Conductive ink, preparation method therefor and use thereof

By mixing a solvent with a boiling point below or equal to 150°C with an organic conductive material to form a conductive ink, the problems of low production efficiency and poor film quality in the prior art are solved, and efficient and uniform preparation of conductive films are achieved.

WO2024244909A1PCT designated stage expired Publication Date: 2024-12-05SHENZHEN GUANGYI TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/091285
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-06
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

During the preparation process, the existing conductive inks use high boiling point solvents, resulting in slow solvent volatility, long drying time, affecting production efficiency, and poor quality of the conductive films formed.

Method used

A solvent with a boiling point below or equal to 150°C is used to mix it with an organic conductive material to form a conductive ink, simplifying the preparation process and improving the uniformity and conductivity of the film.

Benefits of technology

The solvent volatility rate of conductive ink is improved, the film formation time is shortened, and the conductive film formed is uniform, flat and dense, with excellent conductivity and production efficiency, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024091285_05122024_PF_FP_ABST
    Figure CN2024091285_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of conductive inks, and provides a conductive ink, a preparation method therefor and the use thereof. On the basis of the total weight of the conductive ink being 100%, the conductive ink comprises the following components in percentage by weight: 1-85% of an organic conductive material and 15-99% of a solvent, the solvent being a solvent of which the boiling point is lower than or equal to 150℃. The conductive ink provided by the present application comprises the organic conductive material and the solvent; since the solvent is a solvent of which the boiling point is lower than or equal to 150℃, the conductive ink of the present application can be dried quickly during coating, thus achieving high production efficiency. In addition, formed transparent conductive film layers are uniform, flat and compact, achieving good product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive ink, preparation method and application thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application number 202310637931.1 filed with the Patent Office of China on May 31, 2023, entitled “A conductive ink, its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present invention relates to the field of conductive ink technology, and in particular to a conductive ink and a preparation method and application thereof. Background Art

[0004] Conductive materials are key components of optoelectronic devices such as light-emitting diodes, solar cells, electrochromic devices, touch screens, defrost windows, and electromagnetic shielding. Among various types of conductive materials, the inorganic conductive material indium tin oxide (ITO) occupies the main market share of conductive materials worldwide due to its excellent optical transmittance and outstanding electrical properties in the visible light region. However, the film formed by ITO has disadvantages such as strong rigidity, high brittleness, and low stress, which cannot meet the development needs of roll-to-roll product manufacturing processes and flexible products. In addition, the indium contained in ITO is a rare earth element with scarce reserves. As the market demand for ITO increases, the price of indium has soared, and the supply of indium has gradually become highly restricted.

[0005] Therefore, there is an urgent need to develop high-performance and low-cost alternatives to ITO, such as metal mesh, carbon nanotubes, graphene, metal oxides, and organic conductive materials. Organic conductive materials are particularly popular due to their advantages such as solution processability, mechanical robustness, and low cost. For example, n-type conducting polymers, as a type of organic conductive material, possess both efficient electron transport and high carrier concentration, resulting in films made from n-type conducting polymers having excellent electrical properties and high transmittance comparable to ITO.

[0006] To prepare thin films containing organic conductive materials, conventional methods typically use polar aprotic solvents such as dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) to dissolve organic conductive materials, such as n-type conductive polymers. However, during the film formation process, the solvents must evaporate. These solvents have high boiling points and low saturated vapor pressures at room temperature, resulting in slow evaporation and prolonged drying times during the preparation process, often requiring overnight drying. This significantly impacts production efficiency.

[0007] Summary of the Invention

[0008] The purpose of this application is to provide a conductive ink and its preparation method and application, aiming to solve the problems of slow volatilization rate and low working efficiency of existing conductive inks due to the use of high-boiling point solvents.

[0009] To achieve the above application objectives, the technical solutions adopted in this application are as follows:

[0010] In a first aspect, the present application provides a conductive ink, which, based on the total weight of the conductive ink being 100%, comprises the following components in percentage by weight: 1 to 85% of an organic conductive material and 15 to 99% of a solvent; wherein the solvent is a solvent having a boiling point lower than or equal to 150°C.

[0011] In a second aspect, the present application provides a method for preparing a conductive ink, comprising: providing the components of the conductive ink of the present application; and mixing an organic conductive material and a solvent to obtain the conductive ink.

[0012] In a third aspect, the present application provides a conductive film, which is made from the conductive ink provided by the present application or the conductive ink prepared by the preparation method provided by the present application.

[0013] In a fourth aspect, the present application provides a conductive substrate, comprising: a substrate layer and an electrode layer disposed on the substrate layer, wherein the electrode layer comprises the conductive film provided in the present application.

[0014] In a fifth aspect, the present application provides an electrochromic film, the electrochromic film comprising a first substrate layer, a first electrode layer, an electrochromic medium layer, a second electrode layer and a second substrate layer stacked in sequence, wherein at least one of the first electrode layer and the second electrode layer comprises the conductive film provided in the present application; or, the electrochromic film comprises a first substrate layer, a first electrode layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence, wherein the first electrode layer comprises the conductive film provided in the present application, or both the first electrode layer and the second electrode layer comprise the conductive film provided in the present application; or The electrochromic film includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, a second electrode layer and a second substrate layer stacked in sequence, wherein the second electrode layer includes the conductive film provided in the present application, or the first electrode layer and the second electrode layer both include the conductive film provided in the present application; or, the electrochromic film includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence, wherein at least one of the first electrode layer, the second electrode layer, the ion storage layer and the electrochromic layer includes the conductive film provided in the present application.

[0015] In a sixth aspect, the present application provides an electrochromic device, comprising at least one substrate layer and the electrochromic film provided by the present application, wherein the substrate layer and the electrochromic film are stacked.

[0016] In the seventh aspect, the present application provides a terminal product, including the electrochromic film provided by the present application or the electrochromic device provided by the present application, wherein the terminal product includes any one of a rearview mirror, a curtain wall, a car sunroof, a car side window, a car windshield, an electronic product housing, glasses, a vehicle, and a display panel.

[0017] Compared with the prior art, this application has the following beneficial effects:

[0018] The conductive ink provided in the first aspect of the present application comprises an organic conductive material and a solvent. Since the solvent has a boiling point of less than or equal to 150°C, even if the boiling point of the solvent contained in the conductive ink is lowered, its corresponding saturated vapor pressure is increased. Therefore, when the conductive ink of the present application is used to prepare a conductive film, the solvent evaporates faster and dries easily, thereby improving production efficiency. Moreover, since the boiling point of the solvent is low, its volatilization is also easier and more comprehensive, so that the conductive film formed by the conductive ink has advantages such as uniformity, flatness, and density. In addition, since the conductive ink contains an organic conductive material, such as an n-type conductive polymer, which has high conductive properties, the conductive film prepared from the conductive ink also has excellent electrical conductivity, which can improve the electrical conductivity rate of the conductive film.

[0019] The second aspect of the present application provides a method for preparing a conductive ink, which can obtain a conductive ink by mixing an organic conductive material and a solvent. Since the solvent has a boiling point of less than or equal to 150°C, the prepared conductive ink is easy to dry when used to prepare a conductive film, and the production efficiency is high. Moreover, the formed conductive film has the advantages of being uniform, flat, and dense. Moreover, since the conductive ink contains an organic conductive material, such as an n-type conductive polymer, which has high conductive properties, the conductive film prepared from the conductive ink prepared by the preparation method has excellent electrical conductivity, which can improve the electrical conductivity rate of the conductive film. In addition, the preparation method is simple and easy, has low operating conditions and low cost, and is suitable for mass production.

[0020] The conductive film provided in the third aspect of the present application is made from the conductive ink provided by the present application or the conductive ink prepared by the preparation method provided by the present application. Since the solvent in the conductive ink has a boiling point lower than or equal to 150°C, even if the boiling point of the solvent contained in the conductive ink is lowered, its corresponding saturated vapor pressure is increased. Therefore, when the conductive ink of the present application is used to prepare the conductive film, the solvent evaporates faster and is easy to dry, thereby improving production efficiency; and since the boiling point of the solvent is low, its volatilization is also easier and more comprehensive, so that the conductive film formed by the conductive ink has the advantages of being uniform, flat, and dense; in addition, since the conductive ink contains organic conductive materials, such as n-type conductive polymers, which have high conductive properties, the conductive film prepared from the conductive ink also has excellent electrical conductivity, which can improve the electrical conductivity rate of the conductive film.

[0021] The conductive substrate provided in the fourth aspect of the present application has the advantages of being uniform, flat, dense and having an excellent electrical conductivity rate, since the electrode layer arranged on the substrate layer includes the conductive film provided in the present application. Therefore, the quality of the formed conductive substrate is better and more suitable for the preparation of various devices or products.

[0022] The electrochromic film provided in the fifth aspect of the present application includes a first substrate layer, a first electrode layer, an electrochromic medium layer, a second electrode layer and a second substrate layer stacked in sequence; or includes a first substrate layer, a first electrode layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence; or includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, a second electrode layer and a second substrate layer stacked in sequence; or includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence. Since at least one of the first electrode layer, the second electrode layer, the ion storage layer and the electrochromic layer includes the conductive film provided in the present application, wherein the conductive film is made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application, and the conductive film has the advantages of uniformity, flatness, density and excellent electrical conductivity, when the electrode layer contains the conductive film, the resistance distribution of the electrode layer can be made more uniform and the electrical conductivity rate can be made better. When the ion storage layer or the electrochromic layer contains the conductive film, the ion storage layer or the electrochromic layer can have more uniform and rapid ion or electron transmission characteristics, which makes the electrochromic film of the present application have excellent performance such as more uniform color change and faster color change efficiency.

[0023] The electrochromic device provided in the sixth aspect of the present application comprises at least one substrate layer and the electrochromic film provided in the present application, wherein the substrate layer and the electrochromic film are stacked, that is, the electrochromic film is arranged on the substrate layer, or sandwiched between the substrate layers, so that the electrochromic film can be better supported, especially when sandwiched between the substrate layers, the electrochromic film can be better protected by the substrate layer; and, since the electrochromic film in the electrochromic device comprises the conductive film provided in the present application, the electrochromic device also has excellent performance such as more uniform and rapid color change.

[0024] The terminal product provided in the seventh aspect of the present application includes the electrochromic film provided in the present application or the electrochromic device provided in the present application, that is, the terminal product includes the conductive film provided in the present application, so that the terminal product provided in the present application has advantages such as excellent color-changing performance. When the terminal product is applied to devices such as transportation vehicles (such as automobiles), electronic products (such as consumer electronics) or buildings, the device can have more excellent color-changing performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments or descriptions of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0026] FIG1 is a schematic structural diagram of a conductive substrate provided in some embodiments of the present application;

[0027] FIG2 is a schematic structural diagram of an electrochromic film provided in some embodiments of the present application;

[0028] FIG3 is a schematic structural diagram of electrochromic films provided in other embodiments of the present application;

[0029] FIG4 is a schematic structural diagram of an electrochromic film provided in some other embodiments of the present application;

[0030] FIG5 is a schematic structural diagram of electrochromic films provided in some other embodiments of the present application;

[0031] FIG6 is a schematic structural diagram of an electrochromic device provided in some embodiments of the present application;

[0032] FIG7 is a picture of a conductive film formed by coating the conductive ink provided in Example 1 of the present application on the surface of a PET substrate;

[0033] FIG8 is a picture of a conductive film formed by coating the conductive ink provided in Example 2 of the present application on the surface of a PET substrate;

[0034] FIG9 is a picture of a conductive film formed by coating the conductive ink provided in Example 3 of the present application on the surface of a PET substrate;

[0035] FIG10 is a picture of a conductive film formed by coating the conductive ink provided in Example 4 of the present application on the surface of a PET substrate;

[0036] FIG11 is a picture of a conductive film formed by coating the conductive ink provided in Example 5 of the present application on the surface of a PET substrate;

[0037] FIG12 is a picture of a conductive film formed by coating the conductive ink provided in Comparative Example 1 of the present application on the surface of a PET substrate;

[0038] FIG13 is a picture of a conductive film formed by coating the conductive ink provided in Comparative Example 2 of the present application on the surface of a PET substrate;

[0039] FIG14 is a schematic diagram of the cyclic voltammetry curve of the conductive film prepared in Example 1 of the present application.

[0040] Explanation of the main component symbols: 1-electrochromic device; 2-substrate layer; 21-first substrate layer; 22-second substrate layer; 3-electrochromic film; 31-conductive substrate; 311-substrate layer; 3111-first substrate layer; 3112-second substrate layer; 312-electrode layer; 3121-first electrode layer; 3122-second electrode layer; 32-electrochromic medium layer; 321-ion storage layer; 322-electrolyte layer; 323-electrochromic layer. DETAILED DESCRIPTION

[0041] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.

[0042] In this application, the term "and / or" describes the relationship between associated objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0043] In this application, "at least one" means one or more, and "many" means two or more. "At least one selected from..." or similar expressions refer to any combination of these items, including any combination of a single or multiple types. For example, "at least one selected from a, b or c", or "at least one selected from a, b and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple.

[0044] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0045] The terms used in the embodiments of the present application are for the purpose of describing specific embodiments only and are not intended to limit the present application. The singular forms "a", "an", "the" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise.

[0046] The weights of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the mass described in the examples of this application may be a mass unit known in the chemical industry, such as μg, mg, g, kg, etc.

[0047] The terms "first" and "second" are used solely for descriptive purposes to distinguish objects, such as substances, from one another and should not be understood to indicate or imply relative importance or to implicitly specify the quantity of the technical features being referred to. For example, without departing from the scope of the embodiments of this application, a first XX may also be referred to as a second XX, and similarly, a second XX may also be referred to as a first XX. Thus, features defined as "first" or "second" may explicitly or implicitly include one or more of such features.

[0048] Some embodiments of the present application provide a conductive ink, which includes the following components in weight percentage based on the total weight of the conductive ink as 100%: 1 to 85% of an organic conductive material and 15 to 99% of a solvent; wherein the solvent has a boiling point lower than or equal to 150°C.

[0049] The conductive ink provided in the embodiment of the present application includes an organic conductive material and a solvent. Since the solvent has a boiling point of less than or equal to 150°C, even if the boiling point of the solvent contained in the conductive ink is lowered, its corresponding saturated vapor pressure is increased. Therefore, when the conductive ink of the embodiment of the present application is used to prepare a conductive film, its solvent evaporates faster and dries easily, thereby improving production efficiency; and since the boiling point of the solvent is low, its volatilization is also easier and more comprehensive, so that the conductive film formed by the conductive ink has advantages such as uniformity, flatness, and density; in addition, since the conductive ink contains an organic conductive material, such as an n-type conductive polymer, which has high conductive properties, the conductive film prepared from the conductive ink also has excellent electrical conductivity, which can improve the electrical conductivity rate of the conductive film.

[0050] The conductive ink includes an organic conductive material having a weight percentage of 1 to 85%. In some embodiments, the weight percentage of the organic conductive material may be 5 to 80%. In other embodiments, the weight percentage of the organic conductive material may also be 1 to 75% or 1 to 60%. For example, the weight percentage of the organic conductive material may be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, etc.

[0051] In some embodiments, the organic conductive material may include a transparent organic conductive material. Thus, a conductive film made of a conductive ink containing the transparent organic conductive material may not only have conductive properties but also have high optical transparency, thereby improving the applicability of the conductive ink.

[0052] In some embodiments, the organic conductive material may include an n-type conductive polymer. In other embodiments, the organic conductive material may include a transparent n-type conductive polymer, such as poly(benzodifurandione) (PBFDO). For example, the n-type conductive polymer may be selected from the n-type conductive polymers shown in Formula I below:

[0053] Wherein, X is O (oxygen), S (sulfur) or Se (sellenium), m and n are both integers greater than 0, R1 and R2 are independently selected from H and C1-C 10 At least one of the alkyl groups, M + In some embodiments, C1-C 10The alkyl group may be an alkyl group containing 1 to 10 carbon atoms, such as methyl CH3-, ethyl CH3CH2-, propyl CH3CH2CH2-, etc. In other embodiments, C1-C 10 The alkyl group may include a straight chain alkyl group or a branched chain alkyl group, such as n-butyl CH3CH2CH2CH2-, isobutyl (CH3)2CHCH2-, sec-butyl CH3CH2(CH3)CH-, tert-butyl (CH3)3C-, etc. In some other embodiments, in the above formula I, X may be O, R1 and R2 may both be H, M + It can be a proton, such as H + .

[0054] In particular, n-type conductive polymers, such as those shown in Formula I or PBFDO, are n-doped to create a strong interaction between the polymer backbone and the good solvents (e.g., water, isopropyl alcohol, ethanol, etc.) of the embodiments of the present application. This allows the n-type conductive polymer to exhibit good solubility and solution processability without the need for alkyl side chains or surfactants. Furthermore, when conductive inks containing n-type conductive polymers are used to prepare conductive films, the resulting conductive films can exhibit advantages such as high conductivity and excellent stability, and even high optical transparency, thereby enhancing the applicability of the conductive inks.

[0055] In some embodiments, the conductive ink includes a solvent having a boiling point of 150° C. or lower. For example, the solvent may have a weight percentage of 15-99%. The weight percentage of the solvent may be 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, etc. Within this weight percentage range, the organic conductive material is easily dissolved to form the conductive ink, and the conductive ink can be used to form a conductive film with high and uniform conductivity.

[0056] The inventors of this application have discovered that when a conductive ink is applied to a substrate to form a conductive film, film formation time is crucial for optimizing nucleation, crystal growth, and industrial production efficiency for organic conductive materials (e.g., n-type conductive polymers). Typically, initial nucleation of n-type conductive polymers is caused by supersaturation, a state in which the liquid (solvent) contains more dissolved solids (solutes) than it can accommodate at a given temperature. This supersaturation is primarily due to solvent evaporation. Therefore, the vapor pressure or boiling point of the solvent in the conductive ink is crucial for controlling the crystallization rate of the organic conductive material or the film formation time of the conductive ink.

[0057] In view of this, in some embodiments, the solvent of the conductive ink can be a solvent with a boiling point lower than or equal to 150°C. In other embodiments, the solvent of the conductive ink can be a solvent with a boiling point lower than or equal to 120°C. In still other embodiments, the solvent of the conductive ink can be a solvent with a boiling point lower than or equal to 100°C. Thus, by using a solvent with a lower boiling point to dissolve the organic conductive material, the solvent can evaporate (volatize) faster during the film formation process of the conductive ink, so that the conductive ink can be in a supersaturated state, thereby facilitating the crystallization nucleation process of the organic conductive material. As a result, the film formation time of the conductive ink can be significantly shortened, thereby improving its film formation efficiency and thus improving the efficiency of industrial production.

[0058] Furthermore, because DMSO contains a hydrophilic sulfinyl group and two hydrophobic methyl groups in its structure, it is miscible with water or most organic solvents except petroleum ether, and can dissolve about 80% of compounds, such as most water-soluble compounds and fat-soluble compounds. Therefore, DMSO is generally considered a universal solvent. In the prior art, when organic materials need to be dissolved, DMSO or DMF with similar properties, or a mixture of DMSO and DMF, is usually selected. However, DMSO and DMF not only have high boiling points, but also have strong polarity and high surface tension. When a solution containing them (such as conductive ink) is coated on a substrate to form a film, the substrate is usually required to have a strong surface energy, which requires the substrate to be subjected to additional high-intensity hydrophilic treatment in advance, which is a relatively complicated process. In addition, when the surface energy of the substrate is less than the surface tension of the solvent, the conductive ink tends to quickly aggregate on the substrate or roll back from the edge of the substrate, which easily leads to poor uniformity of the film formed on the substrate, resulting in poor quality of the conductive film formed.

[0059] In view of this, in some embodiments, the solvent of the conductive ink can be a hydrophilic solvent. In other embodiments, the solvent of the conductive ink can be a hydrophilic solvent with a boiling point lower than or equal to 150°C. In still other embodiments, the solvent of the conductive ink can be a hydrophilic solvent with a boiling point lower than or equal to 120°C. In still other embodiments, the solvent of the conductive ink can be a hydrophilic solvent with a boiling point lower than or equal to 100°C. In this case, since the solvent is a hydrophilic solvent, when the conductive ink is applied to the substrate, there is no need to perform additional hydrophilic treatment on the substrate in advance. A conductive film with high conductivity and uniformity can be formed on the substrate. The conductive film has good quality and has the advantages of simple process and low cost.

[0060] In some embodiments, the solvent may include a good solvent. In other embodiments, the good solvent may be selected from at least one of water, isopropyl alcohol, and ethanol. For example, it may be one of water, isopropyl alcohol, and ethanol, or a mixture of any two of water, isopropyl alcohol, and ethanol, or a mixture of water, isopropyl alcohol, and ethanol. Generally, good solvents such as water, isopropyl alcohol, and ethanol can have a strong interaction with the polymer backbone of the organic conductive material (e.g., n-type conductive polymer), and their polarities match each other. Thus, the organic conductive material (e.g., n-type conductive polymer) can be better dissolved in these good solvents, thereby improving the uniformity of the conductive ink formed.

[0061] In some embodiments, when the good solvent includes water, the weight percentage of the organic conductive material is 5-80%, and it is understood that the weight percentage of water is 20-95%. In other embodiments, when the good solvent includes isopropyl alcohol or ethanol, the weight percentage of the organic conductive material is 1-60%, and it is understood that the weight percentage of isopropyl alcohol or ethanol is 40-99%. In still other embodiments, when the good solvent includes at least two of water, isopropyl alcohol, and ethanol, the weight percentage of the organic conductive material is 1-75%, and it is understood that the total weight percentage of water, isopropyl alcohol, and ethanol is 25-99%. Therefore, different good solvents can be selected to dissolve the organic conductive material according to actual needs to ensure the excellent performance of the conductive ink formed.

[0062] In some embodiments, the solvent may include a poor solvent. In other embodiments, the poor solvent may be selected from at least one of isobutanol, tert-butanol, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methyl ethyl ether, and propionaldehyde. For example, the poor solvent may be selected from isobutanol, tert-butanol, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methyl ethyl ether, and propionaldehyde. It may also be a mixture of any two or more of isobutanol, tert-butanol, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methyl ethyl ether, and propionaldehyde. Thus, different poor solvents can be selected according to actual needs to improve the applicability of the prepared conductive ink.

[0063] In some embodiments, the solvent may include a good solvent and a poor solvent. Good solvent and poor solvent are functional terms, and the solvents may be different for different materials. Therefore, the good solvent and poor solvent in the embodiments of the present application are for organic conductive materials. A good solvent refers to a solvent with high solubility for organic conductive materials; a poor solvent refers to a solvent with low solubility for organic conductive materials.

[0064] In some embodiments, when the solvent includes a good solvent and a poor solvent, for example, a mixed solvent of a good solvent and a poor solvent, the weight percentage of the organic conductive material can be 1-40%. It can be understood that the total weight percentage of the good solvent and the poor solvent can be 60-99%.

[0065] In some embodiments, the solvent may include a good solvent and a poor solvent, and the volume of the good solvent may be greater than the volume of the poor solvent. In other embodiments, the volume of the good solvent may be greater than 50% of the total volume of the solvent, that is, the volume of the good solvent is greater than 50% of the total volume of the good solvent and the poor solvent. In this case, by making the volume of the good solvent greater than the volume of the poor solvent, the dissolution effect of the organic conductive material can be optimized in the solvent mixture system of the good solvent and the poor solvent, thereby facilitating the formation of a uniform, smooth, and dense conductive film by the conductive ink.

[0066] In some embodiments, the solvent may include water, and the volume of water is greater than 70% of the total volume of the solvent. That is, when the solvent includes water, ensuring that the volume of water is greater than 70% of the total volume of the solvent can optimize the dissolution effect of the organic conductive material, thereby facilitating the conductive ink to form a uniform, flat, and dense conductive film.

[0067] The conductive ink of the embodiment of the present application can be prepared using the following preparation method.

[0068] Some embodiments of the present application provide a method for preparing a conductive ink, comprising the following steps: S01: providing the components of the conductive ink of the present application; S02: mixing an organic conductive material and a solvent to obtain a conductive ink.

[0069] The preparation method of the conductive ink provided in the embodiment of the present application is to obtain the conductive ink by mixing an organic conductive material and a solvent. Since the solvent has a boiling point lower than or equal to 150°C, the prepared conductive ink is easy to dry when used to prepare a conductive film, and the production efficiency is high. Moreover, the formed conductive film has the advantages of being uniform, flat, and dense. Moreover, since the conductive ink contains an organic conductive material, such as an n-type conductive polymer, which has high conductive properties, the conductive film prepared from the conductive ink prepared by the preparation method has excellent electrical conductivity, which can improve the electrical conductivity rate of the conductive film. In addition, the preparation method is simple and easy, has low operating conditions and low cost, and is suitable for mass production.

[0070] Among them, the conductive ink in step S01 is the conductive ink of the embodiment of the present application. Therefore, the specific types and contents of the various component raw materials of the conductive ink of the embodiment of the present application provided in step S01 are the same as those shown in the conductive ink of the embodiment of the present application. In order to save space, they will not be repeated here.

[0071] In some embodiments, in step S02 , the solvent may include a good solvent, and the step of mixing the organic conductive material and the solvent may include: mixing the organic conductive material and the good solvent and then sequentially performing a first ultrasonic treatment and a first stirring treatment.

[0072] In other embodiments, in step S02, the solvent may include a good solvent and a poor solvent, and the step of mixing the organic conductive material and the solvent may include: mixing the organic conductive material and the good solvent, sequentially performing a first ultrasonic treatment and a first stirring treatment to obtain a mixed solution of the organic conductive material and the good solvent; then adding the poor solvent to the mixed solution, and sequentially performing a second ultrasonic treatment and a second stirring treatment. This facilitates the full dissolution of the organic conductive material in the solvent, thereby achieving an optimal dispersion effect.

[0073] In some embodiments, the power of the first ultrasonic treatment may be 100-200 W, the ultrasonic time may be 0.5-1 hour, the rotation speed of the first stirring treatment may be 1200-1500 rpm, and the stirring time may be 0.5-4 hours. In other embodiments, the power of the second ultrasonic treatment may be 100-200 W, the ultrasonic time may be 0.5-1 hour, the rotation speed of the second stirring treatment may be 1200-1500 rpm, and the stirring time may be 0.5-4 hours.

[0074] Some embodiments of the present application provide a conductive film, which is made from the conductive ink provided in the embodiments of the present application or the conductive ink prepared by the preparation method provided in the embodiments of the present application. Since the solvent in the conductive ink is a solvent with a boiling point lower than or equal to 150°C, even if the boiling point of the solvent contained in the conductive ink is lowered, its corresponding saturated vapor pressure is increased. Therefore, when the conductive ink of the present application is used to prepare the conductive film, its solvent evaporates faster and is easy to dry, thereby improving production efficiency; and since the boiling point of the solvent is low, its volatilization is also easier and more comprehensive, so that the conductive film formed by the conductive ink has the advantages of uniformity, flatness, and density; in addition, since the conductive ink contains organic conductive materials, such as n-type conductive polymers, which have high conductive properties, the conductive film prepared from the conductive ink also has excellent electrical conductivity, which can improve the electrical conductivity rate of the conductive film.

[0075] In some embodiments, the conductive film can serve as both an electrode layer in an electrochromic film. In other embodiments, the conductive film can serve as either an ion storage layer or an electrochromic layer in an electrochromic film. In still other embodiments, the conductive film can serve as both an electrode layer and an ion storage layer in an electrochromic film, or both an electrode layer and an electrochromic layer in an electrochromic film.

[0076] As shown in FIG1 , some embodiments of the present application provide a conductive substrate 31 , comprising: a substrate layer 311 and an electrode layer 312 disposed on the substrate layer 311 , wherein the electrode layer 312 comprises the conductive film provided in the embodiments of the present application.

[0077] In some embodiments, the conductive ink provided in the embodiment of the present application or the conductive ink prepared by the preparation method provided in the embodiment of the present application may be coated on the substrate layer by a process such as magnetron sputtering or coating to form an electrode layer including the conductive film provided in the embodiment of the present application on the substrate layer, or to form an ion storage layer or electrochromic layer including the conductive film provided in the embodiment of the present application by coating on the electrode layer. Taking the coating method as an example, the substrate layer or the substrate layer including the electrode layer may be placed flat on the scraping table, and a clean wire rod may be placed on the machine table, the lock may be clamped, and then an appropriate amount of conductive ink may be sucked with a pipette, and the liquid may be discharged parallel to the wire rod at a distance of 1 to 2 cm from the offline rod, and then the equipment may be started to automatically coat according to the set parameters. After air drying at room temperature, the formed film material may be placed in an oven for drying, and the conductive film may be formed on the substrate layer or the electrode layer.

[0078] In some embodiments, the base layer 311 may include a flexible substrate, such as a polyethylene terephthalate (PET) substrate, a flexible glass substrate, a polyimide (PI) substrate, or a polydimethylsiloxane (PDMS) substrate. In other embodiments, the base layer 311 may include a rigid substrate, such as a rigid glass substrate. Thus, depending on actual needs, a conductive ink may be applied to a flexible substrate or a rigid substrate to form a conductive film, thereby forming a flexible conductive substrate or a rigid conductive substrate to accommodate different application scenarios.

[0079] The conductive substrate provided in the embodiment of the present application has an electrode layer arranged on the substrate layer, which includes the conductive film provided by the present application, and the conductive film is made of the conductive ink provided by the present application or the conductive ink prepared by the preparation method provided by the present application. Therefore, the electrode layer on the conductive substrate has the advantages of uniformity, flatness, density and excellent electrical conductivity rate, thereby making the quality of the formed conductive substrate better and more suitable for the preparation of various devices or products.

[0080] Some embodiments of the present application provide an electrochromic film 3. As shown in FIG2 , the electrochromic film 3 may include a first substrate layer 3111, a first electrode layer 3121, an electrochromic medium layer 32, a second electrode layer 3122, and a second substrate layer 3112 stacked in sequence; wherein at least one of the first electrode layer 3121 and the second electrode layer 3122 includes the conductive film provided in the embodiments of the present application.

[0081] The electrochromic medium layer 32 may be in a liquid, sol, or solid state. In some embodiments, the electrochromic medium layer 32 may include liquid crystal (LC), polymer dispersed liquid crystal (PDLC), suspended-particle devices (SPD), micro-blinds, inorganic electrochromic materials, and organic electrochromic materials. Thus, by applying a voltage to the first electrode layer and the second electrode layer, a potential difference is formed across the electrochromic medium layer, driving the ions or electrons between the electrochromic medium layers to embed or de-embed, thereby causing the electrochromic film to exhibit a change in color or transmittance as a whole, thereby causing a transition between a colored state (e.g., blue, black, or other colors) and a faded state (e.g., transparent), or a transition between a colored state, an intermediate state (any color between the colored state and the faded state, such as light blue or light black), and a faded state.

[0082] In some embodiments, the first electrode layer 3121 or the second electrode layer 3122 may include the conductive film provided in the embodiments of the present application, that is, the first electrode layer 3121 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application, and accordingly, the second electrode layer 3122 may be made of other materials, such as indium tin oxide (ITO). Alternatively, the second electrode layer 3122 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application, and accordingly, the first electrode layer 3121 may be made of other materials, such as indium tin oxide (ITO). In other embodiments, the first electrode layer 3121 and the second electrode layer 3122 may include the conductive film provided in the embodiments of the present application, that is, the first electrode layer 3121 or the second electrode layer 3122 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application.

[0083] The electrochromic film provided in the embodiment of the present application includes a first base layer, a first electrode layer, an electrochromic medium layer, a second electrode layer and a second base layer stacked in sequence. Since at least one of the first electrode layer and the second electrode layer includes the conductive film provided in the embodiment of the present application, the conductive film has the advantages of uniformity, flatness, density and excellent electrical conductivity rate, thereby making the resistance distribution of the electrode layer of the electrochromic film more uniform and the electrical conductivity rate more excellent, which makes the electrochromic film of the present application have excellent performance such as more uniform color change and faster color change efficiency.

[0084] Some embodiments of the present application provide an electrochromic film. As shown in FIG3 , the electrochromic film 3 may include a first substrate layer 3111, a first electrode layer 3121, an electrolyte layer 322, an electrochromic layer 323, a second electrode layer 3122, and a second substrate layer 3112 stacked in sequence; wherein the first electrode layer 3121 includes the conductive film provided in the embodiments of the present application, or the first electrode layer 3121 and the second electrode layer 3122 both include the conductive film provided in the embodiments of the present application.

[0085] In some embodiments, the first electrode layer 3121 may include a conductive film provided in an embodiment of the present application, that is, the first electrode layer 3121 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application, and accordingly, the second electrode layer 3122 may be made of other materials, such as indium tin oxide (ITO), etc. Of course, the second electrode layer 3122 may also be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application. In this case, the first electrode layer 3121 can not only serve as a conductive layer of the electrochromic film, but also serve as an ion storage layer in the electrochromic film, thereby having both high conductivity and excellent ion storage or ion transport properties.

[0086] The electrochromic film provided in some embodiments of the present application includes a first substrate layer, a first electrode layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence, at least the first electrode layer includes the conductive film provided in the present application, and the first electrode layer and / or the second electrode layer can serve as the conductive layer of the electrochromic film. Because the electrode layer has the advantages of uniformity, flatness, density and excellent electrical conductivity rate, the resistance distribution of the conductive layer of the electrochromic film is more uniform and the electrical conductivity rate is better, which makes the electrochromic film of the present application have excellent performances such as more uniform color change and faster color change efficiency; in addition, the first electrode layer can also serve as the ion storage layer of the electrochromic film. Because the electrode layer has the advantages of uniformity, flatness, density and excellent electrical conductivity rate, the ion storage layer of the electrochromic film has more uniform and faster ion transmission characteristics, which makes the electrochromic film of the present application have excellent performances such as more uniform and faster color change.

[0087] Some embodiments of the present application provide an electrochromic film. As shown in FIG4 , the electrochromic film 3 may include a first substrate layer 3111, a first electrode layer 3121, an ion storage layer 321, an electrolyte layer 322, a second electrode layer 3122, and a second substrate layer 3112 stacked in sequence; wherein the second electrode layer 3122 includes the conductive film provided in the embodiments of the present application, or both the first electrode layer 3121 and the second electrode layer 3122 include the conductive film provided in the embodiments of the present application.

[0088] In some embodiments, the second electrode layer 3122 can be made of the conductive ink provided in this application or the conductive ink prepared by the preparation method provided in this application. Accordingly, the first electrode layer 3121 can be made of other materials, such as indium tin oxide (ITO). Of course, the first electrode layer 3121 can also be made of the conductive ink provided in this application or the conductive ink prepared by the preparation method provided in this application. In this case, the second electrode layer 3122 can not only serve as the conductive layer of the electrochromic film, but also serve as the electrochromic layer in the electrochromic film, thereby having both high conductivity and excellent color-changing properties.

[0089] The electrochromic film provided in some embodiments of the present application includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, a second electrode layer and a second substrate layer stacked in sequence, at least the second electrode layer includes the conductive film provided in the present application, the first electrode layer and / or the second electrode layer can serve as the conductive layer of the electrochromic film, because the electrode layer has the advantages of uniformity, flatness, density and excellent electrical conductivity rate, thereby making the resistance distribution of the conductive layer of the electrochromic film more uniform and the electrical conductivity rate more excellent, which makes the electrochromic film of the present application have excellent performances such as more uniform color change and faster color change efficiency; on the other hand, the second electrode layer can also serve as the electrochromic layer of the electrochromic film, because the electrode layer has the advantages of uniformity, flatness, density and excellent electrical conductivity rate, thereby making the electrochromic layer of the electrochromic film have more uniform and rapid color change characteristics, which makes the electrochromic film of the present application have excellent performances such as more uniform and rapid color change.

[0090] Some embodiments of the present application provide an electrochromic film. As shown in FIG5 , the electrochromic film 3 may include a first substrate layer 3111, a first electrode layer 3121, an ion storage layer 321, an electrolyte layer 322, an electrochromic layer 323, a second electrode layer 3122, and a second substrate layer 3112, which are sequentially stacked. At least one of the first electrode layer 3121, the ion storage layer 321, the electrochromic layer 323, and the second electrode layer 3122 includes a conductive film provided in an embodiment of the present application. In some embodiments, as shown in FIG5 , the sequentially stacked ion storage layer 321, the electrolyte layer 322, and the electrochromic layer 323 may form the electrochromic medium layer 32 as described above.

[0091] In some embodiments, the first electrode layer 3121 or the second electrode layer 3122 may include the conductive film provided in the embodiments of the present application, that is, the first electrode layer 3121 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application, and accordingly, the second electrode layer 3122 may be made of other materials, such as indium tin oxide (ITO). Alternatively, the second electrode layer 3122 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application, and accordingly, the first electrode layer 3121 may be made of other materials, such as indium tin oxide (ITO). In other embodiments, the first electrode layer 3121 and the second electrode layer 3122 may include the conductive film provided in the embodiments of the present application, that is, the first electrode layer 3121 or the second electrode layer 3122 may be made of the conductive ink provided in the present application or the conductive ink prepared by the preparation method provided in the present application.

[0092] In some embodiments, the ion storage layer 321 may include the conductive film provided in the embodiments of the present application, that is, the ion storage layer 321 may be made of the conductive ink provided in the present application or the conductive ink produced by the preparation method provided in the present application. Accordingly, the electrochromic layer 323 may be made of other materials, such as inorganic electrochromic materials or organic electrochromic materials. In other embodiments, the electrochromic layer 323 may include the conductive film provided in the embodiments of the present application, that is, the electrochromic layer 323 may be made of the conductive ink provided in the present application or the conductive ink produced by the preparation method provided in the present application. Accordingly, the ion storage layer 321 may be made of other materials, such as materials forming an inorganic ion storage layer or an organic ion storage layer. In other embodiments, the ion storage layer 321 and the electrochromic layer 323 may both include the conductive film provided in the embodiments of the present application, that is, the ion storage layer 321 and the electrochromic layer 323 may both be made of the conductive ink provided in the present application or the conductive ink produced by the preparation method provided in the present application.

[0093] In some embodiments, when both the first electrode layer 3121 and the ion storage layer 321 comprise the conductive film provided in the embodiments of the present application, the first electrode layer 3121 and the ion storage layer 321 can be combined into a single layer and made from the conductive ink provided in the present application or the conductive ink produced by the preparation method provided in the present application. In other embodiments, when both the second electrode layer 3122 and the electrochromic layer 323 comprise the conductive film provided in the embodiments of the present application, the second electrode layer 3122 and the electrochromic layer 323 can be combined into a single layer and made from the conductive ink provided in the present application or the conductive ink produced by the preparation method provided in the present application.

[0094] The electrochromic film provided in some embodiments of the present application includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence. Since at least one of the first electrode layer, the ion storage layer, the electrochromic layer and the second electrode layer includes the conductive film provided in the present application, the conductive film can serve as the conductive layer of the electrochromic film on the one hand, and the conductive film has the advantages of being uniform, flat, dense and having an excellent electrical conductivity rate, thereby making the conductive layer resistance of the electrochromic film The conductive film can also serve as the ion storage layer or electrochromic layer of the electrochromic film. Because the conductive film has the advantages of uniformity, flatness, density and excellent electrical conductivity, the ion storage layer or electrochromic layer of the electrochromic film has more uniform and rapid color change characteristics, which makes the electrochromic film of the present application have more uniform and rapid color change and other excellent performance.

[0095] Some embodiments of the present application provide an electrochromic device, which may include at least one substrate layer and the electrochromic film provided in the embodiments of the present application, wherein the substrate layer and the electrochromic film are stacked. The number of substrate layers is not limited, for example, it may be one layer, two layers, or more than two layers. In some embodiments, the substrate layer may be one layer, and the electrochromic film may be disposed on the substrate layer. In other embodiments, as shown in FIG6 , the substrate layer 2 may be two layers, for example, a first substrate layer 21 and a second substrate layer 22, wherein the first substrate layer 21, the electrochromic film 3, and the second substrate layer 22 are stacked in sequence, so that the electrochromic film 3 is sandwiched between the first substrate layer 21 and the second substrate layer 22. In some further embodiments, the substrate layer may also be three layers. For example, after forming the sandwich structure shown in FIG6 , another substrate layer may be further disposed on the side of the first substrate layer 21 or the second substrate layer 22 away from the electrochromic film 3.

[0096] The electrochromic device provided in the embodiments of the present application includes at least one substrate layer and the electrochromic film provided in the embodiments of the present application, wherein the substrate layer and the electrochromic film are stacked, that is, the electrochromic film is arranged on the substrate layer, or sandwiched between two substrate layers, so that the electrochromic film can be better supported, especially when sandwiched between two substrate layers, the electrochromic film can be better protected by the substrate layer; and, because the electrochromic film includes the conductive film provided in the present application, the electrochromic device also has excellent performance such as more uniform and rapid color change.

[0097] The embodiments of the present application also provide a terminal product, including the electrochromic film provided in the embodiments of the present application or the electrochromic device provided in the embodiments of the present application, wherein the terminal product may include any one of a rearview mirror, a curtain wall, a car sunroof, a car side window, a car windshield, a housing of an electronic product, glasses, a vehicle, and a display panel. In some embodiments, the electrochromic film or the electrochromic device can replace the glass or housing of the terminal product. In other embodiments, the electrochromic film or the electrochromic device can be attached to the glass or housing of the terminal product. In yet other embodiments, the electrochromic film or the electrochromic device can also be sandwiched between the glass or housing of the terminal product. In this way, a terminal product with electrochromic properties can be formed to enrich the performance of the terminal product.

[0098] The terminal product provided in the embodiments of the present application includes the electrochromic film provided in the embodiments of the present application or the electrochromic device provided in the embodiments of the present application, so that the terminal product provided in the embodiments of the present application has advantages such as excellent color-changing performance. When the terminal product is applied to devices such as transportation vehicles (such as automobiles), electronic products (such as consumer electronics) or buildings, the device can have even better color-changing performance.

[0099] The following describes the details in conjunction with specific embodiments.

[0100] Example 1

[0101] This embodiment provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0102] Conductive ink, comprising the following components in percentage by weight:

[0103] PBFDO-poly(benzofurandione) 80%,

[0104] Water 20%;

[0105] Among them, the boiling point of water is 100°C.

[0106] The preparation method of conductive ink comprises the following steps:

[0107] S11: According to the components and contents of the conductive ink of Example 1, 8.0 g of poly(benzofurandione) and 2.0 mL of water were measured;

[0108] S12: poly(benzofurandione) was dissolved in water, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 0.5 h to obtain a conductive ink.

[0109] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0110] The conductive ink was coated on a 0.4 m×0.4 m (0.4 m in width and 0.4 m in length) PET substrate and dried at 100° C. for 2 min to obtain a conductive film.

[0111] Example 2

[0112] This embodiment provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0113] Conductive ink, comprising the following components in percentage by weight:

[0114] PBFDO-poly(benzofurandione) 60%,

[0115] Ethanol 40%;

[0116] Among them, the boiling point of ethanol is 78.3°C.

[0117] The preparation method of conductive ink comprises the following steps:

[0118] S11: According to the components and contents of the conductive ink of Example 2, 6.0 g of poly(benzofurandione) and 5.1 mL of ethanol were measured;

[0119] S12: Poly(benzofurandione) was dissolved in ethanol, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 1 h to obtain a conductive ink.

[0120] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0121] The conductive ink was coated on a 0.4 m×0.4 m (0.4 m in width and 0.4 m in length) PET substrate and dried at room temperature and pressure for 30 s to obtain a conductive film.

[0122] Example 3

[0123] This embodiment provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0124] Conductive ink, comprising the following components in percentage by weight:

[0125] PBFDO-poly(benzofurandione) 75%,

[0126] Solvent 25%;

[0127] The solvent is selected from water and ethanol, and the volume ratio of water to ethanol is 10:1, and the boiling points of water and ethanol are 100° C. and 78.3° C. respectively.

[0128] The preparation method of conductive ink comprises the following steps:

[0129] S11: According to the components and contents of the conductive ink of Example 3, 7.5 g of poly(benzofurandione), 2.3 mL of water, and 0.3 mL of ethanol were measured;

[0130] S12: Poly(benzofurandione) was added to a mixed solvent of water and ethanol, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 1 h to obtain a conductive ink.

[0131] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0132] The conductive ink was coated on a 0.4 m×0.4 m (0.4 m in width and 0.4 m in length) PET substrate and dried at 100° C. for 2 min to obtain a conductive film.

[0133] Example 4

[0134] This embodiment provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0135] Conductive ink, comprising the following components in percentage by weight:

[0136] PBFDO-poly(benzofurandione) 40%,

[0137] Solvent 60%;

[0138] The solvent includes water and ethyl acetate, and the volume ratio of water to ethyl acetate is 16:1, and the boiling points of water and ethyl acetate are 100° C. and 77.2° C. respectively.

[0139] The preparation method of conductive ink comprises the following steps:

[0140] S11: According to the components and contents of the conductive ink of Example 4, 4.0 g of poly(benzofurandione), 5.7 mL of water, and 0.39 mL of ethyl acetate were measured;

[0141] S12: Poly(benzofurandione) was added to a mixed solvent of water and ethyl acetate, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 1.5 h to obtain a conductive ink.

[0142] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0143] The conductive ink was coated on a 0.4 m×0.4 m (0.4 m in width and 0.4 m in length) PET substrate and dried at 100° C. for 2 min to obtain a conductive film.

[0144] Example 5

[0145] This embodiment provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0146] Conductive ink, comprising the following components in percentage by weight:

[0147] PBFDO-poly(benzofurandione) 40%,

[0148] Solvent 60%;

[0149] The solvent includes ethanol and ethyl acetate, and the volume ratio of ethanol to ethyl acetate is 30:1, and the boiling points of ethanol and ethyl acetate are 78.3° C. and 77.2° C. respectively.

[0150] The preparation method of conductive ink comprises the following steps:

[0151] S11: According to the components and contents of the conductive ink of Example 5, 4.0 g of poly(benzofurandione), 7.4 mL of ethanol, and 0.21 mL of ethyl acetate were measured;

[0152] S12: Poly(benzofurandione) was added to a mixed solvent of ethanol and ethyl acetate, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 3 h to obtain a conductive ink.

[0153] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0154] The conductive ink was coated on a 0.4 m×0.4 m (0.4 m in width and 0.4 m in length) PET substrate and dried at room temperature and pressure for 1 min to obtain a conductive film.

[0155] Comparative Example 1

[0156] This comparative example provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0157] Conductive ink, comprising the following components in percentage by weight:

[0158] PBFDO-poly(benzodifurandione) 24%,

[0159] Dimethylformamide 76%;

[0160] Among them, the boiling point of dimethylformamide is 153°C.

[0161] The preparation method of conductive ink comprises the following steps:

[0162] S11: According to the components and contents of the conductive ink of Comparative Example 1, 2.4 g of poly(benzofurandione) and 8.0 mL of dimethylformamide were measured;

[0163] S12: Poly(benzofurandione) was added to dimethylformamide, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 3 h to obtain a conductive ink.

[0164] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0165] The conductive ink was coated on a 30 mm×50 mm (30 mm in width and 50 mm in length) PET substrate and dried at room temperature and pressure for 12 h to obtain a conductive film.

[0166] Comparative Example 2

[0167] This comparative example provides a conductive ink and a preparation method thereof, as well as a conductive film prepared from the conductive ink.

[0168] Conductive ink, comprising the following components in percentage by weight:

[0169] PBFDO-poly(benzodifurandione) 24%,

[0170] Dimethyl sulfoxide 76%;

[0171] The boiling point of dimethyl sulfoxide is 189°C.

[0172] The preparation method of conductive ink comprises the following steps:

[0173] S11: According to the components and contents of the conductive ink of Example 5, 2.4 g of poly(benzofurandione) and 6.9 mL of dimethyl sulfoxide were measured;

[0174] S12: Poly(benzofurandione) was added to dimethyl sulfoxide, and ultrasonically treated at a power of 100 W and a temperature of 40° C. for 0.5 h, and then stirred at a rotation speed of 1300 rpm at room temperature for 3 h to obtain a conductive ink.

[0175] The conductive ink or the conductive ink prepared by the conductive ink preparation method is prepared into a conductive film:

[0176] The conductive ink was coated on a 0.4 m×0.4 m (0.4 m in width and 0.4 m in length) PET substrate and dried under heating conditions at 100° C. for 3 h to obtain a conductive film.

[0177] Related performance test analysis:

[0178] 1. The conductive films provided in Examples 1-5 and Comparative Examples 1-2 were photographed using a camera to obtain the surface morphology of each conductive film, as shown in Figures 7-13. Figures 7-11 show that the conductive films formed by applying the conductive inks provided in Examples 1-5 on a PET substrate were uniform, smooth, and dense, indicating good film quality. In contrast, Figures 12 and 13 show that the conductive films formed by applying the conductive inks provided in Comparative Examples 1-2 on a PET substrate exhibited numerous dark spots, uneven solute distribution, and numerous wrinkles, indicating poor film quality.

[0179] 2. In addition, it can be seen from the above embodiments and comparative examples that after the conductive inks provided in Examples 1 to 5 are coated on a PET substrate, during the drying process to form a conductive film, the drying time at room temperature and pressure is 30 seconds to 10 minutes, and the drying time at 100°C heating conditions is 3 seconds to 2 minutes; however, after the conductive inks provided in Comparative Examples 1 to 2 are coated on the same PET substrate, during the drying process to form a conductive film, the drying time at room temperature and pressure is 12 hours or more, and the drying time at 100°C heating conditions is 3 hours or more.

[0180] It can be seen that the conductive ink provided in the embodiment of the present application uses a solvent with a boiling point lower than or equal to 150°C, and the solvent is easy to volatilize. Therefore, the conductive ink provided in the embodiment of the present application is easy to dry after coating and forming a film, which reduces the processing time and improves production efficiency. Moreover, since the boiling point of the solvent is low, it evaporates more easily and comprehensively, so that the film formed by the conductive ink has the advantages of being uniform, flat and dense.

[0181] 3. Take the conductive film prepared in Example 1 and use the four-probe method to measure the sheet resistance of the conductive film. The measured sheet resistance is about 52Ω / cm 2 Typically, ITO conductive films of the same size and thickness have a resistance of about 40-70Ω / cm 2 It can be seen that the conductive film prepared by using the conductive ink provided in the embodiment of the present application has excellent conductive properties that are comparable to those of ITO conductive film.

[0182] 4. The conductive film prepared in Example 1 was cut into 3 cm × 5 cm pieces and subjected to electrochemical testing. The conductive film was used as the working electrode, Ag / AgCl as the reference electrode, and a Pt sheet as the counter electrode. The film was placed in a propylene carbonate (PC) solution containing 0.2 mol / L tetrabutylammonium bis-trifluoromethanesulfonimidate (TBATFSI). Electrochemical testing was performed at a sweep rate of 0.01 V / s between -0.4 V and 1.0 V (vs Ag / AgCl). The cyclic voltammetry (CV) curve of the conductive film is shown in FIG14 . Furthermore, the transmittance of the conductive film was found to vary from 20% to 60%.

[0183] As shown in Figure 14, within the monitored voltage range, different oxidation and reduction reactions alternately occur on the working electrode (conductive film), indicating that the conductive film has a high ion diffusion coefficient and high charge capacitance, proving that the conductive film has relatively excellent ion storage capacity and can be used as an ion storage layer in electrochromic devices. The range of transmittance variation obtained by detection shows that the conductive film also has the ability to change color (change transmittance), and can be used as an electrochromic layer in electrochromic devices.

[0184] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.

Claims

1. A conductive ink, It is characterized in that Taking the total weight of the conductive ink as 100%, the conductive ink comprises the following components in percentage by weight: Organic conductive material 1~85%, Solvent 15-99%; Wherein, the solvent is a solvent with a boiling point lower than or equal to 150°C.

2. The conductive ink according to claim 1, It is characterized in that The solvent is a hydrophilic solvent with a boiling point lower than or equal to 150°C.

3. The conductive ink according to claim 1 or 2, It is characterized in that The solvent includes at least one of a good solvent and a poor solvent.

4. The conductive ink according to claim 3, It is characterized in that The solvent includes the good solvent and the poor solvent, wherein the volume of the good solvent is greater than that of the poor solvent.

5. The conductive ink according to claim 3, It is characterized in that The good solvent is selected from at least one of water, isopropanol and ethanol; and / or The poor solvent is selected from at least one of isobutyl alcohol, tert-butyl alcohol, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methyl ethyl ether and propionaldehyde.

6. The conductive ink according to claim 3, It is characterized in that The solvent includes water, and the volume of the water is greater than 70% of the total volume of the solvent.

7. The conductive ink according to claim 5, It is characterized in that When the good solvent includes water, the weight percentage of the organic conductive material is 5 to 80%; or When the good solvent includes the isopropanol or the ethanol, the weight percentage of the organic conductive material is 1 to 60%; or When the good solvent includes at least two of the water, the isopropanol and the ethanol, the weight percentage of the organic conductive material is 1 to 75%; or When the solvent includes the good solvent and the poor solvent, the weight percentage of the organic conductive material is 1 to 40%.

8. The conductive ink according to claim 1 or 2, It is characterized in that The organic conductive material includes a transparent organic conductive material.

9. The conductive ink according to claim 1 or 2, It is characterized in that The organic conductive material includes an n-type conductive polymer.

10. The conductive ink according to claim 9, It is characterized in that The n-type conductive polymer is selected from the n-type conductive polymer shown in the following formula I; Wherein, X is O, S or Se, m and n are both integers greater than 0, R 1 and R 2 are independently selected from H and C 1 -C 10 At least one of the alkyl groups, M + It is a cation.

11. A method for preparing a conductive ink, It is characterized in that include: Providing the components of the conductive ink according to any one of claims 1 to 10; The organic conductive material and the solvent are mixed to obtain conductive ink.

12. The preparation method according to claim 11, It is characterized in that The solvent includes a good solvent, and the mixing treatment of the organic conductive material and the solvent includes: mixing the organic conductive material and the good solvent and then sequentially performing a first ultrasonic treatment and a first stirring treatment.

13. The preparation method according to claim 11, It is characterized in that The solvent includes a good solvent and a poor solvent, and the mixing process of the organic conductive material and the solvent includes: After mixing the organic conductive material and the good solvent, sequentially performing a first ultrasonic treatment and a first stirring treatment to obtain a mixed solution of the organic conductive material and the good solvent; The poor solvent is added to the mixed solution, and a second ultrasonic treatment and a second stirring treatment are sequentially performed.

14. The preparation method according to claim 12 or 13, It is characterized in that The power of the first ultrasonic treatment and / or the second ultrasonic treatment is 100-200W, and the ultrasonic time is 0.5-1h; and / or The rotation speed of the first stirring treatment and / or the second stirring treatment is 1200-1500 rpm, and the stirring time is 0.5-4 hours.

15. A conductive film, It is characterized in that The conductive film is made from the conductive ink described in any one of claims 1 to 10 or the conductive ink prepared by the preparation method described in any one of claims 11 to 14.

16. A conductive substrate, It is characterized in that It comprises: a base layer and an electrode layer arranged on the base layer, wherein the electrode layer comprises the conductive film according to claim 15.

17. An electrochromic film, It is characterized in that The electrochromic film comprises a first substrate layer, a first electrode layer, an electrochromic medium layer, a second electrode layer and a second substrate layer which are sequentially stacked, wherein at least one of the first electrode layer and the second electrode layer comprises the conductive film according to claim 15; or, The electrochromic film comprises a first substrate layer, a first electrode layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer which are sequentially stacked, wherein the first electrode layer comprises the conductive film according to claim 15, or the first electrode layer and the second electrode layer both comprise the conductive film according to claim 15; or, The electrochromic film comprises a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, a second electrode layer and a second substrate layer which are sequentially stacked, wherein the second electrode layer comprises the conductive film according to claim 15, or the first electrode layer and the second electrode layer both comprise the conductive film according to claim 15; or, The electrochromic film includes a first substrate layer, a first electrode layer, an ion storage layer, an electrolyte layer, an electrochromic layer, a second electrode layer and a second substrate layer stacked in sequence, wherein at least one of the first electrode layer, the second electrode layer, the ion storage layer and the electrochromic layer includes the conductive film as described in claim 15.

18. An electrochromic device, It is characterized in that It comprises at least one substrate layer and the electrochromic film as claimed in claim 17, wherein the substrate layer and the electrochromic film are stacked.

19. A terminal product, It is characterized in that It includes the electrochromic film as claimed in claim 17 or the electrochromic device as claimed in claim 18, wherein the terminal product includes any one of a rearview mirror, a curtain wall, a car sunroof, a car side window, a car windshield, a housing of an electronic product, glasses, a vehicle, and a display panel.

Citation Information

Patent Citations

  • Anti-settling and self-leveling silver nanowire conductive printing ink and method for preparing transparent conducting thin film by using same

    CN104861776A

  • Conductive ink and preparation method thereof

    CN106046918A

  • Transparent conductive film and preparation method thereof

    CN106229036A

  • Spray transparent and conductive ink as well as preparation method and application thereof

    CN107384025A

  • Preparation method of water-based UV conductive ink

    CN108148469A