contains a high-molecular-weight epoxy resin, the blending amount thereof is preferably 50% by mass or less, more preferably 35% by mass or less, and even more preferably 10 to 35% by mass, relative to 100% by mass of the total resin solids content of the low-elasticity, transparent curable resin layer 2. When the blending amount of the high-molecular-weight epoxy resin in the low-elasticity, transparent curable resin layer 2 is equal to or greater than the above-mentioned preferable lower limit, a storage modulus that sufficiently presses the low-elasticity, black curable resin layer 1 into spaces between multiple light-emitting elements is easily obtained. When the blending amount is equal to or less than the preferable upper limit, the low-elasticity, transparent curable resin layer 2 easily fills spaces between multiple light-emitting elements.
[0067] The total amount of epoxy resin in the low-elasticity, transparent, curable resin layer 2 is preferably 10 to 100% by mass, more preferably 20 to 99% by mass, and even more preferably 35 to 95% by mass, relative to 100% by mass of the total resin solids content of the low-elasticity, transparent, curable resin layer 2. When the total amount of epoxy resin in the low-elasticity, transparent, curable resin layer 2 is within the above range, it is possible to control the storage modulus and ensure appropriate fluidity during thermocompression bonding. Furthermore, when the amount is equal to or greater than the above lower limit, it is possible to improve heat resistance after curing.
[0068] (Elastomer) The low-elasticity transparent curable resin layer 2 preferably contains an elastomer in addition to a resin such as an epoxy resin, etc. By containing an elastomer, it becomes easier to control the storage modulus.
[0069] Examples of the elastomer include the same types as those for the low-elasticity black curable resin layer 1. Among them, NBR is preferred because it has good compatibility with epoxy resins, can increase the storage modulus of the low-elasticity transparent curable resin layer 2 at around 150°C, and has good adhesion to the low-elasticity black curable resin layer 1. The preferred weight-average molecular weight of the elastomer is also the same as that for the low-elasticity black curable resin layer 1.
[0070] In particular, when the low-elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. A modified elastomer having a functional group capable of reacting with an epoxy group also functions as a curing agent for the epoxy resin. Furthermore, since it can react with and bond to the epoxy resin, it improves heat resistance and reliability against thermal shock.
[0071] Examples of functional groups capable of reacting with an epoxy group include the same types as those in the low-elasticity black curable resin layer 1. Among these, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, because they can be cured at low temperatures and ensure a long usable time.
[0072] When the low-elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it particularly preferably contains an acid-modified NBR having a carboxy group. Examples of the acid-modified NBR having a carboxy group include the same types as those used for the low-elasticity black curable resin layer 1. Two or more types of modified elastomers having a functional group reactive with an epoxy group may be used in combination.
[0073] The amount of elastomer in the low-elasticity, transparent, curable resin layer 2 is preferably 90% by mass or less, more preferably 1 to 80% by mass, and even more preferably 5 to 65% by mass, relative to 100% by mass of the total resin solids content of the low-elasticity, transparent, curable resin layer 2. When the amount of elastomer in the low-elasticity, transparent, curable resin layer 2 is equal to or greater than the above-mentioned preferable lower limit, film-formability is improved and the film thickness distribution during film formation can be narrowed. When the amount is equal to or less than the preferable upper limit, the low-elasticity, transparent, curable resin layer 2 is likely to fill between multiple light-emitting elements.
[0074] (Curing Agent) When the low-elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it may contain a curing agent for epoxy resins other than the modified elastomer having a functional group reactive with an epoxy group. Examples of the other curing agent include the same curing agents as those used in the low-elasticity black curable resin layer 1. Two or more types of the other curing agents may be used in combination.
[0075] (Curing Catalyst) When the low-elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it may contain a curing catalyst that promotes the curing reaction of the epoxy resin. Examples of the curing catalyst include the same curing catalysts as those used for the low-elasticity black curable resin layer 1, and preferred embodiments are also the same.
[0076] The amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solids content of the low-elasticity transparent curable resin layer 2. Within the above range, curing can be sufficiently promoted, ensuring the usable life of the dry film 100. Two or more types of curing catalysts may be used in combination.
[0077] (Other Components) The low-elasticity transparent curable resin layer 2 may contain a black pigment or black dye in order to suppress uneven light emission and uneven color.
[0078] From the viewpoint of increasing the total light transmittance, when the low-elasticity, transparent, curable resin layer 2 contains carbon black, the blending amount thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less, relative to 100 parts by mass of the total resin solid content. The low-elasticity, transparent, curable resin layer 2 may further contain, as necessary, a resin other than the epoxy resin and the elastomer, a thickener, a defoaming agent and / or a leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.
[0079] <High-elasticity, transparent curable resin layer 3> The high-elasticity, transparent curable resin layer 3 is a layer used in the thermocompression bonding step to sufficiently press the low-elasticity, black curable resin layer 1 and the low-elasticity, transparent curable resin layer 2 between the plurality of light-emitting elements arranged on the element-mounted substrate 10, and remove the low-elasticity, black curable resin layer 1 from above the light-emitting elements.
[0080] [Total Light Transmittance] The highly elastic, transparent, curable resin layer 3 is preferably prepared so that the total light transmittance in the cured state is 50% or more, more preferably 75 to 99.5%, and even more preferably 80 to 99.5%. When the highly elastic, transparent, curable resin layer 3 has a total light transmittance in the cured state that is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side.
[0081] [Storage Elastic Modulus] The high-elasticity, transparent curable resin layer 3 is in an uncured or semi-cured state before being pressed onto the element-mounted substrate 10 and cured. The storage elastic modulus of the high-elasticity, transparent curable resin layer 3 before being cured is greater at 100°C than the storage elastic modulus of the low-elasticity, black curable resin layer 1 before being cured and the low-elasticity, transparent curable resin layer 2 before being cured. The storage elastic modulus of the high-elasticity, transparent curable resin layer 3 before being cured is preferably greater than the storage elastic modulus of the low-elasticity, black curable resin layer 1 before being cured and the low-elasticity, transparent curable resin layer 2 before being cured at 100°C to 150°C.
[0082] In addition, when the storage modulus of the high-elasticity, transparent curable resin layer 3 before curing is greater than the storage modulus of the low-elasticity, black curable resin layer 1 before curing and the low-elasticity, transparent curable resin layer 2 before curing at 100°C and 150°C, the storage modulus of the high-elasticity, transparent curable resin layer 3 before curing is usually greater than the storage modulus of the low-elasticity, black curable resin layer 1 before curing and the low-elasticity, transparent curable resin layer 2 before curing over the entire range of 100°C to 150°C.
[0083] The storage modulus of the highly elastic transparent curable resin layer 3 before curing is 1.0×10 at 100° C. 7 Pa or less, and 4 Pa or more, 1.0×10 7 Pa or less, and 4 Pa or more, 5.0×10 6 It is more preferable that the viscosity is 0.05 Pa or less.
[0084] Since the storage modulus at 100°C of the high-elasticity transparent curable resin layer 3 before curing is within a preferred range, stress is transmitted to the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2 when the layer is pressed against the element-mounted substrate 10, and both the elasticity required to sufficiently remove the low-elasticity black curable resin layer 1 from above the light-emitting elements and the flexibility required to deform in accordance with the unevenness of the multiple light-emitting elements can be achieved, making it easier to sufficiently fill the spaces between the multiple light-emitting elements with the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2.
[0085] If the storage modulus at 100°C of the high-elasticity, transparent, curable resin layer 3 before curing exceeds a preferred upper limit, the high-elasticity, transparent, curable resin layer 3 will have insufficient fluidity and will be less able to deform to conform to the irregularities of the multiple light-emitting elements. This will prevent the low-elasticity, black curable resin layer 1 from being sufficiently removed from only the upper portions of the low-height light-emitting elements, resulting in reduced brightness. Furthermore, it will be difficult to sufficiently press the low-elasticity, black curable resin layer 1 between the multiple light-emitting elements, making it more likely that defects such as air bubbles will occur due to the remaining voids. Furthermore, cracks will occur in the high-elasticity, transparent, curable resin layer 3 during thermocompression bonding, making it more likely that crack-like defects will occur.
[0086] If the storage modulus at 100°C of the high-elasticity, transparent curable resin layer 3 before curing is below the preferred lower limit, it becomes difficult to sufficiently remove the low-elasticity, black curable resin layer 1 from the light-emitting element. Also, the fluidity of the high-elasticity, transparent curable resin layer 3 is too high, which causes the surface of the high-elasticity, transparent curable resin layer 3 to become uneven to fit the light-emitting element after thermocompression bonding, which is likely to result in poor appearance.
[0087] The storage modulus of the highly elastic transparent curable resin layer 3 before curing is 1.0×10 at 150° C. 4 Pa or more, and 4 ~5.0 x 10 7 Pa, and preferably 1.0×10 5 ~1.0 x 10 7 Pa is more preferable.
[0088] If the storage modulus at 150°C of the highly elastic, transparent, curable resin layer 3 before curing exceeds the preferred upper limit, cracks are likely to occur due to cure shrinkage during thermal curing. If the storage modulus at 150°C of the highly elastic, transparent, curable resin layer 3 before curing is equal to or greater than the preferred lower limit, flow during thermal curing can be suppressed, post-curing appearance defects such as repelling can be suppressed, and further, problems are less likely to occur when etching is performed in a subsequent process.
[0089] The storage modulus of the high-elasticity transparent curable resin layer 3 at 100°C before curing is preferably 10 to 1,000 times, and more preferably 30 to 500 times, the storage modulus of each of the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2 before curing. The storage modulus of the high-elasticity transparent curable resin layer 3 at 150°C before curing is preferably 5 to 10,000 times, and more preferably 10 to 1,000 times, the storage modulus of each of the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2.
[0090] [Curable Resin Composition] The high-elasticity transparent curable resin layer 3 is composed of a curable resin composition. As with the low-elasticity black curable resin layer 1, the curable resin composition may be a thermosetting resin composition containing at least one resin selected from an epoxy resin, an acrylic resin, a polyester resin, and a polyurethane resin, and a curing agent. Among these, an epoxy resin composition is preferred because it can be cured at low temperatures and has excellent heat resistance and reliability.
[0091] (Epoxy Resin) Examples of epoxy resins used in the high-elasticity transparent curable resin layer 3 include the same types as those used in the low-elasticity black curable resin layer 1 .
[0092] The highly elastic, transparent, curable resin layer 3 preferably contains a high-molecular-weight epoxy resin having a weight-average molecular weight of 10,000 to 100,000 from the viewpoint of being able to impart an appropriate viscosity during compression bonding to the highly elastic, transparent, curable resin layer 3. It is more preferable that the highly elastic, transparent, curable resin layer 3 contains a high-molecular-weight epoxy resin having a weight-average molecular weight of 10,000 to 35,000 from the viewpoint of having good compatibility with other resin components and being able to dissolve without mixing with a high-boiling-point solvent that may remain in the dry film even after drying.
[0093] By including a high-molecular-weight epoxy resin having a weight-average molecular weight of 10,000 to 100,000 as the epoxy resin used in the highly elastic, transparent, curable resin layer 3, the layer has an appropriate viscosity when heated, and therefore the storage modulus of the highly elastic, transparent, curable resin layer 3 can be adjusted to a preferred range within a temperature range of 100°C to 150°C. The high-molecular-weight epoxy resin used in the highly elastic, transparent, curable resin layer 3 is preferably a phenoxy-type epoxy resin because of its good compatibility with other epoxy resins.
[0094] Phenoxy-type epoxy resins have a relatively large molecular weight among epoxy resins and have an appropriate viscosity when heated, making it possible to adjust the storage modulus of the highly elastic, transparent, curable resin layer 3 to a preferred range within the range of 100°C to 150°C. Furthermore, unlike other thermoplastic resins such as polyester, phenoxy-type epoxy resins can be cured as epoxy resins, which allows for an increase in crosslink density and does not impair the heat resistance of the cured product or the reliability of its performance over long-term use.
[0095] From the viewpoint of ensuring a storage modulus sufficient to compress the low-elasticity black curable resin layer 1 during thermocompression bonding, the glass transition temperature of the phenoxy-type epoxy resin used in the high-elasticity transparent curable resin layer 3 is preferably 100°C or higher.
[0096] Specific examples of phenoxy-type epoxy resins include "1256," "YX7200," "YX8100," and "YX7180" manufactured by Mitsubishi Chemical Corporation, "YP-50," "YP-50S," and "YP-70" manufactured by Nippon Steel Chemical & Material Co., Ltd., "N-690" manufactured by DIC Corporation, and "H-157" and "EXA-192" manufactured by DIC Corporation.
[0097] The blending amount of the high-molecular-weight epoxy resin in the highly elastic, transparent, curable resin layer 3 is preferably 30 to 80% by mass, more preferably 40 to 75% by mass, and even more preferably 45 to 70% by mass, relative to 100% by mass of the total resin solid content of the highly elastic, transparent, curable resin layer 3. The same applies to the preferred blending amount of the phenoxy-type epoxy resin in the highly elastic, transparent, curable resin layer 3.
[0098] Within the above range, the storage modulus can be controlled, and the storage modulus for pressing the low-elasticity black curable resin layer 1 and the high-elasticity transparent curable resin layer 3 into each other during thermocompression bonding can be ensured, allowing the low-elasticity black curable resin layer 1 to be sufficiently removed from above the light-emitting element. Furthermore, flow during thermal curing can be suppressed, preventing poor appearance after curing, such as repelling, and further reducing problems when performing etching in a subsequent process. Furthermore, toughness is improved, making it less likely for crack-like defects to occur during thermocompression bonding. Furthermore, when the content is equal to or less than the above upper limit, the crosslink density of the high-elasticity transparent curable resin layer 3 in the cured state can be increased, improving heat resistance and chemical resistance.
[0099] Furthermore, it is preferable that the epoxy resin used in the highly elastic, transparent, curable resin layer 3 contains a polyfunctional epoxy resin. The polyfunctional epoxy resin increases the crosslink density, thereby further improving the stability of the performance of the cured product of the epoxy resin composition over long-term use and heat resistance. In addition, since the viscosity in the range of 100°C to 150°C is lower than that of phenoxy-type epoxy resins, the storage modulus of the highly elastic, transparent, curable resin layer 3 can be adjusted by combining it with a phenoxy-type epoxy resin.
[0100] Specific examples of polyfunctional epoxy resins include "YX7700", "157S70", and "1032S60" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", and "HP-7200H" manufactured by DIC Corporation.
[0101] The blending amount of the polyfunctional epoxy resin in the highly elastic, transparent, curable resin layer 3 is preferably 90% by mass or less, more preferably 10 to 80% by mass, and even more preferably 20 to 70% by mass, relative to 100% by mass of the total resin solids content of the highly elastic, transparent, curable resin layer 3. Within the above range, the storage modulus of the highly elastic, transparent, curable resin layer 3 during thermocompression bonding can be controlled, and heat resistance and chemical resistance can be imparted in the cured state.
[0102] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the highly elastic, transparent, curable resin layer 3 preferably contains an epoxy resin having a softening point or melting point of 120° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the highly elastic, transparent, curable resin layer 3 contains an epoxy resin having a softening point or melting point of 50 to 105° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.
[0103] The total amount of epoxy resin in the high-elasticity, transparent, curable resin layer 3 is preferably 10 to 100% by mass, more preferably 30 to 99% by mass, and even more preferably 50 to 95% by mass, relative to 100% by mass of the total resin solids content of the high-elasticity, transparent, curable resin layer 3. Within this range, the storage modulus can be controlled, ensuring a storage modulus sufficient to compress the low-elasticity, black curable resin layer 1 during thermocompression bonding. Furthermore, flow during thermal curing can be suppressed, preventing post-curing appearance defects such as repelling, and further reducing the risk of problems during subsequent etching processes. Furthermore, when the amount is equal to or greater than the lower limit, heat resistance in the cured state is improved.
[0104] (Elastomer) The highly elastic, transparent, curable resin layer 3 preferably contains an elastomer in addition to a resin such as an epoxy resin, etc. By containing an elastomer, it becomes easier to control the storage modulus.
[0105] Examples of the elastomer include the same types as those for the low-elasticity black curable resin layer 1. Among them, NBR is preferred because it has good compatibility with epoxy resins, can increase the storage modulus of the high-elasticity transparent curable resin layer 3 at around 150°C, and has good adhesion to the low-elasticity transparent curable resin layer 2. The preferred weight-average molecular weight of the elastomer is also the same as that for the low-elasticity black curable resin layer 1.
[0106] In particular, when the highly elastic, transparent, curable resin layer 3 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group reactive with an epoxy group. A modified elastomer having a functional group reactive with an epoxy group also functions as a curing agent for the epoxy resin. Furthermore, because it can react and bond with the epoxy resin, it improves heat resistance and reliability against thermal shock. Furthermore, the difference in polarity between the functional group reactive with the epoxy resin and the resin skeleton favorably affects dispersibility, resulting in good dispersibility when carbon black is incorporated into the highly elastic, transparent, curable resin layer 3.
[0107] Examples of functional groups capable of reacting with an epoxy group include the same types as those in the low-elasticity black curable resin layer 1. Among these, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, because they can be cured at low temperatures and ensure a long usable time.
[0108] When the high-elasticity transparent curable resin layer 3 is composed of an epoxy resin composition, it particularly preferably contains an acid-modified NBR having a carboxy group. Examples of the acid-modified NBR having a carboxy group include the same types as those used for the low-elasticity black curable resin layer 1. Two or more types of modified elastomers having a functional group reactive with an epoxy group may be used in combination.
[0109] The amount of elastomer in the high-elasticity, transparent, curable resin layer 3 is preferably 0 to 50% by mass, more preferably 1 to 70% by mass, and even more preferably 5 to 50% by mass, relative to 100% by mass of the total resin solids content of the high-elasticity, transparent, curable resin layer 3. Within this range, the storage modulus can be controlled. Furthermore, when the amount is equal to or less than the upper limit, a storage modulus sufficient to compress the low-elasticity, black curable resin layer during thermocompression bonding can be ensured. Furthermore, flow during thermal curing can be suppressed, preventing post-curing appearance defects such as cissing, and further, preventing problems during subsequent etching processes. Furthermore, when the amount is equal to or greater than the lower limit, the dispersibility of carbon black is improved. Furthermore, film-formability is improved, allowing for a narrower film thickness distribution when the epoxy resin composition is applied to form a film.
[0110] (Curing Agent) When the high-elasticity transparent curable resin layer 3 is composed of an epoxy resin composition, it may contain a curing agent for epoxy resins other than the modified elastomer having a functional group reactive with an epoxy group. Examples of the other curing agent include the same curing agents as those used in the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2. Two or more types of the other curing agents may be used in combination.
[0111] (Curing Catalyst) When the high-elasticity, transparent curable resin layer 3 is composed of an epoxy resin composition, it may contain a curing catalyst that promotes the curing reaction of the epoxy resin. Examples of the curing catalyst include the same curing catalysts as those used in the low-elasticity, black curable resin layer 1 and the low-elasticity, transparent curable resin layer 2, and preferred embodiments are also the same.
[0112] The amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solids content of the highly elastic, transparent, curable resin layer 3. Within the above range, curing can be sufficiently promoted, ensuring the usable life of the dry film 100. Two or more types of curing catalysts may be used in combination.
[0113] (Other Components) The highly elastic, transparent, curable resin layer 3 may contain a black pigment or black dye to suppress uneven light emission and color. From the viewpoint of increasing the total light transmittance, when the highly elastic, transparent, curable resin layer 3 contains carbon black, the blending amount thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less, relative to 100 parts by mass of the total resin solids. The highly elastic, transparent, curable resin layer 3 may further contain, as necessary, a resin other than the epoxy resin and elastomer, a thickener, a defoamer and / or leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.
[0114] <Protective Film> The first protective film 6 and the second protective film 7 (hereinafter, the first protective film 6 and the second protective film 7 may be collectively referred to simply as "protective films") have the role of protecting the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3, and can also be used as films onto which a coating liquid of a curable resin composition is applied when these curable resin layers are formed.
[0115] Examples of the protective film that can be used include polyester films such as polyethylene terephthalate and polyethylene naphthalate, films made of thermoplastic resins such as polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, and polystyrene films, and surface-treated paper.
[0116] Among these, polyester films are preferably used from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. The thickness of the protective film is not particularly limited, but is selected appropriately depending on the application within the range of approximately 10 to 150 μm. The surface of the protective film on which the resin layer is to be provided may be subjected to a release treatment.
[0117] <Method for manufacturing dry film> To obtain the dry film 100, first, a second protective film 7 is coated with a coating liquid of a curable resin composition for the high-elasticity, transparent curable resin layer 3 and dried, and a release film is coated with a coating liquid of a curable resin composition for the low-elasticity, transparent curable resin layer 2 and dried. These films are overlaid and laminated so that the high-elasticity, transparent curable resin layer 3 and the low-elasticity, transparent curable resin layer 2 are in contact, and the release film is peeled off, thereby obtaining a laminate in which the low-elasticity, transparent curable resin layer 2, the high-elasticity, transparent curable resin layer 3, and the second protective film 7 are laminated in this order. Next, a first protective film 6 is coated with a coating liquid of a curable resin composition for the low-elasticity, black curable resin layer 1 and dried.
[0118] Thereafter, these are stacked and laminated so that the low-elasticity transparent curable resin layer 2 and the low-elasticity black curable resin layer 1 are in contact with each other, thereby obtaining a laminate in which the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, the high-elasticity transparent curable resin layer 3, and the second protective film 7 are stacked in this order on the first protective film 6.
[0119] The coating liquid of the curable resin composition for the low-elasticity black curable resin layer 1, the coating liquid of the curable resin composition for the low-elasticity transparent curable resin layer 2, and the coating liquid of the curable resin composition for the high-elasticity transparent curable resin layer 3 preferably contain an organic solvent in an amount that provides a viscosity that allows for smooth application. The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, and petroleum-based solvents. Specific examples thereof include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; Examples of suitable solvents include esters such as propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine.
[0120] When carbon black is blended into the coating liquid, carbon black powder or a carbon black dispersion may be added.
[0121] Examples of methods for applying the coating liquid of the curable resin composition for the low-elasticity black curable resin layer 1, the coating liquid of the curable resin composition for the low-elasticity transparent curable resin layer 2, and the coating liquid of the curable resin composition for the high-elasticity transparent curable resin layer 3 include various coaters such as a die coater, gravure coater, roll coater, curtain flow coater, spin coater, bar coater, reverse coater, kiss coater, fountain coater, rod coater, air doctor coater, knife coater, blade coater, cast coater, and screen coater. The drying temperature is preferably 60 to 160°C, preferably 80 to 130°C, and more preferably 90 to 120°C.
[0122] The temperature during lamination is preferably 20 to 120°C, more preferably 30 to 100°C, and even more preferably 40 to 80°C. By setting the temperature during lamination at or above the preferred lower limit, it is possible to ensure sufficient adhesion between the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2, allowing handling even in an uncured or semi-cured state. Furthermore, by setting the temperature during lamination at or below the preferred upper limit, it is possible to prevent the formation of air bubbles and wrinkles. Lamination can be performed using a roll laminator, a press, a vacuum press, or the like.
[0123] <Substrate with elements> As shown in Fig. 2, the substrate with elements 10 has a plurality of light-emitting elements arranged on a substrate 11. Fig. 2 and other figures schematically show a portion where three light-emitting elements (light-emitting element 12, light-emitting element 13, and light-emitting element 14) are arranged.
[0124] There is no limitation on the material of the substrate 11, but a known printed circuit board can be suitably used. Examples of known printed circuit boards include a glass epoxy board, a fluororesin board, and a ceramic board. The light-emitting element is typically a light-emitting diode. The present invention is particularly suitable for use when the light-emitting element is extremely small.
[0125] For example, a light-emitting diode having a height of 1000 nm to 200 μm and a side length of 0.001 to 0.5 mm can be used. For the element-mounted substrate 10 for obtaining mini-LEDs or micro-LEDs, light-emitting diodes of three colors (R, G, and B) or a blue light-emitting diode can be used as the light-emitting element.
[0126] <Method for Manufacturing Light-Emitting Electronic Component> One aspect of the method for manufacturing a light-emitting electronic component of the present invention is a method in which the dry film 100 of the present invention is placed on the surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, with the low-elasticity black curable resin layer 1 in contact with the surface, and the dry film 100 is thermocompression-bonded to fill the spaces between the plurality of light-emitting elements with the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and a portion of the high-elasticity transparent curable resin layer 3, and then heated to cure the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3. Hereinafter, a method for manufacturing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.
[0127] In the manufacturing method of this embodiment, first, as shown in FIG. 2 , a dry film 100 from which the first protective film 6 has been peeled off to expose the low-elasticity black curable resin layer 1 is placed on the surface of the element-mounted substrate 10 on which the light-emitting elements 12, 13, and 14 are arranged, so that the low-elasticity black curable resin layer 1 is in contact with the dry film 100.
[0128] In this case, before compression bonding, the thickness of the low-elasticity black curable resin layer 1 is preferably 10 to 80% of the height of the light-emitting element. The lower limit is more preferably 15% or more, and even more preferably 30% or more. The upper limit is more preferably 70% or less, even more preferably 65% or less, and particularly preferably 55% or less.
[0129] When the thickness of the low-elasticity black curable resin layer 1 is 10% or more of the height of the light-emitting element, the function of preventing light diffusion between the light-emitting elements is sufficient. When the thickness of the low-elasticity black curable resin layer 1 is 15% or more of the height of the light-emitting element, the resin can be sufficiently filled between the light-emitting elements. When the thickness of the low-elasticity black curable resin layer 1 is 30% or more of the height of the light-emitting element, the rate of change in the film thickness of the low-elasticity black curable resin layer 1 after curing is small, and uniform blackness can be achieved throughout the light-emitting electronic component.
[0130] If the thickness of the low-elasticity black curable resin layer 1 is 80% or less of the height of the light-emitting element, a decrease in brightness can be prevented even if there are differences in the tilt or height of the light-emitting element, and light from the light-emitting element is not prevented from reaching the viewer. If the thickness of the low-elasticity black curable resin layer 1 is 70% or less of the height of the light-emitting element, leakage to the outside of the low-elasticity black curable resin layer during thermocompression bonding can be prevented. If the thickness of the low-elasticity black curable resin layer 1 is 55% or less of the height of the light-emitting element, the low-elasticity black curable resin layer 1, which has a light diffusion prevention function, can be appropriately filled between the light-emitting elements.
[0131] The thickness of the low-elasticity transparent curable resin layer 2 before compression bonding is preferably 10 to 80% of the height of the light-emitting element. The lower limit is more preferably 15% or more, and even more preferably 20% or more. The upper limit is more preferably 70% or less, and even more preferably 60% or less.
[0132] When the thickness of the low-elasticity transparent curable resin layer 2 is 10% or more of the height of the light-emitting element, the low-elasticity transparent curable resin layer 2 can sufficiently press the low-elasticity black curable resin layer 1 between the multiple light-emitting elements. When the thickness of the low-elasticity transparent curable resin layer 2 is 15% or more of the height of the light-emitting element, the low-elasticity black curable resin layer 1 can be pressed uniformly during thermocompression bonding, preventing the occurrence of black shading due to variations in the film thickness of the flowed low-elasticity black curable resin layer 1. When the thickness of the low-elasticity transparent curable resin layer 2 is 20% or more of the height of the light-emitting element, the low-elasticity black curable resin layer 1 can be made thinner, making it even less likely that the low-elasticity black curable resin layer 1 will remain on the light-emitting element.
[0133] When the thickness of the low-elasticity, transparent curable resin layer 2 is 80% or less of the height of the light-emitting element, a decrease in brightness can be prevented even if there is a difference in the tilt or height of the light-emitting element.When the thickness of the low-elasticity, transparent curable resin layer 2 is 70% or less of the height of the light-emitting element, leakage of the low-elasticity, transparent curable resin layer 2 to the outside during thermocompression bonding can be prevented.
[0134] The thickness of the highly elastic, transparent, curable resin layer 3 before compression bonding is preferably 10 to 500% of the height of the light emitting element. The lower limit is more preferably 15% or more, and even more preferably 20% or more. The upper limit is more preferably 200% or less, and even more preferably 150% or less.
[0135] When the thickness of the high-elasticity transparent curable resin layer 3 is 10% or more of the height of the light-emitting element, the high-elasticity transparent curable resin layer 3 can remove the low-elasticity black curable resin layer 1 on the light-emitting element, and by not leaving the opaque low-elasticity black curable resin layer 1 on the light-emitting element, light from the light-emitting element does not reach the viewer. When the thickness of the high-elasticity transparent curable resin layer 3 is 15% or more of the height of the light-emitting element, the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2 can be uniformly pressed together during thermocompression bonding, preventing the occurrence of black shading due to variations in the film thickness of the flowed low-elasticity black curable resin layer 1. When the thickness of the high-elasticity transparent curable resin layer 3 is 20% or more of the height of the light-emitting element, the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2 are less susceptible to deformation during thermal curing, making it less likely to cause poor appearance.
[0136] When the thickness of the highly elastic, transparent curable resin layer 3 is 500% or less of the height of the light-emitting element, a uniform film can be formed without differences in residual solvent concentration or unevenness in thermal history in the thickness direction. When the thickness of the highly elastic, transparent curable resin layer 3 is 200% or less of the height of the light-emitting element, the fluidity of the highly elastic, transparent curable resin layer 3 near the upper surface of the light-emitting element can be increased during thermocompression bonding, allowing the low-elasticity, black curable resin layer 1 to be more efficiently removed from above the light-emitting element. When the thickness of the highly elastic, transparent curable resin layer 3 is 150% or less of the height of the light-emitting element, the total light transmittance of the highly elastic, transparent curable resin layer 3 can be increased.
[0137] The total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 before compression bonding is preferably 100 to 550%, more preferably 110 to 400%, and more preferably 120 to 300% of the height of the light-emitting element.
[0138] If the total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 is equal to or greater than the above-mentioned lower limit relative to the height of the light-emitting element, the curable resin can be sufficiently embedded between the light-emitting elements. If the total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 is equal to or less than the above-mentioned upper limit relative to the height of the light-emitting element, thickness unevenness is unlikely to occur during compression bonding, and poor appearance is unlikely to occur on the surface.
[0139] The ratio of the thickness of the low-elasticity black curable resin layer 1 before compression to the total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 before compression is preferably 3 to 70%, more preferably 5 to 60%, and even more preferably 10 to 50%. If the ratio of the thickness of the low-elasticity black curable resin layer 1 before compression to the total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 is equal to or greater than the above-mentioned lower limit, the degree of blackness can be increased and the contrast of the display can be sufficiently improved. If it is equal to or less than the above-mentioned upper limit, the low-elasticity black curable resin layer 1 is less likely to remain on the light-emitting element during compression, and brightness can be sufficiently improved.
[0140] The ratio of the thickness of the low-elasticity transparent curable resin layer 2 before compression to the total thickness of the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3 before compression is preferably 3 to 70%, more preferably 5 to 60%, and even more preferably 10 to 50%. If the ratio of the thickness of the low-elasticity transparent curable resin layer 2 before compression to the total thickness of the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3 before compression is equal to or greater than the above-mentioned lower limit, the low-elasticity transparent curable resin layer 2 can sufficiently press the low-elasticity black curable resin layer 1 between the multiple light-emitting elements. If the ratio is equal to or less than the above-mentioned upper limit, a decrease in brightness can be prevented even if there are differences in the tilt or height of the light-emitting elements.
[0141] The dry film 100 is thermocompressed in the state shown in FIG. 2 to embed the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and a portion of the high-elasticity transparent curable resin layer 3 between the light-emitting elements as shown in FIG. 3. At this time, the low-elasticity black curable resin layer 1 has a low storage modulus and ensures fluidity, making it easy to fill between the light-emitting elements. This is preferable because the high-elasticity transparent curable resin layer 3 and the low-elasticity transparent curable resin layer 2 facilitate its removal from above the light-emitting elements. Furthermore, the low-elasticity transparent curable resin layer 2 also has a relatively low storage modulus and ensures fluidity, making it easy to fill between the light-emitting elements while uniformly pressing the low-elasticity black curable resin layer 1. Furthermore, the high-elasticity transparent curable resin layer 3 has a relatively high storage modulus and is within a deformable range, making it easy to sufficiently remove the low-elasticity black curable resin layer 1 from above the light-emitting elements even if there are differences in the inclination or height of the light-emitting elements.
[0142] The temperature for thermocompression bonding is preferably 80 to 120°C, and more preferably 90 to 110°C. By setting the temperature for thermocompression bonding to 80°C or higher, it is easy to ensure the fluidity of the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2, and the flexibility of the high-elasticity transparent curable resin layer 3. Furthermore, by setting the temperature for thermocompression bonding to 120°C or lower, damage to the light-emitting element is less likely to occur. By setting the temperature for thermocompression bonding to 90 to 110°C, it is possible to more precisely control the fluidity and suppress the occurrence of unevenness and crack-like defects.
[0143] The pressure in thermocompression bonding is preferably 0.05 to 1.0 MPa, more preferably 0.1 to 0.5 MPa. By setting the pressure in thermocompression bonding to the preferred lower limit or more, the low-elasticity black curable resin layer 1 does not remain on the light-emitting element, and light from the light-emitting element does not reach the viewer. By setting the pressure to the preferred upper limit or less, damage to the light-emitting element is unlikely to occur.
[0144] The thermocompression bonding is preferably carried out using a vacuum press that is capable of forming in a vacuum state, which makes it easier to avoid defects caused by air being mixed into the resulting light-emitting electronic component.
[0145] After the pressure bonding, the second protective film 7 is peeled off as shown in Fig. 4, and then the resulting mixture is thermally cured to form the low-elasticity black cured resin layer 1 into a black cured material layer 21 (low-elasticity black cured resin layer 1 in a cured state), the low-elasticity transparent cured resin layer 2 into a first transparent cured material layer 22 (low-elasticity transparent cured resin layer 2 in a cured state), and the high-elasticity transparent cured resin layer 3 into a second transparent cured material layer 23 (high-elasticity transparent cured resin layer 3 in a cured state), as shown in Fig. 5. Thereafter, the resulting mixture is sealed with a sealant 25 as shown in Fig. 6. This results in a light-emitting electronic component 31.
[0146] The curing temperature is preferably 100 to 160°C, more preferably 120 to 150°C. By setting the curing temperature to 100°C or higher, it is possible to cure the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3. By setting the curing temperature to 120°C or higher, it is possible to shorten the curing time for the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3. Furthermore, by setting the curing temperature to the above upper limit temperature or lower, damage to the light-emitting element is unlikely to occur.
[0147] The curing time varies depending on the curing temperature, but is preferably 30 to 360 minutes, more preferably 45 to 180 minutes. At the curing temperature, the storage modulus of the highly elastic, transparent, curable resin layer 3 is relatively high and fluidity is suppressed, thereby suppressing poor appearance after curing. This results in a light-emitting electronic component 31 in which the dry film 100 is pressure-bonded to the surface of the element-mounted substrate 10, on which multiple light-emitting elements are arranged on the substrate 11.
[0148] In the obtained light-emitting electronic component 31, the low-elasticity black cured resin layer 1, the low-elasticity transparent cured resin layer 2, and the high-elasticity transparent cured resin layer 3 are cured to form a black cured material layer 21, a first transparent cured material layer 22, and a second transparent cured material layer 23, respectively, and portions of the black cured material layer 21, the first transparent cured material layer 22, and the second transparent cured material layer 23 are filled between the plurality of light-emitting elements. Note that Fig. 6 shows an example in which the black cured material layer 21 and the first transparent cured material layer 22 are all filled between the plurality of light-emitting elements, and portions of the second transparent cured material layer 23 are filled between the plurality of light-emitting elements.
[0149] Second Embodiment Integrated Encapsulating Sheet Hereinafter, an integrated encapsulating sheet 200 according to a second embodiment will be described. In the description of the second embodiment, components similar to those in the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.
[0150] As shown in FIG. 7 , the integrated encapsulating sheet 200 is basically configured by laminating a low-elasticity black curable resin layer 1, a low-elasticity transparent curable resin layer 2, a high-elasticity transparent curable resin layer 3, and a encapsulating film layer 9.
[0151] For ease of handling, the integrated encapsulating sheet 200 of the present embodiment may further have a protective film on one or both surfaces of the low-elasticity black curable resin layer 1 and the sealing film layer 9. FIG. 7 shows an example in which protective films are provided on both surfaces. Specifically, the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, the high-elasticity transparent curable resin layer 3, the sealing film layer 9, and the second protective film 7 are sequentially laminated on the first protective film 6. Note that if the surface hardness of the sealing film layer 9 is sufficient, the second protective film 7 can be omitted.
[0152] The integrated encapsulating sheet 200 is used such that the low-elasticity black curable resin layer 1 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in Fig. 8. A specific method for obtaining a light-emitting electronic component by pressure bonding the integrated encapsulating sheet 200 to the element-mounted substrate 10 will be described later. The element-mounted substrate 10 is the same as the element-mounted substrate 10 in the first embodiment.
[0153] <Curable Resin Layer> The low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 in this embodiment are the same as those in the dry film 100 of the first embodiment, and preferred aspects are also the same.
[0154] <Sealing Film Layer> The sealing film layer 9 is a layer for protecting the light-emitting element from external physical impact, humidity, moisture, etc. The sealing film layer 9 of this embodiment is composed of a support film layer 4 and a hard coat layer 5 provided on the side of the support film layer 4 opposite to the highly elastic, transparent curable resin layer 3.
[0155] [Total Light Transmittance] The total light transmittance of the sealing film layer 9 as a whole (in this embodiment, the combined total of the support film layer 4 and the hard coat layer 5) is preferably 20 to 80%, more preferably 30 to 80%, and even more preferably 40 to 75%. When the total light transmittance of the sealing film layer 9 is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. When the total light transmittance of the sealing film layer 9 is equal to or less than the upper limit, it is easier to ensure blackness. When the total light transmittance is within the above range, contrast is further improved.
[0156] [Storage Modulus] The storage modulus of the sealing film layer 9 as a whole (in this embodiment, the support film layer 4 and the hard coat layer 5 combined) at 100°C is 1.0 × 10 8 Pa or more, 1.0×10 10 Pa or less, and 9 Pa or more, 9.0×10 9 Pa or less, and 9 Pa or more, 8.0×10 9 It is more preferable that the viscosity is 0.05 Pa or less.
[0157] When the storage modulus of the sealing film layer 9 at 100°C is equal to or less than the preferred upper limit, appropriate flexibility is obtained that does not hinder the flow of the low-elasticity black curable resin layer 1 and the like when pressure-bonded to the element-mounted substrate 10, thereby improving workability and preventing cracks due to pressure.
[0158] When the storage modulus of the sealing film layer 9 at 100°C is equal to or greater than the preferred lower limit, the sealing film layer 9 is less likely to deform when pressed against the element-mounted substrate 10, and pressure can be reliably transmitted to the low-elasticity black curable resin layer 1, etc., preventing defects such as cracking and deformation in the hard coat layer 5.
[0159] <Support Film Layer> The support film layer 4 in the sealing film layer 9 is a layer for protecting the light emitting element from external physical impact, humidity, moisture, and the like.
[0160] [Total Light Transmittance] The total light transmittance of the support film layer 4 alone is preferably 30 to 99%, more preferably 50 to 95%, and even more preferably 70 to 95%. When the total light transmittance of the support film layer 4 alone is equal to or greater than the above lower limit, an inexpensive commercially available film can be used.
[0161] [Resin] The support film layer 4 may be composed of a thermoplastic resin or a thermosetting resin. Examples of resins constituting the support film layer 4 include polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, polycarbonate resin, triacetyl cellulose resin, polymethylpentene resin, phenoxy resin, syndiotactic polystyrene resin, and polyimide resin. In terms of heat resistance, weather resistance, availability, cost, and the like, it is preferable for the support film layer 4 to contain at least one resin selected from polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, and polycarbonate resin. By containing these resins, deformation during pressure bonding can be prevented.
[0162] [Film Thickness] The thickness of the support film layer 4 is preferably 10 to 250 μm, more preferably 20 to 200 μm, and even more preferably 25 to 150 μm. When the thickness of the support film layer 4 is equal to or greater than the preferred lower limit, the support film layer 4 has sufficient strength to protect the element. When the thickness of the support film layer 4 is equal to or less than the preferred upper limit, visibility is improved and costs can be reduced.
[0163] <Hard Coat Layer> [Hardness] The hard coat layer 5 is a layer for protecting the light-emitting electronic component from scratches. The pencil hardness of the surface of the hard coat layer 5 is preferably H or more, more preferably 2H or more, and even more preferably 3H or more.
[0164] [Surface Roughness] The surface roughness Ra of the hard coat layer 5 surface is preferably 0.1 to 1 μm, more preferably 0.2 to 1 μm, and even more preferably 0.3 to 1 μm. When the surface roughness of the hard coat layer 5 is equal to or greater than the preferred lower limit, the reflectance of the surface of the hard coat layer 5 can be reduced. When the surface roughness of the hard coat layer 5 is equal to or less than the preferred upper limit, production becomes easier.
[0165] [Total Light Transmittance] The hard coat layer 5 is preferably prepared so that the total light transmittance is 30 to 99%, more preferably 50 to 99%, and even more preferably 60 to 99%. When the total light transmittance of the hard coat layer 5 is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side.
[0166] [Curable Resin Composition] The hard coat layer 5 is composed of a curable resin composition. Examples of curable resin compositions constituting the hard coat layer 5 include thermosetting resin compositions, ultraviolet curable resin compositions, and electron beam curable resin compositions. Among these, ultraviolet curable resin compositions are preferred. Examples of ultraviolet curable resin compositions include acrylic resins, urethane resins, silicone resins, etc., and may contain one or more of these. Examples of thermosetting resin compositions include acrylic resins, urethane resins, silicone resins, melamine resins, etc., and may contain one or more of these.
[0167] [Fine Particles] The hard coat layer 5 preferably contains fine particles. As the fine particles, inorganic fine particles, organic fine particles, or both can be used. Examples of inorganic fine particles include silica fine particles and titanium fine particles. Examples of organic fine particles include polymethyl methacrylate resin (PMMA resin) and urethane resin. Of these, silica fine particles are preferred. By containing fine particles, it is possible to adjust the surface roughness and improve the surface hardness.
[0168] [Film Thickness] The thickness of the hard coat layer 5 is preferably 0.5 to 20 μm, more preferably 1 to 10 μm, and even more preferably 1.5 to 8 μm. When the thickness of the hard coat layer 5 is equal to or greater than the preferred lower limit, sufficient hardness can be ensured. When the thickness of the hard coat layer 5 is equal to or less than the preferred upper limit, problems such as curling do not occur. The hard coat layer 5 may contain a black pigment or black dye to suppress uneven light emission and color unevenness.
[0169] [Glossiness] The glossiness of the hard coat layer 5 side measured with a glossmeter (JIS-Z-8741) is preferably 1 to 50, more preferably 3 to 30, and even more preferably 5 to 25. When the glossiness of the hard coat layer 5 side is equal to or higher than the lower limit, production is easy. When the glossiness of the hard coat layer 5 is equal to or lower than the preferred upper limit, the visibility of the display is improved.
[0170] <Semitransparent Resin Layer> The sealing film layer 9 may have a semitransparent resin layer provided on one or both surfaces of the support film layer 4. By providing a semitransparent resin layer, the blackness of the display can be increased and the contrast can be improved. Furthermore, when a semitransparent resin layer is provided on the viewer side of the support film layer 4, diffuse reflection of external light by the support film layer 4 can be made less visible.
[0171] [Total Light Transmittance] The translucent resin layer preferably has a total light transmittance of 20 to 80%, more preferably 30 to 80%, and even more preferably 40 to 75%. When the total light transmittance of the translucent resin layer is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side. When the total light transmittance of the translucent resin layer is equal to or less than the upper limit, the degree of blackness is increased, and the contrast improvement effect is further improved.
[0172] [Overall Haze] The translucent resin layer preferably has an overall haze based on JIS K 7136 of 7% or more, more preferably 10 to 70%, and even more preferably 15 to 65%. When the overall haze of the translucent resin layer is equal to or greater than the preferred lower limit, the ability to conceal diffuse reflection of external light in the support film layer 4 is improved. When the overall haze of the translucent resin layer is equal to or less than the preferred upper limit, the degree of blackness can be increased. The overall haze of the translucent resin layer can be adjusted by the compatibility of the carbon black, filler, and resin contained in the translucent resin composition.
[0173] [Storage Modulus] The storage modulus of the semi-transparent resin layer at 100°C is 1.0 × 10 6 Pa or more, and 6 Pa or more, 1.0×10 10 Pa or less, and more preferably 1.0 × 10 7 Pa or more, 5.0×10 9 Pa or less, and more preferably 1.0 × 10 8 Pa or more, 5.0×10 9 It is particularly preferable that the viscosity is 0.05 Pa or less.
[0174] If the thickness of the semitransparent resin layer varies, the degree of blackness may become non-uniform in the surface direction, which may result in spots. When the storage modulus of the semitransparent resin layer at 100°C is equal to or greater than the preferred lower limit, the semitransparent resin layer is less likely to deform when pressure-bonded to the element-mounted substrate 10, and thickness variations are less likely to occur. Therefore, uneven light emission and color unevenness can be suppressed.
[0175] When the storage modulus at 100°C of the semitransparent resin layer is equal to or less than the preferred upper limit, it is easy to prevent cracks from occurring when the semitransparent resin layer is pressure-bonded to the element-mounted substrate 10. In addition, it is easy to ensure adhesion between the semitransparent resin layer and the support film layer 4 or the hard coat layer 5.
[0176] [Semitransparent Resin Composition] The semitransparent resin layer can be composed of a coating film of a semitransparent resin composition containing carbon black, etc., or a cured product thereof. The semitransparent resin composition is a thermoplastic resin composition or a curable resin composition, and is preferably a curable resin composition from the viewpoint of being less likely to deform or the like in durability tests under thermal shock or high humidity.
[0177] Examples of resins contained in the translucent resin composition include epoxy resin, acrylic resin, polyester resin, polyurethane resin, polycarbonate resin, polyimide resin, acrylonitrile butadiene copolymer, styrene butadiene copolymer, vinyl acetate resin, and silicone resin. When the translucent resin composition is a curable resin composition, it is preferably a cured film from the viewpoints of being less prone to deformation and having stable coloring. In other words, it is preferable that the translucent resin composition is cured before being pressure-bonded to the element-mounted substrate 10.
[0178] <Protective Film> The first protective film 6 and the second protective film 7 can be the same as the protective film in the first embodiment, and the preferred aspects are also the same.
[0179] <Method for manufacturing integrated encapsulating sheet> In order to obtain the integrated encapsulating sheet 200, a release sheet is prepared by applying a coating liquid of the curable resin composition for the low elasticity transparent curable resin layer 2 to the release sheet and then drying the coating liquid, and a sealing film layer 9 is prepared by applying a coating liquid of the curable resin composition for the high elasticity transparent curable resin layer 3 to the release sheet and then drying the coating liquid.
[0180] Thereafter, these are stacked and laminated so that the low-elasticity, transparent curable resin layer 2 and the high-elasticity, transparent curable resin layer 3 are in contact with each other, thereby obtaining a laminate (1) in which the high-elasticity, transparent curable resin layer 3 and the low-elasticity, transparent curable resin layer 2 are sequentially stacked on the sealing film layer 9. A second protective film 7 is laminated on the surface of this sealing film layer 9, as necessary.
[0181] A first protective film 6 is prepared by applying a coating liquid of a curable resin composition for the low-elasticity black curable resin layer 1 and drying it, and the release sheet of the laminate (1) is peeled off. The low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2 are placed on top of each other and laminated together so that they are in contact with each other, thereby obtaining an integrated encapsulating sheet 200.
[0182] The sealing film layer 9 in which the hard coat layer 5 is formed on the support film layer 4 is obtained by applying a coating agent for the hard coat layer to the surface of the support film layer 4, drying the coating agent, and then curing the coating agent. When the sealing film layer 9 is obtained by sequentially forming the semitransparent resin layer and the hard coat layer 5 on the support film layer 4, the sealing film layer 9 can be obtained by applying a coating liquid of a semitransparent resin composition for the semitransparent resin layer to the surface of the support film layer 4 and drying the coating liquid, applying a coating agent for the hard coat layer to the surface of the support film layer 4 and then drying the coating liquid, and then curing the coating agent.
[0183] When the sealing film layer 9 is formed by forming a translucent resin layer on one surface of the support film layer 4 and a hard coat layer 5 on the other surface, the sealing film layer 9 can be obtained by applying a coating liquid of a translucent resin composition for the translucent resin layer to one surface of the support film layer 4 and drying it, and then applying a coating agent for the hard coat layer to the other surface and drying it, and then curing it. The coating agent for the hard coat layer may be applied after curing the translucent resin composition.
[0184] <Method for manufacturing a light-emitting electronic component> One aspect of the method for manufacturing a light-emitting electronic component of the present invention is a method in which the integrated encapsulating sheet 200 of the present invention is placed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, with the low-elasticity black curable resin layer 1 in contact with the surface, and the sheet is thermocompression-bonded to fill the spaces between the plurality of light-emitting elements with the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and a portion of the high-elasticity transparent curable resin layer 3, and the sheet is heated to cure these curable resin layers. Hereinafter, a method for manufacturing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.
[0185] In the manufacturing method of the present embodiment, first, as shown in FIG. 8 , the first protective film 6 is peeled off from the surface of the element-mounted substrate 10 on which the light-emitting elements 12, 13, and 14 are arranged, and the integrated encapsulating sheet 200, in which the low-elasticity black cured resin layer 1 is exposed, is placed so that the low-elasticity black cured resin layer 1 is in contact with the surface.
[0186] In this case, before the pressure-bonding, preferred aspects such as the thickness of the low-elasticity black curable resin layer 1, the total thickness of the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3, the total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3, and the ratio of the thicknesses of each layer are the same as those described for the case where the dry film 100 of the first embodiment is used.
[0187] 8, the dry film 100 is thermocompressed to fill the gaps between the light-emitting elements with the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and a portion of the high-elasticity transparent curable resin layer 3. The low-elasticity black curable resin layer 1 has a relatively low storage modulus and ensures fluidity, making it easy to fill gaps between the light-emitting elements and less likely to remain on the light-emitting elements. The low-elasticity transparent curable resin layer 2 also has a relatively low storage modulus and ensures fluidity, making it easy to fill gaps between the light-emitting elements together with the low-elasticity black curable resin layer 1.
[0188] The preferred conditions for thermocompression bonding, such as temperature and pressure, are the same as those described for the case where the dry film 100 of the first embodiment is used. As in the first embodiment, it is also preferable to use a vacuum press machine capable of forming in a vacuum state.
[0189] After the pressure bonding, the second protective film 7 is peeled off as shown in Fig. 10, and then the resulting mixture is thermally cured to form the low-elasticity black cured resin layer 1 into a black cured material layer 21 (low-elasticity black cured resin layer 1 in a cured state), the low-elasticity transparent cured resin layer 2 into a first transparent cured material layer 22 (low-elasticity transparent cured resin layer 2 in a cured state), and the high-elasticity transparent cured resin layer 3 into a second transparent cured material layer 23 (high-elasticity transparent cured resin layer 3 in a cured state), as shown in Fig. 11. This results in a light-emitting electronic component 32.
[0190] In the obtained light-emitting electronic component 32, the low-elasticity black cured resin layer 1, the low-elasticity transparent cured resin layer 2, and the high-elasticity transparent cured resin layer 3 are cured to form a black cured material layer 21, a first transparent cured material layer 22, and a second transparent cured material layer 23, respectively, and portions of the black cured material layer 21, the first transparent cured material layer 22, and the second transparent cured material layer 23 are filled between the plurality of light-emitting elements. Fig. 11 shows an example in which the black cured material layer 21 and the first transparent cured material layer 22 are all filled between the plurality of light-emitting elements, and portions of the second transparent cured material layer 23 are filled between the plurality of light-emitting elements.
[0191] <<Effects>> According to the dry film or integrated encapsulating sheet of the present invention, the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer are soft and fluid during compression bonding. Meanwhile, because the high-elasticity transparent curable resin layer is hard, the stress of compression bonding is sufficiently transmitted to the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer. As a result, the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer can be sufficiently filled between the optical elements. Because the high-elasticity transparent curable resin layer has sufficient hardness, the black curable resin layer on the light-emitting element can be removed even in areas where light-emitting elements with different inclinations or heights are present (i.e., areas where stress is less likely to be applied). As a result, even if the inclination or height of the light-emitting elements differs from one light-emitting element to another, a decrease in brightness can be suppressed without time-consuming etching such as plasma treatment.
[0192] According to the light-emitting electronic component and the method for manufacturing the light-emitting electronic component of the present invention, the highly elastic transparent curable resin layer on the surface side of the dry film is the hardest, so that poor appearance after curing can be suppressed. Because the encapsulating film layer is laminated on the integrated encapsulating sheet, the encapsulating process can be completed with a single pressure bonding. Moreover, even if the height or inclination of the light-emitting element varies, the black curable resin layer on the light-emitting element can be removed. As a result, a light-emitting electronic component with sufficient brightness and blackness can be obtained without increasing production costs or energy consumption.
[0193] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the descriptions of these examples. In the following description, all blending amounts are calculated on a solid content basis.
[0194] <Raw Materials> Details of the raw materials used in each Example and Comparative Example are as follows. [Epoxy Resins] EOCN (registered trademark)-1020-55: Nippon Kayaku Co., Ltd., cresol novolac type multifunctional epoxy resin (solid), softening point 55.7°C, epoxy equivalent 195 g / eq. EPICLON (registered trademark) HP-7200H: DIC Corporation, cyclopentadiene novolac type multifunctional epoxy resin (solid), softening point 82°C, epoxy equivalent 227 g / eq. jER (registered trademark) YX7200B35: Mitsubishi Chemical Corporation, phenoxy type epoxy resin (MEK solution, solid content 35% by mass), glass transition temperature 150°C, epoxy equivalent 8750 g / eq., weight average molecular weight 27,218. [Elastomer] Nipol NX775: manufactured by Nippon Zeon Co., Ltd., a carboxy-modified nitrile rubber, an elastomer having a weight average molecular weight of 208,000.
[0195] [Curing catalyst] Curesol (registered trademark) 2PZ-CN: 1-cyanoethyl-2-phenylimidazole, manufactured by Shikoku Chemical Industries, Ltd. Curesol 2E4MZ: 2-ethyl-4-methylimidazole, manufactured by Shikoku Chemical Industries, Ltd.
[0196] [Carbon Black] Special Black 4: manufactured by Orion Engineered Carbons, gas black, pH 3, average particle size 25 nm.
[0197] [Solvent] MEK: Methyl ethyl ketone, manufactured by Junsei Chemical Co., Ltd. PGM: Propylene glycol monomethyl ether, manufactured by Junsei Chemical Co., Ltd.
[0198] [Support film layer] Cosmoshine (registered trademark) A4300: PET film manufactured by Toyobo Co., Ltd., thickness 75 μm. [Release PET] 1-E: Manufactured by Nippa Corporation, thickness 50 μm. 1-TRE: Manufactured by Nippa Corporation, thickness 50 μm.
[0199] [Resin for hard coat layer] ACRIT (registered trademark) 8KX-078: manufactured by Taisei Fine Chemical Co., Ltd., solid content concentration 40% by mass, UV-curable acrylic polymer, weight average molecular weight 40,000.
[0200] [Fine particles] Chemisnow (registered trademark) MX-500L: manufactured by Soken Chemical & Engineering Co., Ltd., cross-linked acrylic monodisperse particles, average particle diameter 5 μm. [Photoradical polymerization initiator] Omnirad (registered trademark) TPO H: manufactured by IGM Resins B.V.
[0201] <Preparation of Coating Liquid>
[0202] [Coating liquid for transparent curable resin layer] The raw materials having the formulations shown in Table 1 were mixed with a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare coating liquids for transparent curable resin layer (raw material 3-1 to raw material 3-3) with a solid content concentration of 35 mass %. That is, the total blend amount (solid content equivalent) of the raw materials having the formulations shown in Table 1 was 35 mass % with respect to the entire coating liquid obtained.
[0203]
[0204] [Coating Liquid for Low-Elasticity Black Curable Resin Layer] 70 parts by mass of epoxy resin EPICLON HP-7200H (manufactured by DIC Corporation), 30 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Co., Ltd.), 3 parts by mass of curing catalyst Curesol 2PZ-CN (manufactured by Shikoku Chemicals Corporation), and 4 parts by mass of carbon black Special Black 4 (manufactured by Orion Engineered Carbons Co., Ltd.) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a coating liquid for low-elasticity black curable resin layer (raw material 4) with a solids concentration of 35 mass%.
[0205] [Coating Liquid of Translucent Resin Composition] 80 parts by mass of epoxy resin EOCN-1020-55 (manufactured by Nippon Kayaku Co., Ltd.), 20 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Co., Ltd.), 3 parts by mass of curing catalyst Curesol 2E4MZ (manufactured by Shikoku Chemicals Corporation), and 0.5 parts by mass of carbon black Special Black 4 (manufactured by Orion Engineered Carbons Co., Ltd.) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a translucent resin composition (raw material 1) with a solids concentration of 25 mass%.
[0206] [Coating Agent for Hard Coat Layer] 100 parts by mass of hard coat layer resin 8KX-078 (manufactured by Taisei Fine Chemical Co., Ltd.), 4.5 parts by mass of fine particles Chemisnow MX-500L (manufactured by Soken Chemical & Engineering Co., Ltd.), and 0.6 parts by mass of a photoradical polymerization initiator Omnirad TPO H (manufactured by IGM Resins B.V.) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a coating agent for a hard coat layer (raw material 2) with a solid content concentration of 25 mass%.
[0207] <Total Light Transmittance of Each Single Layer> The total light transmittance of Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) was measured in accordance with JIS K 7361 using a haze meter NDH5000 (manufactured by Nippon Denshoku Industries Co., Ltd.).
[0208] The coating liquid for the low-elasticity transparent curable resin layer and the coating liquid for the high-elasticity transparent curable resin layer were applied to Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) using an applicator so that the dry film thickness was 25 μm (50 μm in Comparative Examples 1 and 2), and the film was dried at 120 ° C for 5 minutes. After that, the coating liquid for the low-elasticity transparent curable resin layer or the coating liquid for the high-elasticity transparent curable resin layer was cured by heating in a hot air circulating oven at 150 ° C for 1 hour to obtain a film with each cured transparent curable resin layer. The total light transmittance of the obtained film with the cured transparent curable resin layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361, with the transmitted light through Cosmoshine A4300 being taken as 100%. The measurement results of the total light transmittance of each transparent curable resin layer are shown in Tables 2 and 3.
[0209] The coating liquid for the low-elasticity black curable resin layer was applied to Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) using an applicator so that the dry film thickness was 30 μm, and after drying at 120 ° C for 5 minutes, the coating liquid for the low-elasticity black curable resin layer was cured by heating in a hot air circulating oven at 150 ° C for 1 hour to obtain a film with a cured low-elasticity black curable resin layer. The total light transmittance of the obtained film with a cured low-elasticity black curable resin layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361, with the transmitted light through Cosmoshine A4300 being 100%. The measurement results of the total light transmittance of the low-elasticity black curable resin layer are shown in Tables 2 and 3.
[0210] <Storage Modulus of Each Monolayer> Using an applicator, the coating liquid for a low-elasticity transparent curable resin layer, the coating liquid for a high-elasticity transparent curable resin layer, and the coating liquid for a low-elasticity black curable resin layer were each applied to a release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) so that the dry film thickness would be 40 μm. After drying at 120° C. for 5 minutes, the release PET 1-E was peeled off to obtain monolayer sheets of the low-elasticity transparent curable resin layer, the high-elasticity transparent curable resin layer, and the low-elasticity black curable resin layer, respectively.
[0211] The storage modulus of each of the obtained monolayer sheets at 100°C was measured using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments) at a measurement frequency of 1 Hz and a temperature rise rate of 5°C / min in accordance with JIS K7244. The results are shown in Tables 2 and 3.
[0212] The storage modulus of the obtained highly elastic transparent curable resin layer at 150°C was measured using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments) at a measurement frequency of 1 Hz and a temperature rise rate of 5°C / min in accordance with JIS K7244. The results are shown in Table 2.
[0213] <Substrate with elements for evaluation> A substrate with elements for evaluation was prepared by arranging a plurality of LED light emitting elements, each of which was 0.1×0.2 mm and 65 μm high, on an epoxy glass substrate.
[0214] <Dry Film> [Examples 1 and 2] A coating liquid for a highly elastic, transparent, curable resin layer shown in Table 2 (raw material 3-2 or raw material 3-3) was applied to the release surface of release PET 1-TRE (manufactured by Nippa Corporation, 50 μm) using an applicator so as to give a dry film thickness of 25 μm, and the coating was dried at 120°C for 5 minutes to obtain a first sheet in which the highly elastic, transparent, curable resin layer was supported by the release PET.
[0215] The coating liquid for the low-elasticity, transparent, curable resin layer (raw material 3-1) was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness would be 25 μm, and the coating was dried at 120° C. for 5 minutes to obtain a second sheet in which the low-elasticity, transparent, curable resin layer was supported by the release PET.
[0216] The obtained first sheet and second sheet were overlapped with each other so that the low-elasticity transparent curable resin layer and the high-elasticity transparent curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C. The release PET 1-E used on the second sheet was peeled off to obtain a third sheet.
[0217] Furthermore, the coating liquid (raw material 4) for the low-elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so as to give a dry film thickness of 30 μm, and the coating was dried at 120° C. for 5 minutes to obtain a fourth sheet in which the low-elasticity black curable resin layer was supported by the release PET.
[0218] The obtained third sheet and fourth sheet were overlaid so that the low-elasticity transparent curable resin layer and the low-elasticity black curable resin layer were in contact with each other, and laminated using a roll laminator at 60°C to obtain a dry film for each example.
[0219] [Comparative Example 1]
[0220] The coating liquid for the highly elastic, transparent, curable resin layer (raw material 3-3) was applied onto the release surface of release PET 1-TRE (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness would be 50 μm, and the coating was dried at 120° C. for 5 minutes to obtain a fifth sheet in which the highly elastic, transparent, curable resin layer was supported by the release PET.
[0221] Furthermore, the coating liquid (raw material 4) for the low-elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so as to give a dry film thickness of 30 μm, and the coating liquid was dried at 120° C. for 5 minutes to obtain a sixth sheet in which the low-elasticity black curable resin layer was supported by the release PET.
[0222] The obtained fifth sheet and sixth sheet were overlapped with each other so that the high-elasticity transparent curable resin layer and the low-elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C to obtain a dry film of Comparative Example 1.
[0223] [Mounting of Dry Film] The release PET 1-E on the low-elasticity black curable resin layer side of the dry film of each example was peeled off, and the low-elasticity black curable resin layer was placed in contact with the LED light-emitting element of the evaluation element-attached substrate. Then, using a vacuum press, dry film 1 was filled between the light-emitting elements under conditions of a vacuum degree of 100 hPa, 100°C, 0.36 MPa, and 3 minutes. The release PET 1-TRE in contact with the high-elasticity transparent curable resin layer was peeled off, and the dry film was then heated in an oven at 150°C for 1 hour to thermally cure, thereby obtaining 10 light-emitting electronic components of each example.
[0224] [Brightness after mounting / Brightness before mounting] For ten light-emitting electronic components in each example, the brightness of the light-emitting electronic components before and after mounting the dry film was measured using a Konica Minolta luminance meter CA-410, and the ratio of brightness after mounting / brightness before mounting was calculated by dividing the brightness after mounting by the brightness before mounting. The average value of the results for the ten light-emitting electronic components is shown in Table 2.
[0225]
[0226] As shown in Table 2, it was confirmed that the dry film according to the present invention can suppress the loss of the overall brightness.
[0227] <Sealing film layer> A coating solution of a translucent resin composition was applied to a first surface of a support film layer (Cosmoshine A4300: manufactured by Toyobo Co., Ltd.) using a bar coater so that the dry film thickness was 7 μm, and the coating was dried at 120° C. for 5 minutes, and then heated in a hot air circulating oven at 80° C. for 72 hours to harden the translucent resin composition. Next, a corona treatment was performed on the surface of the translucent resin layer opposite the film layer, and a coating agent for a hard coat layer was applied using a bar coater so that the dry film thickness was 3 μm. Then, after drying at 120° C. for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiating it with ultraviolet light of 1000 kJ / cm 2 , thereby obtaining a sealing film layer in which the semi-transparent resin layer and the hard coat layer were supported by the support film layer.
[0228] <Total Light Transmittance of Sealing Film Layer> The total light transmittance of the obtained sealing film layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361. The results are shown in Table 3.
[0229] <Storage modulus of sealing film layer> The storage modulus of the obtained sealing film layer at 100°C was measured using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments) under conditions of a measurement frequency of 1 Hz and a temperature rise rate of 5°C / min in accordance with JIS K7244. The results are shown in Table 3.
[0230] <Integrated encapsulating sheet> [Examples 3 and 4] The coating liquid for the highly elastic, transparent, curable resin layer shown in Table 3 (raw material 3-2 or raw material 3-3) was applied to the second surface (the surface opposite to the first surface) of the support film layer in the sealing film layer using an applicator so as to give a dry film thickness of 25 μm, and the coating was dried at 120° C. for 5 minutes to obtain a seventh sheet in which the seventh transparent curable resin layer was supported by the release PET.
[0231] The coating liquid for the low-elasticity, transparent, curable resin layer (raw material 3-1) was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 25 μm. The coating was then dried at 120° C. for 5 minutes to obtain an eighth sheet in which the low-elasticity, transparent, curable resin layer was supported on the release PET layer.
[0232] The obtained seventh sheet and eighth sheet were stacked together so that the high-elasticity transparent curable resin layer and the third low-elasticity transparent curable resin layer were in contact with each other, and laminated using a roll laminator at 60°C. The release PET used on the eighth sheet was peeled off to obtain a ninth sheet.
[0233] Furthermore, the coating liquid (raw material 4) for the low-elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness would be 30 μm, and the coating was dried at 120° C. for 5 minutes to obtain a 10th sheet in which the low-elasticity black curable resin layer was supported by the release PET.
[0234] The obtained ninth sheet and tenth sheet were stacked so that the low elasticity transparent curable resin layer and the low elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C to obtain an integrated encapsulating sheet of each Example.
[0235] [Comparative Example 2] The coating liquid for the highly elastic, transparent, curable resin layer (raw material 3-3) was applied to the second surface (the surface opposite to the first surface) of the support film layer of the sealing film layer using an applicator so as to give a dry film thickness of 50 μm. The coating was then dried at 120° C. for 5 minutes to obtain an 11th sheet in which the highly elastic, transparent, curable resin layer was supported on the sealing film layer.
[0236] Furthermore, the coating liquid (raw material 4) for the low-elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness would be 30 μm, and the coating was dried at 120° C. for 5 minutes to obtain a 12th sheet in which the low-elasticity black curable resin layer was supported by the release PET.
[0237] The obtained 11th sheet and 12th sheet were stacked together so that the high elasticity transparent curable resin layer and the low elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C to obtain an integrated encapsulating sheet of Comparative Example 2.
[0238] [Mounting of integrated encapsulating sheet] The release PET 1-E of the integrated encapsulating sheet of each example was peeled off, and the low-elasticity black curable resin layer was placed in contact with the LED light-emitting element of the evaluation element-attached substrate. Thereafter, the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer were filled between the light-emitting elements in a vacuum press under conditions of a vacuum degree of 100 hPa, 100 ° C., 0.36 MPa, and 3 minutes, and then heated in an oven at 150 ° C. for 1 hour to be thermally cured, thereby obtaining 10 light-emitting electronic components of each example.
[0239] [Lab] The Lab values on the hard coat layer side of ten light-emitting electronic components obtained for each example were measured using a spectrophotometer CM-5 manufactured by Konica Minolta in accordance with JIS K 8722. The Lab values of the ten light-emitting electronic components for each example were averaged and the results are shown in Table 3.
[0240] [Brightness after mounting / Brightness before mounting] For 10 light-emitting electronic components in each example, the brightness of the light-emitting electronic components before and after mounting the integrated encapsulant sheet was measured using a Konica Minolta luminance meter CA-410, and the ratio of brightness after mounting / brightness before mounting was calculated by dividing the brightness after mounting by the brightness before mounting. The average value of the results for the 10 light-emitting electronic components is shown in Table 3.
[0241]
[0242] As shown in Table 3, it was confirmed that the dry film according to the present invention can suppress the loss of the overall brightness.
[0243] REFERENCE SIGNS LIST 1 Low-elasticity black curable resin layer 2 Low-elasticity transparent curable resin layer 3 High-elasticity transparent curable resin layer 4 Support film layer 5 Hard coat layer 6 First protective film 7 Second protective film 9 Sealing film layer 10 Substrate with element 11 Substrate 12 Light-emitting element 13 Light-emitting element 14 Light-emitting element 21 Black cured product layer 22 First transparent cured product layer 23 Second transparent cured product layer 25 Sealing material 31 Light-emitting electronic component 32 Light-emitting electronic component 100 Dry film 200 Integrated encapsulating sheet
Claims
1. A dry film that is pressure-bonded to a surface of a substrate having a plurality of light-emitting elements arranged on the substrate, the surface having the plurality of light-emitting elements arranged thereon, the dry film comprising a low-elasticity black curable resin layer, a low-elasticity transparent curable resin layer, and a high-elasticity transparent curable resin layer, which are laminated in this order from the side that will be in direct contact with the substrate during the pressure-bonding.
2. The dry film described in claim 1, wherein the storage modulus of the high elasticity transparent curable resin layer is greater than the storage modulus of the low elasticity transparent curable resin layer and the low elasticity black curable resin layer at 100°C.
3. A dry film according to claim 1 or 2, wherein the storage modulus of the low elasticity transparent curable resin layer is greater than the storage modulus of the low elasticity black curable resin layer at 100°C.
4. The storage modulus of the highly elastic transparent curable resin layer is 1.0×10 at 100° C. 7 The dry film according to claim 1 or 2, wherein the viscosity is 0.1 Pa or less.
5. The storage modulus of the low elasticity black curable resin layer is 1.0 x 10 at 100°C. 5 The dry film according to claim 1 or 2, wherein the viscosity is 0.1 Pa or less.
6. The storage modulus of the low elasticity transparent curable resin layer is 1.0×10 5 The dry film according to claim 1 or 2, wherein the viscosity is 0.1 Pa or less.
7. The storage modulus of the highly elastic transparent curable resin layer is 1.0×10 at 150° C. 5 The dry film according to claim 1 or 2, having a modulus of elasticity of 1 Pa or more.
8. The dry film according to claim 1 or 2, wherein the low elasticity black curable resin layer has a total light transmittance of 0 to 30%.
9. The dry film according to claim 1 or 2, wherein the low elasticity transparent curable resin layer has a total light transmittance of 50% or more.
10. The dry film according to claim 1 or 2, wherein the highly elastic, transparent, curable resin layer has a total light transmittance of 50% or more.
11. The dry film according to claim 1 or 2, wherein the highly elastic transparent curable resin layer comprises a high molecular weight epoxy resin.
12. The dry film according to claim 11, wherein the high molecular weight epoxy resin has a weight average molecular weight of 10,000 to 100,000.
13. The dry film according to claim 11, wherein the highly elastic transparent curable resin layer contains a phenoxy type epoxy resin as the high molecular weight epoxy resin.
14. The dry film according to claim 11, wherein the amount of the high molecular weight epoxy resin is 30 to 80 mass % relative to 100 mass % of the total resin solids content of the highly elastic, transparent, curable resin layer.
15. The dry film according to claim 1 or 2, wherein the low elasticity black curable resin layer comprises an elastomer.
16. The dry film of claim 15, wherein the elastomer is a modified elastomer.
17. The dry film of claim 16, wherein the modified elastomer is an acid-modified acrylonitrile butadiene rubber.
18. The dry film according to claim 1 or 2, wherein the low elasticity black curable resin layer contains carbon black.
19. An integrated sealing sheet comprising the dry film according to claim 1 or 2 and a sealing film layer provided on the opposite side of the high elasticity transparent curable resin layer to the low elasticity transparent curable resin layer.
20. The integral encapsulating sheet according to claim 19, wherein the encapsulating film layer comprises a support film layer and a hard coat layer provided on the side of the support film layer opposite the highly elastic transparent curable resin layer.
21. A light-emitting electronic component comprising: a substrate having a plurality of light-emitting elements arranged on the substrate; and a dry film according to claim 1 or 2 pressed onto the surface of the substrate having the plurality of light-emitting elements arranged thereon; wherein the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and a portion of the high-elasticity transparent curable resin layer are filled between the plurality of light-emitting elements; and the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer are cured.
22. A light-emitting electronic component comprising: an element-mounted substrate having a plurality of light-emitting elements arranged on a substrate; and the integrated encapsulating sheet according to claim 19, which is pressed onto the surface of the element-mounted substrate on which the plurality of light-emitting elements are arranged; the low-elasticity black curable resin layer, and a portion of the low-elasticity transparent curable resin layer and the high-elasticity transparent curable resin layer are filled between the plurality of light-emitting elements; and the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer are cured.
23. A method for manufacturing a light-emitting electronic component, comprising: placing the dry film described in claim 1 or 2 on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the low-elasticity black curable resin layer is in contact with the surface, and thermocompressing the dry film; and curing the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer by heating.
24. The method for producing a light-emitting electronic component according to claim 23, wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is carried out by heating at 100 to 160°C.
25. A method for manufacturing a light-emitting electronic component, comprising: placing the integrated encapsulating sheet described in claim 19 on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the low-elasticity black curable resin layer is in contact with the surface, and thermocompressing the sheet; and curing the low-elasticity black curable resin layer, the low-elasticity transparent curable resin layer, and the high-elasticity transparent curable resin layer by heating.
26. The method for producing a light-emitting electronic component according to claim 25, wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is carried out by heating at 100 to 160°C.
Citation Information
Patent Citations
LED packaging method, LED lamp and LED display
CN115084320A
Sealing sheet, manufacturing method of sealing sheet, light emitting diode device, and manufacturing method of light emitting diode device
JP2013077811A
Adhesive sheet and display body
JP2020169262A
Optical laminate
JP2021161263A
Thermosetting resin composition
JP2023012051A