Silicone tape composition for sensing hydrogen gas having excellent tensile strength and elongation, hydrogen gas sensing silicone tape, and method for manufacturing same

The silicone tape composition with VTP, hTPS, and PdO supported by zeolite and other carriers addresses the lack of field applicability and visibility in hydrogen gas sensing, offering enhanced tensile strength and color change detection for hydrogen gas, suitable for hydrogen fuel cell energy sources and industrial fields.

WO2024248181A1PCT designated stage expired Publication Date: 2024-12-05UNID BTPLUS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/007449
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing hydrogen gas sensing technologies lack field applicability, tensile strength, and color change visibility for immediate detection of abnormal conditions, particularly in hydrogen fuel cell energy sources and industrial fields.

Method used

A silicone tape composition comprising a hydrogen gas detection agent, Vinyl Terminated Polydimethylsiloxane (VTP), Hydride Terminated Polydimethylsiloxane (hTPS), silicone gum, and additives like alumina for improved tensile strength and visibility, with PdO as the hydrogen gas sensing agent supported by carriers like zeolite and TiO2, SiO2, ZnO, and Al2O3, and a platinum catalyst for enhanced functionality.

Benefits of technology

The silicone tape exhibits excellent tensile strength, elongation, and color change visibility, enabling stable and immediate detection of hydrogen gas, suitable for various industrial applications, including hydrogen fuel cell energy sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023007449_05122024_PF_FP_ABST
    Figure KR2023007449_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a silicone tape composition for sensing hydrogen gas, a hydrogen gas sensing silicone tape, and a method for manufacturing same, wherein the silicone tape composition may be simply manufactured in an adhesive or sticky tape form and thus has excellent field applicability, and has excellent tensile strength and color change visibility. The silicone tape composition for sensing hydrogen gas, according to the present invention, comprises a hydrogen-gas-sensing agent, PDMS, and a platinum catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

A silicone tape composition for detecting hydrogen gas with excellent tensile strength and elongation, the silicone tape for detecting hydrogen gas, and a method for producing the same

[0001] The present invention relates to a silicone tape composition for detecting hydrogen gas, a silicone tape for detecting hydrogen gas, and a method for producing the same.

[0002] More specifically, the present invention relates to a silicone tape composition for detecting hydrogen gas, which can be simply manufactured in the form of an adhesive or pressure-sensitive adhesive tape, has excellent field applicability, has excellent tensile strength and color change visibility, and has excellent tensile strength and elongation, the hydrogen gas detecting silicone tape, and a method for manufacturing the same.

[0003] Regarding a hydrogen sensor that detects hydrogen gas used in hydrogen fuel cell energy sources, hydrogen cars, and various industrial fields, there is patent registration number 10-1015088 (February 9, 2011) [Reduced PDMO thin film used in ultra-high sensitivity hydrogen sensor and method for manufacturing the same].

[0004] This registered patent includes a step of artificially producing a PdO thin film using a reactive sputtering technique (reactive DC magnetron sputtering system), and a step of obtaining a Pd thin film with nanocracks formed by subjecting the PdO thin film to a reduction reaction.

[0005] The Pd thin film formed with the above nanocracks has improved hydrogen detection characteristics, suggesting a technology suitable for use in a hydrogen detection sensor.

[0006] There is also a patent registration number 10-1269510 (May 24, 2013) [Hydrogen detection sensor capable of measuring hydrogen concentration].

[0007] This registered patent relates to a hydrogen detection sensor that can continuously measure changes in the concentration of hydrogen gas by changing the resistance value corresponding to changes in the concentration of hydrogen gas.

[0008] Specifically, it includes a hydrogen detection unit that is hydrogenated when in contact with hydrogen gas, and when the hydrogen detection unit is hydrogenated, the resistance value of the hydrogen detection unit changes, has a first resistance value change rate at a first concentration of hydrogen gas, and has a second resistance value change rate that is different from the first resistance value change rate at a second concentration of hydrogen gas that is different from the first concentration.

[0009] However, these two patents and other prior literature are unrelated to the field applicability aspect or the technology that improves the visibility of color changes to enable immediate detection of abnormal conditions.

[0010] Accordingly, the present invention aims to provide a silicone tape composition for detecting hydrogen gas, which can be simply manufactured in the form of an adhesive or sticky tape, has excellent field applicability, has excellent tensile strength and color change visibility, and has excellent tensile strength and elongation, and a hydrogen gas detecting silicone tape, and a manufacturing method thereof.

[0011] In order to achieve the above purpose, the silicone tape composition for detecting hydrogen gas according to the present invention

[0012] It is composed of a hydrogen gas detector, VTP (Vinyl Terminated Polydimethylsiloxane), hTPS (Hydride Terminated Polydimethylsiloxane), and silicone gum.

[0013] In addition, the silicone tape composition for detecting hydrogen gas according to the present invention

[0014] Further comprising some or all of a visibility enhancer, an adhesion enhancer, a curing retardant, an adhesion enhancer, and a tensile strength enhancer,

[0015] The above discoloration visibility enhancer is alumina,

[0016] The above curing retardant is methylvinylcyclosiloxane (MVC),

[0017] The above hydrogen gas detector uses PdO, and the carrier is some or all of zeolite, TiO2, SiO2, ZnO, and Al2O3.

[0018] It is preferable to include 300 to 500 parts by weight of VTP, 120 to 150 parts by weight of hTPS, and 7,000 to 12,000 parts by weight of silicone gum for 100 parts by weight of hydrogen gas detector.

[0019] Furthermore, the hydrogen gas sensing silicone tape and the manufacturing method thereof according to the present invention are made using the above composition.

[0020] The present invention provides a silicone tape composition for detecting hydrogen gas, which is in the form of a tape with excellent field applicability, has excellent tensile strength and color change visibility, and has excellent tensile strength and elongation, a silicone tape for detecting hydrogen gas, and a method for manufacturing the same.

[0021] Figure 1 is a comparative photograph of a hydrogen gas sensing silicone tape according to the present invention before and after exposure to hydrogen gas.

[0022] Figure 2 is a manufacturing process diagram of a hydrogen gas detector.

[0023] Hereinafter, the present invention will be described in detail.

[0024] The present invention is susceptible to various modifications and takes various forms, and thus, implementation examples (or examples) are described in detail herein. However, this is not intended to limit the present invention to a specific disclosed form, and it should be understood that all modifications, equivalents, and alternatives fall within the spirit and technical scope of the present invention.

[0025] The terminology used in this specification is only used to describe specific implementations (or examples) and is not intended to limit the present invention. The singular expression includes plural expressions unless the context clearly indicates otherwise. In this application, it should be understood that the terms such as ~comprises~ or ~consists of~ indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0026] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and will not be interpreted in an idealized or overly formal sense unless explicitly defined herein.

[0027] The hydrogen gas detection silicone tape composition according to the present invention, the hydrogen gas detection silicone tape, and the manufacturing method thereof are as follows:

[0028] It is composed of a hydrogen gas detector, VTP (Vinyl Terminated Polydimethylsiloxane), hTPS (Hydride Terminated Polydimethylsiloxane), and silicone gum.

[0029] Specifically, it is preferable to include 300 to 500 parts by weight of VTP, 120 to 150 parts by weight of hTPS, and 7,000 to 12,000 parts by weight of silicone gum for 100 parts by weight of hydrogen gas detector.

[0030] It is also desirable to add a discoloration visibility enhancer to the tape and a catalyst, especially a platinum catalyst.

[0031] It is preferred that this discoloration visibility enhancer be alumina, in which case the alumina also helps to improve the tensile strength of the tape.

[0032] In addition, the present invention preferably further includes a curing retarder, and the curing retarder may be methylvinylcyclosiloxane (MVC).

[0033] Basically, it is desirable to use PdO (Palladium Oxide) as a hydrogen gas detector.

[0034] In addition, it is preferable that the hydrogen gas detector be contained in a carrier considering ease of operation, material stability, and preservation, and examples of the carrier include porous materials such as zeolite, TiO2, SiO2, ZnO, and Al2O3 (one, some, or all of these may be used), among which zeolite is suitable.

[0035] That is, PdCl2 is mixed and supported on zeolite, which is a carrier.

[0036] [Correction under Rule 91 13.06.2023] Furthermore, the principle of hydrogen gas detection is as follows, and the discoloration before and after hydrogen gas detection using the tape according to the present invention can be confirmed in the comparative photo of Fig. 1.

[0037] PdO (Brown) + H2 → Pd (Gray) + H2O

[0038] [Correction pursuant to Rule 91, June 13, 2023][Deleted]

[0039] [Correction pursuant to Rule 91, June 13, 2023][Deleted]

[0040] [Description of the composition's ingredients]

[0041] The hydrogen gas detection silicone tape according to the present invention preferably employs a silicone tape so that it can be stably applied to various fields, and the silicone tape uses silicone to which a vinyl group and a hydrogen (H) group have been added to improve functionality (a silicone to which a hydroxyl (OH) group has been added (Hydroxyl-Terminated Polydimethylsiloxane (HTPS)) is added only in comparative examples). In addition, it is preferable that the curing reaction of the silicone be an addition reaction type and use a platinum (Pt) catalyst.

[0042] ○ Vinyl terminated polydimethylsiloxane (hereinafter referred to as 'PDMS')

[0043] It serves as the backbone of silicon.

[0044] ○ PDMS with terminal hydrogen groups (Hydride terminated PDMS)

[0045] It acts as a cross-linker.

[0046] ○ PDMS with terminal hydroxyl groups (Hydroxyl terminated PDMS) (used only in comparative examples as follows)

[0047] It provides adhesive properties unique to hydroxyl groups (adhesion to the adherend can be secured by providing -OH, which does not participate in additional curing).

[0048] ○ Pt catalyst

[0049] Induces a curing reaction of silicone.

[0050] <Silicone 반응 예>

[0051] Hydride terminated PDMS + Vinyl terminated PDMS (using Pt catalyst)

[0052]

[0053] {Source: Gelest catalog}

[0054] In addition, the fillers for hydrogen gas detection are as follows.

[0055] ○ PdO / Carrier

[0056] PdO exhibits discoloration properties when reacted with hydrogen gas, and zeolite, TiO2, SiO2, ZnO, and Al2O3 act as carriers for PdO, with zeolite being suitable.

[0057] ○ Alumina (Al22O3)

[0058] It maximizes the visibility of color change (color contrast effect) of PdO (i.e., it functions as a color change visibility enhancer) and also helps increase the tensile strength of the tape.

[0059] ○ Curing inhibitor

[0060] Inhibitor MVC (methylvinylcyclosiloxane), a curing retardant, is used.

[0061] The present invention can be better understood through specific manufacturing examples, examples, and comparative examples (see [Table 1] and [Table 2]).

[0062] [Manufacturing Example: Manufacturing of the entire composition and tape for manufacturing a hydrogen gas detection silicone tape]

[0063] ● Manufacturing of hydrogen gas detector

[0064] As can be seen in the process diagram of Fig. 2,

[0065] 1. Mix and support the PdO precursor and water (H2O) with the substrate (zeolite, TiO2, or ZnO). The PdO precursor (PdCl2) is added at 2 to 4 phr relative to the carrier.

[0066] 2. Stir for 10 minutes, the reaction temperature is room temperature (RT) to 60 ℃, 3. pH Control; Adjust the pH of the solution to 7 using dilute hydrochloric acid.

[0067] 3. Stir for 60 minutes, and the reaction temperature is room temperature to 60 ℃.

[0068] 4. Pressure filter using a filter (0.2 ㎛ Membrane filter with washing).

[0069] 5. Dry for 12 hours (drying temperature: 120 ℃) ​​to obtain PdO / carrier powder.

[0070] ● Manufacturing of hydrogen gas detection silicone tape

[0071] ○Raw material mixing ratio

[0072] The components of each example and comparative example below are mixed based on 100 parts by weight of PdO / Zeolite, a hydrogen gas detector.

[0073] Meanwhile, in this embodiment, PDMS (VTP) having a terminal vinyl group can be used by mixing those having different viscosities to help secure dispersion characteristics for the PdO / carrier, which is a hydrogen gas detector. For example, it is suitable to mix and use 90 to 120 parts by weight of VTP having a viscosity of 20,000 cps and 40 to 60 parts by weight of VTP having a viscosity of 65,000 cps for 100 parts by weight of VTP having a viscosity of 1,000 cps.

[0074] ○ Three Roll Milling

[0075] It is a process of crushing / dispersing particles (fillers) present in the above mixed composition,

[0076] In particular, a dispersion liquid is manufactured by crushing / dispersing hydrogen gas detector particles in silicon (RV100), and milling is performed with a gap of 20 ㎛ for the roll into which the raw material is fed and a gap of 5 ㎛ for the roll from which the raw material is discharged.

[0077] ○ Planetary Mixing

[0078] The above dispersion and the remaining composition are mixed using a planetary mixer.

[0079] ○ Observation of film formation and hydrogen gas discoloration

[0080] Coat the PET substrate with a moisture film thickness of 300 ㎛, dry at 70 to 150°C for 7 to 30 minutes, and then cure at 100 to 150°C for 10 to 13 minutes to form a film.

[0081] Meanwhile, as in Examples 8 and 11, the adhesive layer is prepared by additionally coating a pressure-sensitive adhesive (PSA) on the surface of the cured silicone tape. This PSA is coated to a dry film thickness of 30 to 60 ㎛, dried at 70 to 150°C for 5 minutes, and then cured at 100 to 150°C for 10 minutes.

[0082] The cured film is exposed to hydrogen gas to observe discoloration. The hydrogen gas exposure condition is 4% H2 gas to observe discoloration.

[0083] [Examples and Comparative Examples]

[0084] Classification (Unit: parts by weight) Example ① Example ② Example ③ Example ④ Example ⑤ Example ⑥ Example ⑦ Example ⑧ VTP 18.04 18.04 20.48 21.95 29.25 29.25 27.72 20.49 Silicone GUM 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 hTPS- Crosslinker 6.80 6.80 7.73 6.49 9.72 9.72 10.46 7.72 HTPS- 50 cps 0.000.000.000.000.000.000.000.000.00 Catalyst- Pt Catalyst 0.600.600.930.770.580.290.940.47Filler - Al2O3 15.009.9017.0417.0417.0417.0523.0717.05Inhibitor 0.200.150.170.140.220.270.230.17Hydrogen gas detector 15.5025.775.854.887.327.307.915.85MS- adhesion promoter 5.025.165.859.767.327.307.915.85Hydrogen gas detector Zeolite carrier Zeolite Zeolite Zeolite Zeolite Zeolite Zeolite Adhesive layer - PressureSensitiveAdhesive Grant Grant ×××× Grant ×

[0085] Classification (Unit: parts by weight) Example ⑨ Example ⑩ Example ⑪ Comparative Example ① Comparative Example ② Comparative Example ③ Comparative Example ④ Comparative Example ⑤ VTP 20.50 27.72 27.72 40.56 40.54 40.50 40.51 45.62 Silicone GUM 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 100.00 hTPS- Crosslinker 7.73 10.46 10.46 12.17 6.08 4.04 3.87 3.87 HTPS- 50 cps 0.000.000.00 14.00 13.94 13.97 13.98 14.51 Catalyst- Pt Catalyst 0.24 0.94 0.94 0.60 0.21 1.21 0.15 0.15 Filler - Al2O3 17.04 23.07 23.07 17.12 16.5 116.28 16.26 16.85 Inhibitor 0.17 0.23 0.23 0.16 0.15 0.15 0.17 0.17 Hydrogen gas detector 5.8 5 7.9 17.9 15.06 5.06 5.07 5.22 5.41 MS- adhesion promoter 5.8 5 7.9 17.9 15.06 5.06 5.07 5.06 5.08 Hydrogen gas detector Zeolite carrier TiO2ZnOzeolitezeolitezeolitezeolitezeoliteAdhesive layer-PressureSensitiveAdhesive×Given××××××

[0086] *VTP=Vinyl Terminated Polydimethylsiloxane

[0087] *hTPS=Hydride Terminated Polydimethylsiloxane

[0088] *HTPS = Hydroxyl Terminated Polydimethylsiloxane

[0089] *MS = Methacylate Silane

[0090] [Experimental Example - Measurement of Tensile Strength and Elongation]

[0091] Classification Tensile strength (N / ㎟) Elongation (%) Adhesion Example 13.51310200 Example 23.80301200 Example 34.8729710 Example 43.8240620 Example 54.6731020 Example 63.9732015 Example 74.56353150 Example 84.3134520 Example 93.5943930 Example 104.35350125 Example 114.2634715 Comparative Example 12.8026520 Comparative Example 21.4633420 Comparative Example 30.9869025 Comparative Example 41.3179615 Comparative Example 51.2872820

[0092] As can be confirmed from the above experimental example [Table 3], the present invention provides a silicone tape composition for hydrogen gas detection, which has excellent tensile strength and elongation compared to the comparative example, the hydrogen gas detection silicone tape, and a manufacturing method thereof. As in the comparative example, when adding silicone (Hydroxyl Terminated Polydimethylsiloxane (HTPS)) to which a hydroxyl (OH) group is assigned, it was confirmed that the tensile strength and elongation were adversely affected compared to the intention of imparting adhesive properties unique to hydroxyl groups.

[0093] Specifically, in the hydrogen gas detection silicone tape composition having excellent tensile strength and elongation according to the present invention, the hydrogen gas detection silicone tape, and the manufacturing method thereof, it is preferable to include 5.00 to 30.0 parts by weight of a hydrogen gas detection agent, 15.00 to 30.00 parts by weight of VTP, and 6.00 to 12.00 parts by weight of hTPS, per 100.00 parts by weight of silicone gum.

[0094] In addition, it is preferable to include 0.20 to 1.00 parts by weight of a catalyst (e.g., Pt catalyst), 15.00 to 25.00 parts by weight of a filler (e.g., alumina (Al2O3)), 0.10 to 0.30 parts by weight of a curing inhibitor (e.g., MVC (methylvinylcyclosiloxane), and 4.00 to 10.00 parts by weight of an adhesion promoter (e.g., MS = Methacylate Silane).

[0095] The adhesive layer can be optionally applied as needed.

[0096] More specifically and comprehensively, as can be confirmed in the experimental example table above, with respect to tensile strength and elongation performance, it is more preferable that VTP is 20.00 to 30.00 parts by weight (see Examples ③ to ⑧, ⑩, ⑪) for 100.00 parts by weight of silicone gum, and it is most preferable that VTP is 25.00 to 30.00 parts by weight (see Examples ⑩, ⑪).

[0097] In addition, it is more preferable that the hydrogen gas detector be 4.80 to 8.00 parts by weight, hTPS be 7.70 to 11.00 parts by weight, the catalyst be 0.45 to 1.00 parts by weight, the filler be 17.00 to 25.00 parts by weight, and the curing retardant be 0.10 to 0.23 parts by weight. (See Examples ③ to ⑧, ⑩, and ⑪ above.)

[0098] In the above description, conventionally known techniques related to the silicon tape composition for detecting hydrogen gas, the silicon tape for detecting hydrogen gas, and the manufacturing method thereof are omitted, but those skilled in the art can easily guess, infer, and reproduce them.

Claims

1. A silicone tape composition for detecting hydrogen gas, comprising a hydrogen gas detector, VTP (Vinyl Terminated Polydimethylsiloxane), hTPS (Hydride Terminated Polydimethylsiloxane), and silicone gum.

2. In paragraph 1, A silicone tape composition for detecting hydrogen gas, characterized in that it further comprises a visibility enhancing agent.

3. In paragraph 2, A silicone tape composition for detecting hydrogen gas, characterized in that the above discoloration visibility improving agent is alumina.

4. In paragraph 1, A silicone tape composition for detecting hydrogen gas, characterized in that it further comprises an adhesive improver.

5. In paragraph 1, A silicone tape composition for detecting hydrogen gas, characterized in that a curing retarder is further added.

6. In paragraph 5, A silicone tape composition for detecting hydrogen gas, characterized in that the curing retardant is methylvinylcyclosiloxane (MVC).

7. In any one of paragraphs 1 to 6, A silicone tape composition for detecting hydrogen gas, characterized in that an adhesion promoter is further added.

8. In any one of paragraphs 1 to 6, A silicone tape composition for detecting hydrogen gas, characterized in that a tensile strength enhancer is further added.

9. In any one of paragraphs 1 to 6, A silicone tape composition for detecting hydrogen gas, characterized in that the hydrogen gas detector uses PdO and the carrier is some or all of zeolite, TiO2, SiO2, ZnO, and Al2O3.

10. In any one of paragraphs 1 to 6, A silicone tape composition for detecting hydrogen gas, comprising 5.00 to 30.0 parts by weight of a hydrogen gas detector, 15.00 to 30.00 parts by weight of VTP, and 6.00 to 12.00 parts by weight of hTPS, per 100.00 parts by weight of silicone rubber.

11. Silicon for detecting hydrogen gas, manufactured using a composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Hydrogen-sensitive discoloration detection adhesive tape, and preparation method and application thereof

    CN111662650A

  • Adhesive film

    JP2019052255A

  • Apparatus and method for treating substrate

    KR1020210035571A

  • Memory module and electronic system including the same

    KR1020240167258A

  • Plasma generating device

    KR102255874B1