Intermediate film for laminated glass, production method for intermediate film for laminated glass, and laminated glass

The interlayer film configuration with a specific absorbance ratio in laminated glass addresses the issue of high haze values during heat resistance tests, ensuring safety and performance by using a thermoplastic resin and polyethylene terephthalate film combination, effectively reducing glass fragment scattering.

WO2024247473A1PCT designated stage expired Publication Date: 2024-12-05SEKISUI CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013550
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-04-02
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional interlayer films with polyethylene terephthalate films in laminated glass exhibit high haze values during heat resistance tests at 100°C, leading to increased scattering of glass fragments upon damage, compromising safety and performance.

Method used

An interlayer film configuration with a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer, where the ratio of absorbance A at 1930 nm to absorbance B at 1705 nm is 0.50 or less, is used to maintain low haze values during heat resistance tests, enhancing safety and performance.

Benefits of technology

The proposed interlayer film configuration effectively suppresses haze values in laminated glass during heat resistance tests, ensuring safety and maintaining low scattering of glass fragments even when subjected to high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013550_05122024_PF_FP_ABST
    Figure JP2024013550_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an intermediate film for laminated glass that comprises a polyethylene terephthalate film and can still be kept to a low haze value when a laminated glass has undergone heat resistance testing at 100°C. An intermediate film for laminated glass according to the present invention comprises, in order, a first resin layer that includes a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer that includes a thermoplastic resin, the ratio of the absorbance A at a wavelength of 1930 nm to the absorbance B at a wavelength of 1705 nm being no more than 0.50.
Need to check novelty before this filing date? Find Prior Art

Description

Interlayer film for laminated glass, method for producing interlayer film for laminated glass, and laminated glass

[0001] The present invention relates to an interlayer film for laminated glass used to obtain laminated glass and a method for producing the same. The present invention also relates to laminated glass using the interlayer film for laminated glass.

[0002] Laminated glass is excellent in safety because it generates only a small amount of glass fragments even when broken by external impact. For this reason, laminated glass is widely used in automobiles, railway vehicles, aircraft, ships, buildings, etc. Laminated glass is manufactured by sandwiching an interlayer film between a pair of glass sheets.

[0003] In order to improve heat insulation properties and strength, an interlayer including a polyethylene terephthalate film is sometimes used. An interlayer including a polyethylene terephthalate film is disclosed in, for example, Patent Document 1 listed below.

[0004] JP 2010-265165 A

[0005] As a test for laminated glass using an interlayer film, a heat resistance test at 100°C may be performed in which the laminated glass is left standing in an environment at 100°C for a predetermined period of time.

[0006] However, laminated glass using a conventional interlayer film including a polyethylene terephthalate film exhibits a high haze value when subjected to a heat resistance test at 100° C. The problem of a high haze value of laminated glass when subjected to a heat resistance test at 100° C. occurs only when an interlayer film including a polyethylene terephthalate film is used, and does not occur when an interlayer film not including a polyethylene terephthalate film is used.

[0007] An object of the present invention is to provide an interlayer film for laminated glass that can maintain a low haze value when laminated glass is subjected to a heat resistance test at 100°C, even though the interlayer film includes a polyethylene terephthalate film. Another object of the present invention is to provide a method for producing the interlayer film for laminated glass. A further object of the present invention is to provide laminated glass using the interlayer film for laminated glass.

[0008] This specification discloses the following interlayer film for laminated glass, a method for producing an interlayer film for laminated glass, and laminated glass.

[0009] Item 1. An interlayer film for laminated glass comprising, in this order, a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer containing a thermoplastic resin, wherein the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm is 0.50 or less.

[0010] Item 2. The interlayer film for laminated glass according to Item 1, wherein the polyethylene terephthalate film is a multilayer polyethylene terephthalate film having two or more polyethylene terephthalate layers and no metal layer, or a metal layer-containing polyethylene terephthalate film having a polyethylene terephthalate layer and a metal layer.

[0011] Item 3. The interlayer film for laminated glass according to Item 1 or 2, wherein the thermoplastic resin contained in the first resin layer includes a polyvinyl acetal resin, and the thermoplastic resin contained in the second resin layer includes a polyvinyl acetal resin.

[0012] Item 4. A method for producing an interlayer film for laminated glass according to any one of Items 1 to 3, comprising the steps of obtaining a laminate including, in this order, a layer for forming a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a layer for forming a second resin layer containing a thermoplastic resin, and curing the laminate so that the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm in the obtained interlayer film is 0.50 or less.

[0013] Item 5. A method for producing an interlayer film for laminated glass according to any one of Items 1 to 3, comprising a step of curing at least one of the first resin layer-forming layer containing a thermoplastic resin and the second resin layer-forming layer containing a thermoplastic resin, so that the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm in the resulting interlayer film is 0.50 or less.

[0014] Item 6. A laminated glass comprising a first laminated glass member, a second laminated glass member, and the interlayer film for laminated glass according to any one of Items 1 to 3, wherein the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.

[0015] The interlayer film for laminated glass according to the present invention comprises, in this order, a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer containing a thermoplastic resin, and has a ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm of 0.50 or less. Because the interlayer film for laminated glass according to the present invention has the above configuration, when the laminated glass is subjected to a heat resistance test at 100°C, the haze value can be kept low, even though the interlayer film comprises a polyethylene terephthalate film.

[0016] Fig. 1 is a diagram for explaining a method for calculating absorbance A at a wavelength of 1930 nm and absorbance B at a wavelength of 1705 nm. Fig. 2 is a cross-sectional view schematically showing an interlayer film for laminated glass according to one embodiment of the present invention. Fig. 3 is a cross-sectional view schematically showing an example of laminated glass using the interlayer film for laminated glass shown in Fig. 2.

[0017] The present invention will be described in detail below.

[0018] (Interlayer Film for Laminated Glass) The interlayer film for laminated glass according to the present invention (sometimes abbreviated as "interlayer film" in this specification) is used in laminated glass.

[0019] The interlayer film includes, in this order, a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer containing a thermoplastic resin, wherein the first resin layer is disposed on a first surface side of the polyethylene terephthalate film, and the second resin layer is disposed on a second surface side of the polyethylene terephthalate film opposite to the first surface.

[0020] The interlayer film may have a three-layer structure consisting of the first resin layer, the polyethylene terephthalate film, and the second resin layer. The interlayer film may have a structure of three or more layers, a structure of ten or fewer layers, or a structure of five or fewer layers. When the polyethylene terephthalate film included in the interlayer film has multiple layers, the polyethylene terephthalate film having multiple layers is counted as one layer when counting the number of layers of the interlayer film. A polyethylene terephthalate film having multiple layers can be regarded as a single layer component in the interlayer film as a whole.

[0021] In the interlayer film, the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm (absorbance A / absorbance B) is 0.50 or less.

[0022] The absorbance A corresponds to the absorbance of water, and the absorbance B corresponds to the absorbance of a methylene group. The inventors have found that, when the ratio (absorbance A / absorbance B) is 0.50 or less, the haze value can be kept low when a heat resistance test is performed on a laminated glass at 100°C, even though the interlayer film includes a polyethylene terephthalate film. Therefore, the haze value of a laminated glass using the interlayer film is unlikely to increase even when the laminated glass is used in a high-temperature environment, for example.

[0023] The ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm (absorbance A / absorbance B) is preferably 0.06 or more, more preferably 0.10 or more, preferably 0.48 or less, more preferably 0.45 or less, even more preferably 0.40 or less, even more preferably 0.35 or less, even more preferably 0.30 or less, particularly preferably 0.25 or less, and most preferably 0.20 or less. When the ratio (absorbance A / absorbance B) is at least the lower limit, the adhesion between the interlayer film and the laminated glass member can be further improved. When the ratio (absorbance A / absorbance B) is at most the upper limit, the effects of the present invention can be more effectively exhibited.

[0024] The absorbance A at a wavelength of 1930 nm is preferably 0.01 or more, more preferably 0.02 or more, and preferably 0.10 or less, more preferably 0.08 or less, and even more preferably 0.05 or less. When the absorbance A is equal to or greater than the lower limit, the adhesion between the interlayer film and the laminated glass member can be further improved. When the absorbance A is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited.

[0025] The absorbance A and the absorbance B are measured as follows.

[0026] (1) Preparation of Laminated Glass X The above interlayer film is placed between two sheets of clear glass conforming to JIS R3202: 1996 to prepare laminated glass X (laminated glass for absorbance measurement). The laminated glass X is preferably prepared as follows.

[0027] The interlayer film is sandwiched between two 2 mm thick clear glass sheets conforming to JIS R3202:1996 to obtain a laminate. The obtained laminate is placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes. The degassed laminate is then transferred to an oven and held at 90°C for 30 minutes for vacuum pressing to pre-bond the laminate. The pre-bonded laminate is then compressed in an autoclave at 135°C and a pressure of 1.2 MPa for 20 minutes to obtain laminated glass X.

[0028] (2) Measurement of Absorbance In the obtained laminated glass X, a position 3 cm from one end toward the other end is designated as the first position, and a position 5 cm from one end toward the other end is designated as the second position. The one end and the other end are opposite ends of the laminated glass X. The absorbance at each of the first and second positions of the laminated glass X is measured using a near-infrared spectrophotometer (for example, the "V-570" manufactured by JASCO Corporation) under conditions of a bandwidth of 2 nm, a scanning speed of 1000 nm / min, a scanning range of 1550 nm to 2050 nm, and a data acquisition interval of 0.5 nm. At the same wavelength, the absorbance at the first position and the absorbance at the second position are averaged. An absorbance spectrum is created from the averaged absorbance.

[0029] In the prepared absorbance spectrum, the line connecting the position of absorbance at a wavelength of 1873 nm and the position of absorbance at a wavelength of 1984 nm is defined as the baseline for absorbance A. The absolute value of the difference between the absorbance at a wavelength of 1930 nm on the baseline for absorbance A and the absorbance at a wavelength of 1930 nm on the prepared absorbance spectrum is defined as the absorbance A of the interlayer film at a wavelength of 1930 nm.

[0030] In the prepared absorbance spectrum, the position of absorbance at a wavelength of 1670 nm is defined as the baseline for absorbance B. The absolute value of the difference between the absorbance at a wavelength of 1670 nm on the prepared absorbance spectrum and the absorbance at a wavelength of 1705 nm on the prepared absorbance spectrum is defined as the absorbance B of the interlayer film at a wavelength of 1705 nm.

[0031] FIG. 1 is a diagram illustrating a method for calculating absorbance A at a wavelength of 1930 nm and absorbance B at a wavelength of 1705 nm. FIG. 1 shows an example of an absorbance spectrum created from an average absorbance obtained by averaging the absorbance at the first position and the absorbance at the second position. As shown in FIG. 1, the absorbance A is the absolute value of the difference between the absorbance at a wavelength of 1930 nm on the baseline for absorbance A and the absorbance at a wavelength of 1930 nm on the absorbance spectrum. Also, as shown in FIG. 1, the absorbance B is the absolute value of the difference between the absorbance at a wavelength of 1670 nm on the absorbance spectrum and the absorbance at a wavelength of 1705 nm on the absorbance spectrum.

[0032] The laminated glass X is produced for measuring absorbance. The interlayer film may be used to produce a laminated glass (laminated glass product) using a laminated glass component other than two sheets of clear glass conforming to JIS R3202:1996, or a laminated glass (laminated glass product) using a laminated glass component other than clear glass.

[0033] An interlayer film having the ratio (absorbance A / absorbance B) of 0.50 or less can be obtained, for example, by the method for producing an interlayer film described below.

[0034] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings.

[0035] FIG. 2 is a cross-sectional view that schematically illustrates an interlayer film for laminated glass according to one embodiment of the present invention.

[0036] The interlayer film 11 shown in FIG. 2 is used to obtain laminated glass. The interlayer film 11 is an interlayer film for laminated glass. The interlayer film 11 includes a polyethylene terephthalate film 1, a first resin layer 2, and a second resin layer 3. The first resin layer 2 is disposed and laminated on a first surface 1a side of the polyethylene terephthalate film 1. The second resin layer 3 is disposed and laminated on a second surface 1b side of the polyethylene terephthalate film 1 opposite the first surface 1a. The polyethylene terephthalate film 1 is an intermediate layer. The first resin layer 2 and the second resin layer 3 are each protective layers, and in this embodiment, are surface layers. The polyethylene terephthalate film 1 is disposed and sandwiched between the first resin layer 2 and the second resin layer 3. Therefore, the intermediate film 11 has a multilayer structure in which a first resin layer 2, a polyethylene terephthalate film 1, and a second resin layer 3 are laminated in this order (first resin layer 2 / polyethylene terephthalate film 1 / second resin layer 3).

[0037] Other layers may be disposed between the first resin layer 2 and the polyethylene terephthalate film 1, and between the polyethylene terephthalate film 1 and the second resin layer 3. It is preferable that the first resin layer 2 and the polyethylene terephthalate film 1, and the polyethylene terephthalate film 1 and the second resin layer 3 are directly laminated together. Examples of such other layers include an adhesive layer.

[0038] Other details of the components constituting the interlayer film and laminated glass according to the present invention will be described below.

[0039] (Polyethylene terephthalate film) The polyethylene terephthalate film (PET film) contains polyethylene terephthalate. The inclusion of a polyethylene terephthalate film in the interlayer film can improve heat insulation properties and strength. Furthermore, the inclusion of a polyethylene terephthalate film in the interlayer film can effectively prevent components contained in one resin layer from migrating to the other resin layer.

[0040] Examples of the polyethylene terephthalate film include a single-layer polyethylene terephthalate film having one polyethylene terephthalate layer and no metal layer, a multilayer polyethylene terephthalate film having two or more polyethylene terephthalate layers and no metal layer, and a metal layer-containing polyethylene terephthalate film having a polyethylene terephthalate layer and a metal layer.

[0041] The polyethylene terephthalate film may be the single-layer polyethylene terephthalate film, the multi-layer polyethylene terephthalate film, or the metal layer-containing polyethylene terephthalate film.

[0042] From the viewpoint of further enhancing the heat-shielding property, the polyethylene terephthalate film is preferably the multilayer polyethylene terephthalate film or the metal layer-containing polyethylene terephthalate film.

[0043] The multilayer polyethylene terephthalate film has two or more polyethylene terephthalate layers, and may have two, two or more, three or more, five or more, 1,000 or less, 100 or less, or 50 or less polyethylene terephthalate layers.

[0044] The metal layer-containing polyethylene terephthalate film may have one, two, two or more, three or more, five or more, 1,000 or less, 100 or less, or 50 or less of the polyethylene terephthalate layers.

[0045] The metal layer-containing polyethylene terephthalate film may have one, two, two or more, three or more, five or more, 1,000 or less, 100 or less, or 50 or less metal layers. Examples of materials for the metal layer include aluminum, copper, silver, gold, palladium, and alloys containing these. Only one type of material for the metal layer may be used, or two or more types may be used in combination.

[0046] In the metal layer-containing polyethylene terephthalate film, the metal layer is preferably disposed on the outer surface of the polyethylene terephthalate layer, and at least one of the surface layers is preferably the metal layer.

[0047] In the metal layer-containing polyethylene terephthalate film, the metal layer is preferably a metal sputtering layer. The metal sputtering layer can be formed by metal sputtering. A coating layer of a metal or a mixed oxide of metals may be applied to both sides or one side of the metal layer. Examples of materials for the coating layer include ZnO, Al 2 O 3 , Ga2 O 3 , InO 3 , MgO, Ti, NiCr, and Cu.

[0048] The metal layer-containing polyethylene terephthalate film may have a dielectric layer. In the metal layer-containing polyethylene terephthalate film, any number of metal layers and dielectric layers may be alternately laminated on a polyethylene terephthalate layer. In a metal layer-containing polyethylene terephthalate film having a dielectric layer, it is preferable that all of the metal layers and dielectric layers are alternately laminated, but there may be a structure in which some of the layers are not alternately laminated, such as metal layer / dielectric layer / metal layer / dielectric layer / metal layer / metal layer / dielectric layer / metal layer. Examples of materials for the dielectric layer include indium oxide.

[0049] (First Resin Layer and Second Resin Layer) <Thermoplastic Resin> The first resin layer contains a thermoplastic resin (hereinafter may be referred to as thermoplastic resin (1)). The thermoplastic resin (1) preferably contains a polyvinyl acetal resin. The first resin layer preferably contains a polyvinyl acetal resin as the thermoplastic resin (1). The second resin layer contains a thermoplastic resin (hereinafter may be referred to as thermoplastic resin (2)). The thermoplastic resin (2) preferably contains a polyvinyl acetal resin. The second resin layer preferably contains a polyvinyl acetal resin as the thermoplastic resin (2).

[0050] The thermoplastic resin (1) and the thermoplastic resin (2) may be the same or different. The thermoplastic resin (1) and the thermoplastic resin (2) may each be used alone or in combination of two or more.

[0051] In the following description, the common components of the thermoplastic resin (1) and the thermoplastic resin (2) will be simply referred to as "thermoplastic resin."

[0052] Examples of the thermoplastic resin include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, polyvinyl alcohol resin, polyolefin resin, polyvinyl acetate resin, polystyrene resin, and ionomer resin. Thermoplastic resins other than these may also be used.

[0053] The thermoplastic resin is preferably a polyvinyl acetal resin. The combined use of a polyvinyl acetal resin and a plasticizer further enhances the adhesive strength of the resin layer to other layers such as laminated glass members and polyethylene terephthalate films.

[0054] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol can be obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally within the range of 70 mol% to 99.9 mol%.

[0055] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, even more preferably 1500 or more, even more preferably 1600 or more, particularly preferably 2600 or more, most preferably 2700 or more, and preferably 5000 or less, more preferably 4000 or less, and even more preferably 3500 or less. When the average degree of polymerization is equal to or greater than the lower limit, the penetration resistance of the laminated glass is further improved. When the average degree of polymerization is equal to or less than the upper limit, the resin layer is easily formed.

[0056] The average degree of polymerization of the polyvinyl alcohol is determined by a method in accordance with JIS K6726 "Testing methods for polyvinyl alcohol."

[0057] The number of carbon atoms in the acetal group contained in the polyvinyl acetal resin is not particularly limited. The aldehyde used in producing the polyvinyl acetal resin is not particularly limited. The number of carbon atoms in the acetal group in the polyvinyl acetal resin is preferably 3 to 5, and more preferably 3 or 4. When the number of carbon atoms in the acetal group in the polyvinyl acetal resin is 3 or more, the glass transition temperature of the resin layer is sufficiently low.

[0058] The aldehyde is not particularly limited. In general, an aldehyde having 1 to 10 carbon atoms is suitably used. Examples of the aldehyde having 1 to 10 carbon atoms include propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, formaldehyde, acetaldehyde, and benzaldehyde. The aldehyde is preferably propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-hexylaldehyde, or n-valeraldehyde, more preferably propionaldehyde, n-butyraldehyde, or isobutyraldehyde, and even more preferably n-butyraldehyde. The above aldehydes may be used alone or in combination of two or more.

[0059] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin is preferably 15 mol% or more, more preferably 18 mol% or more, even more preferably 20 mol% or more, particularly preferably 28 mol% or more, preferably 40 mol% or less, more preferably 35 mol% or less, and even more preferably 32 mol% or less. When the hydroxyl group content is above the lower limit, the adhesive strength of the resin layer is further increased. On the other hand, when the hydroxyl group content is below the upper limit, the flexibility of the resin layer is increased, making the resin layer easier to handle.

[0060] The hydroxyl group content of the polyvinyl acetal resin is a molar fraction calculated by dividing the amount of ethylene groups having hydroxyl groups by the total amount of ethylene groups in the main chain, and is expressed as a percentage. The amount of ethylene groups having hydroxyl groups can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0061] The degree of acetylation (acetyl group amount) of the polyvinyl acetal resin is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, preferably 30 mol% or less, more preferably 25 mol% or less, even more preferably 20 mol% or less, particularly preferably 15 mol% or less, and most preferably 3 mol% or less. When the degree of acetylation is above the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is improved. When the degree of acetylation is below the upper limit, the moisture resistance of the laminated glass is improved.

[0062] The degree of acetylation is a molar fraction calculated by dividing the amount of ethylene groups having acetyl groups by the total amount of ethylene groups in the main chain, and is expressed as a percentage. The amount of ethylene groups having acetyl groups can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0063] The degree of acetalization of the polyvinyl acetal resin (or the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 60 mol% or more, more preferably 63 mol% or more, and preferably 85 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less. When the degree of acetalization is equal to or greater than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0064] The degree of acetalization is determined as follows. First, the amount of ethylene groups to which hydroxyl groups are bonded and the amount of ethylene groups to which acetyl groups are bonded are subtracted from the total amount of ethylene groups in the main chain to determine the value. The obtained value is divided by the total amount of ethylene groups in the main chain to determine the molar fraction. The value expressed as a percentage of this molar fraction is the degree of acetalization.

[0065] The hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree are preferably calculated from the results of measurements made in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral." However, measurements made in accordance with ASTM D1396-92 may also be used. When the polyvinyl acetal resin is a polyvinyl butyral resin, the hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree can be calculated from the results of measurements made in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0066] The content of polyvinyl acetal resin in 100% by weight of the thermoplastic resin contained in the first resin layer is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The content of polyvinyl acetal resin in 100% by weight of the thermoplastic resin contained in the first resin layer is preferably 100% by weight or less. It is preferable that the main component (50% by weight or more) of the thermoplastic resin of the first resin layer is polyvinyl acetal resin.

[0067] The content of polyvinyl acetal resin in 100% by weight of the thermoplastic resin contained in the second resin layer is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The content of polyvinyl acetal resin in 100% by weight of the thermoplastic resin contained in the second resin layer is preferably 100% by weight or less. The main component (50% by weight or more) of the thermoplastic resin of the second layer is preferably polyvinyl acetal resin.

[0068] <Plasticizer> From the viewpoint of further increasing the adhesive strength of the resin layer, it is preferable that the first resin layer contains a plasticizer (hereinafter, may be referred to as plasticizer (1)). From the viewpoint of further increasing the adhesive strength of the resin layer, it is preferable that the second resin layer contains a plasticizer (hereinafter, may be referred to as plasticizer (2)). When the thermoplastic resin contained in the resin layer is a polyvinyl acetal resin, it is particularly preferable that the resin layer contains a plasticizer. It is preferable that the layer containing a polyvinyl acetal resin contains a plasticizer.

[0069] In the following description, the components common to the plasticizer (1) and the plasticizer (2) will be simply referred to as "plasticizer."

[0070] The plasticizer is not particularly limited. Any conventionally known plasticizer can be used as the plasticizer. Only one type of plasticizer may be used, or two or more types may be used in combination.

[0071] Examples of the plasticizer include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, organic phosphate plasticizers, and organic phosphite plasticizers. The plasticizer is preferably an organic ester plasticizer. The plasticizer is preferably a liquid plasticizer.

[0072] Examples of the monobasic organic acid ester include glycol esters obtained by reacting glycol with a monobasic organic acid. Examples of the glycol include triethylene glycol, tetraethylene glycol, and tripropylene glycol. Examples of the monobasic organic acid include butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, n-nonylic acid, decylic acid, and benzoic acid.

[0073] Examples of the polybasic organic acid ester include ester compounds of a polybasic organic acid and an alcohol having a linear or branched structure and having 4 to 8 carbon atoms. Examples of the polybasic organic acid include adipic acid, sebacic acid, and azelaic acid.

[0074] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylpropanoate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, and diethylene glycol di-2-ethylbutylene. Examples of suitable organic ester plasticizers include diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, diethylene glycol dibenzoate, dipropylene glycol dibenzoate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacate, and a mixture of a phosphate ester and an adipate. Organic ester plasticizers other than those listed above may also be used as the organic ester plasticizer. Furthermore, adipate esters other than the above-mentioned adipate esters may also be used as the adipate ester.

[0075] Examples of the organic phosphoric acid plasticizer include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.

[0076] The plasticizer is preferably a diester plasticizer represented by the following formula (1):

[0077]

[0078] In the above formula (1), R1 and R2 each represent an organic group having 2 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group, or an n-propylene group, and p represents an integer of 3 to 10. In the above formula (1), R1 and R2 each preferably represent an organic group having 5 to 10 carbon atoms, and more preferably represent an organic group having 6 to 10 carbon atoms.

[0079] The plasticizer preferably includes triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH), or triethylene glycol di-2-ethylpropanoate. The plasticizer more preferably includes triethylene glycol di-2-ethylhexanoate (3GO) or triethylene glycol di-2-ethylbutyrate (3GH), and even more preferably includes triethylene glycol di-2-ethylhexanoate (3GO).

[0080] The content of the plasticizer (1) contained in the first resin layer relative to 100 parts by weight of the thermoplastic resin (1) contained in the first resin layer is defined as content (1). The content (1) is preferably 25 parts by weight or more, more preferably 30 parts by weight or more, even more preferably 35 parts by weight or more, preferably 75 parts by weight or less, more preferably 60 parts by weight or less, even more preferably 50 parts by weight or less, and particularly preferably 40 parts by weight or less. When the content (1) is equal to or greater than the lower limit, the penetration resistance of the laminated glass is further improved. When the content (1) is equal to or less than the upper limit, the transparency of the laminated glass is further improved.

[0081] The content of the plasticizer (2) contained in the second resin layer relative to 100 parts by weight of the thermoplastic resin (2) contained in the second resin layer is defined as content (2). The content (2) is preferably 25 parts by weight or more, more preferably 30 parts by weight or more, even more preferably 35 parts by weight or more, preferably 75 parts by weight or less, more preferably 60 parts by weight or less, even more preferably 50 parts by weight or less, and particularly preferably 40 parts by weight or less. When the content (2) is equal to or greater than the lower limit, the penetration resistance of the laminated glass is further improved. When the content (2) is equal to or less than the upper limit, the transparency of the laminated glass is further improved.

[0082] <Heat-shielding substance> The interlayer preferably contains a heat-shielding substance. The first resin layer preferably contains a heat-shielding substance. The first resin layer may not contain a heat-shielding substance. The second resin layer preferably contains a heat-shielding substance. The second resin layer may not contain a heat-shielding substance. Only one type of heat-shielding substance may be used, or two or more types may be used in combination.

[0083] The heat-shielding material preferably contains at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound, or contains heat-shielding particles. In this case, the heat-shielding material may contain both the component X and the heat-shielding particles.

[0084] Component X: The interlayer film preferably contains at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound. The first resin layer preferably contains the component X. The second resin layer preferably contains the component X. Only one component X may be used, or two or more components X may be used in combination.

[0085] There are no particular restrictions on the component X. As the component X, conventionally known phthalocyanine compounds, naphthalocyanine compounds, and anthracyanine compounds can be used.

[0086] Examples of the component X include phthalocyanine, phthalocyanine derivatives, naphthalocyanine, naphthalocyanine derivatives, anthracyanine, and anthracyanine derivatives. The phthalocyanine compound and the phthalocyanine derivative preferably have a phthalocyanine skeleton. The naphthalocyanine compound and the naphthalocyanine derivative preferably have a naphthalocyanine skeleton. The anthracyanine compound and the anthracyanine derivative preferably have an anthracyanine skeleton.

[0087] From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the component X is preferably at least one selected from the group consisting of phthalocyanine, phthalocyanine derivatives, naphthalocyanine, and naphthalocyanine derivatives, and more preferably at least one of phthalocyanine and phthalocyanine derivatives.

[0088] From the viewpoint of effectively improving the heat-shielding properties and maintaining a higher visible light transmittance for a long period of time, the component X preferably contains a vanadium atom or a copper atom. The component X preferably contains a vanadium atom, and also preferably contains a copper atom. The component X is more preferably at least one of a phthalocyanine containing a vanadium atom or a copper atom and a derivative of a phthalocyanine containing a vanadium atom or a copper atom. From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the component X preferably has a structural unit in which an oxygen atom is bonded to a vanadium atom.

[0089] In 100% by weight of the layer containing the component X (the first resin layer or the second resin layer), the content of the component X is preferably 0.0005% by weight or more, more preferably 0.005% by weight or more, even more preferably 0.01% by weight or more, particularly preferably 0.02% by weight or more, preferably 0.2% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.05% by weight or less, and particularly preferably 0.04% by weight or less. When the content of the component X is equal to or greater than the lower limit and equal to or less than the upper limit, the heat-shielding properties are sufficiently high and the visible light transmittance is sufficiently high. For example, it is possible to achieve a visible light transmittance of 70% or more.

[0090] Heat-shielding particles: The interlayer preferably contains heat-shielding particles. The first resin layer preferably contains the heat-shielding particles. The second resin layer preferably contains the heat-shielding particles. The heat-shielding particles are a heat-shielding substance. Use of the heat-shielding particles can effectively block infrared rays (heat rays). Only one type of the heat-shielding particles may be used, or two or more types may be used in combination.

[0091] From the viewpoint of further enhancing the heat-shielding properties of the laminated glass, the heat-shielding particles are more preferably metal oxide particles, and the heat-shielding particles are preferably particles formed from a metal oxide (metal oxide particles).

[0092] Infrared rays, which have wavelengths of 780 nm or more, which are longer than visible light, have a smaller amount of energy than ultraviolet rays. However, infrared rays have a large thermal effect, and when infrared rays are absorbed by a substance, they are released as heat. For this reason, infrared rays are generally called heat rays. By using the above heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Here, heat-shielding particles refer to particles that can absorb infrared rays.

[0093] Specific examples of the heat-shielding particles include metal oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, tungsten oxide particles (sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, etc.), tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, and silicon-doped zinc oxide particles; and lanthanum hexaboride (LaB 6 ) particles, etc. Heat-shielding particles other than these may also be used. Metal oxide particles are preferred because of their high heat-ray shielding function, and ATO particles, GZO particles, IZO particles, ITO particles, or tungsten oxide particles are more preferred, with ITO particles or tungsten oxide particles being particularly preferred. In particular, tin-doped indium oxide particles (ITO particles) are preferred because of their high heat-ray shielding function and ease of availability, and tungsten oxide particles are also preferred.

[0094] From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the tungsten oxide particles are preferably metal-doped tungsten oxide particles. The "tungsten oxide particles" include metal-doped tungsten oxide particles. Specific examples of the metal-doped tungsten oxide particles include sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles.

[0095] From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, cesium-doped tungsten oxide particles are particularly preferred. From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the cesium-doped tungsten oxide particles are represented by the formula: Cs 0.33 WO 3 Preferably, the tungsten oxide particles are represented by the formula:

[0096] The average particle size of the heat-shielding particles is preferably 0.01 μm or more, more preferably 0.02 μm or more, and preferably 0.1 μm or less, more preferably 0.05 μm or less. When the average particle size is equal to or greater than the lower limit, the heat ray shielding property is sufficiently high. When the average particle size is equal to or less than the upper limit, the dispersibility of the heat-shielding particles is high.

[0097] The "average particle size" refers to the volume average particle size. The average particle size can be measured using a particle size distribution analyzer ("UPA-EX150" manufactured by Nikkiso Co., Ltd.) or the like.

[0098] In 100% by weight of the layer containing the heat-shielding particles (the first resin layer or the second resin layer), the content of the heat-shielding particles (particularly the content of the tungsten oxide particles) is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, even more preferably 1% by weight or more, particularly preferably 1.5% by weight or more, preferably 6% by weight or less, more preferably 5.5% by weight or less, even more preferably 4% by weight or less, particularly preferably 3.5% by weight or less, and most preferably 3% by weight or less. When the content of the heat-shielding particles is equal to or more than the above lower limit and equal to or less than the above upper limit, the heat-shielding property becomes sufficiently high, and the visible light transmittance becomes sufficiently high.

[0099] <Metal Salt> The interlayer film preferably contains at least one metal salt (hereinafter sometimes referred to as metal salt M) selected from alkali metal salts and alkaline earth metal salts. The first resin layer preferably contains the metal salt M. The second resin layer preferably contains the metal salt M. Alkaline earth metals refer to six metals: Be, Mg, Ca, Sr, Ba, and Ra. The use of the metal salt M makes it easy to control the adhesion between the interlayer film and a laminated glass member such as a glass plate, or the adhesion between each layer in the interlayer film. Only one type of the metal salt M may be used, or two or more types may be used in combination.

[0100] The metal salt M preferably contains at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, and Ba. The metal salt M contained in the interlayer film more preferably contains at least one metal selected from K and Mg.

[0101] Furthermore, alkali metal salts of organic acids having 2 to 16 carbon atoms and alkaline earth metal salts of organic acids having 2 to 16 carbon atoms can be used as the metal salt M. The metal salt M may include a magnesium salt of a carboxylic acid having 2 to 16 carbon atoms or a potassium salt of a carboxylic acid having 2 to 16 carbon atoms.

[0102] Examples of the magnesium salts of carboxylic acids having 2 to 16 carbon atoms and the potassium salts of carboxylic acids having 2 to 16 carbon atoms include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutanoate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.

[0103] The total content of Mg and K in the layer containing the metal salt M (first resin layer or second resin layer) is preferably 5 ppm or more, more preferably 10 ppm or more, even more preferably 20 ppm or more, and preferably 300 ppm or less, more preferably 250 ppm or less, and even more preferably 200 ppm or less. When the total content of Mg and K is at least the above lower limit and at most the above upper limit, the adhesion between the interlayer film and the laminated glass member (e.g., glass plates) or the adhesion between the layers in the interlayer film can be more effectively controlled.

[0104] <Ultraviolet Shielding Agent> The interlayer film preferably contains an ultraviolet ray shielding agent. The first resin layer preferably contains an ultraviolet ray shielding agent. The second resin layer preferably contains an ultraviolet ray shielding agent. By using an ultraviolet ray shielding agent, the visible light transmittance of the laminated glass is more unlikely to decrease even after long-term use. Only one type of ultraviolet ray shielding agent may be used, or two or more types may be used in combination.

[0105] The ultraviolet screening agent includes an ultraviolet absorbing agent, and the ultraviolet screening agent is preferably an ultraviolet absorbing agent.

[0106] Examples of the ultraviolet screening agent include ultraviolet screening agents containing metal atoms, ultraviolet screening agents containing metal oxides, ultraviolet screening agents having a benzotriazole structure (benzotriazole compounds), ultraviolet screening agents having a benzophenone structure (benzophenone compounds), ultraviolet screening agents having a triazine structure (triazine compounds), ultraviolet screening agents having a malonic acid ester structure (malonic acid ester compounds), ultraviolet screening agents having an oxalic acid anilide structure (oxalic acid anilide compounds), and ultraviolet screening agents having a benzoate structure (benzoate compounds).

[0107] Examples of the ultraviolet shielding agent containing the metal atom include platinum particles, platinum particles whose surfaces are coated with silica, palladium particles, and palladium particles whose surfaces are coated with silica. The ultraviolet shielding agent is preferably not a heat-shielding particle.

[0108] The ultraviolet screening agent is preferably an ultraviolet screening agent having a benzotriazole structure, an ultraviolet screening agent having a benzophenone structure, an ultraviolet screening agent having a triazine structure, or an ultraviolet screening agent having a benzoate structure, more preferably an ultraviolet screening agent having a benzotriazole structure or an ultraviolet screening agent having a benzophenone structure, and even more preferably an ultraviolet screening agent having a benzotriazole structure.

[0109] Examples of the ultraviolet screening agent containing a metal oxide include zinc oxide, titanium oxide, and cerium oxide. Furthermore, the surface of the ultraviolet screening agent containing a metal oxide may be coated. Examples of the coating material for the surface of the ultraviolet screening agent containing a metal oxide include insulating metal oxides, hydrolyzable organosilicon compounds, and silicone compounds.

[0110] Examples of the insulating metal oxide include silica, alumina, zirconia, etc. The insulating metal oxide has a band gap energy of, for example, 5.0 eV or more.

[0111] Examples of the ultraviolet screening agent having a benzotriazole structure include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole ("Tinuvin P" manufactured by BASF), 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole ("Tinuvin 320" manufactured by BASF), 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin 326" manufactured by BASF), and 2-(2'-hydroxy-3',5'-di-amylphenyl)benzotriazole ("Tinuvin 328" manufactured by BASF). Due to their excellent ultraviolet screening performance, the ultraviolet screening agent is preferably an ultraviolet screening agent having a benzotriazole structure containing a halogen atom, and more preferably an ultraviolet screening agent having a benzotriazole structure containing a chlorine atom.

[0112] Examples of the ultraviolet screening agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF).

[0113] Examples of the ultraviolet screening agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF).

[0114] Examples of the ultraviolet screening agent having a malonic acid ester structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl-2,2-(1,4-phenylenedimethylidene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.

[0115] Commercially available ultraviolet screening agents having the malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).

[0116] Examples of the ultraviolet screening agent having an oxalic acid anilide structure include oxalic acid diamides having an aryl group substituted on the nitrogen atom, such as N-(2-ethylphenyl)-N'-(2-ethoxy-5-t-butylphenyl)oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl)oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxalanilide ("Sanduvor VSU" manufactured by Clariant).

[0117] Examples of the ultraviolet screening agent having a benzoate structure include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF).

[0118] The content of the ultraviolet ray blocking agent in 100% by weight of the layer containing the ultraviolet ray blocking agent (first resin layer or second resin layer) is preferably 0.1% by weight or more, more preferably 0.2% by weight or more, even more preferably 0.3% by weight or more, particularly preferably 0.5% by weight or more, preferably 2.5% by weight or less, more preferably 2% by weight or less, even more preferably 1% by weight or less, and particularly preferably 0.8% by weight or less. When the content of the ultraviolet ray blocking agent is equal to or greater than the above lower limit, the decrease in visible light transmittance after a period of time can be further suppressed. When the content of the ultraviolet ray blocking agent is equal to or less than the above upper limit, the decrease in visible light transmittance of the interlayer film and laminated glass after a period of time can be significantly suppressed.

[0119] <Antioxidant> The interlayer film preferably contains an antioxidant. The first resin layer preferably contains an antioxidant. The second resin layer preferably contains an antioxidant. Only one type of antioxidant may be used, or two or more types may be used in combination.

[0120] Examples of the antioxidant include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. The phenol-based antioxidants are antioxidants having a phenol skeleton. The sulfur-based antioxidants are antioxidants containing sulfur atoms. The phosphorus-based antioxidants are antioxidants containing phosphorus atoms.

[0121] The antioxidant is preferably a phenol-based antioxidant or a phosphorus-based antioxidant.

[0122] Examples of the phenolic antioxidant include 2,6-di-t-butyl-p-cresol (BHT), butylhydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy-5- Examples of antioxidants include tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butyric acid glycol ester, and bis(3-t-butyl-4-hydroxy-5-methylbenzenepropanoate)ethylenebis(oxyethylene). One or more of these antioxidants are preferably used.

[0123] Examples of the phosphorus-based antioxidant include tridecyl phosphite, tris(tridecyl)phosphite, triphenyl phosphite, trinonylphenyl phosphite, bis(tridecyl)pentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl ester phosphorous acid, and 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, etc. One or more of these antioxidants are preferably used.

[0124] Examples of commercially available antioxidants include "IRGANOX 245" manufactured by BASF, "IRGAFOS 168" manufactured by BASF, "IRGAFOS 38" manufactured by BASF, "Sumilizer BHT" manufactured by Sumitomo Chemical Co., Ltd., "H-BHT" manufactured by Sakai Chemical Industry Co., Ltd., and "IRGANOX 1010" manufactured by BASF.

[0125] In order to maintain a high visible light transmittance of the interlayer film and the laminated glass for a long period of time, the content of the antioxidant is preferably 0.03 wt% or more, and more preferably 0.1 wt% or more, relative to 100 wt% of the layer containing the antioxidant (the first resin layer or the second resin layer). Furthermore, since the effect of adding the antioxidant becomes saturated, the content of the antioxidant is preferably 2 wt% or less, relative to 100 wt% of the layer containing the antioxidant (the first resin layer or the second resin layer).

[0126] <Other Components> The first resin layer and the second resin layer may each contain, as necessary, additives such as a light stabilizer, a coupling agent, a dispersant, a surfactant, a flame retardant, an antistatic agent, a pigment, a dye, an adhesion modifier other than a metal salt, a moisture-resistant agent, a fluorescent brightener, and an infrared absorber. Only one type of each of the other components may be used, or two or more types may be used in combination.

[0127] (Other Details of the Interlayer Film for Laminated Glass) The thickness of the interlayer film is not particularly limited. From the viewpoint of practical use and of sufficiently increasing the penetration resistance and bending rigidity of the laminated glass, the thickness of the interlayer film is preferably 0.1 mm or more, more preferably 0.25 mm or more, and preferably 3 mm or less, more preferably 1.5 mm or less. If the thickness is equal to or greater than the lower limit, the penetration resistance and bending rigidity of the laminated glass will be further improved. If the thickness is equal to or less than the upper limit, the transparency of the interlayer film will be further improved.

[0128] The interlayer film may be an interlayer film having a uniform thickness or an interlayer film having a varying thickness. The cross-sectional shape of the interlayer film may be rectangular or wedge-shaped. When the cross-sectional shape of the interlayer film is wedge-shaped (when the interlayer film has a varying thickness), the thickness of the interlayer film refers to the average thickness.

[0129] Examples of methods for producing the interlayer film include the following production method (1) and the following production method (2). The production method for the interlayer film is preferably the following production method (1) or the following production method (2).

[0130] The method for producing an interlayer film (1) includes a step of obtaining a laminate including, in this order, a first resin layer-forming layer containing a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer-forming layer containing a thermoplastic resin, and a step of curing the laminate so that the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm (absorbance A / absorbance B) of the obtained interlayer film is 0.50 or less.

[0131] The step of curing the laminate is preferably carried out before the interlayer film is disposed between the first laminated glass member and the second laminated glass member.

[0132] The method (2) for producing an interlayer film includes a step of curing at least one layer selected from the first resin layer-forming layer containing a thermoplastic resin and the second resin layer-forming layer containing a thermoplastic resin, so that the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm (absorbance A / absorbance B) in the resulting interlayer film is 0.50 or less. This step may be a step of curing the first resin layer-forming layer, a step of curing the second resin layer-forming layer, or a step of curing each of the first resin layer-forming layer and the second resin layer-forming layer.

[0133] In the method (2) for producing the interlayer film, it is preferable to include, after the curing step, a step of obtaining a laminate having a first resin layer-forming layer, a polyethylene terephthalate film, and a second resin layer-forming layer in this order.

[0134] In the step of obtaining the laminate in the interlayer film manufacturing methods (1) and (2), the method for obtaining the laminate is not particularly limited, and examples thereof include a method in which the first resin layer-forming layer, a polyethylene terephthalate film, and a second resin layer-forming layer are laminated in this order.

[0135] The curing step in the interlayer film manufacturing methods (1) and (2) is preferably step (A) of maintaining the film in an environment with a curing temperature of 20°C to 30°C and a curing humidity of 10% to 40% RH for 6 hours or longer, or step (B) of maintaining the film in an environment with a curing temperature of 40°C to 60°C and a curing humidity of 85% to 99% RH for 8 minutes or shorter. In this case, it is easy to adjust the ratio (absorbance A / absorbance B) to 0.50 or less. In particular, when the curing temperature is 20°C to 30°C, the curing humidity during curing must be kept fairly low in order to adjust the ratio (absorbance A / absorbance B) to 0.50 or less.

[0136] From the viewpoint of more easily controlling the ratio (absorbance A / absorbance B), it is preferable that the curing temperature, curing humidity, and curing time in the step (A) and the step (B) each satisfy the following conditions:

[0137] The curing temperature in the step (A) is preferably 22°C or higher, more preferably 23°C or higher, and preferably 28°C or lower, more preferably 27°C or lower. The curing humidity in the step (A) is preferably 15% RH or higher, more preferably 20% RH or higher, and preferably 35% RH or lower, more preferably 30% RH or lower. The curing time in the step (A) is preferably 7 hours or higher, more preferably 8 hours or higher. There is no particular limitation on the upper limit of the curing time in the step (A). The curing time in the step (A) is, for example, 24 hours or shorter.

[0138] The curing temperature in step (B) is preferably 43°C or higher, more preferably 45°C or higher, and preferably 58°C or lower, more preferably 55°C or lower. The curing humidity in step (B) is preferably 90% RH or higher, more preferably 93% RH or higher, and preferably 98% RH or lower, more preferably 97% RH or lower. The curing time in step (B) is preferably 7 minutes or shorter, more preferably 6 minutes or shorter. There is no particular limitation on the lower limit of the curing time in step (B). The curing time in step (B) is, for example, 0.5 minutes or longer.

[0139] (Laminated Glass) The laminated glass according to the present invention includes a first laminated glass member, a second laminated glass member, and an interlayer film. In the laminated glass according to the present invention, the interlayer film is disposed between the first laminated glass member and the second laminated glass member.

[0140] FIG. 3 is a cross-sectional view that schematically shows an example of laminated glass that uses the interlayer film for laminated glass shown in FIG. 2 .

[0141] The laminated glass 31 shown in Fig. 3 includes a first laminated glass member 21, a second laminated glass member 22, and an interlayer film 11. The interlayer film 11 is disposed and sandwiched between the first laminated glass member 21 and the second laminated glass member 22.

[0142] A first laminated glass member 21 is laminated on a first surface 11a of the interlayer film 11. A second laminated glass member 22 is laminated on a second surface 11b opposite to the first surface 11a of the interlayer film 11. The first laminated glass member 21 is disposed and laminated on the outer surface 2a of the first resin layer 2. The second laminated glass member 22 is disposed and laminated on the outer surface 3a of the second resin layer 3.

[0143] Examples of the first and second laminated glass members include glass plates and PET (polyethylene terephthalate) films. The laminated glass includes not only laminated glass in which an interlayer film is sandwiched between two glass plates, but also laminated glass in which an interlayer film is sandwiched between a glass plate and a PET film or the like. The laminated glass is a laminate including glass plates, and preferably includes at least one glass plate. It is preferable that the first laminated glass member and the second laminated glass member are each a glass plate or a PET film, and that the laminated glass includes a glass plate as at least one of the first laminated glass member and the second laminated glass member. It is particularly preferable that both the first and second laminated glass members are glass plates.

[0144] Examples of the glass plate include inorganic glass and organic glass. Examples of the inorganic glass include float glass, heat-absorbing glass, heat-reflecting glass, polished glass, patterned glass, lined glass, and green glass. The organic glass is a synthetic resin glass that replaces inorganic glass. Examples of the organic glass include polycarbonate plates and poly(meth)acrylic resin plates. Examples of the poly(meth)acrylic resin plates include polymethyl(meth)acrylate plates.

[0145] The first laminated glass member is preferably a first glass plate, and the second laminated glass member is preferably a second glass plate.

[0146] The thickness of each of the first and second laminated glass members is preferably 1 mm or more, more preferably 1.8 mm or more, even more preferably 2 mm or more, particularly preferably 2.1 mm or more, and preferably 5 mm or less, more preferably 3 mm or less. Furthermore, when the first and second laminated glass members are glass plates, the thickness of the glass plates is preferably 1 mm or more, more preferably 1.8 mm or more, even more preferably 2 mm or more, particularly preferably 2.1 mm or more, and preferably 5 mm or less, more preferably 3 mm or less, and even more preferably 2.6 mm or less. When the first and second laminated glass members are PET films, the thickness of the PET films is preferably 0.03 mm or more, and preferably 0.5 mm or less.

[0147] The method for producing the laminated glass is not particularly limited. First, an interlayer film is sandwiched between the first laminated glass member and the second laminated glass member to obtain a laminate. Next, the air remaining between the first laminated glass member, the second laminated glass member, and the interlayer film is removed, for example, by passing the obtained laminate through a pressure roll or placing it in a rubber bag and suctioning it under reduced pressure. Thereafter, a pre-bonded laminate is obtained by pre-bonding at about 70 to 110°C. Next, the pre-bonded laminate is placed in an autoclave or pressed at about 120 to 150°C and a pressure of 1 to 1.5 MPa. In this manner, a laminated glass can be obtained. Each layer may be laminated during the production of the laminated glass.

[0148] The interlayer film and the laminated glass can be used in automobiles, railway vehicles, aircraft, ships, buildings, etc. The interlayer film and the laminated glass can also be used for applications other than these. The interlayer film and the laminated glass are preferably interlayer films and laminated glass for vehicles or buildings, and more preferably interlayer films and laminated glass for vehicles. The interlayer film and the laminated glass can be used for automobile windshields, side windows, rear windows, roof glass, backlight glass, etc. The interlayer film and the laminated glass are preferably used in automobiles. The interlayer film is preferably used to obtain laminated glass for automobiles.

[0149] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0150] The polyvinyl acetal resin used was acetalized using n-butylaldehyde having a carbon number of 4. The degree of acetalization (degree of butyralization), degree of acetylation, and hydroxyl group content of the polyvinyl acetal resin were measured by a method conforming to JIS K6728 "Testing Methods for Polyvinyl Butyral." Note that when measured by ASTM D1396-92, the values ​​shown were similar to those obtained by the method conforming to JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0151] (Thermoplastic resin) Polyvinyl acetal resin (PVB, average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1 mol%, acetalization degree 68.5 mol%)

[0152] (Plasticizer) 3GO: Triethylene glycol di-2-ethylhexanoate

[0153] (Metal salt) Mg mixture (a 50:50 (weight ratio) mixture of magnesium 2-ethylbutyrate and magnesium acetate)

[0154] (UV Screening Agent) Tinuvin 326: 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin 326" manufactured by BASF)

[0155] (Antioxidant) BHT: 2,6-di-t-butyl-p-cresol

[0156] The following polyethylene terephthalate films were prepared:

[0157] Nano90S (multilayer polyethylene terephthalate film, Sumitomo 3M's "Multilayer Nano 90S", thickness 75 μm) XIR-75 (metal layer-containing polyethylene terephthalate film, Southwall Technologies' "XIR-75", thickness 50 μm) Lumirror T60 (single layer polyethylene terephthalate film, Toray Industries' "Lumirror T60", thickness 100 μm) ST-22 (multilayer polyethylene terephthalate film, Toray Industries' "ST-22", thickness 100 μm)

[0158] The curing conditions described below are shown in Table 1 below.

[0159]

[0160] Example 1 Preparation of Layer for Forming First Resin Layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a composition for forming the first resin layer.

[0161] PVB: 100 parts by weight 3GO: 40 parts by weight Mg mixture: an amount that results in a magnesium content of 70 ppm in the resulting first resin layer Tinuvin 326: an amount that results in a magnesium content of 0.2% by weight in the resulting first resin layer BHT: an amount that results in a magnesium content of 0.2% by weight in the resulting first resin layer

[0162] The obtained composition for forming the first resin layer was extruded by an extruder to obtain a layer for forming the first resin layer.

[0163] Preparation of Layer for Forming Second Resin Layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a composition for forming the second resin layer.

[0164] PVB: 100 parts by weight 3GO: 40 parts by weight Mg mixture: an amount that results in a magnesium content of 70 ppm in the resulting second resin layer Tinuvin 326: an amount that results in a magnesium content of 0.2% by weight in the resulting second resin layer BHT: an amount that results in a magnesium content of 0.2% by weight in the resulting second resin layer

[0165] The obtained composition for forming the second resin layer was extruded by an extruder to obtain a layer for forming the second resin layer.

[0166] The obtained first resin layer forming layer and second resin layer forming layer were cured under the curing condition A shown in Table 1, respectively.

[0167] Next, the first resin layer-forming layer, the polyethylene terephthalate film shown in Table 2, and the second resin layer-forming layer were laminated in this order, and pressed with a pressure roll at 100°C and 0.2 MPa to obtain an interlayer film. In the obtained interlayer film, the first resin layer and the second resin layer were each rectangular, and the thickness of the first resin layer and the second resin layer was each 380 µm.

[0168] Preparation of laminated glass: Two 2 mm thick clear glass sheets conforming to JIS R3202:1996 were prepared. The obtained interlayer film was sandwiched between the two clear glass sheets to obtain a laminate. The obtained laminate was placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes, then transferred to an oven in the degassed state and held at 90°C for 30 minutes for vacuum pressing to pre-bond the laminate. The pre-bonded laminate was then bonded in an autoclave for 20 minutes under conditions of 135°C and a pressure of 1.2 MPa to obtain a laminated glass (10 cm long x 10 cm wide). The obtained laminated glass corresponds to the above-mentioned laminated glass X.

[0169] Examples 2 to 8 and Comparative Examples 1 to 6 Interlayer films and laminated glasses (laminated glass X) were obtained in the same manner as in Example 1, except that the type of polyethylene terephthalate film and the curing conditions were changed as shown in the table below.

[0170] (Reference Examples A to F) Interlayer films and laminated glasses (laminated glass X) were obtained in the same manner as in Example 1, except that no polyethylene terephthalate film was used and the curing conditions were changed as shown in the table below.

[0171] (Evaluation) (1) Absorbance In the obtained laminated glass (laminated glass X), a position 3 cm from one end toward the other end was designated as the first position, and a position 5 cm from one end toward the other end was designated as the second position. The absorbance at each of the first and second positions of laminated glass X was measured using a near-infrared spectrophotometer ("V-570" manufactured by JASCO Corporation) under the following conditions: bandwidth 2 nm, scanning speed 1000 nm / min, scan range 1550 nm to 2050 nm, and data acquisition interval 0.5 nm. Next, the absorbance at the first position and the absorbance at the second position were averaged at the same wavelength, and an absorbance spectrum was created from the averaged absorbance.

[0172] In the prepared absorbance spectrum, the line connecting the position of absorbance at a wavelength of 1873 nm and the position of absorbance at a wavelength of 1984 nm was defined as the baseline for absorbance A. The absolute value of the difference between the absorbance at a wavelength of 1930 nm on the baseline for absorbance A and the absorbance at a wavelength of 1930 nm on the prepared absorbance spectrum was defined as the absorbance A of the interlayer film at a wavelength of 1930 nm.

[0173] The absolute value of the difference between the absorbance at a wavelength of 1670 nm on the prepared absorbance spectrum and the absorbance at a wavelength of 1705 nm on the prepared absorbance spectrum was taken as the absorbance B of the interlayer film at a wavelength of 1705 nm.

[0174] Furthermore, the ratio (absorbance A / absorbance B) was calculated from the obtained absorbance A and absorbance B.

[0175] (2) Heat Resistance Test at 100° C. (Haze Value) The obtained laminated glass (Laminated Glass X) was placed in an incubator at 100° C. The haze values ​​of the laminated glass before being placed in the incubator and the laminated glasses after being placed in the incubator for 7 days, 14 days, 28 days, and 56 days were measured as follows.

[0176] In the obtained laminated glass (laminated glass X), a position 3 cm from one end toward the other end was designated as a first position, and a position 5 cm from one end toward the other end was designated as a second position. The haze value was measured at each of the first and second positions in accordance with JIS K6714. The average of the haze value at the first position and the haze value at the second position was designated as the haze value of the laminated glass.

[0177] The haze value of the laminated glass before being left standing in the incubator was subtracted from the haze value of the laminated glass after being left standing in the incubator for 56 days, and the difference was taken as the change in haze value (Day 0 to Day 56).

[0178] Details and results are shown in Tables 2 to 5 below.

[0179]

[0180]

[0181]

[0182]

[0183] As shown in Tables 2 to 4, when the ratio (absorbance A / absorbance B) is 0.50 or less, the haze value can be kept low when the laminated glass is subjected to a heat resistance test at 100°C, even though the interlayer film includes a polyethylene terephthalate film. On the other hand, as shown in Table 5, when the interlayer film does not include a polyethylene terephthalate film, the problem of the laminated glass having an increased haze value does not occur when the heat resistance test at 100°C is performed.

[0184] REFERENCE SIGNS LIST 1...Polyethylene terephthalate film 1a...First surface 1b...Second surface 2...First resin layer 2a...Outer surface 3...Second resin layer 3a...Outer surface 11...Interlayer film 11a...First surface 11b...Second surface 21...First laminated glass member 22...Second laminated glass member 31...Laminated glass

Claims

1. An interlayer film for laminated glass comprising, in this order, a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a second resin layer containing a thermoplastic resin, wherein the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm is 0.50 or less.

2. The interlayer film for laminated glass according to claim 1, wherein the polyethylene terephthalate film is a multilayer polyethylene terephthalate film having two or more polyethylene terephthalate layers and no metal layer, or a metal layer-containing polyethylene terephthalate film having a polyethylene terephthalate layer and a metal layer.

3. The interlayer film for laminated glass according to claim 1 or 2, wherein the thermoplastic resin contained in the first resin layer comprises a polyvinyl acetal resin, and the thermoplastic resin contained in the second resin layer comprises a polyvinyl acetal resin.

4. A method for producing an interlayer film for laminated glass according to any one of claims 1 to 3, comprising the steps of obtaining a laminate comprising, in this order, a layer for forming a first resin layer containing a thermoplastic resin, a polyethylene terephthalate film, and a layer for forming a second resin layer containing a thermoplastic resin, and curing the laminate so that the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm in the obtained interlayer film is 0.50 or less.

5. A method for producing an interlayer film for laminated glass according to any one of claims 1 to 3, comprising a step of curing at least one of the layer for forming a first resin layer containing a thermoplastic resin and the layer for forming a second resin layer containing a thermoplastic resin, so that in the obtained interlayer film, the ratio of absorbance A at a wavelength of 1930 nm to absorbance B at a wavelength of 1705 nm is 0.50 or less.

6. A laminated glass comprising: a first laminated glass component; a second laminated glass component; and the interlayer film for laminated glass according to any one of claims 1 to 3, wherein the interlayer film for laminated glass is disposed between the first laminated glass component and the second laminated glass component.

Citation Information

Patent Citations

  • Intermediate film for sandwich glass as well as sandwich glass and method for manufacturing the same

    JP2001226153A

  • Laminated glass and method for manufacturing the same

    JP2010265165A

  • Polyvinyl acetal resin for interlayer film

    JP2015067477A

  • Laminated glass comprising functional film

    JP2018008867A