Curable resin composition

The curable resin composition, featuring modified polyolefin A and B with a nanocrystalline structure and moisture-curable functional groups, addresses the issues of high viscosity and poor heat-resistant creep in conventional compositions, offering excellent coatability and heat-resistant properties for adhesive applications.

WO2024248150A1PCT designated stage expired Publication Date: 2024-12-05TOYOBO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/020107
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-30
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional curable resin compositions face issues with high viscosity, affecting coating properties, and poor heat-resistant creep properties, limiting their application in adhesive materials.

Method used

A curable resin composition comprising modified polyolefin A and B, with a nanocrystalline structure, where polyolefin B is an ethylene-butylene-propylene copolymer, and includes a moisture-curable functional group, a moisture curing accelerator, and a catalyst, resulting in a composition with improved melt viscosity and heat-resistant creep properties.

Benefits of technology

The composition exhibits excellent coatability in the molten state and enhanced heat-resistant creep properties, making it suitable for use as a hot melt adhesive with improved flexibility and adhesive strength across various environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention provides a curable resin composition which has excellent coatability in a molten state and exhibits excellent creep characteristics even in a high-temperature environment. The present invention specifically provides a curable resin composition which contains a modified polyolefin A and a modified polyolefin B, wherein: the modified polyolefin A has a chemical structure that is obtained by grafting a moisture-curable functional group to a polyolefin a; the modified polyolefin B has a chemical structure that is obtained by grafting a moisture-curable functional group to a polyolefin b; the polyolefin b has a nanocrystalline structure; and the melt viscosity of the curable resin composition is 35,000 cps or less at 140°C.
Need to check novelty before this filing date? Find Prior Art

Description

Curable resin composition

[0001] The present invention relates to a curable resin composition.

[0002] Hot melt adhesives have traditionally been used in fields such as building materials, automotive interior materials, and electrical component assembly because they can bond in a short time and do not contain solvents. For example, automotive interior materials (ceilings, doors, seats, etc.) are composed of molded products and skin materials. Polyolefin molded products (polypropylene, polyethylene, etc.) are mainly used as the molded products, and polyolefin skin materials are mainly used as the skin materials. Automotive interior materials are produced by bonding these molded products and skin materials with hot melt adhesives using methods such as press bonding and vacuum forming.

[0003] Curable resin compositions are widely used as materials for hot melt adhesives (see, for example, Patent Documents 1 and 2). Patent Document 1 describes a curable resin composition comprising a styrene block copolymer graft-polymerized with an acrylic monomer, and a silane coupling agent blended therein. Patent Document 2 describes a curable resin composition comprising a reaction product of a modified polyolefin resin modified with an unsaturated carboxylic acid and / or a derivative thereof, and a compound having a functional group reactive with the modified polyolefin resin and a reactive silyl group.

[0004] Japanese Patent Publication No. 2000-303047 Japanese Patent Publication No. 2010-059319

[0005] However, when the curable resin composition described in Patent Document 1 is applied to a substrate, there is a problem in coatability due to high viscosity. Also, the curable resin composition described in Patent Document 2 has a problem in that it is poor in heat creep resistance.

[0006] The present invention has been made in view of the above, and an object of the present invention is to provide a curable resin composition that has excellent coatability in a molten state and excellent heat creep resistance after a curing reaction.

[0007] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the following specific curable resin composition has excellent coatability in a molten state and excellent heat creep resistance after a curing reaction, and have thus completed the present invention.

[0008] The present invention encompasses, for example, the subject matter described in the following items: Item 1. A curable resin composition containing modified polyolefin A and modified polyolefin B, wherein modified polyolefin A has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin a, modified polyolefin B has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin b, said polyolefin b having a nanocrystalline structure, and wherein the melt viscosity of said curable resin composition at 140°C is 35,000 cps (= mPa s) or less.

[0009] The curable resin composition of the present invention exhibits excellent coatability in a molten state and excellent heat creep resistance after the curing reaction.

[0010] 1 is a diagram showing a bonded sample in a method for evaluating heat creep resistance; and FIG. 2 is a diagram showing the relationship between a measurement sample and a weight in a method for evaluating heat creep resistance.

[0011] Hereinafter, a curable resin composition according to an embodiment of the present invention will be described. In the following, the notation "to" indicating a numerical range means "less than" or "exceeding," unless otherwise specified. In other words, "A to B" means "A or more and B or less."

[0012] <Curable Resin Composition> The curable resin composition of the present invention is a curable resin composition containing modified polyolefin A and modified polyolefin B. When 100 parts by mass of the combined total of modified polyolefin A and modified polyolefin B is immersed in xylene at 100°C for 1 hour, preferably 25 to 40 parts by mass remain undissolved, and when immersed in xylene at 120°C for 1 hour, preferably 0.1 to 5 parts by mass remain undissolved. The curable resin composition of the present invention may further contain, in addition to modified polyolefin A and modified polyolefin B, a moisture-cure accelerator C, a moisture-cure catalyst D, a diluent, a tackifier, a wax, an antioxidant, etc. The curable resin composition of the present invention can be produced by melt-kneading the constituent components thereof, and may be cooled and solidified to form granules or powder, or may be dissolved or dispersed in a solvent to form a liquid.

[0013] <Modified Polyolefin A and Modified Polyolefin B> The modified polyolefin A in the present invention has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin a. The modified polyolefin B in the present invention has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin b. The chemical structure obtained by grafting refers to the chemical structure in a grafted state, and for example, modified polyolefin A can also be expressed as "a chemical structure in which a moisture-curable functional group is grafted onto polyolefin a."

[0014] Examples of the polyolefin a or the polyolefin b include homopolymers of α-olefins polymerized from monomer components such as ethylene, propylene, 1-butene, isobutene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene; copolymers of ethylene with α-olefins other than ethylene, such as ethylene-propylene copolymers, ethylene-propylene-butylene copolymers, and ethylene-propylene-isobutylene copolymers; Examples of the polyolefin-based polymer include copolymers of α-olefins with other monomers copolymerizable with α-olefins (for example, conjugated or non-conjugated dienes such as butadiene, 1,4-hexadiene, 7-methyl-1,6-octadiene, 1,8-nonadiene, and 1,9-decadiene; cyclic olefins such as cyclopropene, cyclobutene, cyclopentene, cyclohexene, norbornene, and dicyclopentadiene); copolymers of isobutylene and isoprene; polychloroprene; polyisoprene; copolymers of isoprene or butadiene with acrylonitrile and / or styrene; and polybutadiene. Among the polyolefin-based polymers described above, in the present invention, from the viewpoint of adhesion of the curable resin composition to polyolefins and the like, preferred are propylene homopolymers, ethylene-propylene copolymers, ethylene-propylene-butylene copolymers, and ethylene-propylene-isobutylene copolymers, with propylene homopolymers being more preferred.

[0015] The polyolefin a is preferably a polypropylene-based polymer, and more preferably a homopolypropylene. The melting point of the polyolefin a is preferably 100 to 190°C, more preferably 120 to 170°C, and even more preferably 130 to 160°C. The glass transition temperature of the polyolefin a is preferably -20 to 5°C, more preferably -15 to 0°C, and even more preferably -10 to 0°C. The melt viscosity of the polyolefin a at 140°C is preferably 20,000 cps or less, more preferably 15,000 cps or less, and even more preferably 10,000 cps or less, with a lower limit of approximately 1,000 cps, although not critical. The polyolefin a preferably satisfies two or more of the above-mentioned ranges of composition, melting point, glass transition temperature, and melt viscosity, and more preferably satisfies all of them.

[0016] The polyolefin b is particularly preferably an ethylene-butylene-propylene copolymer. The melting point of the polyolefin b is preferably 100 to 190°C, more preferably 130 to 170°C, and even more preferably 120 to 150°C. The glass transition temperature of the polyolefin b is preferably -20 to 20°C, more preferably -20 to 15°C, and even more preferably -20 to -10°C. The polyolefin b preferably satisfies two or more of the above-mentioned composition, melting point, and glass transition temperature ranges, and more preferably satisfies all of them.

[0017] The modified polyolefin A and the modified polyolefin B can be produced by known methods. For example, they can be produced by grafting moisture-curable functional groups onto the polyolefin a and the polyolefin b in the presence of a radical initiator or by electron beam irradiation. The grafting reaction may be carried out on the polyolefin a and the polyolefin b individually, or on a mixture of the polyolefin a and the polyolefin b. Examples of the radical initiator include peroxide initiators such as dicumyl peroxide, t-butylperoxyisopropyl carbonate, di-t-butyl peroxide, t-butyl perbenzoate, benzoyl peroxide, cumene hydroperoxide, t-butyl peroctoate, methyl ethyl ketone peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, lauryl peroxide, t-butyl peracetate, t-butyl-α-cumyl peroxide, di-t-butyl peroxide, methyl ethyl ketone ... Examples of the radical initiator include dicumyl peroxide, di-t-amyl peroxide, t-amyl peroxybenzoate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, α,α'-bis(t-butylperoxy)-1,3-diisopropylbenzene, α,α'-bis(t-butylperoxy)-1,4-diisopropylbenzene, 2,5-bis(t-butylperoxy)-2,5-dimethylhexane, and 2,5-bis(t-butylperoxy)-2,5-dimethyl-3-hexyne. These radical initiators can be used alone or in combination of two or more. Among these, dicumyl peroxide and t-butylperoxyisopropyl carbonate are preferred.

[0018] Examples of moisture-curable functional groups used in the synthesis of modified polyolefin A and modified polyolefin B include an isocyanate group and a hydrolyzable silyl group. During the synthesis, a compound having a moisture-curable functional group is grafted onto the polyolefin a and the polyolefin b, and a silane-modified monomer containing a hydrolyzable silyl group and an ethylenically unsaturated group can be suitably used as the compound from the viewpoint of reactivity control. Such a silane-modified monomer can be, for example, a compound represented by the following formula (1): X n R 3-n -Si-Y (1) (wherein Y is an ethylenically unsaturated group, X is a hydrolyzable silyl group, R is an alkyl group, and n is an integer of 1 to 3).

[0019] Examples of the hydrolyzable group in the above formula (1) include halogen, alkoxy groups, alkenyloxy groups, acyloxy groups, amino groups, aminooxy groups, oxime groups, and amide groups. The alkoxy group is preferably a methoxy group. The number of these hydrolyzable groups bonded to one silicon atom is selected from the range of 1, 2, and 3. The number of hydrolyzable groups bonded to one silicon atom may be one or more. Furthermore, a hydrolyzable group and a non-hydrolyzable group may be bonded to one silicon atom. As the hydrolyzable group bonded to the silicon group, an alkoxy group (such as a monoalkoxy group, a dialkoxy group, or a trialkoxy group) is preferred because of its ease of handling. In the above formula (1), n ​​is preferably 3. Examples of the ethylenically unsaturated group contained in the silane-modified monomer include a vinyl group, an aryl group, an acrylic group, and a methacrylic group. Preferred silane-modified monomers having an ethylenically unsaturated group include vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, and 3-methacryloxypropyltrimethoxysilane.

[0020] The amount of radical initiator used in producing modified polyolefin A and modified polyolefin B is preferably 0.5 to 10 parts by mass, more preferably 0.75 to 8 parts by mass, and even more preferably 1 to 5 parts by mass, per 100 parts by mass of the total amount of polyolefin a and polyolefin b (or the amount of that polyolefin when only one of them is used as a raw material). When the amount of radical initiator is 0.5 parts by mass or more, the graft reaction proceeds sufficiently, improving the room temperature adhesive strength, adhesive strength in high-temperature environments, and creep properties of the cured curable resin composition or hot-melt adhesive using the curable resin composition. When the amount of radical initiator is 10 parts by mass or less, side reactions such as homopolymerization of the silane-modified monomer or decomposition reaction of the polyolefin are suppressed.

[0021] The amount of the silane-modified monomer used in producing modified polyolefin A and modified polyolefin B is preferably 0.5 to 10 parts by mass, more preferably 0.75 to 8 parts by mass, and particularly preferably 1 to 8 parts by mass, per 100 parts by mass of the total amount of polyolefin a and polyolefin b (or the amount of the polyolefin a when only one of them is used as a raw material). When the amount of the silane-modified monomer used is 0.5 parts by mass or more, the graft polymerization reaction proceeds sufficiently, and the heat creep resistance and adhesive strength after aging of the curable resin composition and hot melt adhesives using the curable resin composition are further improved. When the amount of the silane-modified monomer used is 10 parts by mass or less, side reactions such as homopolymerization of the silane-modified monomer and decomposition reaction of polyolefin a are further suppressed.

[0022] The melt viscosity of the modified polyolefin A at 140°C is preferably 35,000 mPa·s or less, more preferably 25,000 mPa·s or less, even more preferably 15,000 mPa·s or less, and most preferably 10,000 mPa·s or less, with the lower limit being, but not limited to, about 1,000 mPa·s. When the melt viscosity of the modified polyolefin A at 140°C is 35,000 mPa·s or less, the curable resin composition and the hot melt adhesive using the curable resin composition can be easily applied to an adherend.

[0023] The melt viscosity of the curable resin composition of the present invention containing the modified polyolefin A and the modified polyolefin B is 35,000 mPa s or less, preferably 34,000 mPa s or less, more preferably 33,000 mPa s or less, and the lower limit is not particularly limited but is about 30,000 mPa s. When the melt viscosity of the curable resin composition at 140°C is 35,000 mPa s or less, the curable resin composition and the hot melt adhesive using the curable resin composition can be easily applied to an adherend.

[0024] The melt viscosities of the modified polyolefin A and the curable resin composition were measured using a Brookfield type viscometer (e.g., Brookfield DVNXRVTJG type). The measurement conditions and determination method were as follows. 11 g of sample was placed in the measurement chamber of the Brookfield type viscometer (Brookfield DVNXRVTJG type), heated to 200°C to melt the sample, and then cooled to 140°C, and the viscosity was measured in accordance with the melt viscosity test method for hot melt adhesives of JIS K6862. The spindle No. 27 used in the measurement was set to a rotation speed of 5 rpm.

[0025] The melting point (Tm) of the modified polyolefin A is preferably 120°C to 170°C, more preferably 130°C to 160°C. When the melting point of the modified polyolefin A is 120°C or higher, the adhesive strength at around room temperature and in a high-temperature environment of the curable resin composition or the hot-melt adhesive using the curable resin composition cured under any environment, and the creep properties in a high-temperature environment are improved. When the melting point of the modified polyolefin A is 170°C or lower, the curable resin composition and the hot-melt adhesive using the curable resin composition can be applied without affecting the adherend.

[0026] The melting point (Tm) of the modified polyolefin B is preferably 120°C to 170°C, more preferably 120°C to 150°C. When the melting point of the modified polyolefin B is 120°C or higher, the adhesive strength at around room temperature and in a high-temperature environment of the curable resin composition or the hot-melt adhesive using the curable resin composition cured under any environment, and the creep properties in a high-temperature environment are improved. When the melting point of the modified polyolefin B is 170°C or lower, the curable resin composition and the hot-melt adhesive using the curable resin composition can be applied without affecting the adherend.

[0027] The melting points (Tm) of modified polyolefin A and modified polyolefin B were determined by DSC measurement using a differential scanning calorimeter (DSC, for example, DuPont V4.OB2000). The measurement conditions and determination method were as follows: 10 mg of a sample was heated from 25°C to 200°C at a rate of 25°C / min under a nitrogen atmosphere, held at 200°C for 5 minutes, and then cooled to 25°C at a rate of 25°C / min. The sample was then heated from 25°C to 200°C at a rate of 25°C / min. The melting point (Tm) was determined as the peak top of the endothermic peak observed at the highest temperature side of the heat of fusion absorption curve detected during this heating process.

[0028] The modified polyolefin A and the modified polyolefin B may or may not have an observable glass transition point. When a glass transition point is observable, the glass transition temperature (Tg) is preferably 15° C. or lower, more preferably −20° C. to 10° C. When the glass transition temperatures of the modified polyolefin A and the modified polyolefin B are 15° C. or lower, the curable resin composition does not become too hard even in a low-temperature environment, and can maintain adhesion to a substrate.

[0029] The glass transition temperatures (Tg) of modified polyolefin A and modified polyolefin B were determined from the temperature dependence of dynamic viscoelasticity. The measurement conditions and determination method were as follows. Using a "DVA-200" manufactured by IT Measurement & Control Co., Ltd., the storage modulus (E') and loss modulus (E'') were measured at a sample thickness of approximately 0.5 mm, attachment mode: tension-compression mode, frequency: 10 Hz, temperature: -100°C to 200°C, and heating rate: 4°C / min, and the loss tangent (tan δ) was calculated. The peak top temperature of the loss tangent tan δ (loss modulus E'' / storage modulus E') in the dynamic viscoelasticity measurement was taken as the glass transition temperature (Tg) [°C].

[0030] The number average molecular weight of the modified polyolefin A is preferably 2,000 to 10,000, more preferably 4,000 to 6,000. When the number average molecular weight of the modified polyolefin A is 2,000 or more, the adhesive strength at room temperature and in a high-temperature environment of the cured curable resin composition or the hot-melt adhesive using the curable resin composition, as well as the creep properties in a high-temperature environment, are improved. When the number average molecular weight of the modified polyolefin A is 10,000 or less, the curable resin composition and the hot-melt adhesive using the curable resin composition can be easily applied to an adherend.

[0031] The number average molecular weight of the modified polyolefin B is preferably 50,000 to 100,000, more preferably 80,000 to 100,000. When the number average molecular weight of the modified polyolefin B is 50,000 or more, the room temperature adhesive strength and adhesive strength in a high temperature environment, as well as creep characteristics, of the cured curable resin composition or hot melt adhesive using the curable resin composition are improved. When the number average molecular weight of the modified polyolefin B is 100,000 or less, the curable resin composition and the hot melt adhesive using the curable resin composition can be easily applied to an adherend.

[0032] The number average molecular weights of Modified Polyolefin A and Modified Polyolefin B are polystyrene-equivalent values ​​determined by GPC (gel permeation chromatography, in accordance with DIN 55 672). The measurement conditions and determination method were as follows: GPC measurement device: HLC-8321GPC / HT (manufactured by Tosoh Corporation) Column: Waters Styragel HT3,4,6E Detector: RI Solvent: ortho-dichlorobenzene (containing 0.5 mg / mL of butylated hydroxyltoluene) Measurement temperature: 140°C Flow rate: 0.3 mL / min Sample concentration: 1.2 to 1.7 mg / mL Injection volume: 200 μL Analysis program: GPC data processing system (TOSOH)

[0033] It is preferable that polyolefin b and / or modified polyolefin B have a controlled nanocrystalline structure. Polyolefin b is preferably a thermoplastic polyolefin-based elastomer in which the crystalline / amorphous structure of the polymer is controlled on the nano-order, and the crystals have a network structure on the nano-order. Suitable examples include, but are not limited to, TAFMER (registered trademark) PN-2070, PN-3560, PN-2060, and PN-20300 manufactured by Mitsui Chemicals, Inc. The nanocrystalline structure-controlled polyolefin resin of the present invention has a crystal size controlled on the nano-order, whereas conventional polyolefins have a crystal size on the micron order. Therefore, compared to conventional polyolefin resins, it is often superior in transparency, heat resistance, flexibility, rubber elasticity, and the like. In the present invention, since modified polyolefin B has a controlled nanocrystalline structure, the flexibility of the resulting curable resin composition and hot melt adhesives using the curable resin composition at low temperatures (0°C) is significantly improved. By improving flexibility at low temperatures, the adhesive surface is less likely to peel when the hot melt adhesive cools and solidifies during the bonding process and when the bonded body is used in a cold environment. On the other hand, when a polyolefin resin without a controlled nanocrystalline structure is used, the flexibility of the resulting curable resin composition and the hot melt adhesive using the curable resin composition at low temperatures (0°C) is poor, and the adhesive surface is more likely to peel.

[0034] The breaking elongation at low temperature (0°C) of the resulting curable resin composition and the hot melt adhesive using the curable resin composition in an uncured state is not particularly limited, but is preferably 300% or more, more preferably 350% or more, and even more preferably 400% or more. When the breaking elongation is 300% or more, the hot melt adhesive tends to be difficult to peel at the bonding surface during the process of cooling and solidifying in the bonding step.

[0035] The breaking elongation at low temperature (0°C) after curing and aging of the resulting curable resin composition and the hot melt adhesive using the curable resin composition is not particularly limited, but is preferably 200% or more, more preferably 250% or more, and even more preferably 300% or more. When the breaking elongation is 200% or more, the bonded body tends to be less likely to peel at the adhesive surface when used in a cold environment.

[0036] The content of modified polyolefin B is preferably 5 to 15 parts by mass, more preferably 7 to 13 parts by mass, and even more preferably 9 to 11 parts by mass, per 100 parts by mass of modified polyolefin A. Within this content range, the flexibility of the curable resin composition and the hot melt adhesive using the curable resin composition in a low-temperature environment is improved. Furthermore, the adhesive strength at room temperature and in a high-temperature environment, as well as the creep properties in a high-temperature environment, of the cured curable resin composition or the hot melt adhesive using the curable resin composition are improved.

[0037] It is preferable that when a total of 100 parts by mass of modified polyolefin A and modified polyolefin B is immersed in xylene at 100° C. for 1 hour, 25 to 40 parts by mass remains undissolved, and when immersed in xylene at 120° C. for 1 hour, 0.1 to 5 parts by mass remains undissolved. When the content is within the above range, excellent coatability in a molten state and excellent heat creep resistance are exhibited.

[0038] <Moisture Curing Accelerator C> The curable resin composition of the present invention may contain a moisture curing accelerator C. Preferred examples of the moisture curing accelerator C include, but are not limited to, acid-modified polyolefin CA and rosin compound CB having an acid functional group. The moisture curing accelerator C may be used alone or in combination of two or more types. The moisture curing accelerator C preferably has an acid functional group and satisfies at least one of a melting point of 70 to 100°C and a softening point of 100 to 140°C.

[0039] The acid-modified polyolefin CA is preferably, but not limited to, one obtained by grafting at least one of an α,β-unsaturated carboxylic acid and its acid anhydride (acid functional group) onto a polyolefin resin. Polyolefin resin refers to a polymer primarily composed of a hydrocarbon skeleton, such as a homopolymer of an olefin monomer, exemplified by ethylene, propylene, butene, butadiene, isoprene, etc., or a copolymer with other monomers, or a hydrogenated or halogenated version of the above homopolymer or copolymer. The acid-modified polyolefin CA is preferably one obtained by grafting at least one of an α,β-unsaturated carboxylic acid and its acid anhydride onto at least one of polyethylene, polypropylene, and propylene-α-olefin copolymer.

[0040] Propylene-α-olefin copolymers are copolymers of propylene as the main component with an α-olefin. As the α-olefin, for example, one or more of ethylene, 1-butene, 1-heptene, 1-octene, 4-methyl-1-pentene, vinyl acetate, etc. can be used. Among these α-olefins, ethylene and 1-butene are preferred. The ratio of the propylene component to the α-olefin component in the propylene-α-olefin copolymer is not limited, but the propylene component is preferably 50 mol% or more, and more preferably 70 mol% or more.

[0041] Examples of at least one of α,β-unsaturated carboxylic acids and acid anhydrides thereof (acid functional groups) include maleic acid, itaconic acid, citraconic acid, and their acid anhydrides. Among these, acid anhydrides are preferred, and maleic anhydride is more preferred. Specific examples include maleic anhydride-modified polypropylene, maleic anhydride-modified propylene-ethylene copolymer, maleic anhydride-modified propylene-butene copolymer, and maleic anhydride-modified propylene-ethylene-butene copolymer, and these acid-modified polyolefins can be used alone or in combination of two or more.

[0042] The method for producing the acid-modified polyolefin CA is not particularly limited, and examples thereof include a radical graft reaction (i.e., a reaction in which radical species are generated on a polymer that will become the main chain, and an unsaturated carboxylic acid and an acid anhydride are graft polymerized using the radical species as a polymerization initiation point).

[0043] Preferred examples of the acid-modified polyolefin CA include PMA-T, PMA-F2, PMA-HM (all trade names, chlorinated maleic acid-modified polyolefins, manufactured by Toyobo Co., Ltd.), PMA-KH, PMA-L, PMA-LZ (all trade names, maleic acid-modified polyolefins, manufactured by Toyobo Co., Ltd.), Umex 1001, Umex 1010, Umex 100TS, Umex 5500 (all trade names, manufactured by Sanyo Chemical Industries, Ltd.), and the like.

[0044] The melting point (Tm) of the acid-modified polyolefin CA is preferably in the range of 70°C to 100°C. By setting it below the upper limit, excellent coatability and good heat creep resistance properties are achieved. The melting point (Tm) was determined by DSC measurement using a differential scanning calorimeter (DuPont, V4.OB2000 model). 10 mg of sample was heated from 25°C to 200°C at 25°C / min under a nitrogen atmosphere, held at 200°C for 5 minutes, and then cooled to 25°C at 25°C / min. The temperature was then raised from 25°C to 200°C at 25°C / min. The peak top of the endothermic peak observed on the highest temperature side of the heat of fusion absorption curve detected during this heating process was taken as the melting point (Tm).

[0045] Preferred examples of the rosin compound CB having an acid functional group include unsaturated acid-modified rosin obtained by adding an unsaturated acid such as maleic acid, fumaric acid, or acrylic acid by a Diels-Alder addition reaction, more specifically, maleopimaric acid obtained by adding maleic acid to rosin, fumaropimaric acid obtained by adding fumaric acid, and acrylopimaric acid obtained by adding acrylic acid, etc. Examples of esterified rosin include alkyl esters of rosin, glycerin ester obtained by esterifying rosin with glycerin, and pentaerythritol ester obtained by esterifying rosin with pentaerythritol, etc.

[0046] Specific examples of rosin compounds CB having an acid functional group include Hariestar DS-70L, Halitack R-80, Halitack FK100, Halitack FK125, Halitack SE10, Halitack F85, Halitack PH, Halitack F-75, Halitack FG-90, Halitack T-80, Halitack M-453, Halitack 4740, Halitack MSR-4, Halitack 28JA, Halitack PCJ, and Halitack AS-5 (all trade names, manufactured by Harima Chemicals Co., Ltd.). , Pine Crystal KE-100, Pine Crystal KE-311, Pine Crystal KE-590, Pine Crystal KE-359, Pine Crystal KE-604, Pine Crystal KE-140, Pine Crystal D-6011 (all trade names, manufactured by Arakawa Chemical Industries, Ltd.), Super Ester A-75, Super Ester A-100, Super Ester A-115, Super Ester A-125 (all trade names, manufactured by Arakawa Chemical Industries, Ltd.), and the like.

[0047] The softening point of the rosin compound CB having an acid functional group is preferably 100°C to 140°C. By setting the softening point to the upper limit or less, excellent coatability and heat creep resistance are achieved. In the present invention, the softening point of the rosin compound refers to a value measured using an RSP-202 (manufactured by RIGO Corporation) in accordance with JIS K6863, the softening point test method for hot melt adhesives.

[0048] The moisture curing accelerator C is preferably contained in an amount of 0.5 to 15 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 5 to 10 parts by mass, per 100 parts by mass of the total of the modified polyolefin A and the modified polyolefin B.

[0049] <Moisture Curing Catalyst D> The curable resin composition of the present invention may contain a moisture curing catalyst D. The moisture curing catalyst D is not particularly limited as long as it can promote the reaction of the moisture-curable functional groups of the modified polyolefin A and / or modified polyolefin B, typically the dehydration condensation reaction of the hydrolyzable silyl groups. Examples of the moisture curing catalyst D include organic bases, organic acids, carboxylic acids, and organometallic compounds (including organic titanates and complexes, or carboxylates of lead, cobalt, iron, nickel, zinc, and tin). Examples of organic bases include tertiary amines. Examples of organometallic compounds include dibutyltin dilaurate, dioctyltin maleate, dibutyltin diacetate, dibutyltin dioctate, stannous acetate, stannous octoate, lead naphthenate, zinc caprylate, and cobalt naphthenate. The moisture curing catalyst D may be used alone or in combination of two or more types. When the moisture curing catalyst D is contained in the present invention, the content of the moisture curing catalyst D is preferably 0.0001 to 10.0 parts by mass, more preferably 0.0005 to 5.0 parts by mass, and particularly preferably 0.001 to 0.5 parts by mass, relative to 100 parts by mass of the curable resin composition. When the content is 0.0001 to 10.0 parts by mass, the curable resin composition and the hot melt adhesive using the curable resin composition can be easily applied to an adherend.

[0050] <Diluents> The curable resin composition of the present invention may further contain one or more diluents. These diluents are generally used to reduce the viscosity of the curable resin composition. Such diluents are typically used in an amount of less than about 50 parts by weight, preferably less than about 40 parts by weight, and more preferably less than about 35 parts by weight, per 100 parts by weight of the curable resin composition of the present invention. Specific examples of such diluents include, but are not limited to, white mineral oil (e.g., Kaydol® oil available from Witco), Shellflex® 371 naphthenic oil (available from Shell Oil Company), and Calsol 5550 (a naphthenic oil from Calumet Lubricants).

[0051] <Tackifier> The curable resin composition of the present invention may further contain one or more tackifiers. When a tackifier is contained in the present invention, the proportion of the tackifier in 100% by mass of the curable resin composition is usually less than 50% by mass, preferably less than 40% by mass, and more preferably less than 35% by mass. Examples of tackifier resins include, but are not limited to, aliphatic, alicyclic, and aromatic hydrocarbons and modified hydrocarbons and hydrogenated products thereof; terpenes and modified terpenes and hydrogenated products thereof; rosin and rosin derivatives and hydrogenated products thereof; and mixtures thereof. A wide variety of known commercially available tackifiers can be used, including, for example, Eastotac H-100, Eastotac H-115, Eastotac H130, and Eastotac H142 (all trade names, manufactured by Eastman Chemical Co.), Escorez 5300, Escorez 5400, Escorez 5600, and Escorez 5637 (all trade names, manufactured by ExxonMobil Chemical Co.), Wingtack Extra and Hercolite 2100 (all trade names, manufactured by Goodyear Chemical Co.), Zonatac 105, and Zonatac 501 Lite (all trade names, manufactured by Arizona Examples include products manufactured by Nippon Chemiphar Chemical Co., Ltd.

[0052] Waxes The curable resin composition of the present invention may further contain one or more waxes. When a wax is included, it is present in an amount of less than 30% by weight, preferably less than 20% by weight, and more preferably less than 15% by weight, based on 100% by weight of the curable resin composition. Useful waxes include paraffin waxes, microcrystalline waxes, high-density, low-molecular-weight polyethylene waxes, pyrolysis waxes, by-product polyethylene waxes, Fischer-Tropsch waxes, oxidized Fischer-Tropsch waxes, and functionalized waxes (e.g., hydroxystearamide waxes and fatty amide waxes). It is common in the art to use the term "synthetic high-melting-point waxes" to include high-density, low-molecular-weight polyethylene waxes, by-product polyethylene waxes, and Fischer-Tropsch waxes.

[0053] <Antioxidant> The curable resin composition of the present invention may further contain one or more antioxidants. When an antioxidant is contained, the content of the antioxidant in 100% by mass of the curable resin composition is usually 0.5% by mass or less, preferably 0.2% by mass or less. As the antioxidant, a wide variety of known antioxidants can be used, and examples thereof include hindered phenol-based antioxidants (Irganox (registered trademark) 565, 1010, and 1076 manufactured by Ciba-Geigy); phosphite-based antioxidants (Irgafos (registered trademark) 168 manufactured by Ciba-Geigy); Cyanox (registered trademark) LTDP manufactured by Cytec Industries; and Ethanox (registered trademark) 1330 manufactured by Albemarle.

[0054] The moisture curing conditions for the curable resin composition are not particularly limited, and conditions typically employed when forming an adhesive layer using a moisture-curable hot melt adhesive may be used. The curing conditions for the curable resin composition layer are not particularly limited, but the curing temperature is preferably 20 to 80°C, more preferably 50 to 80°C. The curing time is preferably 1 to 14 days, more preferably 7 to 14 days. The humidity is preferably 20% RH to 80% RH, more preferably 50% RH to 80% RH, although immersion in water at the curing temperature for the curing time is also preferred.

[0055] The present invention provides the following aspects of the invention. Item 1. A curable resin composition containing modified polyolefin A and modified polyolefin B, wherein modified polyolefin A has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin a, and modified polyolefin B has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin b, and polyolefin b has a nanocrystalline structure, and the melt viscosity of the curable resin composition is 35,000 cps or less at 140°C. Item 2. The curable resin composition according to Item 1 above, wherein polyolefin b is an ethylene-butylene-propylene copolymer. Item 3. The curable resin composition according to Item 1 or 2 above, wherein polyolefin b has a melting point of 100 to 190°C. Item 4. The curable resin composition according to any one of Items 1 to 3 above, wherein polyolefin b has a glass transition temperature of -20 to 20°C. Item 5. The curable resin composition according to any one of Items 1 to 4, wherein the modified polyolefin B is contained in an amount of 5 to 15 parts by mass per 100 parts by mass of the modified polyolefin A. Item 6. The curable resin composition according to any one of Items 1 to 5, wherein the polyolefin a is polypropylene. Item 7. The curable resin composition according to any one of Items 1 to 6, wherein the polyolefin a has a melting point of 100 to 190°C. Item 8. The curable resin composition according to any one of Items 1 to 7, wherein the polyolefin a has a glass transition temperature of -20 to 5°C. Item 9. The curable resin composition according to any one of Items 1 to 8, wherein the polyolefin a has a melt viscosity at 140°C of 20,000 cps or less. Item 10. The curable resin composition according to any one of Items 1 to 9, further comprising 0.5 to 15 parts by mass of a moisture curing accelerator C per 100 parts by mass of the total of the modified polyolefin A and the modified polyolefin B. Item 11. Item 12. The curable resin composition according to item 10, wherein the moisture curing accelerator C has an acid functional group and satisfies at least one of a melting point of 70 to 100° C. and a softening point of 100 to 140° C. Item 13. The curable resin composition according to item 10 or 11, wherein the moisture curing accelerator C is an acid-modified polyolefin.Item 13. The curable resin composition according to any one of Items 10 to 12, wherein the acid functional group contained in the acid-modified polyolefin is maleic anhydride. Item 14. The curable resin composition according to Items 10 or 11, wherein the moisture curing accelerator C is a rosin compound having an acid functional group. Item 15. The curable resin composition according to any one of Items 1 to 9, further comprising 0.0001 to 10.0 parts by mass of a moisture curing catalyst D per 100 parts by mass of the modified polyolefin A and the modified polyolefin B combined, wherein the moisture curing catalyst D is an organometallic compound. Item 16. The curable resin composition according to any one of Items 1 to 15, wherein when 100 parts by mass of the modified polyolefin A and the modified polyolefin B combined is immersed in xylene at 100°C for 1 hour, 25 to 40 parts by mass remains undissolved, and when immersed in xylene at 120°C for 1 hour, 0.1 to 5 parts by mass remains undissolved. Item 17. 17. A hot melt adhesive comprising the curable resin composition according to any one of items 1 to 16.

[0056] First, each component used in preparing the curable resin composition (hot melt adhesive) will be described.

[0057] <Polyolefin a> Polyolefin a-1: Eastoflex P1010 (melting point: 152°C, glass transition temperature: -4°C, number average molecular weight: 5000, manufactured by Eastman Chemical Company) Polyolefin a-2: Lmodu s400 (melting point: 80°C, glass transition temperature: 6°C, number average molecular weight: 25000, manufactured by Idemitsu Kosan Co., Ltd.)

[0058] <Polyolefin b> Polyolefin b-1: Tafmer PN2070 (melting point: 140°C, glass transition temperature: -14°C, number average molecular weight: 90200, has a nanocrystalline structure, manufactured by Mitsui Chemicals, Inc.) Polyolefin b-2: Tafmer DF940 (melting point: 77°C, does not have a nanocrystalline structure, manufactured by Mitsui Chemicals, Inc.)

[0059] <Moisture Cure Accelerator C> Moisture curing accelerator C-1: PMA-L (acid value: 7 to 8 mgKOH / g, melting point: 70°C, manufactured by Toyobo Co., Ltd.) Moisture curing accelerator C-2: Haritack 4740 (acid value: 25 to 35 mgKOH / g, softening point: 115 to 125°C, manufactured by Harima Chemicals Co., Ltd.) Moisture curing accelerator C-3: Haritack MSR-4 (acid value: 120 to 150 mgKOH / g, softening point: 120 to 135°C, manufactured by Harima Chemicals Co., Ltd.) Moisture curing accelerator C-4: Harie Star AS-5 (acid value: 185 to 210 mgKOH / g, softening point: 160°C, manufactured by Harima Chemicals Co., Ltd.) Moisture curing accelerator C-5: Pine Crystal KE-604 (acid value: 230 to 245 mg KOH / g, softening point: 124 to 134°C, manufactured by Arakawa Chemical Industries, Ltd.)

[0060] <Moisture Curing Catalyst D> Moisture Curing Catalyst D-1: Neostan U-100 (manufactured by Nitto Kasei Co., Ltd.)

[0061] <Production of Modified Polyolefin Composition> 1) Production of Modified Polyolefin Composition X Modified polyolefin composition X was produced for use in evaluating the properties of modified polyolefin compositions in a state where moisture curing had hardly occurred. Modified polyolefin composition X was a composition that did not contain moisture curing accelerator C or moisture curing catalyst D.

[0062] Polyolefin, KBM-503 (3-methacryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Polymer Co., Ltd.), and PERBUTYL (registered trademark) I (t-butyl peroxy isopropyl monocarbonate, manufactured by NOF Corporation) in the blending ratios shown in Table 1 were added through the supply port of a twin-screw extruder (KZW15TW-45 / 60MG-NH(-2200) manufactured by Technovel Corporation (screw outer diameter 15 mm, L / D=60)), and while vacuum degassing was performed from the end of the twin-screw extruder, the mixture was kneaded at a barrel temperature of 160°C and an extrusion rate of 1.0 to 1.5 kg / h, to obtain a modified polyolefin composition X.

[0063]

[0064] 2) Preparation of Modified Polyolefin Composition Y Modified polyolefin composition Y was prepared for use in evaluating the properties of the modified polyolefin composition after moisture curing. Modified polyolefin composition Y is a composition containing moisture curing accelerator C or moisture curing catalyst D.

[0065] Modified polyolefin composition X and moisture curing accelerator C or moisture curing catalyst D in the blending ratios shown in Tables 2 and 3 were charged into a benchtop kneader (PBV-0.1 manufactured by Irie Shokai Co., Ltd.), and the mixture was uniformly mixed and dissolved while heating at 170°C for 1 hour, thereby obtaining modified polyolefin composition Y.

[0066] <Evaluation Method> Evaluations in the examples and comparative examples were carried out by the following measurement methods.

[0067] 1) Evaluation of Coatability The coatability of the modified polyolefin composition X was evaluated based on its melt viscosity at 140°C. If the melt viscosity at 140°C is 35,000 mPa·s or less, it is evaluated as having no problems in practical use. ◯: The melt viscosity at 140°C is 35,000 mPa·s or less. ×: The melt viscosity at 140°C is greater than 35,000 mPa·s. The melt viscosity was measured using a Brookfield-type viscometer (DVNXRVTJG, manufactured by Brookfield) as follows. 11 g of sample was placed in a measurement chamber, heated to 200°C to melt, and then cooled to 140°C. The melt viscosity was measured in accordance with the melt viscosity test method for hot melt adhesives of JIS K6862. The spindle No. 27 used in the measurement was set to a rotation speed of 5 rpm.

[0068] 2) Measurement of Gel Fraction Using a 500 μm thick spacer, the modified polyolefin composition X was pressurized and formed into a film under conditions of 10 MPa and 30 seconds in an environment of 140°C, to obtain a film sample. The obtained film sample was cut out to a mass of 0.25 g. The cut sample was placed in an Erlenmeyer flask (50 mL), xylene (25 mL) was added, the flask was covered, and the mixture was left for 1 hour under conditions of 100°C or 120°C. Thereafter, the mixture was filtered through a 200-mesh wire mesh and dried together with the wire mesh under vacuum at 70°C. The mass of the dried sample was measured, and the gel fraction was calculated according to the following formula: Gel fraction (%) = (mass of dried sample (g) / 0.25 g) × 100

[0069] 3) Measurement of Heat Creep Resistance Modified polyolefin composition Y was pressurized using a 200 μm thick spacer at 10 MPa for 30 seconds in a 140°C environment to form a film sample. The resulting film sample was cut into a width of 25 mm and a length of 25 mm. The cut sample was placed between the following adherends 1 and 2 together with a 100 μm spacer, and pressurized at 0.1 MPa for 30 seconds in a 160°C environment to prepare an adhesive sample (Figure 1). The film sample and adhesive sample were prepared using an "SA-302 Tabletop Test Press" manufactured by Tester Sangyo Co., Ltd., using a PP plate (thickness: 2 mm) as adherend 1 and cotton canvas No. 9 as adherend 2.

[0070] The prepared adhesive sample was cured in 60°C hot water for 7 days and then aged in a 23°C, 50% RH environment for 1 day to obtain a measurement sample. A weight was placed on the edge of the adhesive surface of the obtained measurement sample so that a 100g load was applied vertically (Figure 2). After 24 hours in a temperature environment of 90°C, 100°C, 110°C, 120°C, or 130°C, a peel length of less than 10 mm was evaluated as "Good" and a peel length of 10 mm or more was evaluated as "Poor." Note that if the evaluation was "Good" at 110°C or higher, it was determined that the heat creep resistance was sufficiently high for practical use.

[0071] 4) Measurement of Breaking Elongation Using a 500 μm thick spacer, modified polyolefin composition X or modified polyolefin Y was pressurized and formed into a film under conditions of 10 MPa for 30 seconds in a 140°C environment, to obtain a film sample. The obtained film sample was cut into a width of 10 mm and a length of 50 mm. Of the cut samples, those derived from modified polyolefin composition X were used as is, while those derived from modified polyolefin Y were cured in 60°C hot water for 7 days and then aged in a 23°C, 50% RH environment for 1 day. Then, a tensile strength test was carried out under the following conditions using an RTA-100 "TENSILON universal material testing machine" manufactured by ORIENTEC Co., Ltd. Temperature: 0±2°C (in a constant temperature and humidity chamber) Distance between chucks: 20 mm Tensile speed: 300 mm / min

[0072] The compositions and properties of the modified polyolefin compositions are shown in Tables 1 to 3. The results in Tables 2 and 3 confirm that the curable resin compositions of the present invention have excellent coatability in a molten state and excellent heat creep resistance after the curing reaction. In contrast, when modified polyolefin B was not included (Comparative Example 1), it was confirmed that the heat creep resistance was poor. When modified polyolefin B did not have a nanocrystalline structure (Comparative Example 3 using polyolefin b-2), it was confirmed that the elongation at break at 0°C and the heat creep resistance were poor. When the melt viscosity at 140°C exceeded 35,000 cps (Comparative Examples 2, 4, and 5), it was confirmed that problems with coatability occurred.

[0073] The curable resin composition of the present invention has excellent coatability and heat creep resistance after the curing reaction, and can be suitably used as a hot melt adhesive.

[0074]

[0075]

[0076] The curable resin composition of the present invention has excellent coatability in a molten state, allowing for easy application and lamination to an adherend, and also cures rapidly after cooling and solidifying, thereby exhibiting excellent heat creep resistance. The curable resin composition of the present invention can be used for a variety of purposes, such as adhesives, sealants, waterproofing materials, paints and coating materials, lining materials, sealing materials, pressure-sensitive adhesives, adhesive tapes, pressure-sensitive adhesive sheets, pressure-sensitive adhesives, and adhesive-processed products.

[0077] 1. Adherend 1 2. Adhesive layer 3. Adherend 2 4. Weight

Claims

1. A curable resin composition comprising modified polyolefin A and modified polyolefin B, wherein the modified polyolefin A has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin a, the modified polyolefin B has a chemical structure obtained by grafting a moisture-curable functional group onto polyolefin b, the polyolefin b having a nanocrystalline structure, and the melt viscosity of the curable resin composition at 140°C is 35,000 cps or less.

2. The curable resin composition according to claim 1, wherein the polyolefin b is an ethylene-butylene-propylene copolymer.

3. The curable resin composition according to claim 1, wherein the melting point of said polyolefin b is 100 to 190°C.

4. The curable resin composition according to claim 1, wherein the polyolefin b has a glass transition temperature of -20 to 20°C.

5. The curable resin composition according to claim 1, wherein the modified polyolefin B is contained in an amount of 5 to 15 parts by mass per 100 parts by mass of the modified polyolefin A.

6. The curable resin composition according to claim 1, wherein the polyolefin a is polypropylene.

7. The curable resin composition according to claim 1, wherein the melting point of said polyolefin a is 100 to 190°C.

8. The curable resin composition according to claim 1, wherein the polyolefin a has a glass transition temperature of -20 to 5°C.

9. The curable resin composition according to claim 1, wherein the melt viscosity of said polyolefin a at 140°C is 20,000 cps or less.

10. The curable resin composition according to claim 1, further comprising 0.5 to 15 parts by mass of a moisture curing accelerator C relative to a total of 100 parts by mass of the modified polyolefin A and the modified polyolefin B.

11. The curable resin composition according to claim 10, wherein the moisture curing accelerator C has an acid functional group and satisfies at least one of a melting point of 70 to 100°C and a softening point of 100 to 140°C.

12. The curable resin composition according to claim 10, wherein the moisture curing accelerator C is an acid-modified polyolefin.

13. The curable resin composition according to claim 12, wherein the acid functional group contained in the acid-modified polyolefin is maleic anhydride.

14. The curable resin composition according to claim 10, wherein the moisture curing accelerator C is a rosin compound having an acid functional group.

15. The curable resin composition according to claim 1, further comprising 0.0001 to 10.0 parts by mass of a moisture curing catalyst D per 100 parts by mass of the combined total of the modified polyolefin A and the modified polyolefin B, the moisture curing catalyst D being an organometallic compound.

16. The curable resin composition according to claim 1, in which when a combined total of 100 parts by mass of modified polyolefin A and modified polyolefin B is immersed in xylene at 100°C for 1 hour, 25 to 40 parts by mass remain undissolved, and when immersed in xylene at 120°C for 1 hour, 0.1 to 5 parts by mass remain undissolved.

17. A hot melt adhesive comprising the curable resin composition according to any one of claims 1 to 16.

Citation Information

Patent Citations

  • Modified propylene polymer, composition thereof, and laminate containing the same

    JP2010106069A

  • Method for producing a functionalized thermoplastic elastomer

    JP2016512855A

  • Silane-modified polyolefin, silane-modified polyolefin composition, silane crosslinked polyolefin, and molding including the same, crosslinked molding, and 3D network fiber aggregate

    JP2023128798A

  • Silane-modified polypropylene, silane-modified polypropylene composition, silane crosslinked polypropylene, and molding including the same, crosslinked molding, 3D network fiber aggregate, and crosslinked molding of 3D network fiber aggregate

    JP2023128806A

  • Hot-melt adhesive composition, method for using hot-melt adhesive composition, automobile interior material, precoated surface material for automobile interior, and method for producing automobile interior material

    WO2018100672A1