Method for producing semiconductor photoelectrode

The method of growing and annealing indium gallium nitride thin films with a metal layer deposition addresses the surface roughness issue, enabling a uniform protective layer and sustained solar energy conversion efficiency in semiconductor photoelectrodes.

WO2024247230A1PCT designated stage expired Publication Date: 2024-12-05NT T INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/020524
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The manufacturing of semiconductor photoelectrodes, particularly indium gallium nitride thin films, faces challenges due to high surface roughness, which hinders the formation of a uniform protective layer, leading to decreased solar energy conversion efficiency as a result of etching reactions and impaired light transmission.

Method used

A method involving the growth of n-type gallium nitride and indium gallium nitride thin films, followed by annealing in a nitrogen or ammonia atmosphere, and the deposition of a metal layer for heat treatment, effectively reduces surface roughness and allows for the formation of a thin, uniform protective layer.

Benefits of technology

This approach enhances the longevity of solar energy conversion efficiency by suppressing etching reactions and maintaining high efficiency over extended periods by reducing surface roughness and ensuring effective light transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023020524_05122024_PF_FP_ABST
    Figure JP2023020524_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This method for producing a semiconductor photoelectrode includes: a step in which a first semiconductor thin film 12 of an n-type gallium nitride is formed on a substrate 11; a step in which a second semiconductor thin film of indium gallium nitride is grown on the surface of the first semiconductor thin film 12; a step in which the grown second semiconductor thin film 13 is subjected to an annealing treatment in a nitrogen or ammonia atmosphere; a step in which a metal layer 14 is formed on the surface of the second semiconductor thin film 13 after the annealing treatment; and a step in which the semiconductor thin film on which the metal layer 14 is formed is subjected to a heat treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing semiconductor photoelectrodes

[0001] The present disclosure relates to a method for manufacturing a semiconductor photoelectrode.

[0002] There is a device that generates hydrogen through a water splitting reaction using a semiconductor photoelectrode (Non-Patent Document 1). This device has an oxidation tank and a reduction tank. An aqueous solution and an oxidation electrode are placed in the oxidation tank. An aqueous solution and a reduction electrode are placed in the reduction tank. The oxidation tank and reduction tank are connected via a proton exchange membrane. The oxidation electrode and reduction electrode are electrically connected by a conductor.

[0003] The water splitting reaction using a photocatalyst consists of a water oxidation reaction and a proton reduction reaction. When light is irradiated onto an n-type photocatalytic material, electrons and holes are generated and separated within the photocatalyst. The holes move to the surface of the photocatalytic material and contribute to the water oxidation reaction. Meanwhile, the electrons move to the reduction electrode and contribute to the proton reduction reaction. Ideally, this oxidation-reduction reaction proceeds, resulting in the water splitting reaction.

[0004] Oxidation reaction: 2H2O + 4h + → O2 + 4H + Reduction reaction: 4H + + 4e - → 2H2

[0005] The oxidation electrode is a semiconductor thin film. For example, the oxidation electrode is a gallium nitride thin film grown on a sapphire substrate. When the gallium nitride thin film is irradiated with light in an aqueous solution, the target water oxidation reaction occurs on the gallium nitride surface, and a side reaction, an etching reaction of gallium nitride (GaN), occurs. As the etching reaction progresses, the reaction field where the target reaction can proceed decreases, and the solar energy conversion efficiency decreases within a few hours.

[0006] Etching reaction: 2GaN + 3H2O + 6h + → N2 + Ga2O3 + 6H +

[0007] S. Yotsuhashi, et al., “CO2Conversion with Light and Water by GaN Photoelectrode”, Japanese Journal of Applied Physics, The Japan Society of Applied Physics, 2012, Volume 51, pp. 02BP07-1-02BP07-3

[0008] Therefore, a structure that suppresses the etching reaction by forming a protective layer on the gallium nitride thin film can be considered, which minimizes contact between the aqueous solution and the gallium nitride thin film. If the protective layer is made thick, light transmission will be hindered depending on the thickness of the protective layer. It is preferable that the thickness of the protective layer is as thin as possible, such as approximately 5 nm or less.

[0009] Furthermore, among gallium nitride thin films, indium gallium nitride thin films with a high indium composition are expected to achieve high efficiency by responding to visible light.

[0010] However, it is difficult to form high-quality indium gallium nitride thin films with a high indium composition. High-indium gallium nitride thin films have a high surface roughness. When the surface roughness exceeds a few nanometers, it can be difficult to uniformly coat the surface with an ultrathin protective layer.

[0011] In order to uniformly coat the surface of an indium gallium nitride thin film with a high indium composition with an extremely thin protective layer, it is necessary to reduce the roughness of the indium gallium nitride thin film.

[0012] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a technique capable of reducing the roughness of an indium gallium nitride thin film.

[0013] A method for manufacturing a semiconductor photoelectrode according to one aspect of the present disclosure includes the steps of forming a first semiconductor thin film of n-type gallium nitride on a substrate, growing a second semiconductor thin film of indium gallium nitride on a surface of the first semiconductor thin film, and annealing the second semiconductor thin film in a nitrogen or ammonia atmosphere after the second semiconductor thin film has been grown, forming a metal layer on the surface of the second semiconductor thin film after the annealing, and heat-treating the semiconductor thin film with the metal layer formed thereon.

[0014] According to the present disclosure, a technique can be provided that can reduce the roughness of an indium gallium nitride thin film.

[0015] Fig. 1 is a flowchart showing an example of a method for manufacturing a semiconductor photoelectrode according to the present disclosure. Fig. 2 is a cross-sectional view showing an example of the configuration of a semiconductor photoelectrode according to the present disclosure. Fig. 3 is a diagram showing an overview of an apparatus for performing an oxidation-reduction reaction test.

[0016] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the description of the drawings, the same parts are designated by the same reference numerals and the description thereof will be omitted.

[0017] First, referring to Figure 3, an apparatus 100 used in an oxidation-reduction reaction test will be described. The apparatus 100 includes a light source 101, an oxidation tank 102, a reduction tank 103, a proton exchange membrane 104, and a lead wire 106. The oxidation tank 102 contains an oxidation electrode 121 and an aqueous solution 122. The oxidation tank 102 is provided with a light-receiving window 124. The light-receiving window 124 receives light from the light source 101 to the oxidation electrode 121. The reduction tank 103 contains a reduction electrode 131 and an aqueous solution 132.

[0018] In the oxidation bath 102, the oxidation electrode 121 is in contact with an aqueous solution 122. The oxidation electrode 121 is made of a nitride semiconductor, titanium oxide, amorphous silicon, etc. The aqueous solution 122 is, for example, an aqueous sodium hydroxide solution, an aqueous potassium hydroxide solution, or hydrochloric acid.

[0019] In the reduction tank 103, the reduction electrode 131 is in contact with an aqueous solution 132. The reduction electrode 131 is a metal or a metal compound, such as nickel, iron, gold, platinum, silver, copper, indium, or titanium. The aqueous solution 132 is, for example, an aqueous solution of potassium hydrogen carbonate, sodium hydrogen carbonate, potassium chloride, or sodium chloride.

[0020] The proton exchange membrane 104 is sandwiched between the oxidation chamber 102 and the reduction chamber 103. Protons are generated in the oxidation chamber 102. The generated protons diffuse into the reduction chamber 103 through the proton exchange membrane 104. The proton exchange membrane 104 is, for example, a perfluorocarbon material. The purple perfluorocarbon material is composed of a hydrophobic Teflon (registered trademark) skeleton made of carbon and fluorine, and perfluoro side chains with sulfonic acid groups. The proton exchange membrane 104 is, for example, Nafion (registered trademark).

[0021] The oxidation electrode 121 and the reduction electrode 131 are electrically connected by a conductor 106. Electrons move from the oxidation electrode 121 to the reduction electrode 131 via the conductor 106.

[0022] The light source 101 is, for example, a xenon lamp, a mercury lamp, a halogen lamp, a solar simulant, sunlight, or a combination thereof. The light source 101 emits light of a wavelength that can be absorbed by the material that constitutes the oxide electrode 121. For example, in the case of the oxide electrode 121 made of gallium nitride, the wavelength that can be absorbed by the oxide electrode 121 is 365 nm or shorter.

[0023] 3, the oxidation electrode 121 is, for example, a gallium nitride thin film grown on a sapphire substrate. When the gallium nitride thin film is irradiated with light in an aqueous solution, the target water oxidation reaction occurs on the gallium nitride surface, and a side reaction, an etching reaction of gallium nitride (GaN), occurs. As the etching reaction progresses, the reaction field where the target reaction can proceed decreases, and the solar energy conversion efficiency decreases within a few hours.

[0024] Therefore, a structure that suppresses the etching reaction by forming a protective layer on the gallium nitride thin film can be considered, which prevents contact between the aqueous solution and the gallium nitride thin film as much as possible. To achieve light transmission, it is preferable that the protective layer be as thin as possible, such as less than 5 nm.

[0025] Furthermore, among gallium nitride thin films, indium gallium nitride thin films with a high indium composition are expected to achieve high efficiency by responding to visible light.

[0026] The method for manufacturing a semiconductor photoelectrode according to the present disclosure forms a high-indium-composition indium gallium nitride thin film into a high-quality thin film. This makes it possible to form an extremely thin and uniform protective layer on the indium gallium nitride thin film. Furthermore, the formation of an extremely thin and uniform protective layer on the indium gallium nitride thin film enables the solar energy conversion efficiency to be extended over a long period of time.

[0027] A method for manufacturing a semiconductor photoelectrode according to the present disclosure will be described with reference to FIGS.

[0028] First, in step S1, a first semiconductor thin film 12 of n-type gallium nitride is formed on a substrate 11. In step S2, a second semiconductor thin film 13 of indium gallium nitride is grown on the surface of the first semiconductor thin film 12 formed in step S1. The processes in steps S1 and S2 are performed by metal organic chemical vapor deposition (MOCVD).

[0029] After the second semiconductor thin film 13 is grown in step S2, it is annealed in a nitrogen or ammonia atmosphere in step S3. Step S3 is performed in a nitrogen atmosphere furnace, an ammonia atmosphere furnace, or an MOCVD growth furnace. The annealing is preferably performed at a temperature in the range of 700 to 1100°C for 1 to 30 minutes.

[0030] In step S4, a metal layer 14 serving as a protective layer is formed on the surface of the second semiconductor thin film 13 after the annealing treatment in step S3. Step S4 is performed by physical vapor deposition such as vacuum deposition or sputtering, chemical vapor deposition such as metalorganic vapor phase epitaxy, or liquid phase epitaxy. While nickel (Ni) is used for the metal layer in this disclosure, this is not limiting. The metal layer may also be made of one or more metals selected from the group consisting of nickel, cobalt (Co), copper (Cu), tungsten (W), tantalum (Ta), palladium (Pd), ruthenium (Ru), iron (Fe), zinc (Zn), and niobium (Nb). The thickness of the metal layer is 1 nm to 10 nm. A thickness of 1 nm to 3 nm is particularly desirable, as it allows sufficient light transmission.

[0031] In step S5, the semiconductor thin film on which the metal layer has been formed in step S4 is heat-treated. In the present disclosure, the heat treatment is performed on a hot plate, but this is not limitative. The heat treatment may also be performed in an electric furnace. In the present disclosure, the heat treatment atmosphere is air, but it may also be an oxygen atmosphere.

[0032] Next, the results of an oxidation-reduction reaction test using the device according to the present disclosure will be described. In the test, the temperature, time, and atmosphere conditions in the annealing treatment for producing the oxidation electrode 121 were changed as shown in Table 1, and the amount of hydrogen generated after a predetermined time was measured.

[0033] The aqueous solution used in the following oxidation-reduction reaction test may be a potassium hydroxide aqueous solution or hydrochloric acid, in addition to sodium hydroxide. The aqueous solution 132 in the reduction tank 103 may be a sodium bicarbonate aqueous solution, a potassium chloride aqueous solution, or a sodium chloride aqueous solution, in addition to potassium bicarbonate. While hydrogen is used as the target product in the example, this is not limiting. By changing the reduction electrode or the atmosphere in the cell, it is also possible to generate carbon compounds through the reduction reaction of carbon dioxide, or ammonia through the reduction reaction of nitrogen. The reduction electrode can be changed to, for example, Ni, Fe, Au, Pt, Ag, Cu, In, Ti, Co, or Ru.

[0034] Example 1 In Example 1, an n-GaN substrate was used as the substrate. A silicon-doped n-GaN semiconductor thin film was epitaxially grown on a 2-inch n-GaN substrate by MOCVD. Ammonia gas and trimethylgallium were used as growth sources. Silane gas was used as the n-type impurity source. Hydrogen was used as the carrier gas sent into the growth furnace. The n-GaN film thickness was 2 μm, which is sufficient for light absorption. The carrier density was 3 × 10 cm.

[0035] Next, indium gallium nitride (InGaN) with a 10% indium composition ratio was grown. Ammonia gas, trimethylgallium, and trimethylindium were used as growth sources. Hydrogen was used as the carrier gas sent into the growth furnace. The film thickness was set to 500 nm, sufficient for sufficient light absorption. The film was then annealed in an ammonia atmosphere at 700°C for 1 minute in the growth furnace. After removal from the furnace, the 2-inch semiconductor thin film was cleaved into four equal pieces, one of which was used to fabricate an electrode. The surface was observed with an atomic force microscope (AFM). The average arithmetic roughness of the surface was less than 1 nm.

[0036] Next, Ni was vacuum-deposited onto the semiconductor thin film to a thickness of 1 nm. The film was then placed on a hot plate set to 300°C and heat-treated in air for 1 hour to form a NiO protective layer. The cross section of the sample was observed with a transmission electron microscope (TEM). The NiO film thickness was 2 nm.

[0037] <Oxidation-reduction reaction test> A conducting wire was connected to a portion of the exposed n-GaN surface and soldered using In. It was then covered with epoxy resin so that the indium surface was not exposed. This was installed as the oxidation electrode 121 shown in Figure 3. The aqueous solution 122 in the oxidation layer was a 1 mol / L aqueous solution of sodium hydroxide. The aqueous solution 132 in the reduction tank 103 was a 0.5 mol / L aqueous solution of potassium bicarbonate. The reduction electrode 131 was made of platinum (manufactured by Nilaco). The proton exchange membrane 104 was made of Nafion (registered trademark).

[0038] Nitrogen gas was flowed through each reaction vessel at a rate of 10 ml / min. The area of ​​the oxidation electrode 121 irradiated with light was set to 1 cm 2 The aqueous solution was stirred at a rotation speed of 250 rpm using a stirring bar and a stirrer at the center of the bottom of each reaction vessel. After the atmosphere inside the reaction vessel was sufficiently replaced with nitrogen gas, the light source 101 was fixed so that it faced the surface of the semiconductor photoelectrode fabricated by the above-mentioned procedure on which the NiO protective layer was formed. The light source 101 was a 300 W high-pressure xenon lamp (illuminance 5 mW / cm 2 ) was used to uniformly irradiate the semiconductor photoelectrode with light. Gas samples were taken from each reaction chamber at any time during the light irradiation, and the reaction products were analyzed using a gas chromatograph. As a result, it was confirmed that oxygen was produced in the oxidation chamber 102 and hydrogen was produced in the reduction chamber 103.

[0039] Example 2 After film formation, annealing was performed in a furnace at a temperature of 800°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0040] Example 3 After film formation, annealing was performed in a furnace at a temperature of 900°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0041] Example 4 After film formation, annealing was performed in a furnace at a temperature of 1000°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0042] Example 5 After film formation, annealing was performed in a furnace at a temperature of 1100°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0043] Example 6 After film formation, annealing was performed in a furnace at a temperature of 1100°C for 5 minutes. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0044] Example 7 After film formation, annealing was performed in a furnace at a temperature of 1100°C for 10 minutes. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0045] Example 8 After film formation, annealing was performed in a furnace at a temperature of 1100° C. for 30 minutes. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0046] Example 9 After film formation, annealing was performed in a nitrogen atmosphere at a temperature of 700°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was found to be 1 nm or less.

[0047] <Comparative Example 1> After film formation, annealing was performed in a furnace at a temperature of 600°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was about 10 nm.

[0048] <Comparative Example 2> After film formation, annealing was performed in a furnace at a temperature of 600°C for 30 minutes. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was about 10 nm.

[0049] <Comparative Example 3> After film formation, annealing was performed in a furnace at a temperature of 1200°C for 1 minute. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was about 15 nm.

[0050] <Comparative Example 4> After film formation, annealing was performed in a furnace at a temperature of 1100°C for 60 minutes. The subsequent steps were the same as in Example 1. When the surface was observed with an AFM, the average arithmetic roughness of the surface was about 15 nm.

[0051] Table 1 shows the amount of hydrogen gas produced versus the light irradiation time in the examples and comparative examples.

[0052]

[0053] The amount of each gas produced was normalized by the surface area of ​​the semiconductor photoelectrode. In all cases, hydrogen was produced upon light irradiation.

[0054] The amounts of hydrogen generated in Examples 1 to 4 are compared with those in Comparative Examples 1 and 2. There is no significant difference in the amount generated immediately after light irradiation. Differences in the amount generated were observed as time passed from the start of light irradiation. In Comparative Examples 1 and 2, the amount of hydrogen generated was reduced by approximately 30% 100 hours after light irradiation. On the other hand, in Examples 1 to 4, the amount of hydrogen generated was maintained at approximately 10% after 100 hours after light irradiation. Compared to Comparative Example 1, Examples 1 to 4, which were annealed at a higher temperature, have improved surface flatness, and it is believed that the etching reaction is suppressed by the formation of a uniform protective layer. Furthermore, no effect was observed even when the annealing time was extended, as in Comparative Example 2.

[0055] In the case of Comparative Example 3, the amount of oxide generated immediately after light irradiation was low. This is thought to be because the annealing treatment was carried out at a high temperature, which rather worsened the crystallinity of the semiconductor thin film.

[0056] The amount of oxide generated immediately after light irradiation was also low in Comparative Example 4. This is thought to be because the annealing treatment time was long, which rather worsened the crystallinity of the semiconductor thin film.

[0057] In Example 9, the same effect as in Example 1 was obtained. It is believed that ammonia or nitrogen is preferable as the N source material effective for improving the quality of InGaN.

[0058] As described above, the method for manufacturing a semiconductor photoelectrode disclosed herein involves growing an indium gallium nitride thin film with a high indium composition and then performing an annealing treatment. This reduces the surface roughness of the semiconductor photoelectrode and makes it possible to form an extremely thin and uniform protective layer. The method for manufacturing a semiconductor photoelectrode disclosed herein can achieve a long life of solar energy conversion efficiency.

[0059] The present disclosure is not limited to the above-described embodiments, and various modifications are possible within the scope of the gist of the present disclosure.

[0060] REFERENCE SIGNS LIST 11 Substrate 12 n-type gallium nitride semiconductor thin film 13 Indium gallium nitride semiconductor thin film 14 Metal layer 100 Apparatus 101 Light source 102 Oxidation chamber 103 Reduction chamber 104 Proton exchange membrane 106 Conductor 121 Oxidation electrode 122, 132 Aqueous solution 131 Reduction electrode

Claims

1. A method for manufacturing a semiconductor photoelectrode, comprising the steps of: forming a first semiconductor thin film of n-type gallium nitride on a substrate; growing a second semiconductor thin film of indium gallium nitride on a surface of the first semiconductor thin film; annealing the second semiconductor thin film in a nitrogen or ammonia atmosphere after the second semiconductor thin film has been grown; forming a metal layer on the surface of the second semiconductor thin film after the annealing; and heat treating the semiconductor thin film with the metal layer formed thereon.

2. The method for producing a semiconductor photoelectrode according to claim 1, wherein the step of forming the first semiconductor thin film and the step of growing the second semiconductor thin film are carried out by metal organic chemical vapor deposition.

3. The method for producing a semiconductor photoelectrode according to claim 1, wherein the annealing treatment is carried out at a temperature in the range of 700°C to 1100°C for 1 minute to 30 minutes.

Citation Information

Patent Citations

  • Light-emitting diode

    JP2013084955A

  • Method for producing nitride semiconductor photoelectrode

    WO2020116151A1

  • Subpixel light emitting diodes for direct view display and methods of making the same

    WO2021236382A1