Low-temperature agglomerated highly-reflected electrodes from metallic nanoparticles
Patent Information
- Application Number
- PCT/CN2024/095943
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-05
Smart Images

Figure CN2024095943_05122024_PF_FP_ABST
Abstract
Description
LOW-TEMPERATURE AGGLOMERATED HIGHLY-REFLECTED ELECTRODES FROM METALLIC NANOPARTICLES
[0001] Cross-refence to Related Applications:
[0002] The present application claims the priorities from the U.S. provisional patent application serial number 63 / 504,796 filed May 30, 2023, and the disclosure of which is incorporated herein by reference in its entirety.Field of the Invention:
[0003] The present invention generally relates to the field of optoelectronic devices including large-area organic solar cells (OSCs) and specifically focuses on solution-processed top electrodes (STEs) for promoting the development of large-area OSCs.Background of the Invention:
[0004] Optoelectronic devices have attracted much attention in the past decades. For example, organic Solar Cells (OSCs) show interesting features of their lightweight, flexibility, low cost, and simple fabrication process. To date, the power conversion efficiency (PCE) of OSCs has achieved over 19%for single junction cells and over 20%for tandem cells. To promote the industrialization of OSCs, large-area devices are highly desirable. However, large-area devices have much more complex and exacting requirements, such as material restriction, deposition methods, and layer thickness of multi-layered device structures, etc.
[0005] Many efforts have contributed to the large-area OSCs. In general, most of the reports selected the rear electrodes formed by vapor deposition methods, such as thermal evaporation or magnetron sputtering, owing to their homogeneous and compact properties. Zangwill et al. illustrated the general deposition process of these solid films, in which the growth and erosion affect the film deposition synergistically1. The morphological evolution of the thin film growth and smoothing was demonstrated, pointing out the fundamental depositing procedure of ultrasmall components. Nevertheless, thermal evaporation and magnetron sputtering inevitably consume a tremendous amount of energy and are incompatible with high-throughput and large-area manufacturing.
[0006] Differently, solution-processed top electrodes (STEs) with the interesting features of a cost-effective and easy fabrication process can be the potential candidate for promoting large-area OSCs. Regrettably, the reported all-solution processed large-area OSCs presented relatively low efficiency, suffering from unsatisfactory conductivity and reflectance of STEs.
[0007] Silver nanoparticle (AgNP) is a potential candidate for high-quality reflective electrodes owing to its high conductivity and reflectance of bulk material. The formation of AgNP conductive film involves two steps: particle deposition and sintering, in which the ligands on the particles may significantly influence the stacking conditions and sintering process, resulting in complex packing structure and harsh sintering requirements.
[0008] Many researchers have investigated the assembly of nanoparticles with different ligands. A rigid core with a soft ligand shell can assemble into phase characteristic of dense packing and internal surface area minimization, while the length of ligands can determine the packing model of particles between hard and soft balls2. In addition, the selection of suitable ligands can manipulate not only the particle shape and size but also the assembled superlattices, which can significantly affect the packing methods of particles and film qualities. These assembled structures offer excellent opportunities for the subsequent conductive thin film formation, after interparticle tunneling or removing organic ligands. For instance, citrate-covered particles are demonstrated to form assembled particle islands, resulting in a suppressed tunneling barrier and a film’s conductivity of over 4000 S / cm, while other ligands restrain the electron transport of films due to the large interparticle distance3.
[0009] Ligands can be split away from the silver surface after photonic, chemical, plasma, or thermal treatments, contributing to interparticle contact and realizing decent conductivities of sintered particles. The remaining insulating ligands and the spherical shape of particles in the sintered thin films severely limit the film quality and subsequently the optical and electrical properties. Few reported methods can remove the ligands from the particles in films and transform the ‘stacked particles’s tructure to uniform film under a soft posttreatment, which is highly desirable for electronic applications.
[0010] The nano-size Ag particles absorb and scatter light extraordinarily because of the collective oscillation of surface electrons, known as surface plasmon resonance (SPR) 4-7. More ligands remain in the AgNP film may make it harder to lose the ‘stacked particles’s tructure, contributing to more potent SPR effects. Compared with commonly used evaporated or sputtered silver electrodes, AgNP thin films may suffer a significant loss of current density in photovoltaic applications. As a result, few reported works demonstrated high-quality reflective electrodes based on solution-processed AgNPs.Summary of the Invention:
[0011] To address issues such as poor reflectance, challenging post-treatment conditions, and the unclear formation mechanisms from nanoscale materials to bulk electrode film, the present invention introduces specific ligands of the AgNP. In addition, the present invention also provides a compact packing-enabled formation approach to fabricate efficient electrodes with very good electrical conductance and high broadband optical reflectance. This method involves stacking metallic nanoparticles and then sintering them to create highly efficient top electrodes with high conductivity and broad-spectrum reflectance.
[0012] This invention delves into the fundamentals of depositing and sintering silver nanoparticles (AgNPs) using various ligands. It proposes a strategy for selecting the optimal ligand for AgNPs, thereby achieving high-density stacking of AgNP films with excellent electrical and optical properties after sintering at low temperatures. Solution-processed top electrodes using AgNPs have great potential in the high-throughput large-scale industrialization of organic solar cells (OSCs) .
[0013] In a first aspect, the present invention provides a solution-processed metallic nanoparticle reflective electrode, which includes a target substrate and a solution-processed conductive film coated on the target substrate. The solution-processed conductive film inlcudes one or more metallic nanomaterials stabilized by one or more covered ligands. The one or more covered ligands interact with adjacent metallic nanomaterials.
[0014] In one embodiment, the one or more metallic nanomaterials include silver nanoparticles, gold nanoparticles, copper nanoparticles nickel nanoparticles, or aluminum nanoparticles.
[0015] Preferably, the solution-processed metallic nanoparticle reflective electrode includes silver nanoparticles (AgNP) reflective electrode.
[0016] In one embodiment, the one or more metallic nanomaterials include metal nanoparticles with particle size of 1-200 nm, and a dispersity of >1mg / mL. The one or more metallic nanomaterials are in a shape of particle, wire, rod, or plate.
[0017] In one embodiment, the target substrate includes silicon wafer, or glass.
[0018] In one embodiment, the one or more covered ligands include short-chain molecular materials with 2-20 carbons in the main chain.
[0019] In one embodiment, the solution-processed metallic nanoparticle reflective electrode realizes a sheet resistance of lower than 20Ω / sq. Preferably, the solution-processed metallic nanoparticle reflective electrode realizes a sheet resistance of lower than 3Ω / sq.
[0020] In one embodiment, the solution-processed conductive film achieves an average reflectance in the visible region over 90%.
[0021] In one embodiment, the average reflectance of the solution-processed conductive film contains 25%diffused reflection.
[0022] In one embodiment, the solution-processed metallic nanoparticle reflective electrode has a conductivity of at least 30×106 S / m. Preferably, the solution-processed metallic nanoparticle reflective electrode has a conductivity of 42×106 S / m.
[0023] In a second aspect, the present invention also provides a method for forming a solution-processed conductive film, including synthesizing one or more metallic nanomaterials stabilized by one or more covered ligands to form a solution-processed conductive film; stacking the one or more metallic nanomaterials on a target substrate; and agglomerating the one or more metallic nanomaterials to form the solution-processed conductive film.
[0024] In one embodiment, the step of synthesizing one or more metallic nanomaterials stabilized by one or more covered ligands further including adding a catalyst with a boiling point in a range of 30-400 ℃.
[0025] In one embodiment, the catalyst includes N-butylamine, Trimethylamine, dimethylethanolamine, or a combination thereof.
[0026] In one embodiment, the step of coating the one or more metallic nanomaterials on a target substrate is conducted by spin coating, spray coating, blade coating, slot-die coating, or dip coating.
[0027] In one embodiment, the step of agglomerating the one or more metallic nanomaterials includes low-temperature thermal annealing of the one or more metallic nanomaterials within a temperature range of 75-150℃.
[0028] In one embodiment, the one or more metallic nanomaterials have a particle size of 1-200 nm, and a dispersity of >1mg / mL in a solvent.
[0029] In one embodiment, the one or more metallic nanomaterials include silver nanoparticles, gold nanoparticles, copper nanoparticles nickel nanoparticles, or aluminum nanoparticles.
[0030] In one embodiment, the one or more covered ligands include a short-chain molecular material with 2-20 carbons in the main chain.
[0031] In one embodiment, the short-chain molecular material includes gallic acid (GA) , and wherein carboxylic acid groups in the GA molecule interact with silver and generate ionic bonds, and hydroxyl groups in the GA also interacts with silver and being connected by hydrogen bonds.
[0032] In one embodiment, the one or more metallic nanomaterials are in a shape of particle, wire, rod, or plate.
[0033] In one embodiment, the target substrate includes silicon wafer, or glass.
[0034] In a third aspect, the present invention provides an evaporation-free organic solar cell, which includes a top electrode, an active layer, and a bottom electrode. The top electrode is a solution-processed metallic nanoparticle reflective electrode. The organic solar cell exhibits a power conversion efficiency of at least 10%for a large-area device.
[0035] In one embodiment, the evaporation-free organic solar cell further contains at least one interfacial layer. The at least one interfacial layer includes a hole transport layer and / or an electron transport layer.
[0036] The following are the novel features of the invention that are not present in current technology:
[0037] (1) Simple process: the process only requires metal nanoparticles deposition and low-temperature agglomerating, excluding the need for harmful chemicals, solvents, and harsh pre-and post-treatment during top electrode deposition;
[0038] (2) Excellent film quality: it achieves an impressively low sheet resistance of 1.6 Ω / sq, indicating efficient charge transportation;
[0039] (3) Good optical reflection in broad region: the agglomerated electrode shows ultrahigh average light reflection (> 92%) in visible region. Also, it can contain 25%diffused reflection, which is attractive in optoelectronic area;
[0040] (4) Environmentally friendly: the process is conducted at low temperatures and does not require or generate toxic raw materials or by-products;
[0041] (5) Low energy consumption in production: the process does not require high temperatures, high vacuum conditions, or large currents.Brief Description of the Drawings:
[0042] Embodiments of the invention are described in more detail hereinafter with reference to the drawings, in which:
[0043] FIG. 1A depicts a schematic diagram of the room-temperature synthesis process of silver nanoparticles. The inset image is a SEM image of AgNPs. FIG. 1B depicts a schematic diagram of spray-coating AgNPs. A patterned cover mask introduces the pattern of rear electrodes. The inset photographs are the top and bottom views of an actual OSC with a spray-coated AgNP electrode. FIGs. 1C-1D shows TEM images of AgNPs before and after annealing with a scale bar of 20 nm. The inset images are the corresponding electron diffraction patterns with a scale bar of 5 1 / nm. FIG. 1E depicts a comparison of conductivities and average reflectance (400-900 nm) of three electrodes: a commonly reported agglomerated AgNPs with oleyamine as ligands (AgNP-OA) , evaporated silver (E-Ag) , and the agglomerated AgNPs assisted with gallic acid of the present invention;
[0044] FIG. 2A shows a molecular structure of gallic acid (GA) ; FIG. 2B-2C depicts a schematic diagram of two contacted AgNPs with GA or oleylamine (OA) , and as ligands. FIG. 2D shows a molecular structure of OA. FIG. 2E shows a TEM image of the one-layer distribution of AgNPs with GA ligands. FIG. 2F depicts a schematic diagram of the one-layer distribution of AgNPs with GA ligands. FIG. 2G depicts a schematic diagram of the one-layer distribution of AgNPs with OA ligands. FIG. 2H shows a TEM image of the one-layer distribution of AgNPs with OA ligands. FIG. 2I depicts a schematic diagram of agglomerating process at a low temperature of AgNPs with GA ligands. FIG. 2J depicts a schematic diagram of the stacking process at a low temperature of AgNPs with GA ligands. FIG. 2K depicts a schematic diagram of the stacking process at a low temperature of AgNPs with OA ligands. FIG. 2L depicts a schematic diagram of the agglomerating process at a low temperature of AgNPs with OA ligands. FIGs. 2I-2L shows SEM images of stacked AgNPs before and after low-temperature annealing. FIG. 2M depicts the reflectance spectrum and the conductivities-temperature curves of centimeter-level AgNPs thin films. The photograph of AgNP-GA and AgNP-OA films before and after thermal agglomerating for 10 min. The annealing temperature is 100 ℃ for AgNP-GA and 250 ℃ for AgNP-OA, respectively;
[0045] FIG. 3A shows a schematic diagram of electrostatic adherence. FIG. 3B shows a schematic diagram of smoothing steps. FIG. 3C shows a schematic diagram of stacked condition after continuously stacking and smoothing. FIG. 3D shows a TEM image of stacking conditions of AgNP-GA after 1 cycle, 2 cycle, and 4 cycle.
[0046] FIG. 4A shows an AFM image of AgNPs before annealing with an area of 1 μm ×1 μm. FIG. 4B shows an AFM image of AgNPs after annealing with an area of 1 μm × 1 μm. The RMSs of the films are marked in the images;
[0047] FIG. 5 depicts the time-varying TEM of AgNP-GA and AgNP-OA;
[0048] FIG. 6 shows TEM images of AgNP-PVP and AgNP-TCA. The average particle size of both cases is around 50 nm;
[0049] FIG. 7 depicts conductivity-temperature curves of AgNPs thin films;
[0050] FIG. 8 depicts XRD of AgNP-OA and AgNP-GA thin films before and after annealing at 130℃ for 5 min;
[0051] FIG. 9A depicts the resistance evolution of AgNP-GA films annealed at stepwise temperatures. The dash lines represent the resistances of sintered AgNP-OA film and evaporated silver thin film. FIG. 9B depicts the total (solid lines) and diffused (dash lines) reflectance spectrum of evaporated silver, sintered AgNP-GA, and sintered AgNP-OA films;
[0052] FIG. 10A shows a schematic diagram of the resistance measurement. The film is deposited on the 17 mm × 17 mm glass substrates, and the resistance is measured diagonally in a 14 mm × 14 mm square area by a multimeter. FIG. 10B shows a natural photograph of the resistance measurement. The AgNP film is annealed at 130 ℃ for 5 min;
[0053] FIG. 11A depicts the total and diffuse reflectance of AgNP films with different thicknesses contributed by the drops of solution in the spin-coating process. FIG. 11B depicts transmittance spectra of AgNP films with different thicknesses contributed by the drops of solution in the spin-coating process. FIG. 11C depicts a statistic diagram of the average reflectance and the corresponding sheet resistance of AgNP films with different thicknesses. FIG. 11D shows the cross-section SEM of the AgNP film prepared with 20 drops of solution in the coating process;
[0054] FIG. 12A shows a group of schematic diagrams of the GA ligand interacting with AgNP. The decarboxylic reaction and ligand dissociation induced by the annealing process is also demonstrated in the diagram. FIG. 12B shows the optical microscope images of gallic acid before and after annealing at 100 ℃ and 130 ℃. The spot on the right corner is used for positioning. FIGs. 12C shows O1s core-level spectra of AgNP films before and after annealing at 100 ℃ and 130 ℃ for 15 min. The relevant peak data are marked in the spectra;
[0055] FIG. 13 depicts FTIR spectra of GA powers before and after the annealing in a humid environment;
[0056] FIG. 14A depicts Ag 3d, O 1s and C 1s XPS spectras of AgNP films before and after the annealing process at 100 ℃ and 130 ℃ for 15 min. FIG. 14B depicts Ag, C, and O mass concentration of AgNP films before and after the annealing process;
[0057] FIG. 15 depicts C1s core-level spectra of AgNP films before and after annealing at 100 ℃ and 130 ℃ for 15 min. The relevant peak data are marked in the spectra;
[0058] FIG. 16A shows the cross-section SEM image of the OSC with the structure of glass / ITO / PEDOT: PSS / D18-Cl: N3: PC61BM / PEI-Zn / SAE. FIG. 16B depicts the J-V characteristics of champion large-area devices with SAE. The inset image is the top view of a large-area device with an area of 1 cm2. FIG. 16C depicts the evolution of PCE for large-area OSCs (≥1 cm2) with a solution-processed top electrode. FIG. 16D depicts electrochemical impedance spectroscopy (EIS) of OSC devices with the structure of ITO / PEDOT: PSS / P3HT: PCBM / PEI-Zn / E-Ag or AgNP. The inset diagram is the equivalent circuit of OSC device. FIG. 16E depicts light intensity dependence of JSC and VOC of OSCs with the structure of ITO / PEDOT: PSS / P3HT: PCBM / PEI-Zn / E-Ag or AgNP;
[0059] FIG. 17 shows the illustrative structure diagrams of D18-Cl, N3, and PC61BM;
[0060] FIG. 18A shows a schematic diagram of spray coating AgNPs. The pattern of rear electrodes is introduced by a patterned cover mask. The below photograph is the top and bottom view of the real OSC device. FIG. 18B shows a photograph of the portable spray gun with an electrical air pump;
[0061] FIG. 19A depicts statistical characteristics of the OSC devices (0.08 cm2) measured with AM 1.5G. FIG. 19B depicts the characteristics of champion devices with E-Ag and SAE;
[0062] FIG. 20A depicts UPS spectra of AgNP films before and after the annealing process at 75 ℃, 100 ℃, and 130 ℃. FIG. 20B shows a schematic energy diagram of the OSC device with different rear electrodes;
[0063] FIG. 21 depicts the EQE spectrum and the corresponding integrated JSC of the SAE-based OSCs. The integrated JSC is 26.17 mA / cm2;
[0064] FIG. 22A depicts a comparison of normal and inverted device structure. FIG. 22B depicts a comparison of normal device structures with various ETLs. FIG. 22C depicts a comparison of inverted devices with various ETLs. FIG. 22D depicts a comparison of devices with various active layers;
[0065] FIGs. 23A-23D depict MPPT stability of ITO / PEDOT: PSS / P3HT: PCBM / PEI-Zn / E-Ag or AgNP devices at air condition (T= 30 ℃; RH= 60%) , including VOC, JSC, FF and PCE;
[0066] FIG. 24A depicts EL spectra of organic LEDs with E-Ag and AgNP-GA electrodes. FIG. 24B depicts current density of E-Ag and AgNP under different voltages. FIG. 24C depicts EQE-J characteristics of OLED devices with E-Ag and AgNP-GA electrodes;
[0067] FIG. 25A shows a schematic diagram of the synthesis process of silver nanoparticles at room temperature. FIG. 25B shows the SEM images for GA*1 and GA*3 films. The scale bar is 500 nm. FIG. 25C depicts the particle diameter distribution of GA*1 and GA*3. The dash histograms are counted numbers, and the lines are fitted distribution curves. FIG. 25D depicts the fitted particle diameter distribution for fresh AgNPs and AgNPs after 30 days of storage;
[0068] FIGs. 26A-26D depict the respective distribution diagrams for fresh GA*1, GA*1 after 30 days of storage, fresh GA*3, and GA*3 after 30 days of storage. The histograms are calculated proportions, and the lines are fitted distribution curves;
[0069] FIG. 27 depicts Zeta potential of AgNP-GA at 25 ℃;
[0070] FIG. 28 shows Grazing-Incidence Small-Angle X-ray Scattering (GISAXS) images of AgNP-OA, AgNP-GA and sintered AgNP-GA thin films; and
[0071] FIG. 29A depicts GASAXS data of AgNP-OA and AgNP-GA before and after sintering. FIG. 29B depicts the structure factor of AgNP-OA and AgNP-GA.Detailed Description:
[0072] In the following description, ligand-assisted Ag nanoparticle (AgNP) electrodes and its preparation process are set forth as preferred examples. It will be apparent to those skilled in the art that modifications, including additions and / or substitutions may be made without departing from the scope and spirit of the invention. Specific details may be omitted so as not to obscure thetinvention; however, the disclosure is written to enablfe one skilled in the art to practice the teachings herein without undue experimentation.
[0073] The commonly used STE materials are conductive polymers, carbon-based nanomaterials, and metal-based materials. The most famous conductive polymer for the solution-processed electrode is the PEDOT: PSS, which shows good conductivity after treatments and great flexibility. Nevertheless, the intense light absorbance induced by the nature of the material limits its potential for performing as reflective electrodes. The serious wetting problems also make it hard to be deposited on the top of OSCs. Carbon-based materials, including carbon nanotubes (CNT, 1D) and graphene (2D) , also suffer from similar problems and are hard to perform as ideal reflective electrodes.
[0074] Moreover, the poor inter-piece or inter-tube contact significantly increases the resistance of the electrodes. Metal-based materials such as Ag nanowires, Ag micro-particles or -plates inks, and AgNPs have been intensively investigated because of their high conductivity in bulk materials. However, AgNWs cannot perform as reflective electrodes due to the low coverage ratio of the network structure. Commercial Ag inks usually contain various additives which may increase the penetration risk during the solution process. In addition, the micron-size Ag components in the inks make it hard to fabricate uniform films and ideal interfaces with the underlying layer. Thus, the silver nanoparticle shall be a potential candidate for STE application because of its high conductivity and reflectance of the bulk material and high coverage of the film formation.
[0075] The present invention addresses the problem by providing a ligand-dominated formation of metallic nanoparticle electrodes for enabling fully solution-processed large-area high-performance organic solar cells. In particular, the present invention provides a solution-processed metallic nanoparticle reflective electrode, which includes a target substrate and a solution-processed conductive film coated on the target substrate. The solution-processed conductive film includes one or more metallic nanomaterials stabilized by one or more covered ligands. The one or more covered ligands interact with adjacent metallic nanomaterials.
[0076] Gallic acid (GA) performs as a reductant and stabilized ligand for AgNP synthesis. The short-chain molecular structure and multiple interactions with AgNP benefit the high space proportion of silver in particles and compact packing during deposition, contributing to a tightly stacked AgNP thin film with a higher density of silver compared to AgNP films with other ligands. Furthermore, unlike commonly-used ligands, GA can decompose at low temperatures and release from the AgNP films, contributing to a facile sintering process for AgNPs and producing a relatively pure silver film.
[0077] In one embodiment, the one or more metallic nanomaterials may include silver nanoparticles, gold nanoparticles, copper nanoparticles nickel nanoparticles, or aluminum nanoparticles. Preferably, the solution-processed metallic nanoparticle reflective electrode comprises silver nanoparticles reflective electrode.
[0078] In one embodiment, the target substrate may include silicon wafer, or glass.
[0079] In one embodiment, the one or more covered ligands may include short-chain molecular materials with 2-20 carbons in the main chain.
[0080] The steps to realize solution-processed top electrodes with AgNPs are as follows:
[0081] (1) synthesizing AgNPs with opportune ligands to achieve ideal particle size and dispersity in a solvent; and
[0082] (2) stacking the AgNP thin film on a target substrate; and
[0083] (3) sintering the AgNPs to form the solution-processed conductive film.
[0084] In one embodiment, the step of synthesizing one or more metallic nanomaterials stabilized by one or more covered ligands further including adding a catalyst with a boiling point in a range of 30-400 ℃. The catalyst may include N-butylamine, Trimethylamine, dimethylethanola, or a combination thereof.
[0085] In one embodiment, step of coating the one or more metallic nanomaterials on a target substrate may be conducted by spin coating, spray coating, blade coating, slot-die coating, or dip coating.
[0086] In one embodiment, the step of agglomerating the one or more metallic nanomaterials includes low-temperature thermal annealing of the one or more metallic nanomaterials within a temperature range of 75-150℃.
[0087] In one embodiment, the short-chain molecular material may include gallic acid (GA) , and wherein carboxylic acid groups in the GA molecule interact with silver and generate ionic bonds, and hydroxyl groups in the GA also interacts with silver and being connected by hydrogen bonds.
[0088] In one embodiment, the solution-processed metallic nanoparticle reflective electrode realizes a sheet resistance of lower than 20Ω / sq, as well as achieving an average reflectance in the visible region over 50%. For instance, the sheet resistance is lower than 15Ω / sq, lower than 10Ω / sq, or lower than 5Ω / sq. The average reflectance in the visible region is more than 60%, 70%, 80%, or 90%.
[0089] Preferably, the present invention provides a strategy for electrodes for electronic applications based on a spray-coated, highly reflective AgNP electrode with a sheet resistance of 1.6 Ω·sq-1 and average reflectance of 92%.
[0090] In one embodiment, the reflectance of the solution-processed conductive film contains 25%diffused reflection.
[0091] In one embodiment, the AgNP electrodes can show a thickness in a range of 200-400 nm.
[0092] Preferably, the AgNP electrodes have a thickness of 300 nm.
[0093] In another aspect, the present invention provides an evaporation-free organic solar cell (OSC) . It includes a top electrode using said AgNP electrodes, an active layer and a bottom electrode. Benefiting from the superior electrical and optical properties of the AgNP electrodes, evaporation-free OSCs exhibit a record PCE of at least 10%for a large-area device (1 cm2) , outperforming other fully solution-processed large-area OSCs.
[0094] Preferably, the organic solar cell exhibits a power conversion efficiency of at least 14.69%for a large-area device.
[0095] In another embodiment, the evaporation-free organic solar cell further includes at least one interfacial layer. The at least one interfacial layer may include a hole transport layer and / or an electron transport layer.
[0096] In one embodiment, the solution-processed metallic nanoparticle reflective electrode has a conductivity of at least 30×106 S / m. Preferably, the solution-processed metallic nanoparticle reflective electrode has a conductivity of 42×106 S / m.
[0097] In conclusion, the present invention provides a strategy for electrodes for electronic applications based on a spray-coated, highly reflective AgNP electrode with a sheet resistance of 1.6 Ω·sq-1 and average reflectance of 92%. Fundamentally, the bottom-up process of metallic nanoparticles with different ligands is systematically studied. Ligands with compact structures and multiple functional groups, such as gallic acid, can lead to a high space proportion of metal in stacked films and compact packing during the stacking procedure.
[0098] EXAMPLE
[0099] Example 1
[0100] Regents and Materials
[0101] Silver acetate dihydrate (AgAC·2H2O, 99%) , gallic acid (GA, 98%) , n-butylamine (NBA, 99%) , methanol (MeOH, 99.5%) , ethanol (EtOH, 99.5%) , polyethylenimine (PEI, branched, Mn 25000) , zinc acetate dihydrate (ZnAC2·2H2O, 99.9%) , and 2-methoxyethanol (99%) are purchased from J&K. PEDOT: PSS (Al4083) is purchased from H. C. Starck GmbH, Germany. D18-Cl and N3 are purchased from eFlexPV Limited. Chloroform (CF, 99.9%) and 1-chloronaphthalene (CN, 97%) were purchased from Sigma-Aldrich. AgNP-PVP and AgNP-TCA are purchased from Zhongkekeyou.
[0102] Particle, thin film electrode, and device characterization
[0103] The surface charge of nanoparticles is characterized by ZetaView Nanoparticle Tracking Analyzer. The surface morphology of the AgNP films before and after annealing is characterized by scanning electron microscopy (SEM, Hitachi S4800 FEG) , transmission electron microscopy (TEM, Philips Tecnai G2 20 S-TWIN) , and atomic force microscopy (AFM, NT-MDT NTEGRA, taping mode) . The optical characteristics are measured by UV-Vis spectroscopy (SHIMADZU UV-2600) . The total and diffused reflectance are measured with an integrating sphere attachment. The resistance and sheet resistance are measured by the multimeter and the four-point probe, respectively. The X-ray photoelectron spectroscopy (XPS) and ultraviolet photoelectron spectroscopy (UPS) of the AgNP films annealed at different temperatures are conducted by Physical Electronics PHI 5802. The device performances of OSCs are characterized by Keithley 2635 under AM 1.5G irradiation (100 mA / cm2) . The light intensity is calibrated by a silicon reference cell (ISO 17025-certified KG3-filtered) . The device areas of the OSCs are 0.08 and 1 cm2, controlled by the shadow masks.
[0104] Example 2-Preparation of GA-assisted AgNPs
[0105] AgNP-GA was synthesized by a room temperature process, as shown in FIG. 25A reduced from silver acetate dihydrate (AgAC·2H2O) . Silver acetate dihydrate (AgAC·2H2O) was selected as the Ag source, dispersed in methanol. Gallic acid (GA) was employed as the reductant and stabilizer in this system.
[0106] Firstly, AgAC·H2O (0.167 g) was added into methanol (6 mL) and stirred for 5 min. At the same time, gallic acid (0.092 g for GA*1 or 0.276 g for GA*3) was dissolved in methanol (10 mL) . The fully dissolved GA solution was quickly added into the AgAC solution dropwise and kept stirring fiercely. After 10 minutes, n-butylamine (10 uL) was dropped into the stirred solution, and the solution reacted for another 10 minutes. The product was centrifuged and washed with methanol (15 mL) three times. The final sediment was dispersed in 1 mL ethanol and kept in the refrigerator before being used.
[0107] The reaction mechanism can be dispersed as follows: Ag+ + GA-→ Ag-GA, (1) NBA + MeOH → NBAH+ + MeO-, (2) GA (C-OH) (reductant) + Ag-GA + MeO-→ GA (C=O) + Ag↓ + MeOH + GA-, (3) NBAH+ + GA-→ NBA + GA. (4)
[0108] FIG. 1A presented the facile synthesis process of GA-assisted AgNPs. N-butylamine (NBA) was selected as the catalyst because of its low boiling point. The inset scanning electron microscope (SEM) image exhibited the morphology of particles. Notably, the GA-assisted AgNPs presented a uniform distribution of particle size and superior storage stability, which was compatible with commercial applications.
[0109] Example 3-Preparation of GA-assisted AgNP electrode in an evaporation-free organic solar cell
[0110] Performing as the solution-processed top electrodes on OSCs, AgNPs should be coated gently on the top of the device with few influences on the underneath layers. Spin-coating, blade-coating, spray-coating, and slot-casting are commonly used methods for solution-processed deposition. Compared to other methods, spray-coating deposition is least affected by the solvents due to the rapid evaporation of microdroplets. Therefore, the AgNP electrodes were fabricated by spray coating with a portable spray gun, as shown in FIG. 1B. A cover mask was employed during spray-coating to introduce the expected patterns. The top and bottom views of an actual OSC with a spray-coated electrode were also exhibited in FIG. 1B, demonstrating no visible damage after AgNPs deposition.
[0111] Moreover, the fresh AgNP electrodes were barely conductive because of the insulating ligands between particles. Typically, the thermal agglomerating process for AgNP electrodes was conducted at over 200 ℃, which was incompatible with OSC manufacture. Differently, the present invention employed a low-temperature agglomerating process to improve the conductivity of AgNP films. The TEM images of AgNPs before and after annealing were conducted to verify the agglomerating process, as shown in FIGs. 1C-1D. The corresponding electron diffraction patterns were also shown in the inset images. Prior to the annealing process, the boundaries between AgNPs were distinct. However, after annealing, these boundaries vanish, suggesting interparticle contact, which enhanced the conductivity of the film. In the electron diffraction patterns, the diffraction rings of Ag presented a polycrystalline structure. In contrast, the annealed AgNPs showed the same rings with some conspicuous spots, indicating that the Ag-based film generated some strong lattice orientations in the polycrystalline structure. This result was consistent with the TEM images. As a result, the annealed AgNP electrodes achieved high conductivity.
[0112] GA-assisted AgNP electrodes presented simultaneously higher conductivity and reflectance. A widely reported AgNP synthesized with common oleyamine (AgNP-OA) , and an evaporated silver film (E-Ag) weres used for comparison in FIG. 1E. The conductivities and average reflectances (400-900 nm) , which were the most critical characteristics of rear electrodes, presented as 26×106 S / m and 47%for AgNP-OA, 34×106 S / m and 94%for E-Ag, and 42×106 S / m and 92%for GA-assisted AgNP electrodes. The GA-assisted AgNPs showed the best performance among all solution-processed rear electrodes to our best knowledge, comparable to evaporated ones and much higher than the AgNP-OA. In a word, GA-assisted AgNPs presented great potential as a rear electrode due to its superior electrical and optical properties.
[0113] Although the AgNP-GA thin films exhibited a great performance of conductivity and reflectance, the fundamental mechanism to realize high-quality particle-related electrodes is not clear yet. Thus, a comprehensive elaboration on thin film formation with metallic nanoparticles was demonstrated in FIG. 2.
[0114] To declare the outstanding role of ligands in film formation, GA and OA were chosen as candidates. During the bottom-up formation process from nanoparticles to bulk films, the organic ligands significantly influenced the film quality in several aspects: Firstly, the molecular structure and chain length of ligands determined the microscopic morphology of AgNPs. GA and OA, which had different molecular structures and carbon chain lengths (shown in FIGs. 2A-2D) , were employed as the stabilized ligands of AgNPs. FIGs. 2B-2C displayed the schematic diagram of two contacted GA-covered and OA-covered AgNPs. GA had a compact molecular structure and several functional groups which were able to interact with AgNP, while OA contained only one functional group, which was able to interact with Ag, and a long carbon chain tail.
[0115] As a result, the AgNP-GA and AgNP-OA were recognized as ‘hard’ and ‘soft’ spheres, respectively, during the stacking of particles. Moreover, because of the steric hindrance, there were always outward-facing functional groups of GA, which might interact with neighborhood particles, benefiting the electrostatic adherence ability of AgNP-GA. On the contrary, the long carbon chain tails of OA prevented the interaction between particles.
[0116] The schematic diagrams of the particle assembly of AgNP-GA and AgNP-OA were shown in FIGs. 2F-2G. The adherence ability of AgNP-GA contributed to a compactly contacted cluster of particles, while AgNP-OA seemed relatively loose. The TEM images of two types of AgNPs were exhibited in FIGs. 2E-2H and showed consistent particle distribution with the previous statements. In addition, the space proportion of silver (Agsp) was significantly influenced by the particle structure. The ratios of the diameter of the silver sphere (D) to the length between spheres (L) were D / L = about 250 of AgNP-GA and D / L = about 3 of AgNP-OA, indicating that the AgNP-GA thin film could achieve a much higher space proportion of silver compared to AgNP-OA. It was assumed that the particles were uniform and stacked in hexagonal close packing. The average density of particles, including metal and ligands, was about 74%. Thus, the maximum Agsp was about 73.1%of AgNP-GA, much larger than 46.6%of the AgNP-OA. It’s worth noting that the space proportion of silver in the thin films greatly affected the particle agglomerating and characteristics of the final products.
[0117] In one embodiment, the one or more metallic nanomaterials had a diameter in a range of 1-900 nm.
[0118] Example 4-Stacking and agglomeration methods
[0119] Similar to other solid thin film stacking, the nanoparticle stacking method was also combined with stacking and smoothing processes at the same time. However, the electrostatic adherence ability made the stacking a little different from others. FIGs. 3A-3C were the schematic diagrams of the particle stacking procedure, containing adherence and smoothing steps. The stacking procedure could be described as follows: (1) The particles in the first layer were closely packed due to electrostatic incorporation during the initial stage. Only a small portion of smaller particles sit on the edges of larger ones; otherwise, they would displace the particles underneath; (2) As the stacking and smoothing of AgNPs continue, a majority of the particles settled onto the substrate, enhancing the density of AgNPs in the first layer. This increased density stabilized the layer, facilitating the formation of subsequent layers.
[0120] The detailed stacking procedure of AgNP-GA was shown in FIG. 3D, the TEM images with different spray cycles demonstrated consistent results as the above statements. Thus, the schematic diagrams of stacked AgNP-GA and AgNP-OA were demonstrated in FIGs. 2J-2K, in which the former was a little bit tighter than the latter because of the electrostatic adherence process.
[0121] To be employed as conductive thin films on optoelectronic devices, AgNPs must be agglomerated by a soft treatment, such as low-temperature annealing. Thus, both types of AgNPs were annealed at 100 ℃, and the schematic diagrams were exhibited in FIGs. 2I-2L. Also, the corresponding SEM images of AgNPs before and after annealing were attached below. The annealed AgNP-GA film demonstrated a continuous surface with some larger-scaled crystal-like morphology. While the OA-covered particles failed to sinter because of the thermal stable ligand and large interspace. The AFM images of as-cast and agglomerated AgNP-GA films were shown in FIGs. 4A-4B. Their route mean squares (RMS) were 5.252 nm and 12.332 nm, respectively, indicating that the roughness of the AgNP films increased after thermal agglomerating. The suitable roughness of Ag films could benefit diffuse reflectance.
[0122] In one embodiment, the low-temperature thermal annealing was conducted under 75℃ -150 ℃ for 5-20 minutes.
[0123] In addition, the time-varying TEM was conducted for both types of AgNPs, as shown in FIG. 5. The AgNP-GA easily agglomerated together under the e-beam illustration within 80 s, while AgNP-OA showed negligible change and kept isolated. Such result further proved that ligands significantly influenced the agglomerating process of AgNPs. Finally, at the end of the scale bar, the macroscopic products showed a dramatic difference in their electrical and optical properties (FIG. 2M) . The agglomerating temperature of GA-based particles was lower than 100 ℃, much lower than other commonly used particles, such as AgNP-OA at about 250 ℃ yet still with lower conductivity.
[0124] To avoid the influence of particle size and interparticle distance, polyvinylpyrrolidone (PVP) and trisodium citrate (TCA) -based silver nanoparticles were chosen to study the agglomerating behavior. The average particle sizes of AgNP-GA, AgNP-PVP, and AgNP-TCA were all around 50 nm. The TEM images of them were demonstrated in FIG. 6. PVP is known as a linear polymer with many amino groups on the chain, indicating the chain of PVP may lay on the particle surface, which is different from OA. TCA was selected as a small molecular ligand. AgNP-GA, AgNP-PVP, and AgNP-TCA had similar interparticle distance and particle size, resulting in a similar space proportion of Ag in the packed AgNP films. The thermal agglomerating behavior was demonstrated in FIG. 7. The agglomerating temperature of AgNP-PVP and -TCA were over 200 ℃, while AgNP-GA agglomerated at low than 100 ℃. As a consequence, after controlling for particle size and interparticle distance, GA-based AgNP showed ultralow thermal agglomerating temperature, owing to the unique capacity of its ligand.
[0125] Referring to FIG. 8, XRD measurement is conducted on AgNPs before and after annealing to investigate the sintering behavior. After annealing, the FWHM of Ag peaks in AgNP-GA decreased, suggesting the optimized crystallization of Ag thin film. In contrast, the peaks in AgNP-OA changed negligibly, suggesting a failure of sintering at low temperatures.
[0126] Moreover, the agglomerated AgNP-GA thin film achieved a broad range of high reflectance of over 90%, much higher than that of AgNP-OA (<50%) . The photograph of agglomerated AgNP films showed a great difference, in which GA-based product significantly turned metallic white at a low temperature of about 100 ℃, while the OA-based product showed negligible visible change after agglomerating at 250 ℃. Overall, the number of functional groups and carbon chain length of ligands sequentially influenced microstructure, stacking method, and agglomerating process of the silver particles, and finally presented different characteristics of the thin film. However, the extraordinary performance of AgNP-GA thin films was not solely attributed to the optimized stacking method and small interspace but also to other mechanisms that occurred during agglomeration.
[0127] As conductive electrodes, conductivity and reflectance were essential properties. FIGs. 9A-9B presented the resistance and reflectance of AgNP films. Step-wised temperatures were used for annealing the AgNP films. The resistances of each sample were recorded at different periods. FIG. 10A was the schematic diagram of the resistance measurement. The films were deposited on the 17 mm × 17 mm glass substrates, and the resistance was measured diagonally in a 14 mm × 14 mm square area by a multimeter.
[0128] A natural photograph of the resistance measurement was shown as an example in FIG. 10B. The resistances of the as-cast films were too large to be measured. It rapidly decreased to lower than 10 Ω with an annealing temperature higher than 100 ℃ in 5 min. The resistances of these samples after 15 minutes of annealing were 9.8×105 Ω for 75 ℃, 135 Ωfor 90 ℃, 2.2 Ω for 100 ℃, 0.6 Ω for 115 ℃, and 0.2 Ω for 130 ℃, respectively. In comparison, the evaporated silver electrode with a thickness of 100 nm had a resistance of 1.4 Ω, similar to the AgNP film annealed at 100 ℃. This demonstrated the significant potential of the AgNP film as conductive electrodes, owing to its exceptional conductivity.
[0129] Even if the temperature was 75℃, the AgNPs could be agglomerated slowly but steadily. This was beneficial for temperature-sensitive applications. The reflectance spectra of the agglomerated AgNP films and evaporated Ag electrodes were exhibited in FIG. 9B. The fully agglomerated AgNP film presented a similar reflectance to the evaporated Ag electrode in the long wavelength region. The highest reflectance of the SAE was 96%, making it ideal for use as a rear electrode in photovoltaic applications. The slightly low reflectance of the SAE in the short wavelength region was caused by the film's original particle shape and pinhole structure, which may slightly decrease the light reabsorption in solar cells. In contrast, the diffuse reflectance of the SAE was much higher than evaporated Ag. The average diffuse reflectance in the visible region was about 25%. High reflectance haze and the aperiodic nanoscale surface undulation may benefit light absorption in the solar cells, contributed by the light scattering and light distribution manipulation. This favorable effect induced by SAE may cover the slight reflectance shortage and improve the final absorption efficiency of solar cells.
[0130] The electrical and optical characteristics of AgNP films with different thicknesses were exhibited in FIGs. 11A-11D. The samples were prepared by a spin-coating process with different solution drops. The reflectance of the films increased along with the drop times, and the transmittance decreased as expected. FIG. 11C showed the statistic diagram of the average reflectance and the corresponding sheet resistance. When only one drop solution was used in deposition, the film presented poor conductivity because of the poor coverage of AgNPs. The diffuse reflectance of one drop sample also proved it. The diffuse reflectance spectrum of one drop sample showed a wavelength-independent performance, indicating the sizeable uncovered area, which was consistent with the conductivity characterization. Two or more drops of solution could fabricate an electrode with good conductivity and suitable reflectance. Referring to FIG. 11D, the cross-section SEM was measured to check the thickness of AgNP film deposited by the drop-wised spin-coating method. Twenty drops of solution spun at 2000 rpm led to a 1440 nm-thick film. In a word, the solution-processed AgNP films exhibited superior electrical and optical properties for rear electrodes.
[0131] The sintering mechanism of the AgNPs is crucial in selecting the specific ligand. Before delving into the sintering mechanism, it is essential to describe the stabilizing effect of the GA material first. The carboxylic acid groups (COO-) in the GA molecule easily interacted with Ag, forming ionic bonds due to their negative and positive charges, respectively. Simultaneously, hydroxyl groups in GA also interacted with Ag, forming connections through hydrogen bonds (FIG. 12A) . The bonds strongly connected the GA and AgNPs in dispersing solution, and GA coverage prevented the aggregation of particles. Thus, sufficient GA ligands guaranteed the storage stability of AgNPs.
[0132] Unlike other stabilizing ligands, which typically consist of long-chain molecules, GA undergoes a decarboxylation reaction at a relatively low temperature (< 100 ℃) , assisted by a small amount of water. The decomposition process was verified by FTIR spectra of GA powers before and after annealing assisted with moisture, as demonstrated in FIG. 13. After the annealing process, the gallic acid powder generated two peaks at 2358 cm-1 and 1717 cm-1, representing CO2 and unsaturated ester, respectively. It verified that the decarboxylation of GA occurred during the heating process, and part of the carboxyl group was esterified with a hydroxyl group. At the same time, the peaks of carboxyl decreased a lot, consistent with the above statement. When the ionic bonds disappeared because of the decarboxylic reaction, the surface of AgNP became unstable.
[0133] After continuous annealing or annealing at a higher temperature, the hydrogen bonds between Ag and hydroxy were not strong enough to protect the AgNP surface. Pyrogallol or remaining GA may become isolated, and the AgNPs quickly sintered with each other. This statement of thermal decomposition was proved by the optical microscope (OM) images and X-ray photoelectron spectra (XPS) measurement, as shown in FIGs. 12B-12C. GA powder was annealed at different temperatures and observed by OM. The spot at the right corner was a marked point for positioning. There was a slight deformation after annealing at 100 ℃, indicating that the decarboxylic reaction of GA occurred. After annealing at 130 ℃, the GA almost disappeared, indicating the full decomposition of GA.
[0134] Moreover, fresh AgNP film and AgNP films annealed at different temperatures for 15 minutes were prepared to measure XPS characteristics. In FIG. 14A, the peaks of Ag 3d5 / 2 and Ag 3d3 / 2 were located at 368.2 eV and 374.2 eV, respectively. No peak shift occured during the whole annealing process. FIG. 14A also showed the O 1s and C 1s XPS spectra of the as-cast and the annealed AgNP films. The core-level spectra and relevant peak data were exhibited in FIGs. 12G-12I and FIG. 15. The energies were consistent with reported values for similar chemical bonds8-10. The peaks at 530.9 eV and 533.5 eV, representing C=O and C-OH, showed few changes after annealing at 100 ℃ for 15 min. However, the peak at 532.6 eV, assigned to -COOH, decreased significantly after annealing, indicating the removal of carboxyl groups. The ratio of carboxyl to the sum of hydroxyl and carbonyl decreased from 57.5%to 29.1%, demonstrating that 49%of carboxyl had been successfully decarboxylated. After annealing at 130 ℃ for 15 min, all the peaks decreased at a similar ratio, consistent with the statement of ligand removal. This declaration was also proved in the C 1s core-level spectra, in which four peaks were found and assigned to corresponding bonds. The peaks at 284.6 eV, 285.8 eV, 287.5 eV, and 288.4 eV represented the C=C, C-OH, C=O, and COOH, respectively. A plasmon loss peak induced by conductive materials also existed and located at 290.8 eV. The C-OH, C=O, and COOH peaks decreased along with the increased temperature, indicating that the decarboxylic reaction occured during the process. In conclusion, the annealing process on AgNP films could successfully produce the decarboxylic reaction and massively remove the GA or pyrogallol ligands from the AgNP surface.
[0135] FIG. 14B exhibited the Ag, C, and O mass concentrations in the as-cast and annealed AgNP films. The statistical data of the mass concentrations were listed in Table 1. The mass concentration of Ag increased from 85.60%to 88.80%and 92.37%after the 100 ℃ and 130 ℃annealing process. In contrast, the C and O concentrations in the AgNP films significantly reduced, especially at 130 ℃. It proved that the thermal treatment massively removed the organic compounds and made the film approach a relatively pure metallic structure. As a result, the sintered AgNP electrodes with few organic components successfully achieved high conductivity and high broadband reflectance.
[0136] Table 1-The statistical data of the mass concentrations of the Ag, C, and O elements in AgNP films before and after the annealing process.
[0137] Example 5
[0138] Organic solar cell fabrication
[0139] In this example, the high-performance device structure of organic solar cells was glass / ITO / PEDOT: PSS / D18-Cl: N3 / PEI-Zn / evaporated Ag (E-Ag) or SAE. The glass / ITO substrates (15 Ω sq-1) were cleaned with detergent, acetone, and ethanol by ultrasonic cleaning successively. Each cleaning process lasted for 15 minutes. The cleaned substrates were stored in ethanol for reserve. The ITO substrates were blown with N2 and treated with ultraviolet ozone (UVO) for 15 minutes. PEDOT: PSS was deposited on the treated substrates by spin-coating at 4000 rpm for 40 s and annealed at 150 ℃ for 20 min. After cooling down, the substrates were transferred into the N2-filled glovebox for the following depositions. D18-Cl: N3: PC61BM (5 mg: 7 mg: 0.5mg in 1 mL chloroform with 0.5 vol%1-chloronaphthalene as additive) solutions were prepared in advance. It was dynamically spin-coated on the PEDOT: PSS films at 2500 rpm for 30 s and annealed at 90 ℃ for 10 min. The PEI-Zn was prepared following the reported literature (1 mg PEI, 10 uL H2O, and 0.075g ZnAC2·2H2O are dissolved in 1 mL 2-methoxyethanol) . The PEI-Zn precursor was deposited on the active layers by dynamic spin-coating at 3000 rpm for 30 s and annealed at 100 ℃ for 10 min.
[0140] Then, the resulting samples were deposited with top electrodes to complete the fabrication. The evaporated silver electrodes (100 nm) were deposited in the high-vacuum thermal evaporation system. SAEs were fabricated by spin-or spray-coating process. AgNP solution (30 uL) was dynamic spin-coated at 3000 rpm drop by drop and annealed at 130 ℃ for 5 min. A portable spray gun was employed for coating the SAE. The diluted AgNP solution (300 uL, 1: 10 in ethanol) was sprayed on the samples covered with a patterned mask. The annealing process was also conducted to sinter the electrodes.
[0141] The universal applications of SAE were prepared on various structures assisted with many materials. The preparation and deposition of each material were as follows: P3HT: PC61BM (20mg: 20mg in 1mL Dichlorobenzene) was coated at 700 rpm for 40 s and slowly grew for 1 h. PBDB-T: ITIC (10mg: 10mg in 1mL Chlorobenzene with 0.3 vol%DIO) was coated at 2500 rpm for 40 s and annealed at 100 ℃ for 10 min. MoO solution was prepared following previous work and coated at 2500 rpm for 40 s. PEDOT: PSS (0.5%triton) was a mixture of PEDOT: PSS and 0.5 vol%triton x100. It was coated on the active layer at 2000 rpm for 40 s and annealed at 140 ℃ for 10 min. ZnO s-g was prepared by dissolving zinc acetate dehydrate (Zn (CH3COO) 2·2H2O, 110 mg) in ethanolamine (NH2CH2CH2OH, 30 μL) , and 2-methoxyethanol (1 mL) with vigorous stirring for 12 h. It was deposited by spin coating at 4000 rpm for 40 s and annealing at 150 ℃ for 20 min.
[0142] The solution-processed AgNP electrode was employed in OSCs to demonstrate its suitability for electronic devices. The device structure was glass / ITO / PEDOT: PSS / D18-Cl: N3: PC61BM / PEI-Zn / SAE. FIG. 16A showed the cross-section scanning electron microscope (SEM) image of the OSC. D18-Cl and N3 were employed as the absorption materials for high-performance OSCs, and the illustrative structure diagrams of D18-Cl, N3, and PC61BM were exhibited in FIG. 17. PEI-Zn was chosen to replace commonly used electron-transporting layers, such as PDINO and ZnO nanoparticles, due to its polymer compounds, which could withstand solution deposition of top electrodes. The amine groups in PEI-Zn were expected to interact with AgNPs and helped to form an ideal interface. The AgNPs were uniformly deposited on the top of the device, and the underlying layers kept in good condition after the spray-coating deposition. The SAE was deposited by spray-coating with a portable spray gun, as shown in FIGs. 18A-18B. The OSCs with evaporated silver rear electrodes (E-Ag) were also fabricated for comparison. The statistical characteristics of the OSCs were exhibited in FIGs. 19A-19B, and the relevant data were listed in Table 2.
[0143] Table 2-The statistical characteristics of the OSC devices with E-Ag and SAE measured with AM 1.5G. The device area is 0.08 cm2.
[0144] All the devices were measured under A. M. 1.5 illumination and calibrated with a standard silicon cell. The SAE-based OSCs presented an average open-circuit voltage (VOC) of 0.802 V, slightly lower than the E-Ag-based devices. The possible reason for the decrement may be the lower work function of the rear electrodes. The work functions of SAEs were characterized by ultraviolet photoelectron spectroscopy (UPS) , as presented in FIG. 20A. The SAE sintered at 130 ℃ showed a work function of -4.45 eV, slightly lower than the E-Ag (-4.30 eV) . The schematic energy diagram of the OSC with different rear electrodes was also exhibited in FIG. 20B. Rear electrodes in the conventional OSCs performed as the cathode and contacted with an electron transporting layer (ETL) . Generally, the small energy offset between ETL and cathode resulted in a high electron extraction efficiency. The energy offset between PEI-Zn and SAE was larger than that between PEI-Zn and E-Ag, indicating slight energy loss at the interface. It was also expressed in the average fill factor, decreasing from 72%to 67.66%. However, benefiting from the excellent reflecting properties of SAEs, containing high total and diffuse reflectance, the OSCs'a verage current density (JSC) increased from 26.59 mA / cm2 (E-Ag) to 27.04 mA / cm2 (SAE) . The EQE spectrum and the corresponding integrated JSC of the SAE-based OSCs were exhibited in FIG. 21. The integrated JSC was 26.17 mA / cm2, considered within the test error range. As a result, the average power conversion efficiencies (PCEs) were 15.92%for E-Ag and 14.67%for SAE. The J-V characteristics of champion devices with E-Ag and SAE were diagramed in FIG. 19B. The SAE-based OSC showed a VOC of 0.815 V, JSC of 27.16 mA / cm2, and FF of 68.85%, contributing to the champion PCE of 15.23%. The decrement in the device performance may mainly cause by the unsuitable work function and the imperfect interfacial contact induced by particle movement during the sintering process. The performance of the evaporation-free device could be improved with further interfacial research. Nevertheless, this represented the highest performance achieved by OSCs with a solution-processed top electrode. A large area device (1 cm2) was fabricated, and the J-V curve was shown in FIG. 16B. It presented a VOC of 0.817 V, JSC of 26.90 mA / cm2, and FF of 66.85%, resulting in the highest PCE of 14.69%. The inset photo was the large-area OSC with SAE. FIG. 16C exhibited the evolution of large-area OSCs with various solution-processed top electrodes, such as PEDO: PSS, AgNW, Ag ink, AgNP, and composite materials. Notably, devices utilizing SAE demonstrated superior performance compared to all previously reported ones in terms of large-area performance. Therefore, the exceptional performance of SAE-based OSCs highlighted the potential of SAE for evaporation-free OSCs and large-scale applications.
[0145] To verify the universality of this new electrode, various OSC devices were fabricated and demonstrated in FIGs. 22A-22D and Table 3. FIGs. 22 A-22D depicted the universal application of AgNP-GA electrode on various structures of OSCs. The solid lines represented devices with evaporated Ag electrodes and dash lines represented devices. AgNP electrodes were employed on the conventional and inverted structure with the device structure of ITO / PEDOT: PSS / P3HT: PCBM / ZnONP / AgNP and ITO / ZnO / P3HT: PCBM / MoO / AgNP, respectively. Different ETLs and HTLs were used to contact AgNP electrodes. For example, ZnO nanoparticles and PEI-Zn worked as ETL in conventional OSCs, and MoO and PEDOT: PSS worked as HTL in inverted OSCs.
[0146] Table 3-Summary of device structures and performance parameters of various OSCs made from AgNP-GA electrodes and evaporated Ag electrodes.
[0147] In addition, three kinds of active layers were employed to present the universal of AgNP electrodes. All the above devices were displayed together with reference devices with evaporated Ag electrodes and showed ideal power conversion efficiencies on the same level. Electrochemical impedance spectroscopy (EIS) measurement was used for analyzing the charge behavior in OSC devices, and the results were displayed in FIG. 16D. After fitting with the classical PV model, the series resistance (RS) , transfer resistance (R1) , and charge recombination resistance (R2) could be achieved (for device with E-Ag, RS = 27.5 Ω, R1 = 260 Ω, R2 = 1375 Ω; for device with AgNP, RS = 27.8 Ω, R1 = 250 Ω, R2 = 1592 Ω. ) . The transfer resistance of the OSC device with AgNP electrode changed little compared to the reference device with E-Ag electrode. And recombination resistance showed a slight and acceptable reduction.
[0148] To further investigate the charge recombination dynamics, the light intensity (IL) dependence of J-V characteristics was analyzed at ranging from 10 to 100 mW / cm2 (FIG. 16E) . Then, dependence of JSC on the light intensity was exhibited to quantify the bimolecular recombination. The slops of the logarithm of JSC to the logarithm of IL of OSC with E-Ag and AgNP electrodes were 0.991 and 0.997, respectively, and both were close to 1. It demonstrated the absence of bimolecular recombination in both devices. Moreover, to evaluate the trap-related recombination, the dependence of VOC on IL was measured and shown in FIG. 16E. Typically, the VOC and logarithm of IL followed the relationship: VOC∝n (kT / q) ln (IL) ,
[0149] where k was Boltzmann's constant, T was the temperature in Kelvin, and q was the elementary charge. The fitted n for E-Ag and AgNP-related devices were 1.11 and 1.13, respectively. A little bit higher n value for AgNP one represented slightly more trap-assisted recombination in this device. Overall, the AgNP-GA electrode demonstrated similar characteristics in OSCs. In addition, the operation stability of OSCs with E-Ag and AgNP-GA was measured and shown in FIGs. 23A-23D. The measurement was conducted in air condition (T= 30 ℃; RH= 60%) and under continuous light tracking at the maximum power point. The device structures were glass / ITO / PEDOT: PSS / P3HT: PCBM / PEI-Zn / E-Ag or AgNP. Compared with evaporated Ag, solution-processed AgNP electrodes displayed a little bit of poor stability at the first 80 h, indicating that the AgNP electrode was not as compact as evaporated Ag and made oxygen and moisture permeate into the device quickly.
[0150] However, the long-term stability (180 h) of the two devices was similar, suggesting AgNP electrode did not contribute to other chemical or interface degradations. In general, the isolation of oxygen and moisture for OSCs could be solved by ideal encapsulation. As a result, the AgNP STE would not destroy the device stability compared with evaporated one. These results were expected to exhibit AgNP electrode’s universal for the OSC community. Furthermore, LEDs were known as important components in the optoelectronic area. An OLED device with a common structure of ITO / PEDOT: PSS / TAPC / Alq / LiF / E-Ag or AgNP is also exhibited in FIGs. 24A-24C. The AgNP electrode worked well on the top of the OLED device and contributed to the almost same EL spectrum as the reference device, peaking at 529 nm. The turn-on voltages were 5.3 V for E-Ag and 5.8 V for AgNP. A little bit higher voltage in J-V curves indicated a slightly worse charge injection at the interface. The EQE of these two devices was 1.49%and 1.41%, respectively, both of which were at similar levels. In conclusion, solution-processed AgNP electrodes could also perform well on top of OLED devices.
[0151] Example 6
[0152] Effect of GA concentration on the particle size distributions and the storage stability
[0153] As shown in Example 2, when GA was added to the Ag-source solution, it quickly connected to the Ag+ (shown in equation 1) and made the dispersion uniform. The NBA acted as a catalyst for accelerating the reaction. In equation 3, the hydroxy in GA reduced the Ag+and generated Ag particles. Finally, the GA (COOH) became the stabilized ligands at the surface of Ag nanoparticles due to the interaction between -COOH and Ag.
[0154] The amount of the GA significantly influenced the particle size distributions and the storage stability of the products. Two different amounts of GA-based AgNPs (named GA*1 and GA*3) were applied to analyze the influence. FIGs. 25B-25C showed the SEM images and the particle size distribution of the AgNP films of GA*1 (9.2 mg / mL) and GA*3 (27.6 mg / mL) . It found that a large amount of GA significantly changed the particle size distribution. GA*3 presented a slightly smaller average particle size (45.7 nm) than GA*1 (51.4 nm) . However, the standard deviations of particle sizes for GA*1 and GA*3 were 21.1 nm and 13.2 nm, indicating that the size distribution of GA*3 was much more uniform than GA*1. The possible mechanism of the distribution change was that large amounts of GA ligand in the solution could mix well with the Ag source at the beginning of the reaction. All the Ag sources reduced at a similar rate and stopped growing at a similar period because of the high intensity of stabilized ligands.
[0155] On the contrary, the absence of gallic acid (GA) resulted in isolated silver sources, which reacted rapidly and aggregated into larger particles. Moreover, the lack of GA ligand in the final products contributed to poor storage stability (FIG. 25D) . After low-temperature storage for 30 days, the particle size distribution of GA*1 significantly changed. The average size of AgNPs almost doubled, and the largest particle reached 170 nm, which was adverse for film deposition. The GA*3 showed superior storage stability and almost consistent size distribution after 30 days. The respective distribution diagrams for GA*1 and GA*3 at different periods were presented in FIG. 26.
[0156] Sufficient GA ligands in the synthesis process helped to control the reaction speed and achieved particles of uniform size. Additionally, they improved the storage stability of AgNPs, benefiting from GA's stabilizing effects. Good storage stability is an indispensable feature of nanoparticles for commercial applications. Throughout the rest of the present invention, all the characterizations and applications were based on GA*3 silver nanoparticles (AgNP-GA) . The surface charge of the particles was almost neutral, and the Zeta potential of the AgNP-GA at 25 ℃ was -10.37 mV (FIG. 27) .
[0157] From the 2D plots of the GISAXS in FIG. 28, the nanoparticles with GA as the ligand showed a random packing status while the one with OA packed more orderly, representing by the appearance of a ring-like pattern in GISAXS. The intensity profile along the qr direction was also obtained and shown in FIG. 29A. The main feature of AgNP-GA was located at qr around The feature of AgNP-OA was located at roughly corresponding to the particle size measured via TEM.
[0158] Assuming there are a hard sphere interactions between Ag nanoparticles, the interparticle potential is:
[0159] From the intensity profile in FIG. 29B, the structure factor S (q) could be obtained. The interparticle distance was calculated via the following formula:
[0160] The determined interparticle distances was 3.1nm for AgNP-OA and 0.2 nm for AgNP-GA.
[0161] The solution-processed AgNP electrodes were deposited by spin-or spray-coating processes. AgNP-GA solution (30 uL) was spin-coated at 2000 rpm on the cleaned glass substrates for morphology characteristics and electrical and optical measurements if there was no special instruction. The films were annealed at different temperatures to achieve good conductivity and high reflectance.Industrial Applicability:
[0162] A low-temperature annealing process can rapidly sinter the AgNPs into a highly conductive electrode with high reflectance which can be robustly formed on OSCs as top electrodes without penetrating the underlying layers, assisted by the composite PEI-Zn layer.
[0163] The present invention achieves evaporation-free OSC with a PCE of 15.23%, about 91%of evaporated ones. In catering to the scale-up applications, a large area device (1 cm2) presents a PCE of 14.69%, which is the highest performance of same-size evaporation-free OSCs compared to prior art. Moreover, various structures of OSCs and even OLED have been successfully employed to verify the universality of this AgNP electrode. Overall, the integrated statement of the ligand-dominated stacking and sintering process from the bottom up is a meaningful advancement in the field of metallic nanoparticle synthesis and application. It not only contributes to realizing the high-quality solution-processed electrodes but also will benefit further research in other nanomaterial-related electronic or biological contexts.
[0164] The foregoing description of the present invention has been provided for the purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise forms disclosed. Many modifications and variations will be apparent to the practitioner skilled in the art.
[0165] The embodiments were chosen and described in order to best explain the principles of the invention and its practical application, thereby enabling others skilled in the art to understand the invention for various embodiments and with various modifications that are suited to the particular use contemplated.
[0166] Definitions
[0167] Throughout this specification, unless the context requires otherwise, the word "comprise" or variations such as "comprises" or "comprising" , will be understood to imply the inclusion of a stated integer or group of integers but not the exclusion of any other integer or group of integers. It is also noted that in this disclosure and particularly in the claims and / or paragraphs, terms such as “comprises” , “comprised” , “comprising” and the like can have the meaning attributed to it in U. S. Patent law; e.g., they allow for elements not explicitly recited, but exclude elements that are found in the prior art or that affect a basic or novel characteristic of the present invention.
[0168] Furthermore, throughout the specification and claims, unless the context requires otherwise, the word “include” or variations such as “includes” or “including” , will be understood to imply the inclusion of a stated integer or group of integers but not the exclusion of any other integer or group of integers.
[0169] As used herein and not otherwise defined, the terms "substantially, " "substantial, " "approximately" and "about" are used to describe and account for small variations. When used in conjunction with an event or circumstance, the terms can encompass instances in which the event or circumstance occurs precisely as well as instances in which the event or circumstance occurs to a close approximation. For example, when used in conjunction with a numerical value, the terms can encompass a range of variation of less than or equal to ±10%of that numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%.
[0170] References in the specification to “one embodiment” , “an embodiment” , “an example embodiment” , etc., indicate that the embodiment described can include a particular feature, structure, or characteristic, but every embodiment may not necessarily include the particular feature, structure, or characteristic. Moreover, such phrases are not necessarily referring to the same embodiment. Further, when a particular feature, structure, or characteristic is described in connection with an embodiment, it is submitted that it is within the knowledge of one skilled in the art to affect such feature, structure, or characteristic in connection with other embodiments whether or not explicitly described.
[0171] In the methods of preparation described herein, the steps can be carried out in any order without departing from the principles of the invention, except when a temporal or operational sequence is explicitly recited. Recitation in a claim to the effect that first a step is performed, and then several other steps are subsequently performed, shall be taken to mean that the first step is performed before any of the other steps, but the other steps can be performed in any suitable sequence, unless a sequence is further recited within the other steps. For example, claim elements that recite “Step A, Step B, Step C, Step D, and Step E” shall be construed to mean step A is carried out first, step E is carried out last, and steps B, C, and D can be carried out in any sequence between steps A and E, and that the sequence still falls within the literal scope of the claimed process. A given step or sub-set of steps can also be repeated. Furthermore, specified steps can be carried out concurrently unless explicit claim language recites that they be carried out separately.
[0172] Other definitions for selected terms used herein may be found within the detailed description of the present invention and apply throughout. Unless otherwise defined, all other technical terms used herein have the same meaning as commonly understood to one of ordinary skill in the art to which the present invention belongs.
[0173] References: The disclosures of the following references are incorporated by reference
[0174] 1. G. Steven Bales, Robijn Bruinsma, Elliott A. Eklund, R.P.U. Karunasiri, Joseph Rudnick and A. Zangwill, Science, 1990, 249, 264-268.
[0175] 2. R. L. Whetten, M.N. Shafigullin, J.T. Khoury, T.G. Schaaff, I. Vezmar, M.M. Alvarez and A. Wilkinson, Acc. Chem. Res., 1999, 32, 397-406.
[0176] 3. H. Moreira, J. Grisolia, N.M. Sangeetha, N. Decorde, C. Farcau, B. Viallet, K. Chen, G. Viau and L. Ressier, Nanotechnology, 2013, 24, 095701.
[0177] 4. K.G. Stamplecoskie and J.C. Scaiano, J. Am. Chem. Soc., 2010, 132, 1825-1827.
[0178] 5. X. Ding, C.H. Liow, M. Zhang, R. Huang, C. Li, H. Shen, M. Liu, Y. Zou, N. Gao, Z. Zhang, Y. Li, Q. Wang, S. Li and J. Jiang, J. Am. Chem. Soc., 2014, 136, 15684-15693.
[0179] 6. H. Ammari, Y. Deng and P. Millien, Arch. Ration. Mech. Anal., 2015, 220, 109-153.
[0180] 7. S. -H. Jeong, H. Choi, J.Y. Kim and T. -W. Lee, Part. Part. Syst. Charact., 2015, 32, 164-175.
[0181] 8. S.T. Jackson and R.G. Nuzzo, Appl. Surf. Sci., 1995, 90, 195-203.
[0182] 9. J.Y.Y. Loh and N.P. Kherani, Molecules, 2019, 24, 3818.
[0183] 10. G. Greczynski and L.Hultman, Prog. Mater. Sci.., 2020, 107, 100591.
Claims
1.A solution-processed metallic nanoparticle reflective electrode, comprising:a target substrate;a solution-processed conductive film coated on the target substrate, wherein the solution-processed conductive film comprises one or more metallic nanomaterials stabilized by one or more covered ligands,wherein the one or more covered ligands interact with adjacent metallic nanomaterials.2.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the one or more metallic nanomaterials comprise silver nanoparticles, gold nanoparticles, copper nanoparticles nickel nanoparticles, or aluminum nanoparticles.3.The solution-processed metallic nanoparticle reflective electrode of claim 2, wherein the solution-processed metallic nanoparticle reflective electrode comprises silver nanoparticles reflective electrode.4.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the one or more metallic nanomaterials comprise metal nanoparticles with Particle size of 1-200 nm, and a dispersity of >1mg / mL in solvent.5.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the one or more metallic nanomaterials are in a shape of particle, wire, rod, or plate.6.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the target substrate comprises silicon wafer, or glass.7.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the one or more covered ligands comprise short-chain molecular materials with 2-20 carbons in the main chain.8.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the solution-processed metallic nanoparticle reflective electrode realizes a sheet resistance of lower than 20Ω / sq.9.The solution-processed metallic nanoparticle reflective electrode of claim 8, wherein the solution-processed metallic nanoparticle reflective electrode realizes a sheet resistance of lower than 3Ω / sq.10.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the solution-processed conductive film achieves an average reflectance in the visible region over 90%.11.The solution-processed metallic nanoparticle reflective electrode of claim 10, the average reflectance of the solution-processed conductive film contains 25%diffused reflection.12.The solution-processed metallic nanoparticle reflective electrode of claim 1, wherein the solution-processed metallic nanoparticle reflective electrode has a conductivity of at least 30×106 S / m.13.The solution-processed metallic nanoparticle reflective electrode of claim 12, wherein the solution-processed metallic nanoparticle reflective electrode has a conductivity of 42×106 S / m.14.A method for forming a solution-processed conductive film, comprising:synthesizing one or more metallic nanomaterials stabilized by one or more covered ligands to form a solution-processed conductive film;stacking the one or more metallic nanomaterials on a target substrate; and agglomerating the one or more metallic nanomaterials to form the solution-processed conductive film.15.The method of claim 14, wherein step of synthesizing one or more metallic nanomaterials stabilized by one or more covered ligands further comprising adding a catalyst with a boiling point in a range of 30 to 400℃.16.The method of claim 15, wherein the catalyst comprises N-butylamine, Trimethylamine, dimethylethanolamine, or a combination thereof.17.The method of claim 14, wherein step of coating the one or more metallic nanomaterials on a target substrate is conducted by spin coating, spray coating, blade coating, slot-die coating, or dip coating.18.The method of claim 14, wherein step of agglomerating the one or more metallic nanomaterials comprises low-temperature thermal annealing of the one or more metallic nanomaterials within a temperature range of 75-150℃.19.The method of claim 14, wherein the one or more metallic nanomaterials have a particle size of 1-200 nm, and a dispersity of >1mg / mL.20.The method of claim 19, wherein the one or more metallic nanomaterials comprise silver nanoparticles, gold nanoparticles, copper nanoparticles nickel nanoparticles, or aluminum nanoparticles.21.The method of claim 14, wherein the one or more covered ligands comprise a short-chain molecular material with 2-20 carbons in the main chain.22.The method of claim 20 or claim 21, wherein the short-chain molecular material comprises gallic acid (GA) , and wherein carboxylic acid groups in the GA molecule interact with silver and generate ionic bonds, and hydroxyl groups in the GA also interacts with silver and being connected by hydrogen bonds.23.The method of claim 14, wherein the one or more metallic nanomaterials are in a shape of particle, wire, rod, or plate.24.The method of claim 14, wherein the target substrate comprises silicon wafer, or glass.25.An evaporation-free organic solar cell, comprising:a top electrode, wherein the top electrode is a solution-processed metallic nanoparticle reflective electrode;an active layer;a bottom electrode,wherein the organic solar cell exhibits a power conversion efficiency of at least 10%for a large-area device.26.The evaporation-free organic solar cell of claim 25, wherein the evaporation-free organic solar cell further comprises at least one interfacial layer.27.The evaporation-free organic solar cell of claim 26, wherein the at least one interfacial layer comprises a hole transport layer and / or an electron transport layer.
Citation Information
Patent Citations
Method for preparing transparent electrode of crystalline silicon solar cell
CN102544223A
Conductive metal paste composition and method of manufacturing the same
CN102651248A
Preparation method for crystalline silicon solar cell nanometer transparent buried gate electrode
CN102983212A
Metal nanoparticles and methods of making same
CN111511484A