Silicon nitride sintered body, machine part using same, and bearing

The silicon nitride sintered body with controlled hardness and sintering aid distribution addresses the processing challenges and wear resistance issues, achieving effective workability and product life in bearing applications.

WO2024242152A1PCT designated stage expired Publication Date: 2024-11-28NTN CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018924
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-02
Filing Date
2024-05-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Silicon nitride sintered bodies have high hardness, making them difficult to process, which increases costs and time, and lowering hardness to improve workability compromises wear resistance, posing a risk to product life, especially in applications like bearing members.

Method used

A silicon nitride sintered body with a Vickers hardness of 1220 Hv to 1400 Hv, containing rare earth and aluminum elements, and a surface layer with a higher sintering aid component ratio, achieving both workability and mechanical properties, and a rich layer of sintering aid on the surface to enhance processability and mechanical properties.

Benefits of technology

The silicon nitride sintered body maintains mechanical properties while improving workability, ensuring a good product life and reducing processing time and costs, particularly in bearing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018924_28112024_PF_FP_ABST
    Figure JP2024018924_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a silicon nitride sintered body having both workability and favorable mechanical characteristics; a machine part using the same; and a bearing. This silicon nitride sintered body has a Vickers hardness of 1,220-1,400 Hv, the maximum diameter of holes in a surface layer part that is a region within 2 mm from the surface of the silicon nitride sintered body is at most 30 μm, the silicon nitride sintered body has a degree of crystallinity of 75-90% and contains a rare-earth element and an aluminum element, the content of the rare-earth element is 6-13 wt%, in terms of oxide, with respect to the total weight of the silicon nitride sintered body, and the content of the aluminum element is 6-13 wt%, in terms of oxide, with respect to the total weight of the silicon nitride sintered body.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride sintered body, mechanical parts using same, and bearings

[0001] The present invention relates to a silicon nitride sintered body, and a machine part and a bearing using the same.

[0002] Silicon nitride (Si 3 N 4 Because silicon nitride sintered bodies have excellent mechanical properties, thermal conductivity, and electrical insulation, they are increasingly being used in bearing components, engine parts, tool materials, and heat dissipation substrate materials. Silicon nitride sintered bodies are known to be produced using silicon nitride powder as a starting material. Because silicon nitride powder is difficult to sinter, sintering aids are used together with the silicon nitride powder to produce densified silicon nitride sintered bodies. Common examples of such sintering aids include oxides of rare earth elements, aluminum oxide, magnesium oxide, and silicon oxide.

[0003] Because silicon nitride powder is expensive, producing a silicon nitride sintered body using silicon nitride powder tends to increase the price of the silicon nitride sintered body. Therefore, a manufacturing method using silicon powder (metallic silicon powder), which is less expensive than silicon nitride powder, as a starting material and then reactively sintering it to produce a silicon nitride sintered body has attracted attention (e.g., Patent Documents 1 to 3). One such manufacturing method is known as the PS-RBSN (Post-Sintering of Reaction Bonded Silicon-Nitride) method. The PS-RBSN method includes a first step of nitriding a compact formed from silicon powder by heat treatment at a temperature of, for example, about 1100°C to 1450°C in a nitrogen gas-containing environment, and a second step of densifying the nitride obtained in the first step by heat treatment at a temperature of, for example, about 1600°C to 1950°C.

[0004] JP 2004-149328 A JP 2008-247716 A JP 2013-49595 A JP 2019-036695 A JP 2021-95317 A

[0005] While silicon nitride sintered bodies have excellent mechanical properties, they are difficult to process due to their extremely high hardness (the Vickers hardness of typical silicon nitride sintered bodies is approximately 1400 to 1500 Hv). This increases the processing time and may result in higher costs. For example, a technology has been proposed to improve processability by adjusting the concentration of the processing fluid (Patent Document 4), but concentration control is difficult, making stable processing difficult. On the other hand, lowering hardness to improve processability also reduces wear resistance (see Patent Document 5). Therefore, using silicon nitride sintered bodies in bearing components, etc., may lead to a shortened product life.

[0006] The present invention has been made in view of the above circumstances, and has as its object to provide a silicon nitride sintered body that combines workability with good mechanical properties, and a mechanical part and a bearing that use the same.

[0007] The silicon nitride sintered body according to one embodiment of the present invention is characterized in that it has a Vickers hardness of 1220 Hv or more and 1400 Hv or less, and that the maximum diameter of pores in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body, is 30 μm or less. Note that the silicon nitride sintered body also includes a form in which there are no pores in the surface layer.

[0008] The silicon nitride sintered body is characterized by having a crystallinity of 75% or more and 90% or less.

[0009] The silicon nitride sintered body contains a rare earth element and an aluminum element, and the content of the rare earth element is 6% by weight or more and 13% by weight or less, calculated as oxide, relative to the total weight of the silicon nitride sintered body, and the content of the aluminum element is 6% by weight or more and 13% by weight or less, calculated as oxide, relative to the total weight of the silicon nitride sintered body.

[0010] The total content of the rare earth element and the aluminum element is 15% by weight or more and 26% by weight or less in terms of oxides relative to the total weight of the silicon nitride sintered body.

[0011] The rare earth element is characterized by including at least one element selected from the group consisting of Y, Ce, Nd, and Eu.

[0012] The silicon nitride sintered body has a Vickers hardness of 1250 Hv or more and 1320 Hv or less, a crystallinity of 75% or more and 85% or less, contains a rare earth element and an aluminum element, and does not contain a transition metal element, the content of the rare earth element being 7.5% to 13% by weight, calculated as oxide, relative to the total weight of the silicon nitride sintered body, the content of the aluminum element being 7.5% to 13% by weight, calculated as oxide, relative to the total weight of the silicon nitride sintered body, the total content of the rare earth element and the aluminum element being 15% to 26% by weight, calculated as oxide, relative to the total weight of the silicon nitride sintered body, and the rare earth element being Y or Ce.

[0013] A machine component of the present invention is characterized by using the silicon nitride sintered body according to one aspect of the present invention. The machine component is characterized by being a rolling element.

[0014] The bearing of the present invention is characterized by using the above rolling elements.

[0015] Another embodiment of the present invention provides a silicon nitride sintered body containing a sintering aid component including a rare earth element and an aluminum element, characterized in that the surface layer contains more of the sintering aid component than the central portion, and the ratio of the sintering aid component in the surface layer to the central portion (also simply referred to as the component ratio) is 1.10 or more and less than 1.40. In this embodiment, the "surface layer" refers to the region of the silicon nitride sintered body from the surface to a depth of 0.25 mm, and the "central portion" refers to the region other than the surface layer.

[0016] A rich layer containing a large amount of the sintering aid component is formed on the surface layer, and the depth of the rich layer from the surface of the silicon nitride sintered body is 0.12 mm or more and less than 0.19 mm.

[0017] The content of the rare earth element is 6% by weight or more and 15% by weight or less, calculated as oxide, relative to the total weight of the silicon nitride sintered body, and the content of the aluminum element is 6% by weight or more and 15% by weight or less, calculated as oxide, relative to the total weight of the silicon nitride sintered body.

[0018] The total content of the rare earth element and the aluminum element is 18% by weight or more and 22% by weight or less in terms of oxides relative to the total weight of the silicon nitride sintered body.

[0019] The rare earth element is Ce, and the silicon nitride sintered body is characterized in that it does not contain any transition metal elements.

[0020] a rich layer containing a large amount of the sintering aid component is formed on the surface layer, the rich layer has a depth from the surface of the silicon nitride sintered body of 0.12 mm or more and less than 0.19 mm; the content of the rare earth element is 6 to 15 wt % inclusive, calculated as oxide, relative to the total weight of the silicon nitride sintered body; the content of the aluminum element is 6 to 15 wt % inclusive, calculated as oxide, relative to the total weight of the silicon nitride sintered body; the total content of the rare earth element and the aluminum element is 18 to 22 wt % inclusive, calculated as oxide, relative to the total weight of the silicon nitride sintered body; the rare earth element is Ce; and the silicon nitride sintered body does not contain a transition metal element.

[0021] A machine part of the present invention is a polished product of the silicon nitride sintered body of another embodiment of the present invention. The machine part is also characterized in that it is a rolling element.

[0022] The bearing of the present invention is characterized by using the above rolling elements.

[0023] According to one embodiment of the present invention, by specifying the maximum pore size (and further the crystallinity) while maintaining a low Vickers hardness of the silicon nitride sintered body, it is possible to achieve both processability and good mechanical properties, and when processed into products such as bearing members, a good product life can be achieved.

[0024] In another embodiment of the silicon nitride sintered body of the present invention, the surface layer contains more sintering aid components than the center portion, and the ratio of the sintering aid components in the surface layer to the center portion is 1.10 or more but less than 1.40, so that, for example, a sintering aid-rich layer is formed in the surface layer, which can achieve both workability and good mechanical properties. As a result, when processed into products such as bearing members, a good product life can be achieved.

[0025] Fig. 1 is a longitudinal sectional view showing an example of a bearing of the present invention. Fig. 2 is a longitudinal sectional view showing another example of a bearing of the present invention. Fig. 3 is a longitudinal sectional view showing another example of a bearing of the present invention. Fig. 4 is an image showing the surface layer and the center portion that were the measurement targets in a test example. Fig. 5 is a diagram showing an outline of a crushing test.

[0026] One embodiment of the present invention will be described below. (Silicon nitride sintered body) The silicon nitride sintered body of this embodiment is mainly composed of a crystalline phase of silicon nitride and contains an appropriate amount of a glass phase (amorphous phase) made of a sintering aid, etc. The sintering aid, etc. will be described later.

[0027] The silicon nitride sintered body of this embodiment has a Vickers hardness of 1220 Hv or more and 1400 Hv or less. By setting the Vickers hardness to 1400 Hv or less, which is lower than that of ordinary silicon nitride sintered bodies, workability is improved. Furthermore, by setting the Vickers hardness to 1220 Hv or more, mechanical properties such as wear resistance are ensured.

[0028] In this embodiment, the Vickers hardness is preferably 1250 Hv or more, and may be 1280 Hv or more. From the viewpoint of processability, the Vickers hardness is preferably 1350 Hv or less, and may be 1320 Hv or less. The Vickers hardness is measured by the method described in the examples below.

[0029] Furthermore, in the silicon nitride sintered body of this embodiment, the maximum diameter of the pores in the surface layer, which is a region within 2 mm from the surface, is 30 μm or less. The maximum diameter of the pores may be 25 μm or less, or in this embodiment, the body may not have any pores. By having a maximum diameter of pores of 30 μm or less, it is possible to maintain mechanical properties while maintaining low hardness, and when the silicon nitride sintered body is processed into products such as bearing rolling elements, it is possible to obtain a good product life. The pores in the surface layer refer to those present in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body, and refer to pores present entirely in the surface layer. The maximum diameter of the pores in the surface layer refers to the diameter of the largest pore among the pores present in the surface layer. When producing a silicon nitride sintered body, the maximum diameter of the pores can be adjusted by adjusting the content of the base material (silicon nitride or silicon) used as a raw material and / or the amount of sintering aid added.

[0030] The maximum diameter of pores is a value measured for pores that are entirely present in the surface layer portion in the cross section of a test piece prepared by the method described in the Examples below. The maximum diameter of pores can be calculated by the method described in the Examples below.

[0031] The silicon nitride sintered body may also have inclusions (I) in the surface layer, which is a region within 2 mm from the surface. The inclusions (I) contain components other than silicon nitride, such as inclusions (It) containing transition metal elements and inclusions (Is) containing non-nitrided silicon elements. The inclusions (It) are derived from, for example, a sintering aid containing a transition metal element (usually an oxide of a transition metal element) used in the production of the silicon nitride sintered body, such as a silicide of a transition metal element. The inclusions (Is) are, for example, aggregates of non-nitrided silicon elements, and it is preferable that the inclusions (Is) are not included or that their presence ratio is low. The inclusions refer to those that are entirely present in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body.

[0032] The silicon nitride sintered body preferably does not contain a transition metal element. In other words, in this case, the silicon nitride sintered body does not have inclusions (It). The transition metal element is an element contained in Groups 3 to 11 of the IUPAC Periodic Table, such as Fe, Ti, Cr, and Mn.

[0033] The silicon nitride sintered body of this embodiment preferably has a crystallinity of 75% or more and 90% or less. Here, the crystallinity of the silicon nitride sintered body means the ratio of the crystalline phase to all components constituting the silicon nitride sintered body, and is calculated from the XRD diffraction pattern of a mirror-polished cut surface of the silicon nitride sintered body using the following formula: Crystallinity (%) = crystalline peak area / (crystalline peak area + amorphous peak area) × 100

[0034] Specifically, the crystallinity of a silicon nitride sintered body is the "peak area of ​​crystalline silicon nitride and other crystalline components in the XRD diffraction pattern" divided by the "sum of the peak areas of all components constituting the sintered body in the XRD diffraction pattern." Here, crystalline silicon nitride is crystalline silicon nitride having an α-, β-, or γ-type crystal structure. Furthermore, all components constituting the sintered body include, for example, silicon, silicon nitride, and components derived from sintering aids that promote sintering during heat treatment in producing silicon nitride.

[0035] When a silicon nitride sintered body is produced using silicon powder and a sintering aid, for example, by the PS-RBSN method (two-stage sintering method), the sintering aid becomes the main component of the amorphous phase in the sintered body under certain conditions. The PS-RBSN method is a two-stage sintering method that includes a silicon nitriding step and a subsequent sintering step. For example, when a compact made of silicon powder and a sintering aid is heat-treated in a nitrogen atmosphere by the PS-RBSN method, the silicon is completely nitrided and all of the sintering aid is amorphous. The crystallinity is calculated as follows: "peak area of ​​crystalline silicon nitride in the XRD diffraction pattern" / "sum of the peak areas of all components constituting the sintered body in the XRD diffraction pattern." Furthermore, when the silicon is completely nitrided and a portion of the sintering aid is crystalline, the crystallinity is calculated as "peak area of ​​crystalline components derived from crystalline silicon nitride and the sintering aid in the XRD diffraction pattern" / "sum of the peak areas of all components constituting the sintered body in the XRD diffraction pattern."

[0036] The raw material for the silicon nitride sintered body may be silicon nitride powder alone, silicon powder, or silicon powder and a sintering aid. The raw material and manufacturing method for the silicon nitride sintered body may be any raw material as long as a silicon nitride sintered body is obtained, and the manufacturing method is not limited to the PS-RBSN method. The atmospheric gas used during the heat treatment may be nitrogen gas, or a mixture of nitrogen gas with hydrogen gas or argon gas.

[0037] The crystallinity of the silicon nitride sintered body may be 78% or more, or 81% or more. The crystallinity may be 87% or less, or 85% or less. By having the crystallinity of the silicon nitride sintered body in the range of 75% to 90%, it is possible to easily maintain mechanical properties while maintaining low hardness, and when the silicon nitride sintered body is processed into products such as rolling elements of bearings, it is easy to obtain a good product life.

[0038] The silicon nitride sintered body of this embodiment may contain a rare earth element and / or an aluminum element. When the silicon nitride sintered body contains a rare earth element, the content of the rare earth element is preferably 6 to 13 wt % in terms of oxide relative to the total weight of the silicon nitride sintered body. When the silicon nitride sintered body contains an aluminum element, the content of the aluminum element is preferably 6 to 13 wt % in terms of oxide relative to the total weight of the silicon nitride sintered body.

[0039] Examples of rare earth elements include yttrium (Y), lanthanum (La), cerium (Ce), samarium (Sm), neodymium (Nd), dysprosium (Dy), europium (Eu), erbium (Er), etc. Among these, yttrium (Y), cerium (Ce), neodymium (Nd), and europium (Eu) are preferred.

[0040] The silicon nitride sintered body preferably contains a rare earth element in the amorphous phase, more preferably one or more elements selected from the group consisting of Y, Ce, Nd, and Eu. The silicon nitride sintered body may also contain a rare earth element in the crystalline phase.

[0041] The content of the rare earth element is more preferably 6.5 wt% or more, or may be 7.0 wt% or more, or may be 7.5 wt% or more, calculated as oxide, relative to the total weight of the silicon nitride sintered body. The content of the rare earth element is more preferably 12.5 wt% or less, or may be 11.5 wt% or less, or may be 10.5 wt% or less.

[0042] The aluminum content is preferably 6.5 wt% or more, or may be 7.0 wt% or more, or may be 7.5 wt% or more, calculated as oxide, relative to the total weight of the silicon nitride sintered body. The aluminum content is more preferably 12.5 wt% or less, or may be 11.5 wt% or less, or may be 10.5 wt% or less. When the silicon nitride sintered body contains a rare earth element and an aluminum element, the aluminum content (in oxide terms) may be within ±5 wt%, ±2 wt%, or ±1 wt% of the rare earth element content (in oxide terms), or may be the same as the rare earth element content.

[0043] By ensuring that the rare earth element and aluminum element contents in the silicon nitride sintered body are within the above ranges, when producing a silicon nitride sintered body by the PS-RBSN method, the nitriding reaction of the raw material silicon powder (metallic silicon powder) can be promoted, and the subsequent sintering can be promoted, making it easier to achieve the Vickers hardness, maximum pore diameter, and crystallinity of the silicon nitride sintered body within the desired ranges. The rare earth element and aluminum element contents can be adjusted by the amount of sintering aid containing a rare earth element (e.g., a rare earth element oxide) or a sintering aid containing an aluminum element (e.g., aluminum oxide) added to the raw material.

[0044] The total content of the rare earth element and aluminum element is preferably 15% by weight or more and 26% by weight or less in terms of oxides based on the total weight of the silicon nitride sintered body.

[0045] The above contents of rare earth elements and aluminum elements may be determined using an X-ray fluorescence analyzer (XRF), an energy dispersive X-ray analyzer (EDX), or an inductively coupled plasma (ICP) optical emission analyzer. Specifically, the contents of rare earth elements and aluminum elements in the silicon nitride sintered body are determined using the above analyzer, and the oxides of rare earth elements (RE) (RE 2 O 3 or REO 2 ) and aluminum oxide (Al 2 O 3The elements of the other components constituting the silicon nitride sintered body are also analyzed using the above-mentioned analyzer, and the total weight of the silicon nitride sintered body is calculated to determine the above-mentioned contents of rare earth elements and aluminum element. When silicon (metal silicon powder) is contained in the raw material powder used to manufacture the silicon nitride sintered body, and the silicon is nitrided to Si 3 N 4 In this case, the Si content in the silicon nitride sintered body is 3 N 4 The weight of the rare earth element oxide and aluminum oxide is 1.67 times the weight of silicon. Therefore, by taking into account the weight change when silicon is nitrided, the contents of the rare earth element oxide and aluminum oxide can be calculated from the composition of the raw material powder.

[0046] A particularly preferred embodiment of the silicon nitride sintered body of this embodiment is a silicon nitride sintered body containing rare earth elements and aluminum elements but not containing transition metal elements, having a Vickers hardness of 1250 Hv to 1320 Hv, a maximum diameter of pores in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body, of 30 μm or less, a crystallinity of 75% to 85%, and containing one or more elements selected from the group consisting of Y, Ce, Nd, and Eu in the amorphous phase, the content of rare earth elements being 6% to 13% by weight, calculated as oxides, relative to the total weight of the silicon nitride sintered body, and the content of aluminum elements being 6% to 13% by weight, calculated as oxides, relative to the total weight of the silicon nitride sintered body. Furthermore, it is preferable that the total content of rare earth elements and aluminum elements be 15% to 26% by weight, calculated as oxides, relative to the total weight of the silicon nitride sintered body. Furthermore, the above-mentioned numerical ranges can be appropriately combined with the above-mentioned embodiment.

[0047] The shape of the silicon nitride sintered body of this embodiment is not particularly limited, and may be selected appropriately depending on the application from spherical, cylindrical, conical, truncated conical, rectangular parallelepiped, etc., but spherical is preferable. The size of the silicon nitride sintered body is also not particularly limited, and for example, if it is spherical, the diameter can be 0.5 cm to 10 cm, and if it is cylindrical, the base diameter can be 0.5 cm to 15 cm and the height can be 3 cm to 20 cm.

[0048] (Production of Silicon Nitride Sintered Body) A method for producing a silicon nitride sintered body generally includes a mixing step of mixing a raw material powder containing silicon nitride powder or silicon powder and a sintering aid, a molding step of molding the mixed raw material powder into a green compact, and a sintering step of sintering the green compact. After the sintering step, the silicon nitride sintered body may be polished, if necessary. The silicon nitride sintered body in this embodiment preferably contains silicon powder as a raw material and uses the PS-RBSN method (two-stage sintering method) for the sintering step.

[0049] In the mixing step, for example, the raw material powders are mixed dry without using water or an organic solvent. In this case, it is preferable to mix without using a binder component. The particle size of the powder after mixing is not particularly limited, but it is preferable that D90 is 10 μm or more and 100 μm or less. It is also preferable that D50 is 2 μm or more and 10 μm or less. By having D90 and / or D50 within the above range, a dense silicon nitride sintered body can be obtained while exhibiting good fluidity and moldability. Note that D50 and D90 are the cumulative 50% diameter and cumulative 90% diameter on a volume basis, respectively, and can be obtained by laser diffraction / scattering particle size distribution measurement, etc.

[0050] Alternatively, wet granulation may be performed in the mixing step to obtain a granulated powder as a mixture. In this case, the raw material powder and binder component are mixed with water and / or an organic solvent (e.g., ethanol) to form a slurry, which is then spray-dried and granulated to obtain a granulated powder. An organic binder or the like is used as the binder component, and is added in an amount of, for example, 1% by weight to 10% by weight based on the total raw material powder.

[0051] In the molding step, the mixture obtained in the mixing step is molded into a predetermined shape by a known molding method such as CIP (cold isostatic pressing) or press molding to obtain a green compact. For example, in the case of a spherical shape, a spherical green compact is formed by press molding such as cold isostatic pressing, and then the green compact is processed in a green processing device to obtain a green sphere.

[0052] The sintering process involves, for example, heating the resulting green compact in a nitrogen atmosphere from a temperature in the range of, for example, 800°C to 1200°C to the sintering temperature at a predetermined heating rate, and then holding the temperature for a predetermined time (for example, 5 to 8 hours) to perform heat treatment to sinter it. By heating the green compact without holding it at the predetermined temperature before sintering it at the sintering temperature, manufacturing efficiency can be improved. The heating rate is, for example, 2.0°C / min or more but less than 10°C / min, preferably 2.0°C / min or more but less than 5.0°C / min, and may be 2.0°C / min or more but 4.0°C / min or less. The sintering temperature is, for example, 1600°C to 1950°C, preferably 1600°C to 1800°C, and more preferably 1650°C to 1750°C. By raising the temperature relatively slowly and controlling the nitriding rate of silicon, it becomes easier to densify the sintered body, reduce the surface hardness, and reduce the maximum diameter of the pores present in the surface layer. It also becomes easier to achieve the desired degree of crystallinity.

[0053] In the production of the silicon nitride sintered body, the sintering aid used in the raw material powder may contain a rare earth element, an aluminum element, or a transition metal element. 2 O 3 , CeO 2 , Nd 2 O 3 , and Eu 2 O 3 As the sintering aid containing aluminum, Al 2 O 3 In addition, the sintering aid containing a transition metal element preferably contains Cr. 2 O 3 , TiO 2 , MnO, Fe 2 O 3 Examples include:

[0054] The raw material powder may contain, in addition to silicon powder and a sintering aid, silicon nitride powder and / or an organic binder, and may also contain a sintering aid containing an element other than a rare earth element, an aluminum element, and a transition metal element.

[0055] The content of silicon powder contained in the raw material powder is preferably 65% ​​by weight or more, more preferably 67% by weight or more, and even more preferably 69% by weight or more, based on the total weight of silicon powder, silicon nitride powder, and sintering aid, and may be 71% by weight or more, preferably 80% by weight or less, and may be 78% by weight or less, or may be 76% by weight or less. The raw material powder may or may not contain silicon nitride powder.

[0056] The content of the sintering aid containing a rare earth element (e.g., an oxide of a rare earth element) contained in the raw material powder is preferably 10 wt% or more, more preferably 11 wt% or more, even more preferably 12 wt% or more, and may be 13 wt% or more, relative to the total weight. The content of the rare earth element may be 17.5 wt% or less, may be 16.5 wt% or less, or may be 15.5 wt% or less. The content of the sintering aid containing an aluminum element (e.g., aluminum oxide) contained in the raw material powder is preferably 10 wt% or more, more preferably 11 wt% or more, even more preferably 12 wt% or more, and may be 13 wt% or more, relative to the total weight. The content of the aluminum element may be 17.5 wt% or less, may be 16.5 wt% or less, or may be 15.5 wt% or less. If the content of the sintering aid contained in the raw material powder is low, it is difficult to obtain a dense silicon nitride sintered body, and if the content of the sintering aid is high, the mechanical properties of the silicon nitride sintered body are likely to deteriorate.

[0057] The average particle size of the silicon powder contained in the raw material powder can be, for example, 5 μm or less. When silicon nitride is contained, its average particle size can be, for example, 0.5 μm or less. The average particle size of the sintering aid depends on the type of sintering aid, but is preferably 10 μm or less, and may be 7 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, or 0.4 μm or less. The average particle size is the cumulative 50% diameter on a volume basis, and can be obtained by laser diffraction / scattering particle size distribution measurement, etc.

[0058] The method for producing silicon nitride sintered bodies of this embodiment includes a mixing step of mixing raw material powder containing silicon powder and a sintering aid, a molding step of molding the mixed raw material powder into a powder compact, and a sintering step of sintering the powder compact. The sintering step is a heat treatment step in which the temperature is increased to a sintering temperature at a predetermined rate in a nitrogen atmosphere and then maintained at that sintering temperature for a predetermined period of time. The heating rate is preferably 2.0°C / min or more and less than 5.0°C / min. The sintering temperature is more preferably 1600°C to 1800°C. The sintering aid preferably contains a rare earth oxide and aluminum oxide but does not contain a transition metal oxide. The raw material powder preferably contains 9.5% by weight to 17% by weight of the rare earth oxide and 9.5% by weight to 17% by weight of the aluminum oxide. The above-mentioned numerical ranges can be appropriately combined with the above method.

[0059] Other embodiments are described below. (Other embodiments) Silicon nitride sintered bodies of other embodiments are mainly composed of a crystalline silicon nitride phase and contain an appropriate amount of a glass phase (amorphous phase) composed of a sintering aid containing a rare earth element and an aluminum element. The silicon nitride sintered bodies in question are those whose surfaces have not been polished after sintering.

[0060] In other forms of silicon nitride sintered bodies, for example, the surface layer of the silicon nitride sintered body contains more sintering aid components than the center. This silicon nitride sintered body is obtained by sintering a green compact obtained by pressing raw material powder containing sintering aids. It is thought that the sintering aids become liquid during sintering and are pushed out to the surface layer, resulting in the uneven distribution of the sintering aid components.

[0061] In particular, this embodiment is characterized in that the ratio of the sintering aid component in the surface layer to the center portion is 1.10 or more and less than 1.40. By making the component ratio 1.10 or more and allowing a large amount of the sintering aid component to be present in the surface layer, processability such as polishing is improved. Furthermore, by making the component ratio less than 1.40, it is easier to ensure the mechanical properties of the finished product after processing. This component ratio can be calculated using the method in the examples described below. The component ratio is preferably 1.20 or more, and may be 1.25 or more. Furthermore, from the viewpoint of mechanical properties after processing, it may be 1.35 or less.

[0062] A rich layer containing a higher amount of sintering aid components than other portions is formed on the surface of the silicon nitride sintered body. The rich layer is formed so as to cover the entire surface of the silicon sintered body. The rich layer contains more sintering aid components than the center portion and is formed as a thick layer from the surface. It can be observed using a scanning electron microscope. The depth of the rich layer from the surface of the silicon nitride sintered body is not particularly limited, but if it is too thick, it may be difficult to remove by polishing and may tend to remain on the surface of the finished product. This may lead to a decrease in strength and bearing characteristics. Therefore, the depth of the rich layer from the surface of the silicon nitride sintered body is preferably less than 0.25 mm, more preferably less than 0.19 mm, or even less than 0.16 mm. Furthermore, from the viewpoint of processability, the depth of the rich layer from the surface is preferably 0.10 mm or more, more preferably 0.12 mm or more. The depth of this rich layer can be calculated using the method described in the Examples below.

[0063] In the production of finished products, the rich layer of the silicon nitride sintered body is basically removed by polishing. By using the above-mentioned silicon nitride sintered body, for example, the processing rate is increased, which shortens the processing time and also reduces wear of the grinding stone. As a result, finished products can be produced at low cost.

[0064] Another form of silicon nitride sintered body contains a rare earth element and an aluminum element. In the silicon nitride sintered body, the content of the rare earth element is preferably 6 to 15 wt % in terms of oxide, relative to the total weight of the silicon nitride sintered body, and the content of the aluminum element is preferably 6 to 15 wt % in terms of oxide, relative to the total weight of the silicon nitride sintered body.

[0065] Examples of rare earth elements include yttrium (Y), lanthanum (La), cerium (Ce), samarium (Sm), neodymium (Nd), dysprosium (Dy), europium (Eu), erbium (Er), etc. Among these, it is preferable to contain one or more elements selected from the group consisting of Y, Ce, and La, and it is more preferable to contain Ce because it can promote nitriding even at a relatively low sintering temperature.

[0066] The content of the rare earth element is more preferably 6.5 wt % or more, and may be 7 wt % or more, calculated as oxide, relative to the total weight of the silicon nitride sintered body. The content of the rare earth element is more preferably 14 wt % or less, and may be 12 wt % or less.

[0067] The aluminum content is more preferably 6.5 wt % or more, and may be 7 wt % or more, calculated as oxide, relative to the total weight of the silicon nitride sintered body. The aluminum content is more preferably 14 wt % or less, and may be 12 wt % or less.

[0068] The aluminum element content (in terms of oxide) relative to the rare earth element content (in terms of oxide) may be contained at a ratio of 1:3 to 3:1, or may be contained at a ratio of 1:2 to 2:1. Furthermore, the aluminum element content (in terms of oxide) may be within ±5 wt % of the rare earth element content (in terms of oxide), ±2 wt % or ±1 wt %, or may be the same as the rare earth element content.

[0069] By having the rare earth element and aluminum element contents in the silicon nitride sintered body within the above ranges, for example, when producing a silicon nitride sintered body by the PS-RBSN method, the nitriding reaction of the raw material silicon powder (metallic silicon powder) can be promoted, and the subsequent sintering can be promoted, making it easier to achieve the component ratio of the sintering aid in the surface layer and the center of the silicon nitride sintered body, and the depth of the rich layer within the desired range. The rare earth element and aluminum element contents can be adjusted by the amount of sintering aid containing a rare earth element (e.g., oxide of a rare earth element) or sintering aid containing an aluminum element (e.g., aluminum oxide) added to the raw material.

[0070] The total content of the rare earth element and aluminum element, calculated as oxides, relative to the total weight of the silicon nitride sintered body, is, for example, 15% by weight or more and 26% by weight or less, and preferably 18% by weight or more and 22% by weight or less.

[0071] The silicon nitride sintered body preferably does not contain a transition metal element, which is an element contained in Groups 3 to 11 of the IUPAC periodic table, such as Fe, Ti, Cr, and Mn.

[0072] The silicon nitride sintered body of the other form described above is preferably produced by the PS-RBSN method (two-stage sintering method). The method for producing the silicon nitride sintered body includes a mixing step of mixing raw material powder containing silicon powder and a sintering aid, a molding step of molding the mixed raw material powder into a powder compact, and a sintering step of sintering the powder compact. The mixing step and molding step can be appropriately adopted from the details described above.

[0073] In the sintering step, the obtained green compact is sintered by heat treatment in a nitrogen atmosphere, for example, at 1600°C to 1800°C (preferably 1600°C to 1700°C, more preferably 1600°C to 1650°C), for a predetermined time. The sintering time is set, for example, to 3 hours to 10 hours. Applicable sintering methods include atmospheric pressure sintering, atmospheric pressure sintering, and pressure sintering (hot pressing). In atmospheric pressure sintering, the pressure is set, for example, to 0.1 MPa to 10 MPa. Furthermore, in the sintering step, primary sintering and secondary sintering may be performed under different pressures.

[0074] In the production of the silicon nitride sintered body, the sintering aid used in the raw material powder may contain a rare earth element, an aluminum element, or a transition metal element. 2 O 3 , CeO 2 , and La 2 O 3 It is preferable to use any one of CeO 2 It is more preferable to use Al as the sintering aid containing aluminum. 2 O 3 In addition, the sintering aid containing a transition metal element preferably contains Cr. 2 O 3 , TiO 2 , MnO, Fe 2 O 3 Examples include:

[0075] The raw material powder may contain silicon nitride powder and / or an organic binder in addition to silicon powder and a sintering aid, and may contain a sintering aid containing an element other than a rare earth element, an aluminum element, and a transition metal element. The average particle size of the silicon powder and silicon nitride can be appropriately selected from the above-mentioned average particle sizes.

[0076] The content of silicon powder contained in the raw material powder is preferably more than 60 wt%, more preferably 65 wt% or more, and may be 70 wt% or more, based on the total weight of silicon powder, silicon nitride powder, and sintering aid. It is also preferably less than 85 wt%, more preferably 80 wt% or less. It is preferable that the raw material powder does not contain silicon nitride powder.

[0077] The content of the sintering aid containing a rare earth element (e.g., an oxide of a rare earth element) contained in the raw material powder is preferably 10 wt % or more, and may be 15 wt % or more, or 20 wt % or less, relative to the total weight. The content of the sintering aid containing an aluminum element (e.g., aluminum oxide) contained in the raw material powder is preferably 10 wt % or more, and may be 15 wt % or more, or 20 wt % or less, relative to the total weight. If the content of the sintering aid contained in the raw material powder is low, it is difficult to obtain a dense silicon nitride sintered body, and if the content of the sintering aid is high, the mechanical properties of the silicon nitride sintered body are likely to deteriorate.

[0078] Another method for producing a silicon nitride sintered body includes a mixing step of mixing silicon powder with a raw material powder containing a sintering aid containing a rare earth oxide and aluminum oxide, a molding step of molding the mixed raw material powder into a green compact, and a sintering step of sintering the green compact, and the sintering step is preferably a heat treatment step in which the mixture is held for a predetermined time in a nitrogen atmosphere at a sintering temperature of 1600°C to 1700°C. For example, by using a predetermined amount of sintering aid and sintering at a relatively low sintering temperature (e.g., 1600°C to 1700°C), it becomes easier to adjust the ratio of the sintering aid component, described below, to the desired range.

[0079] Furthermore, the rare earth oxide is CeO 2 Preferably, the raw material powder contains the rare earth oxide and the aluminum oxide in a total amount of 20% by weight or more and 35% by weight or less (more preferably 25% by weight or more and 35% by weight or less) based on the total amount of the raw material powder. Preferably, the raw material powder does not contain a transition metal oxide. The above-mentioned numerical ranges can be appropriately combined with the above method.

[0080] (Uses of Silicon Nitride Sintered Body) The silicon nitride sintered body of each of the above-described forms is polished to meet predetermined product specifications, for example, to obtain a silicon nitride sintered body product. While the use of the product is not particularly limited, due to its excellent mechanical properties, it is preferably used as a mechanical part. Mechanical parts are used, for example, in rolling or sliding parts. The mechanical part of the present invention is a part that uses the silicon nitride sintered body or polished product of the present invention in part or in its entirety. Examples of mechanical parts include sliding members, bearing members, rolling roll materials, compressor vanes, gas turbine blades and other engine parts, cutting tools (chips), etc. Examples of bearing members include raceways such as inner and outer rings, rolling elements for bearings, and cages. The bearing of the present invention is a bearing that includes this mechanical part as part or in its entirety, and examples thereof include rolling bearings, sliding bearings (such as spherical bushings), linear guide bearings, ball screws, linear bearings, etc. In particular, the bearing of the present invention is preferably a rolling bearing using the above silicon nitride sintered body or polished product as the rolling elements for the bearing.

[0081] An example of a bearing according to this embodiment will be described with reference to FIG. 1 . FIG. 1 is a cross-sectional view of a deep groove ball bearing. The rolling bearing 1 comprises an inner ring 2 having an inner ring raceway surface 2a on its outer peripheral surface and an outer ring 3 having an outer ring raceway surface 3a on its inner peripheral surface, which are concentrically arranged. A plurality of balls (rolling elements) 4 are disposed between the inner ring raceway surface 2a and the outer ring raceway surface 3a. These balls 4 are formed of the silicon nitride sintered body described above. The balls 4 are held in place by a cage 5. Openings 8a, 8b at both axial ends of the inner and outer rings are sealed by sealing members 6, and a grease composition 7 is enclosed around at least the balls 4. The grease composition 7 is interposed between the raceway surfaces of the balls 4 and provides lubrication. The type of rolling bearing is not limited to a deep groove ball bearing, and may be an angular contact ball bearing, a thrust ball bearing, or the like.

[0082] Another example of the bearing of this embodiment will be described with reference to FIG. 2 . FIG. 2 is a cross-sectional view of a ball screw. As shown in FIG. 2 , the ball screw has a plurality of balls 15 interposed between a screw groove 12 formed on the outer peripheral surface of a screw shaft 11, which serves as a guide member, and a screw groove 14 formed on the inner peripheral surface of a ball nut 13. The rotational power of the screw shaft 11 (or ball nut 13) is transmitted to the ball nut 13 (or screw shaft 11) via the balls 15, causing the ball nut 13 to move in the axial direction. In FIG. 2 , the balls 15 are formed of the silicon nitride sintered body described above, and the screw shaft 11 and ball nut 13 are formed of steel (e.g., bearing steel or low-carbon steel). A grease composition is filled around the balls 15 between the screw shaft 11 and the ball nut 13, and the ball screw seal member 16 seals the balls 15.

[0083] In the ball screw shown in Figure 2, the ball circulation system is not particularly limited, and any circulation system can be used, such as a tube system, a return tube (pipe) system, a deflector system, an end deflector system, an end cap system, a top system, etc. In any circulation system, the circulation path has a significant effect on the smooth circulation of the balls.

[0084] Specifically, ball screws are used to convert the rotational motion of a motor into linear motion, and can be suitably used in, for example, electric actuators, positioning devices, electric jacks, servo cylinders, electric servo presses, mechanical presses, electric brake devices, transmissions, electric power steering devices, electric injection molding machines, and the like.

[0085] Here, ball screws are required to have wear resistance, toughness, high load capacity, etc. In recent years, with the trend toward miniaturization, there has been an increasing demand for the ability to withstand high loads, as well as the need to suppress hydrogen embrittlement caused by hydrogen generated from lubricants due to slippage or high loads. In the example of Figure 2, the above-mentioned silicon nitride sintered body is used as the ball, which easily meets these requirements and also provides an excellent product life for the ball.

[0086] Furthermore, in a ball screw, if there is a large misalignment due to installation errors or the like when installing the ball screw, there is a risk of twisting (i.e., relative tilt between the screw shaft and the nut). If a moment caused by twisting acts on the ball screw, the load balance within the nut will be disrupted, resulting in areas where the contact pressure increases, which could shorten the lifespan. In response to this, using the above-mentioned silicon nitride sintered body as the balls can improve the circulation performance of the balls, making it easier to suppress a decrease in lifespan.

[0087] Another example of a bearing according to this embodiment will now be described with reference to Fig. 3. Fig. 3 is a cross-sectional view showing an example of a spherical plain bearing. As shown in Fig. 3, spherical plain bearing 21 comprises an inner ring 22 having a spherical outer peripheral surface 22b and an inner peripheral surface 22a formed with a bearing hole 24 through which a support shaft can be inserted, in combination with an outer ring 23 having a concave surface 23a corresponding to outer peripheral surface 22b. In spherical plain bearing 21, at least one of inner ring 22 and outer ring 23 is formed from the above-mentioned silicon nitride sintered body. The material of the other member is not particularly limited and can be, for example, a metal such as an aluminum alloy, stainless steel, or steel; a synthetic resin; or a ceramic other than the above-mentioned silicon nitride sintered body.

[0088] A spherical plain bearing is a self-aligning plain bearing with a spherical sliding surface that can support radial loads and axial loads in both directions. Spherical plain bearings are suitable for oscillating and aligning motions, and are used in the joints of industrial and construction machinery. Spherical plain bearings can be either oil-free (see Figure 3) or oil-lubricated; for example, in the case of oil-lubricated bearings, the inner and outer rings are provided with oil holes and oil grooves. When installing a spherical plain bearing, grease may be applied to the sliding surfaces.

[0089] The present invention will be explained in more detail below based on examples and comparative examples, but the present invention is not limited to these examples.

[0090] Examples 1 to 7, Comparative Examples 1 and 2 Raw material powders were prepared according to the blending ratios shown in Table 1, and dry-mixed for 48 hours in a ball mill at a rotation speed of 200 rpm using silicon nitride balls as media. Note that the specific surface area of ​​the metallic silicon used as the raw material may be adjusted to suppress melting of the metallic silicon and facilitate the progress of the nitriding reaction.

[0091]

[0092] The resulting mixed powder was molded into a spherical green compact with a diameter of 12 mm by the RIP (Rubber Isostatic Pressing) method. During molding, the shape of the rubber mold may be adjusted to prevent cracking of the green compact due to springback of the rubber mold or air stagnation within the rubber mold. For example, a gap may be provided between the mating surfaces of the upper and lower rubber molds. The resulting green compact was heated in a nitrogen atmosphere (pressure: 0.9 MPa) from 800°C to 1750°C (sintering temperature) at a heating rate of 2.5°C / min, and then held for 6 hours to obtain a silicon nitride sintered body.

[0093] The composition ratios of each oxide in the obtained silicon nitride sintered body were calculated from the composition ratios of the raw material powder, assuming that all of the silicon (metallic silicon) contained in the raw material powder was nitrided and that the weight of silicon nitride was 1.67 times the weight of silicon. The values ​​are shown in Table 2.

[0094]

[0095] The obtained spherical silicon nitride sintered body was subjected to ball polishing to G5 in accordance with JIS B 1563 to prepare spherical test pieces of 3 / 8 inch (diameter 9.525 mm).

[0096] <Calculation of Processing Rate> In the above polishing, polishing was performed using a #200 diamond surface plate until the ball diameter reached 9.625 mm. During this process, the ball dimensions were measured every hour in accordance with JIS B 1501, and the processing rate μm / h was calculated. The results are shown in Table 3.

[0097] <Measurement of maximum diameter of pores> The test pieces obtained in the examples and comparative examples were cut at a cross section passing through their centers, and the cut surface was mirror-polished. The mirror-polished cut surface was photographed using a "VHX5000" manufactured by Keyence Corporation, and the photographed image was analyzed using a "WinRoof" manufactured by Mitani Shoji Co., Ltd. to measure the maximum diameter of pores present in the surface layer, which is a region corresponding to a range within 2 mm from the surface of the spherical test piece. The pore diameter was calculated as the square root of the envelope area of ​​the pores (pore diameter = √ (envelope area of ​​pores)). Surface layers that did not contain pores with a diameter of more than 30 μm were evaluated as "A", and those that did contain pores were evaluated as "B". The pores measured were those that were entirely present in the surface layer. The results are shown in Table 3.

[0098] <Measurement of Vickers Hardness> Using the mirror-polished test piece, the Vickers hardness was measured in accordance with JIS R 1610.

[0099] <Calculation of Crystallinity> The crystallinity of the silicon nitride sintered body was calculated based on the XRD diffraction pattern of the mirror-polished cut surface described above, using the following formula: Crystallinity (%) = crystalline peak area / (crystalline peak area + amorphous peak area) × 100

[0100] <Rolling Contact Fatigue Test> Using the test specimens obtained in the examples and comparative examples, and using "6206" manufactured by NTN Corporation as the bearing outer ring, bearing inner ring, and cage, a rolling contact fatigue test was performed at a rotation speed of 3000 rpm, a load of 1.5 GPa, and a test time of 168 hours to evaluate the product life. The lubricant used was "VG56," an additive-free turbine oil manufactured by JXTG Nippon Oil & Energy Corporation. Test specimens that did not peel within the test time were evaluated as "a," and those that peeled were evaluated as "b." The results are shown in Table 3.

[0101]

[0102] As shown in Table 3, Examples 1 to 7, which have a Vickers hardness of 1220 Hv or more and 1400 Hv or less and a maximum pore diameter of 30 μm or less, have a good processing rate (e.g., 10 μm / h or more), and all rolling fatigue test results were "a," indicating excellent peel resistance. The crystallinity of Examples 1 to 7 was within the range of 75% to 90% (specifically, 76% to 88%). The results of the Examples show that the silicon nitride sintered body of the present invention maintains mechanical properties usable for rolling elements and has a good product life, while also achieving improved processability compared to ordinary silicon nitride sintered bodies.

[0103] [Test Examples 1 to 11] Raw material powders were prepared in the compounding ratios shown in Table 4 and dry-mixed in a ball mill. They were then press-molded at a molding pressure of 30 MPa and then molded into a green compact by cold isostatic pressing (200 MPa). The resulting green compact was held at 1650°C for 10 hours in a nitrogen atmosphere (pressure: 0.9 MPa) and then pressure-sintered to obtain a silicon nitride sintered body.

[0104] [Test Example 12] Raw material powders were prepared according to the compounding ratios shown in Table 4, and a predetermined amount of organic binder was added and wet-mixed in a ball mill. The mixture was then press-molded at a molding pressure of 30 MPa and then compacted into a powder compact by cold isostatic pressing (200 MPa). The resulting powder compact was degreased in a degreasing furnace and then held at 1750°C for 4 hours in a nitrogen atmosphere for atmospheric sintering. The atmospheric sintered compact was then subjected to HIP treatment at 1700°C for 1 hour under a nitrogen pressure of 100 MPa.

[0105]

[0106] The composition ratios of each oxide in the obtained silicon nitride sintered body were calculated from the composition ratios of the raw material powder, assuming that all of the silicon (metallic silicon) contained in the raw material powder was nitrided and that the weight of silicon nitride was 1.67 times the weight of silicon. The values ​​are shown in Table 5.

[0107]

[0108] The silicon nitride sintered bodies produced under each condition were used to evaluate their processing characteristics and various physical properties, and polished silicon nitride sintered bodies (machining allowance: 0.2 to 0.25 mm) were used to evaluate their strength and rolling contact fatigue properties. The evaluation results are summarized in Table 6.

[0109] <Calculation of processing rate> According to JIS B 1563, the ball was polished to G5 to prepare a spherical test piece of 3 / 8 inch (diameter 9.525 mm). In the above polishing, the ball was polished using a #200 diamond surface plate until the diameter of the ball reached 9.625 mm. During this process, the ball dimensions were measured every hour according to JIS B 1501, and the processing rate μm / h was calculated. In this test, a processing rate of 10 μm / h or more was considered to be acceptable.

[0110] <Calculation of Auxiliary Agent Ratio and Depth of Auxiliary Agent-Rich Layer> The silicon nitride sintered body (before polishing) prepared as described above was cut at a cross section passing through its center, and the cut surface was mirror-polished. The mirror-polished cut surface was subjected to component analysis of the surface layer and center using a Hitachi scanning electron microscope. An image of the cut surface and its measurement locations are shown in FIG. 4(a). The surface layer measured was a region within 0.25 mm from the surface, and the center was a predetermined region including the center of the cross section. For component analysis, EDX analysis was performed on both the surface and center using a scanning electron microscope at a magnification of 1000x. Specifically, EDX analysis was performed on the surface layer (region from the surface to a depth of 0.25 mm) toward the center at multiple locations, and the average value of the measured values ​​was used as the surface layer value. Note that component analysis of the surface layer was performed at eight or fewer locations on the silicon nitride sintered body. The center was also measured using the same number of fields, and the average value was used as the center value. Specifically, the central portion was scanned in a predetermined area including the center of the cross section, which corresponds to the scanning range of the surface layer. 2 (or La 2 O 3 ) and Al 2 O 3 The detected amount of the auxiliary component in the surface layer (CeO 2 (or La 2 O 3 ) and Al 2 O 3The total amount of detected serotonin (serotonin) was calculated from the analysis results.

[0111] The depth of the rich layer was measured by element mapping using EDX analysis at a magnification of 500, scanning from the surface in the depth direction, and determining the amount of the auxiliary component detected (CeO 2 (or La 2 O 3 ) and Al 2 O 3 Specifically, a line analysis was performed in a region from the surface to 0.5 mm (e.g., two 500x fields of view), and the depth of the rich layer was determined as the end point of the rich layer at the point where the detection intensity became weak (e.g., below a threshold value (20% from the detection intensity at the surface)).

[0112] Figure 4(b) shows a color chart of an electron probe microanalyzer (EPMA), and Figure 4(c) shows an SEM image. These figures also show that a large amount of auxiliary components are present in the surface layer.

[0113] <Crushing Test> A crushing test was conducted as a strength test. A two-ball crushing test was conducted using the above test specimen. The crushing test conformed to JIS B 1501. As shown in FIG. 5, the testing machine had a fixed jig 31 and a movable jig 32, and the movable jig 32 was moved up and down by a crosshead 33. Conical depressions were formed in the fixed jig 31 and the movable jig 32, and two test balls 34 were set between these depressions. The stroke speed of the crosshead 33 was 1.0 × 10 mm / min. The load at which the test balls 34 were crushed was measured. A crushing strength of 20 kN or more was considered to pass.

[0114] <Rolling Contact Fatigue Test> The rolling contact fatigue test was carried out under the same conditions as the above-mentioned rolling contact fatigue test. Test pieces that did not peel off within the test time were rated as passing.

[0115]

[0116] As shown in Table 6, the processing rate was significantly improved when the ratio of the additive in the surface layer to the center was 1.10 or more. In particular, the silicon nitride sintered bodies (Test Examples 7 to 11) produced by the PS-RBSN method had processing rates of 20 μm / h or more, and showed superior processability compared to Test Example 12. Furthermore, when the additive ratio was less than 1.40, good results were obtained in the crushing strength and rolling fatigue tests.

[0117] On the other hand, Test Examples 4 to 6, in which the additive ratio was 1.40 or more, showed a decrease in crushing strength. One possible reason for this is that the sintering additive content in the raw materials was relatively high, at 40 wt.% or more, resulting in a large amount of glass phase formed after sintering. In addition, the deeper the additive-rich layer, the more difficult it is to remove by polishing and the more likely it is to remain on the surface of the finished ball, which may have led to a decrease in strength and bearing characteristics.

[0118] In the rolling fatigue test, the test pieces did not peel off within the test time in Test Examples 7 to 12. On the other hand, peeling due to voids occurred in Test Examples 1 to 3. Furthermore, minute peeling occurred in Test Examples 5 and 6, which resulted in the test being stopped due to abnormal vibration.

[0119] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims rather than the above-described embodiments, and it is intended to include any modifications within the scope of the claims and meanings equivalent to the claims.

[0120] The silicon nitride sintered body of the present invention can be suitably used as a rolling element in bearings such as rolling bearings, linear guide bearings, ball screws, and linear bearings.

[0121] DESCRIPTION OF SYMBOLS 1 Rolling bearing 2 Inner ring 3 Outer ring 4 Rolling element 5 Cage 6 Seal member 7 Grease 8a, 8b Opening 11 Screw shaft 12 Thread groove 13 Ball nut 14 Thread groove 15 Ball 16 Ball screw seal member 21 Spherical plain bearing 22 Inner ring 23 Outer ring 24 Bearing hole 31 Fixed jig 32 Movable jig 33 Crosshead 34 Test ball

Claims

1. A silicon nitride sintered body having a Vickers hardness of 1,220 Hv or more and 1,400 Hv or less, and a maximum diameter of pores in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body, of 30 μm or less.

2. The silicon nitride sintered body according to claim 1, characterized in that the crystallinity of said silicon nitride sintered body is 75% or more and 90% or less.

3. The silicon nitride sintered body according to claim 1, characterized in that the silicon nitride sintered body contains a rare earth element and an aluminum element, and the content of the rare earth element is, in terms of oxide, 6 to 13 weight % of the total weight of the silicon nitride sintered body, and the content of the aluminum element is, in terms of oxide, 6 to 13 weight % of the total weight of the silicon nitride sintered body.

4. A silicon nitride sintered body according to claim 3, characterized in that the total content of said rare earth element and said aluminum element is 15% by weight or more and 26% by weight or less, calculated as oxide, of the total weight of said silicon nitride sintered body.

5. The silicon nitride sintered body according to claim 3, wherein said rare earth element includes at least one element selected from the group consisting of Y, Ce, Nd, and Eu.

6. The silicon nitride sintered body according to claim 1, characterized in that the silicon nitride sintered body has a Vickers hardness of 1250 Hv or more and 1320 Hv or less, a crystallinity of 75% or more and 85% or less, contains rare earth elements and aluminum elements, and does not contain transition metal elements, the rare earth element content is 7.5% or more and 13% or less by weight, calculated as an oxide, of the total weight of the silicon nitride sintered body, the aluminum element content is 7.5% or more and 13% or less by weight, calculated as an oxide, of the total weight of the silicon nitride sintered body, the sum of the rare earth element and the aluminum element content is 15% or more and 26% or less by weight, calculated as an oxide, of the total weight of the silicon nitride sintered body, and the rare earth element is Y or Ce.

7. A machine part using the silicon nitride sintered body according to claim 1.

8. The mechanical part according to claim 7, wherein the mechanical part is a rolling element.

9. A bearing using the rolling element according to claim 8.

Citation Information

Patent Citations

  • Ceramic sintered compact, method of producing the same, and sliding member, bearing ball and bearing using the same

    JP2001192258A

  • Abrasion resistant member of silicon nitride and its manufacturing method

    JP2002326875A

  • Static member for heat engine and its manufacturing method

    JP2002348177A

  • Silicon nitride sintered compact and sliding member using the same

    JP2008285349A

  • Sintered silicon nitride

    JP2011016716A