Structure of activated biochar sphere
By encapsulating wood biochar fragments in calcium alginate hydrogel spheres and combining them with thermosetting polymers and metal salt additives, porous activated biochar spheres are formed, solving the problem of the lack of pores in the biochar sphere structure. This enables efficient adsorption of gold ions and repeated use in a wide range of acidic and alkaline environments.
Patent Information
- Application Number
- PCT/CN2025/093411
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
In existing technologies for separating gold ions from solutions using biochar, the biochar spheres lack an effective pore structure, resulting in low adsorption efficiency and difficulty in repeated use in acidic or alkaline environments.
By encapsulating wood biochar fragments in calcium alginate hydrogel spheres and adding thermosetting polymers and metal salt additives, porous activated biochar spheres are formed. The thermosetting polymers and metal salt additives form a cross-linked structure, and combined with a physical activation process, a turbine layer carbon structure and multi-layered non-uniform channels are generated.
It achieves efficient adsorption of gold ions in the pH range of 2 to 12, with an adsorption rate of over 60%, and the biochar balls have a stable structure and can be reused.
Smart Images

Figure CN2025093411_12112026_PF_FP_ABST
Abstract
Description
Structure of activated biochar balls Technical Field
[0001] This invention relates to an activated biochar ball, and more particularly to a recyclable and reusable activated biochar ball. Background Technology
[0002] To separate gold ions from solution using biochar, and to ensure the biochar can be recycled and reused, current techniques, such as those described in CN 116832774, involve freeze-drying calcium alginate hydrogel spheres, followed by carbonization and acid washing, with a preferred carbonization temperature of 600–700℃. The resulting biomass-derived char particles exhibit a large number of oxygen-containing groups such as quinone and phenolic hydroxyl groups, and operate within a pH range of 1–8. Electron microscopy images at the micrometer scale, as shown in Figures 1 and 2, reveal a smooth and flat surface without obvious pore structures.
[0003] For example, CN 113426385 first utilizes phenolic compounds, aldehyde compounds, chitosan, and sodium alginate to form a homogeneous sol solution, which is then added dropwise to a saturated boric acid solution containing calcium chloride to form gel microspheres. Subsequent aging yields hydrogel microspheres with a double cross-linked structure of calcium alginate and phenolic resin. The hydrogel microspheres are dried at room temperature and pressure and then carbonized, preferably at a carbonization temperature of 850–950℃. The resulting activated biochar microspheres possess a large number of polar groups such as —OH, —NH2, and COOH (COO-). The residual polar groups and heteroatoms can improve the adsorption performance of the carbon aerogel microspheres. At the micrometer scale, electron microscopy images (refer to Figure 3) show that the etched pores have a generally smooth interface. Summary of the Invention
[0004] Activated biochar balls can adsorb gold ions in solution, are recyclable and reusable, and the solution pH should be at least 2–8, or even within the pH 2–12 range. That is, within this pH range, the adsorption rate of standard gold ions using these balls should be at least 60%.
[0005] In one embodiment, a porous spherical structure of activated biochar spheres comprises, at the micrometer scale:
[0006] Multiple carbon particles form a spherical, multi-sized, irregularly stacked structure, wherein each carbon particle includes a corresponding layered edge structure and a corresponding surface layer structure, and the multi-sized fragment particle stacking structure includes:
[0007] A carbon framework is formed by the stacking and connection of carbon particles, wherein the stacking of these carbon particles further forms multiple interparticle voids;
[0008] A porous structure is formed by the interconnection of interparticle voids, wherein the porous structure includes an interface structure formed by multiple layered edge structures through multi-level non-uniform stacking, wherein the layered edge structures are irregular in shape; multiple small particles are discretely distributed and can form small-scale agglomerations on these surface layered structures.
[0009] In one embodiment, a porous spherical structure of activated biochar spheres includes:
[0010] Multiple micrometer-sized carbon particles are irregularly stacked to form millimeter-sized spherical structures;
[0011] These carbon particles each include a corresponding layered edge structure and a corresponding surface hierarchical structure.
[0012] These carbon particles are linked together to form a carbon skeleton;
[0013] The carbon particles include a turbine layer carbon structure, wherein the turbine layer carbon structure includes multiple interlayer spaces and multiple exchangeable metal ions embedded in the interlayer spaces. Attached Figure Description
[0014] Figures 1-2 show electron microscope images of biomass-derived char particles at the micrometer scale, as disclosed in CN 116832774.
[0015] Figure 3 shows an electron microscope image of the activated biochar balls disclosed in CN 113426385 at the micrometer scale.
[0016] Figure 4 is a schematic diagram of the layered edge structure.
[0017] Figure 5 is a schematic diagram of the surface hierarchical structure.
[0018] Figure 6 shows electron microscope images of Leucaena leucantha biochar at the micrometer scale.
[0019] Figure 7 shows the spherical appearance of activated biochar balls according to one embodiment of the present invention.
[0020] Figure 8 shows an electron microscope image of the internal structure of the activated biochar spheres according to one embodiment of the present invention.
[0021] Figure 9 shows the spherical appearance of the activated biochar balls according to another embodiment of the present invention.
[0022] Figure 10 shows an electron microscope image of the internal structure of activated biochar balls according to another embodiment of the present invention.
[0023] Figure 11 shows electron microscope images of the biochar fragments added in the embodiment of the present invention at the micrometer scale. Detailed Implementation
[0024] In one embodiment, lignocellulosic biochar fragments, a thermosetting polymer, and a metal salt additive are encapsulated in calcium alginate hydrogel spheres. The lignocellulosic biochar fragments are dispersed in the cross-linked chains of the hydrogel spheres, while the thermosetting polymer and metal salt additive are uniformly dispersed in water within the hydrogel spheres. The hydrogel spheres are then heated. Initially, the thermosetting polymer in the water dissolves and forms a high-molecular-weight cross-linked structure together with the metal salt additive particles, such as clay mineral particles. Upon continued heating, the hydrogel spheres dehydrate to form sodium alginate-based gel spheres. Subsequently, carbonization and physical activation are performed under nitrogen atmosphere to generate porous activated biochar spheres for easy recycling. In one embodiment, the hydrogel spheres are approximately 3 mm in size, and the activated biochar spheres are approximately 1 mm in size. The metal salt additive particles may be particles of clay minerals or their processed derivatives.
[0025] In one embodiment, wood biochar fragments can serve as the primary carbon source for activated biochar balls. Combined with the cross-linked chains of the sodium alginate-based cross-linked structure, they can strengthen the cross-linked structure of the calcium alginate gel balls. The cross-linked chains integrate the cyclic structure of biochar, such as aromatic rings, which can improve the thermal stability of the cross-linked structure. Thermosetting polymers can act as adhesives, connecting and fixing multiple adjacent cross-linked chains within the gel balls, strengthening the spherical structure of the gel balls, preventing disintegration during high-temperature processing, and can also serve as a secondary carbon source for the activated biochar balls. Metal salt additive particles can act as bridging agents, forming a cross-linked structure together with the thermosetting polymer, thus improving thermal stability. Calcium alginate serves as a carrier for the wood biochar fragments and can also be a secondary carbon source for the activated biochar balls.
[0026] In one embodiment, the gel spheres are carbonized to form biochar spheres, which further strengthens the sphere structure and makes them less susceptible to damage from corrosion or impact. During carbonization, an activation gas, such as carbon dioxide or water vapor, can be injected into a nitrogen environment to simultaneously activate the spheres.
[0027] In one embodiment, in addition to metal salt additives, during the carbonization process of biochar, the organic matter of the biochar releases metal salts, such as alkali metal carbonates, as part of the thermal decomposition reaction. At a carbonization temperature of 600–650°C, the organic matter of the biochar can release all the metal salts, and the biochar can form an initial turbine layer carbon structure. At the physical activation temperature (700–1000°C), the metal salts dissociate into metal ions, which can flow with the molten metal salts. The biochar fragments themselves already contain metal salts. Thermosetting polymers and calcium alginate also produce metal salts during carbonization.
[0028] In one embodiment, after physical activation, the activated biochar spheres develop a layered, turbine-like carbon structure with a wider front and narrower back interlayer space. Metal ions, embedded in these interlayer spaces along with the flow of molten metal salts, can be used for ion exchange. Under high-pressure nitrogen, metal ions can penetrate deeper into the interlayer space, thereby creating a larger interlayer space and more exchangeable metal ions. The physical activation step not only improves the original properties of biochar, such as specific surface area and pore structure, but also provides additional exchangeable metal ions. However, physical activation can further worsen the thermal weight loss of the biochar, weakening the spherical structure of the gel spheres. The formation of a cross-linked structure of thermosetting polymer-metal salt additive particles within the gel spheres helps maintain their spherical structure during physical activation, preventing them from disintegrating into fragments. In one embodiment, the activated biochar spheres contain more than 70% carbon.
[0029] In one embodiment, calcium alginate hydrogel spheres solidify to form a stable cross-linked structure incorporating biochar fragments. The solidified hydrogel spheres contain thermosetting polymer particles, clay mineral particles, and calcium carbonate particles distributed within the water content of the hydrogel spheres. The solidified hydrogel spheres can be dehydrated and dried using atmospheric pressure heating. Initially, during heating, the thermosetting polymer melts and combines with the clay mineral particles to form a second cross-linked structure (polymer-clay mineral cross-linked structure), which permeates the structural voids of the sodium alginate-based gel spheres. After dehydration, the second cross-linked structure provides internal cohesion to the calcium alginate-biochar fragment spheres, strengthening the sphere structure. In one embodiment, during the carbonization process, bio-calcium carbonate helps to form cyclic structures, such as aromatic ring structures, improving the thermal stability of the biochar.
[0030] In one embodiment, the thermosetting polymer may be a phenolic resin, starch, or a processed derivative of starch, such as wheat starch, corn starch, or paste. The metal salt additive particles may be clay minerals or their derivatives, such as aluminosilicate minerals, mica powder, modified kaolin, or calcium carbonate / biocarbonate. The addition of biocarbonate can promote the formation of cyclic structures, such as aromatic rings, in the biochar during carbonization, thereby improving thermal stability. Physical activation may be carbon dioxide activation or steam activation. Steam activation helps to generate additional oxygen-containing functional groups.
[0031] In one embodiment, the millimeter-sized porous activated biochar spheres, at the micrometer scale, have a carbon framework formed by numerous fragmented carbon particles ranging from 10 to 50 micrometers (µm) in size. These fragmented carbon particles possess a layered edge structure (refer to Figure 4) and a surface hierarchical structure (refer to Figure 5). Referring to Figure 4, the layered edge structure includes an upper surface 1, a lower surface 2, and an edge surface 3 connecting the upper surface 1 and the lower surface 2, wherein the upper surface 1 and the lower surface 2 face approximately opposite directions. Referring to Figure 5, the surface hierarchical structure includes an upper surface 4, a lower surface 5, and an edge surface 6 connecting the upper surface 4 and the lower surface 5, wherein the upper surface 4 and the lower surface 5 face approximately the same direction. A single fragmented carbon particle may have multiple layered edges. The 10-50 micrometer (µm) carbon particles aggregate and stack, forming a multi-sized, irregularly stacked structure with a spherical appearance. The fragmented carbon particles connect to form a porous spherical carbon framework, creating voids between the fragmented carbon particles, which connect to form a porous structure.
[0032] In one embodiment, at the micrometer scale, the interface structure between the pore structure and the carbon skeleton of the porous sphere includes multiple irregularly shaped layered edges, forming a non-smooth interface through multi-layered, non-uniform stacking, unlike etched pore structures. The fragmented carbon particles are inconsistent in height, causing adjacent particles to not be on the same plane, resulting in irregular stacking with varying density, forming multi-layered channels that are disordered and exhibit a non-uniform interface structure. Although the carbon skeleton of the biochar sphere originates from a cross-linked structure, at the micrometer scale, the linking pattern of the fragmented carbon particles on the surface of the porous sphere does not exhibit the chain network of a cross-linked structure, nor does it exhibit the channel structure of acacia biochar (refer to Figure 6).
[0033] In one embodiment, at the micrometer scale, small particles approximately 1 micrometer in size contain inorganic salts. These inorganic salt particles aggregate in small areas on the surface of fragmented carbon particles. Overall, the inorganic salt particles are discretely attached to the surface of the carbon particles.
[0034] In the following specific embodiments, unless otherwise specified, the added biochar was obtained from *Leucaena leucocephala*, carbonized at 650°C, and pulverized before being sieved through a 100-mesh screen; the gold ion standard reagent was prepared by adding trivalent gold ions to deionized water at a concentration of 10 ppm; the adsorption rate of gold ions was measured by adding 100 mg of activated biochar balls to 50 mL of the standard reagent, adsorbing for 5 hours, and then measuring the residual amount of trivalent gold ions in the standard reagent; the hydrogel spheres had a particle size of approximately 3 mm; and the mixture was dried under normal pressure. Metal salt additives, such as clay minerals or their processed derivatives, or calcium carbonate / bio-calcium carbonate, were added to a homogeneous aqueous solution based on sodium alginate and stirred to produce uniformly dispersed metal salt additive particles.
[0035] Example 1
[0036] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of starch, 10 g of phenolic resin, 36 g of biochar, and 4 g of mica powder. The mixture was stirred until evenly dispersed in the water to form a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, the solid and liquid phases were separated, and the mixture was heated to 80°C and dried for 2 hours. During this time, the starch and phenolic resin also dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 98.4%. Referring to Figure 7, the spherical appearance of the activated biochar spheres; referring to Figure 8, an electron microscope image of the internal structure of the spheres at the micrometer scale.
[0037] Example 2
[0038] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of phenolic resin, 36 g of biochar, and 4 g of clay minerals. The mixture was stirred until evenly dispersed in the water, forming a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride, dissolving to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation was achieved, and the mixture was heated to 80°C and dried for 2 hours. During this process, the phenolic resin dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 76.8%.
[0039] Example 3
[0040] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of starch, 36 g of biochar, and 4 g of clay minerals. The mixture was stirred until evenly dispersed in the water, forming a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride, dissolving to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct dropwise addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation was achieved, and the mixture was heated to 80°C and dried for 2 hours. During this process, the starch dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 84.7%.
[0041] Example 4
[0042] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of starch, 10 g of phenolic resin, 36 g of biochar, and 4 g of clay minerals. The mixture was stirred until uniformly dispersed in the water to form a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct dropwise addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation was achieved, and the mixture was heated to 80°C and dried for 2 hours. During this process, the starch and phenolic resin dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with steam at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 71.6%. Referring to Figure 9, the spherical appearance of the activated biochar spheres; referring to Figure 10, an electron microscope image of the internal structure of the spheres at the micrometer scale.
[0043] Example 5
[0044] 1 liter of tap water was mixed with 10g sodium alginate, 10g starch, 10g phenolic resin, 36g biochar, 4g clay minerals, and 4g calcium carbonate. The mixture was stirred until uniformly dispersed in the water, forming a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80g calcium chloride, dissolving to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation occurred, and the mixture was heated to 80°C and dried for 2 hours. During this time, the starch and phenolic resin also dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. The adsorption rate of gold ions was 100% for a standard reagent at pH 2 and 100% for a standard reagent at pH 12. The electron microscope (SEM) images of the spheres are shown in Figure 1, showing the sphere's appearance, and Figures 2 and 3, showing the sphere's surface structure at the micrometer scale. Referring to Figure 11, the electron microscope image of the wood biochar fragments added in the example at the micrometer scale shows a smooth interface with a porous surface.
[0045] Component No. 1 Top Surface 2 Bottom Surface 3 Edge Surface 4 Top Surface 5 Bottom Surface 6 Edge Surface
Claims
1. A porous spherical structure of activated biochar spheres, comprising, at the micrometer scale: Multiple carbon particles form a spherical, multi-sized, irregularly stacked structure, wherein each carbon particle includes a corresponding layered edge structure and a corresponding surface layer structure, and the multi-sized, irregularly stacked structure includes: A carbon skeleton is formed by the stacking and connection of these carbon particles, wherein the stacking of these fragmented carbon particles further forms multiple intergranular voids; A porous structure formed by interconnected interparticle voids, wherein the porous structure includes an interface structure formed by multiple layered edge structures through multi-layered non-uniform stacking, wherein the layered edge structures are irregular in shape; Multiple small particles are discretely attached to these carbon particles.
2. The porous spherical structure as described in claim 1, wherein, The layered edge structure includes a first upper surface, a first edge surface, and a first lower surface, wherein the first edge surface connects the first upper surface and the first lower surface, and the first upper surface and the first lower surface face upward and downward, respectively.
3. The porous spherical structure as described in claim 1, wherein, The surface hierarchy structure includes a second upper surface, a second edge surface, and a second lower surface, wherein the second edge surface connects the second upper surface and the second lower surface, and the second upper surface and the second lower surface face the same direction.
4. The porous spherical structure as described in claim 1, wherein, These small particles include inorganic salts.
5. A porous spherical structure of activated biochar balls, comprising: Multiple micrometer-sized carbon particles are irregularly stacked to form millimeter-sized spherical structures; These carbon particles each include a corresponding layered edge structure and a corresponding surface hierarchical structure. These carbon particles are linked together to form a carbon skeleton; The carbon particles include a turbine layer carbon structure, wherein the turbine layer carbon structure includes multiple interlayer spaces and multiple exchangeable metal ions embedded in the interlayer spaces.