Method for manufacturing wiring board having protective film
Through the two-layer coating structure, the problem of insufficient voids and heat resistance in the printed circuit board protection film is solved by using the first photosensitive resin with moderate viscosity and the second photosensitive resin composition with high viscosity, and the integrity of the conductor is achieved Improved coverage and heat resistance.
Patent Information
- Application Number
- CN202010467453.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-05-28
AI Technical Summary
In the prior art, when manufacturing a printed circuit board with thick conductors, it is difficult to effectively prevent voids in the protective film, and the protective film of the thick conductors has shortcomings in terms of heat resistance.
Using a two-layer coating structure, the first coating film is formed by spraying the first photosensitive resin composition with a viscosity of 10 seconds to 50 seconds, and the second coating film is made by a second photosensitive having a viscosity higher than the first layer. The resin composition is formed by spray coating to ensure that the total film thickness of the two coating films after drying exceeds the conductor thickness, and the film thickness of the first coating film after drying is less than or equal to the conductor thickness to prevent sagging.
It effectively prevents the generation of voids in the protective film, and significantly improves the heat resistance and clarity of the protective film of the thick conductor, ensuring the complete coverage of the conductor.
Smart Images

Figure BDA0002513126370000181
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a wiring board such as a printed wiring board having a protective film such as an insulating coating. Background Art
[0002] Wiring boards such as printed wiring boards are used to form a conductor circuit pattern on a substrate, and electronic components are mounted on the pads of the pattern by soldering. In addition, the conductor circuit portion other than the pads is covered with a solder resist film as a protective film. This prevents solder from adhering to unnecessary parts when soldering electronic components on the printed wiring board, and prevents the conductor from being directly exposed to air and corroded by oxidation and humidity.
[0003] In recent years, with the high output of electronic devices such as solar cells for solar power generation and high-power motors installed in vehicles to reduce environmental burden, the conductor circuits of wiring boards are sometimes loaded with high voltages and large currents. Corresponding to the high voltages and large currents loaded on the conductor circuits of wiring boards, the thickness of the conductors tends to increase. When a protective film is formed on a wiring board with a thick conductor (for example, more than 150 μm), in order to give the insulating film basic properties such as heat resistance and insulation, it is required to reliably cover the thick conductor including the edge of the conductor. In order to reliably cover the thick conductor, it is necessary to apply a thicker protective film.
[0004] In addition, as electronic devices become more functional, there is a tendency for the conductor circuit patterns of wiring boards to become finer and the spacing between conductors to become narrower. If the spacing between thick conductors is narrowed, it is sometimes difficult to fill the gaps between the conductors with a protective film, and voids (cavitation) are generated in the protective film between the conductors, and the basic properties such as heat resistance and insulation cannot be fully imparted to the protective film.
[0005] Therefore, a method for manufacturing a printed wiring board in which a curable insulating material is applied (filled) to at least the recessed portion between circuits of a printed wiring board having thick wiring circuits and cured has been proposed, in which the curable insulating material is applied (filled) under reduced pressure (Patent Document 1). Patent Document 1 describes the manufacture of a printed wiring board having thick wiring circuits without voids and flat by applying the curable insulating material under reduced pressure.
[0006] However, the method for manufacturing a printed circuit board in Patent Document 1 has the problem that a decompression process is required and the manufacturing process of the printed circuit board is complicated. In addition, in the method for applying a curable insulating material under reduced pressure in Patent Document 1, the reduction of voids generated in the protective film between conductors is sometimes insufficient, and there is room for improvement in the heat resistance of the protective film.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2008-78595 Summary of the invention
[0010] Problems to be solved by the invention
[0011] In view of the above situation, an object of the present invention is to provide a method for manufacturing a wiring board having a protective film, which can prevent the generation of gaps in the protective film even if the protective film is filled between thick conductors formed on the wiring board, and can also impart excellent heat resistance even if the protective film is formed on thick conductors.
[0012] Means for solving problems
[0013] The gist of the configuration of the present invention is as follows.
[0014] [1] A method for manufacturing a wiring board having a protective film, comprising:
[0015] A first coating film forming step, wherein a first coating film is formed by spraying a first photosensitive resin composition on a wiring board having a substrate and a conductor provided on the substrate, wherein the viscosity of the first photosensitive resin composition is 10 seconds to 50 seconds when measured by an Iwata cup, and the thickness of the first coating film after drying is less than or equal to the thickness of the conductor;
[0016] A second coating film forming step, wherein a second photosensitive resin composition having a higher viscosity than the first photosensitive resin composition is applied on the surface of the first coating film to form the second coating film, and the total thickness of the first coating film after drying and the thickness of the second coating film after drying is greater than the thickness of the conductor.
[0017] [2] The method for producing a wiring board having a protective film according to [1], wherein the second coating film is formed by spraying the second photosensitive resin composition.
[0018] [3] The method for producing a wiring board having a protective film according to [1] or [2], wherein the viscosity of the first photosensitive resin composition is 10 seconds to 30 seconds when measured using an Iwata cup.
[0019] [4] The method for producing a wiring board having a protective film according to [2], wherein the viscosity of the second photosensitive resin composition is 80 seconds to 100 seconds when measured with an Iwata cup.
[0020] [5] The method for producing a wiring board having a protective coating according to any one of [1] to [4], wherein the first coating film is formed by performing a step of spraying the first photosensitive resin composition and then drying the composition a plurality of times.
[0021] [6] The method for producing a wiring board having a protective coating according to any one of [1] to [5], wherein no colorant is compounded in the first coating film.
[0022] [7] A method for manufacturing a wiring board having a protective coating according to any one of [1] to [6], wherein the thickness of the first coating layer in the first coating layer forming step after drying is smaller than the thickness of the conductor by at least 5.0 μm and at most 30 μm.
[0023] [8] The method for manufacturing a wiring board having a protective coating according to any one of [1] to [7], wherein the protective coating is composed of the first coating film and the second coating film.
[0024] [9] The method for manufacturing a wiring board having a protective film according to any one of [1] to [8], wherein the conductor has a thickness of 150 μm or more.
[0025]
[10] A method for manufacturing a wiring board having a protective coating according to any one of [1] to [9], wherein the thickness of the first coating layer after drying is greater than 100 μm and less than 250 μm, and the thickness of the second coating layer after drying is greater than 20 μm.
[0026]
[11] A method for manufacturing a wiring board having a protective film according to any one of [1] to
[10] , wherein the first photosensitive resin composition and the second photosensitive resin composition contain (A) a photosensitive resin containing a carboxyl group, (B) a photopolymerization initiator, (C) a reactive diluent, (D) an epoxy compound, and (E) a non-reactive diluent.
[0027] In the above-mentioned embodiment [1], the protective film has a laminated structure of a first coating film and a second coating film. In addition, the film thickness of the first coating film after drying is less than or equal to the thickness of the conductor, and the total film thickness of the first coating film after drying and the film thickness of the second coating film after drying is greater than the thickness of the conductor, so that the upper surface of the conductor is covered by the second coating film.
[0028] In the above-mentioned embodiment [5], the first coating film is formed by performing a plurality of cycles of a step of forming a coating film of the first photosensitive resin composition and a step of drying the formed coating film, and the step of forming a coating film of the first photosensitive resin composition is performed by spraying the first photosensitive resin composition. Therefore, the first coating film has a structure in which a plurality of dried coating films of the first photosensitive resin composition are stacked.
[0029] Effects of the Invention
[0030] According to a method for manufacturing a wiring board with a protective film of the present invention, a first photosensitive resin composition having a viscosity of more than 10 seconds and less than 50 seconds when measured by an Iwata cup is sprayed to form a first coating film in a manner such that the film thickness after drying is less than or equal to the thickness of the conductor, and then a second photosensitive resin composition having a higher viscosity than the first photosensitive resin composition is applied to form a second coating film in a manner such that the total of the film thickness after drying of the first coating film and the film thickness after drying of the second coating film is greater than the thickness of the conductor. This prevents the generation of voids in the protective film even if it is a protective film filled between thick conductors formed on the wiring board, and further, even a protective film formed on a thick conductor can be imparted with excellent heat resistance.
[0031] According to the aspect of the method for manufacturing a wiring board having a protective film of the present invention, by spraying the second photosensitive resin composition to form the second coating film, it is possible to reliably prevent the generation of voids in the protective film even if the protective film is filled between thick conductors.
[0032] According to the scheme of the manufacturing method of the wiring board with a protective film of the present invention, by making the viscosity of the second photosensitive resin composition greater than 80 seconds and less than 100 seconds when measured by using an Iwata cup, the surface of the protective film can be flattened, and the covering property of the protective film on the etched portion of the conductor can be improved, thereby more reliably covering the entire conductor.
[0033] According to the aspect of the method for manufacturing a wiring board having a protective film of the present invention, since a colorant is not added to the first coating film, the photocurability of the first coating film is improved, the heat resistance of the protective film is further improved, and the protective film can be given excellent clarity.
[0034] According to the scheme of the manufacturing method of the wiring board with a protective film of the present invention, by making the film thickness of the first layer of coating after drying in the first layer of coating forming process smaller than the thickness of the conductor by more than 5.0μm and less than 30μm, it is possible to prevent the first layer of coating from dripping and to improve the covering property of the protective film on the etched portion of the conductor. DETAILED DESCRIPTION
[0035] The following is a description of a method for manufacturing a wiring board with a protective film of the present invention. The method for manufacturing a wiring board with a protective film of the present invention comprises: a first coating film forming step, wherein a first photosensitive resin composition having a viscosity of 10 seconds or more and 50 seconds or less when measured by an Iwata cup is sprayed on a wiring board having a substrate and a conductor disposed on the substrate to form a first coating film, wherein the thickness of the first coating film after drying is equal to or less than the thickness of the conductor; and a second coating film forming step, wherein a second photosensitive resin composition having a higher viscosity than the first photosensitive resin composition is applied on the surface of the first coating film to form a second coating film, wherein the total thickness of the first coating film after drying and the thickness of the second coating film after drying is greater than the thickness of the conductor. It should be noted that the "viscosity" of the photosensitive resin composition in this specification is the viscosity of the photosensitive resin composition at 25°C.
[0036] The protective film having a laminated structure of a first coating film and a second coating film is a cured product of a photosensitive resin composition. The first coating film is a cured product of a first photosensitive resin composition, and the second coating film is a cured product of a second photosensitive resin composition.
[0037] First coating film forming step
[0038] The first coating film forming step is a step of spraying a first photosensitive resin composition having a viscosity of 10 seconds or more and 50 seconds or less when measured by an Iwata cup on a wiring board (e.g., a printed wiring board having a conductor circuit pattern) to form a first coating film, and forming the first coating film in such a way that the film thickness of the first coating film after drying is less than or equal to the thickness of the conductor. For example, after the first photosensitive resin composition is directly sprayed on the wiring board to form a coating film, the formed coating film is dried to form the first coating film. The first coating film becomes the lower layer of the protective film.
[0039] The viscosity of the first photosensitive resin composition is 10 seconds to 50 seconds (50 mPa·s to 380 mPa·s) when measured by an Iwata cup. If the viscosity is less than 10 seconds when measured by an Iwata cup, sagging occurs in the first coating film and a predetermined pattern cannot be formed. In addition, if the viscosity exceeds 50 seconds, the spray discharge liquid of the first photosensitive resin composition cannot be sufficiently finely divided, and voids are easily generated in the first coating film filled between thick conductors (for example, 150 μm or more). In addition, it is difficult to impart heat resistance to the protective film formed on thick conductors of 150 μm or more. In summary, by making the viscosity of the first photosensitive resin composition 10 seconds or more and 50 seconds or less when measured by an Iwata cup, the first coating film can be prevented from sagging, and the spray discharge liquid of the first photosensitive resin composition can be made fine, so that even between thick conductors (for example, 150 μm or more) gaps can be prevented from being generated in the filled first coating film, and excellent heat resistance can be given to the protective film. It should be noted that in this specification, the viscosity in Pa·s is a value measured by a B-type viscometer (sample temperature 25°C, rotation speed 50 rpm).
[0040] The viscosity of the first photosensitive resin composition is not particularly limited as long as it is within the range of 10 seconds or more and 50 seconds or less when measured using an Iwata cup. From the perspective of reliably preventing the first coating film from sagging, the lower limit is preferably 15 seconds (100 mPa·s) when measured using an Iwata cup. On the other hand, from the perspective of reliably preventing the formation of voids in the first coating film filled between thick conductors and further improving the heat resistance of the protective film having the first coating film, the upper limit of the viscosity of the first photosensitive resin composition is preferably 40 seconds (330 mPa·s) when measured using an Iwata cup, and particularly preferably 30 seconds (230 mPa·s) when measured using an Iwata cup. The viscosity of the first photosensitive resin composition can be set within the above-specified range by adjusting the amount of the (E) non-reactive diluent added to the first photosensitive resin composition described later.
[0041] The components of the first photosensitive resin composition are not particularly limited, and include, for example, (A) a carboxyl group-containing photosensitive resin, (B) a photopolymerization initiator, (C) a reactive diluent, (D) an epoxy compound, and (E) a non-reactive diluent. The components of the first photosensitive resin composition are described below.
[0042] (A) Photosensitive resin containing carboxyl group
[0043] The photosensitive resin containing a carboxyl group is not particularly limited, and examples thereof include resins having one or more photosensitive unsaturated double bonds. As the photosensitive resin containing a carboxyl group, examples thereof include polyacid-modified free radical polymerizable unsaturated monocarboxylic acid epoxy resins such as polyacid-modified epoxy (meth) acrylates, which can be obtained by reacting free radical polymerizable unsaturated monocarboxylic acid such as acrylic acid and methacrylic acid (hereinafter sometimes referred to as "(meth) acrylic acid") with at least part of the epoxy groups in a multifunctional epoxy resin having two or more epoxy groups in one molecule to obtain free radical polymerizable unsaturated monocarboxylic acid epoxy resins such as epoxy (meth) acrylates, and reacting the generated hydroxyl groups with polyacids and / or polyacid anhydrides.
[0044] The chemical structure of the multifunctional epoxy resin is not particularly limited as long as it is an epoxy resin with two or more functions. The epoxy equivalent of the multifunctional epoxy resin is not particularly limited, and its upper limit is preferably 3000, more preferably 2000, and particularly preferably 1000. On the other hand, the lower limit of the epoxy equivalent of the multifunctional epoxy resin is preferably 100, and particularly preferably 200. As multifunctional epoxy resin, for example: biphenyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, ε-caprolactone modified epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, cyclic aliphatic multifunctional epoxy resin, glycidyl ester type multifunctional epoxy resin, glycidyl amine type multifunctional epoxy resin, heterocyclic multifunctional epoxy resin, bisphenol modified novolac type epoxy resin, multifunctional modified novolac type epoxy resin, phenol and aromatic aldehyde condensation product type epoxy resin with phenolic hydroxyl group etc. can be enumerated. In addition, the product obtained by introducing halogen atoms such as Br and Cl into these resins can be used. These multifunctional epoxy resins can be used alone, or two or more can be used in combination.
[0045] There is no particular limitation on the free radical polymerizable unsaturated monocarboxylic acid, and examples thereof include (meth) acrylic acid, crotonic acid, tiliac acid, angelic acid, cinnamic acid, etc. Among them, (meth) acrylic acid is preferred from the perspective of easy acquisition and handling. These free radical polymerizable unsaturated monocarboxylic acids can be used alone or in combination of two or more.
[0046] The reaction method of the polyfunctional epoxy resin and the radically polymerizable unsaturated monocarboxylic acid is not particularly limited. For example, the polyfunctional epoxy resin and the radically polymerizable unsaturated monocarboxylic acid can be reacted by stirring and heating them in a suitable diluent such as an organic solvent.
[0047] The free carboxyl groups are introduced into the free radical polymerizable unsaturated monocarboxylic acid epoxy resin by addition reaction of the carboxyl groups of the polyacid and / or polyacid anhydride with the hydroxyl groups generated by the reaction of the polyfunctional epoxy resin and the free radical polymerizable unsaturated monocarboxylic acid. The chemical structure of the polyacid and polyacid anhydride is not particularly limited, and any of saturated and unsaturated ones can be used. As the polyacid, for example, succinic acid, maleic acid, adipic acid, citric acid, tetrahydrophthalic acid, phthalic acid, tetrahydrophthalic acid, 3-methyltetrahydrophthalic acid, 4-methyltetrahydrophthalic acid, 3-ethyltetrahydrophthalic acid, 4-ethyltetrahydrophthalic acid and other tetrahydrophthalic acids; hexahydrophthalic acid, 3-methylhexahydrophthalic acid, 4-methylhexahydrophthalic acid, 3-ethylhexahydrophthalic acid, 4-ethylhexahydrophthalic acid and other hexahydrophthalic acids; methyltetrahydrophthalic acid, endomethylenetetrahydrophthalic acid, methylendomethylenetetrahydrophthalic acid and other tetrahydrophthalic acids; trimellitic acid; pyromellitic acid; and diglycolic acid. As the polyacid anhydride, the anhydrides of the above-mentioned various polyacids can be listed. These polyacids and / or polyacid anhydrides can be used alone or in combination of two or more.
[0048] The method for reacting the radically polymerizable unsaturated monocarboxylic acid-containing epoxy resin with the polybasic acid and / or polybasic acid anhydride is not particularly limited. For example, the radically polymerizable unsaturated monocarboxylic acid-containing epoxy resin and the polybasic acid and / or polybasic acid anhydride may be reacted by stirring and heating the resin in a suitable diluent such as an organic solvent.
[0049] The above-mentioned polyacid-modified unsaturated monocarboxylic acid epoxy resin can also be used as a photosensitive resin containing a carboxyl group. A polyacid-modified free radical polymerizable unsaturated monocarboxylic acid epoxy resin further added with a free radical polymerizable unsaturated group obtained by addition reaction of a compound having one or more free radical polymerizable unsaturated groups and epoxy groups with part of the carboxyl groups in the above-mentioned polyacid-modified unsaturated monocarboxylic acid epoxy resin can also be used as a photosensitive resin containing a carboxyl group. The polyacid-modified free radical polymerizable unsaturated monocarboxylic acid epoxy resin further added with a free radical polymerizable unsaturated group has a chemical structure in which a free radical polymerizable unsaturated group is further introduced into the side chain of the polyacid-modified unsaturated monocarboxylic acid epoxy resin. Therefore, the polyacid-modified free radical polymerizable unsaturated monocarboxylic acid epoxy resin further added with a free radical polymerizable unsaturated group is a resin with further improved photocurability compared with the polyacid-modified unsaturated monocarboxylic acid epoxy resin.
[0050] Examples of compounds having one or more free radical polymerizable unsaturated groups and epoxy groups include glycidyl compounds. Examples of glycidyl compounds include glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, pentaerythritol triacrylate monoglycidyl ether, pentaerythritol trimethacrylate monoglycidyl ether, and the like. One molecule may have one glycidyl group or may have multiple glycidyl groups. In addition, the above-mentioned compounds having one or more free radical polymerizable unsaturated groups and epoxy groups may be used alone or in combination of two or more.
[0051] The method for reacting the polyacid-modified unsaturated monocarboxylic acid epoxy resin with the compound having one or more free radical polymerizable unsaturated groups and epoxy groups is not particularly limited. For example, the polyacid-modified unsaturated monocarboxylic acid epoxy resin and the compound having one or more free radical polymerizable unsaturated groups and epoxy groups can be reacted by stirring and heating in an appropriate diluent such as an organic solvent.
[0052] The acid value of the photosensitive resin containing a carboxyl group is not particularly limited, but from the perspective of reliable alkali development, the lower limit is preferably 30 mgKOH / g, and particularly preferably 40 mgKOH / g. On the other hand, from the perspective of reliably preventing the alkaline developer from dissolving the exposed portion, the upper limit of the acid value of the photosensitive resin containing a carboxyl group is preferably 200 mgKOH / g, and from the perspective of reliably preventing the decrease in moisture resistance and insulation properties of the cured product, it is particularly preferably 150 mgKOH / g.
[0053] The mass average molecular weight of the photosensitive resin containing a carboxyl group is not particularly limited. From the perspective of toughness and dryness to touch of the cured product, the lower limit is preferably 3000, and particularly preferably 5000. On the other hand, from the perspective of good alkali developability, the upper limit of the mass average molecular weight of the photosensitive resin containing a carboxyl group is preferably 200000, and particularly preferably 100000. It should be noted that the "mass average molecular weight" refers to the mass average molecular weight measured at room temperature using gel permeation chromatography (GPC) and calculated by polystyrene conversion.
[0054] Commercially available products of the above-mentioned various carboxyl group-containing photosensitive resins include, for example, SP-4621, SP-4785 (all from Showa Denko K.K.), ZAR-2000, ZFR-1122, FLX-2089, ZCR-1569H, and ZCR-1601H (all from Nippon Kayaku Co., Ltd.). The above-mentioned various carboxyl group-containing photosensitive resins may be used alone or in combination of two or more.
[0055] (B) Photopolymerization initiator
[0056] The photopolymerization initiator is not particularly limited, and examples thereof include (9-ethyl-6-nitro-9H-carbazole-3-yl) [4-(2-methoxy-1-methylethoxy-2-methylphenyl] -, O-acetoxime, 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyl oxime)], ethyl ketone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl] -1-(O-acetoxime), 2-(acetoxyiminomethyl) thioxanthen-9-one, 1,8-octanedione, 1,8-bis[9-ethyl-6-nitro-9H-carbazole-3-yl] -, 1,8-bis(O- Oxime ester photopolymerization initiators such as 1,8-octanedione, 1,8-bis[9-(2-ethylhexyl)-6-nitro-9H-carbazole-3-yl]-, 1,8-bis(O-acetyloxime), (Z)-(9-ethyl-6-nitro-9H-carbazole-3-yl)(4-((1-methoxypropane-2-yl)oxy)-2-methylphenyl)methanone O-acetyloxime; 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-methyl-4'-(methylthio)-2-morpholinopropanophenone, etc. α-Aminoalkyl phenyl ketone-based photopolymerization initiator; benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexyl phenyl ketone, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4′-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert- Butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzil dimethyl ketal, acetophenone dimethyl ketal, ethyl p-dimethylaminobenzoate, 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, bis (2,4,6-trimethylbenzoyl) phenyl phosphine oxide, bis (2,6-dimethoxybenzoyl) -2,4,4-trimethyl-pentyl phosphine oxide, (2,4,6-trimethylbenzoyl) ethoxyphenyl phosphine oxide, etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0057] The content of the photopolymerization initiator is not particularly limited, but is preferably 0.5 to 30 parts by mass, particularly preferably 1.0 to 20 parts by mass, based on 100 parts by mass (solid content, the same below) of the carboxyl group-containing photosensitive resin.
[0058] (C) Reactive diluent
[0059] The reactive diluent is, for example, a photopolymerizable monomer, which is a compound having at least one, preferably two or more photopolymerizable double bonds per molecule. During the exposure treatment, the reactive diluent enhances the photocuring of the first photosensitive resin composition, thereby contributing to the improvement of the acid resistance, heat resistance, and alkali resistance of the cured product of the first photosensitive resin composition. Examples of the reactive diluent include monofunctional (meth)acrylate monomers and difunctional or higher (meth)acrylate monomers. Examples of the (meth)acrylate monomer include: monofunctional (meth)acrylate compounds such as hydroxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, diethylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and stearyl (meth)acrylate; 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, cyclopentyl acrylate, and cyclopentyl acrylate. Bifunctional (meth)acrylate compounds such as ethylene oxide modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, and isocyanurate di(meth)acrylate; trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tri(acryloyloxyethyl)isocyanurate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ε-caprolactone modified dipentaerythritol hexa(meth)acrylate, etc. These may be used alone or in combination of two or more.
[0060] The content of the reactive diluent is not particularly limited, but is preferably 5.0 parts by mass or more and 80 parts by mass or less, and particularly preferably 10 parts by mass or more and 60 parts by mass or less, based on 100 parts by mass of the carboxyl group-containing photosensitive resin.
[0061] (D) Epoxy compounds
[0062] The epoxy compound is a component used to increase the crosslinking density of the cured product and obtain a coating film with sufficient strength. Examples of the epoxy compound include epoxy resins. Examples of the epoxy resins include the same epoxy resins that can be used to prepare the above-mentioned (A) carboxyl-containing photosensitive resin. Specifically, for example, biphenyl epoxy resin, naphthalene epoxy resin, dicyclopentadiene epoxy resin, ε-caprolactone modified epoxy resin, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD epoxy resin and other phenol novolac epoxy resins, o-cresol novolac epoxy resin and other cresol novolac epoxy resins, bisphenol A novolac epoxy resins, cyclic aliphatic multifunctional epoxy resins, glycidyl ester multifunctional epoxy resins, glycidyl amine multifunctional epoxy resins, heterocyclic multifunctional epoxy resins, bisphenol modified novolac epoxy resins, multifunctional modified novolac epoxy resins, condensate epoxy resins of phenols and aromatic aldehydes having phenolic hydroxyl groups, etc. These can be used alone or in combination of two or more.
[0063] The content of the epoxy compound is not particularly limited, but is preferably 10 parts by mass or more and 80 parts by mass or less, and particularly preferably 20 parts by mass or more and 70 parts by mass or less, based on 100 parts by mass of the carboxyl group-containing photosensitive resin.
[0064] (E) Non-reactive diluent
[0065] The non-reactive diluent is a component used to adjust the viscosity of the first photosensitive resin composition to 10 seconds or more and 50 seconds or less when measured by an Iwata cup, and to adjust the drying property of the first photosensitive resin composition. Examples of the non-reactive diluent include organic solvents. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene and xylene; alcohols such as methanol, isopropanol, and cyclohexanol; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; cellosolves such as cellosolves and butyl cellosolves; carbitols such as carbitol and butyl carbitol; esters such as ethyl acetate, butyl acetate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate.
[0066] The content of the non-reactive diluent is not particularly limited as long as the viscosity of the first photosensitive resin composition can be controlled to be within the range of 10 seconds or more and 50 seconds or less when measured by an Iwata cup. For example, it is preferably 50 parts by mass or more and 500 parts by mass or less, and particularly preferably 70 parts by mass or more and 170 parts by mass or less, relative to 100 parts by mass of the photosensitive resin containing a carboxyl group. In addition, the content of the non-reactive diluent is preferably 10% by mass or more and 40% by mass or less, and particularly preferably 15% by mass or more and 35% by mass or less, in the first photosensitive resin composition.
[0067] The first photosensitive resin composition may contain various components, such as a colorant, various additives, and a filler, in addition to the above-mentioned components (A) to (E), as required.
[0068] The colorant is a pigment, a coloring agent, etc., and is not particularly limited. In addition, for the colorant, any color such as a white colorant, a blue colorant, a green colorant, a yellow colorant, a purple colorant, a black colorant, etc. can be used according to the desired color to be given to the first layer of the coating. As the above-mentioned colorant, for example, inorganic colorants such as titanium oxide as a white colorant and carbon black as a black colorant can be listed; phthalocyanine series such as phthalocyanine green as a green colorant and phthalocyanine blue, Leonor blue as a blue colorant, phthalocyanine series such as Cromophtal Yellow as a yellow colorant, organic colorants such as anthraquinone series, etc. It should be noted that the first layer of the coating forms the lower layer of the protective film. Therefore, by not adding a colorant to the first photosensitive resin composition, the photocurability of the first layer of the coating is improved, the heat resistance of the protective film is further improved, and excellent clarity can be given to the protective film.
[0069] As various additives, for example, coupling agents such as silane, titanate, and alumina; latent curing agents such as boron trifluoride-amine complexes, dicyandiamide (DICY) and its derivatives, organic acid hydrazides, diaminomaleonitrile (DAMN) and its derivatives, guanamine and its derivatives, melamine and its derivatives, amine imide (AI) and polyamines; metal salts of acetylacetone such as acetylacetone Zn and acetylacetone Cr, enamine, tin octoate, quaternary sulfonium salts, triphenylphosphine, imidazoles such as 2-mercaptobenzimidazole, imidazolium salts, and thermosetting accelerators such as triethanolamine borate; thixotropic agents such as polycarboxylic acid amides, etc.
[0070] The filler is a component for improving the physical strength of the coating film of the first photosensitive resin composition, that is, the first layer coating film, and examples thereof include talc, barium sulfate, silica, alumina, aluminum hydroxide, and mica.
[0071] The method for producing the first photosensitive resin composition is not limited to a specific method, and for example, the above-mentioned components can be mixed in a predetermined ratio, and then kneaded or mixed at room temperature (e.g., 25° C.) using a kneading means such as a triple roll, a ball mill, a bead mill, a sand mill, or a stirring means such as a super mixer or a planetary mixer. In addition, before the above kneading or mixing, preliminary kneading or preliminary mixing can be performed at room temperature (e.g., 25° C.) as needed.
[0072] Next, a method for spraying the first photosensitive resin composition on a wiring board to form a first coating film on the wiring board is described. The first photosensitive resin composition obtained as described above is applied to, for example, a printed wiring board having a circuit pattern formed by etching copper foil (the thickness of the copper foil as a conductor is, for example, 150 μm or more) using a coating method using a spray coater, i.e., spraying. Regarding the thickness of each coating of the first photosensitive resin composition, for example, when the film thickness after drying is set to 50 to 70 μm, the first photosensitive resin composition is applied with a wet film thickness of 150 to 250 μm to form a coating film. Then, the formed coating film of the first photosensitive resin composition is heated at a temperature of about 70 to 90° C. for about 5 to 15 minutes, and a drying treatment (preliminary drying) is performed to dry the coating film to form a first coating film.
[0073] The first photosensitive resin composition is applied in such a manner that the thickness of the first coating layer after drying is less than or equal to the thickness of the conductor. The thickness of the first coating layer after drying is not particularly limited as long as it is less than or equal to the thickness of the conductor. From the perspective of preventing sagging in the first coating layer and improving the covering property of the protective film on the etched portion of the conductor, it is preferably 5.0 μm or more and 30 μm or less than the thickness of the conductor, and particularly preferably 10 μm or more and 25 μm or less. Therefore, the above-mentioned steps of forming a coating film by spraying and drying the formed coating film can be repeated multiple times as needed to form a first coating film having a desired thickness. When the steps of forming a coating film and drying the formed coating film are repeated multiple times, the first coating film becomes a structure of a dried coating film of a plurality of layers of the first photosensitive resin composition stacked on top of each other.
[0074] The thickness of the first coating layer after drying can be adjusted according to the thickness of the conductor. For example, when the thickness of the conductor is 150 μm to 350 μm, the thickness of the first coating layer after drying is preferably 100 μm to 250 μm, particularly preferably 150 μm to 230 μm.
[0075] Second coating film forming process
[0076] In the second coating film forming step, a second photosensitive resin composition having a higher viscosity than the first photosensitive resin composition is applied on the surface of the first coating film formed as described above, thereby forming a second coating film, and the second photosensitive resin composition is applied in such a manner that the total thickness of the first coating film after drying and the thickness of the second coating film after drying is greater than the conductor thickness of the wiring board. For example, the second photosensitive resin composition is applied directly on the first coating film or through another coating film, and after the coating film is formed, the coating film of the second photosensitive resin composition is dried to form the second coating film. The second coating film becomes the upper layer of the protective film. In addition, when the second coating film is located at the uppermost layer of the protective film, the second photosensitive resin composition can be directly applied on the first coating film to form a protective film composed of the first coating film and the second coating film.
[0077] The method for coating the second photosensitive resin composition on the first coating film is not particularly limited, and known methods such as spray coating, screen printing, bar coating, applicator, blade coating, knife coating, roll coating, gravure coating, etc. can be used. Among them, spray coating using a spray coating machine is preferred from the perspective of reliably preventing the formation of voids in the protective film even when the protective film is filled between thick conductors formed on the wiring board.
[0078] The viscosity of the second photosensitive resin composition is not particularly limited as long as it is higher than the viscosity of the first photosensitive resin composition. When the second photosensitive resin composition is applied by spraying, from the perspective of reliably preventing the protective film from sagging and more reliably covering the entire conductor by improving the covering property of the protective film on the etching portion of the conductor, the lower limit of the viscosity is preferably 70 seconds (500 mPa·s) when measured using an Iwata cup, and particularly preferably 80 seconds (550 mPa·s) when measured using an Iwata cup. On the other hand, from the perspective of flattening the surface of the protective film, the upper limit of the viscosity of the second photosensitive resin composition is preferably 110 seconds (630 mPa·s) when measured using an Iwata cup, and particularly preferably 100 seconds (590 mPa·s) when measured using an Iwata cup. In addition, when the second photosensitive resin composition is applied by a coating method other than spraying such as screen printing, the viscosity of the second photosensitive resin composition is preferably 150 dPa·s or more and 250 dPa·s or less, and particularly preferably 180 dPa·s or more and 220 dPa·s or less. The viscosity of the second photosensitive resin composition can be set within a predetermined range by adjusting the amount of the (E) non-reactive diluent added to the second photosensitive resin composition described later.
[0079] The components of the second photosensitive resin composition are not particularly limited, and include, for example, (A) a photosensitive resin containing a carboxyl group, (B) a photopolymerization initiator, (C) a reactive diluent, (D) an epoxy compound, and (E) a non-reactive diluent. The components (A) to (E) of the second photosensitive resin composition may be the components exemplified and listed in the components (A) to (E) of the first photosensitive resin composition. In addition, the content range of the components (A) to (E) of the second photosensitive resin composition may be the content range exemplified in the components (A) to (E) of the first photosensitive resin composition. Therefore, except for the content of the (E) non-reactive diluent having the function of adjusting the viscosity of the second photosensitive resin composition, the components of the (A) carboxyl group-containing photosensitive resin, (B) photopolymerization initiator, (C) reactive diluent, and (D) epoxy compound of the second photosensitive resin composition can be mixed with the same compounds as those of the first photosensitive resin composition at the same mixing ratio. In addition, the (E) non-reactive diluent of the second photosensitive resin composition can use the same compound as that of the (E) non-reactive diluent of the first photosensitive resin composition.
[0080] In addition, a colorant that matches the desired color of the second coating film may be added to the second photosensitive resin composition as needed. By adding a colorant to the second photosensitive resin composition, a covering power may be imparted to the protective film of the wiring board. In addition to the above-mentioned components (A) to (E), the second photosensitive resin composition may contain various components such as various additives, fillers, etc. as needed, similar to the first photosensitive resin composition.
[0081] The method for producing the second photosensitive resin composition is not limited to a specific method. For example, the above-mentioned components can be mixed in a predetermined ratio, and then kneaded or mixed at room temperature (e.g., 25° C.) using a kneading means such as a triple roll, a ball mill, a bead mill, a sand mill, or a stirring means such as a super mixer or a planetary mixer. In addition, before the above kneading or mixing, preliminary kneading or preliminary mixing can be performed at room temperature (e.g., 25° C.) as needed.
[0082] Next, a method for applying a second photosensitive resin composition to a wiring board to form a second coating film on the wiring board is described. The second photosensitive resin composition obtained as described above is applied to the first coating film formed as described above using the above-mentioned known coating methods such as spraying. Regarding the thickness of each coating of the second photosensitive resin composition, for example, when the film thickness after drying is set to 20 to 50 μm, the coating film of the second photosensitive resin composition is formed by coating with a wet film thickness of 40 to 100 μm. Next, the coating film of the formed second photosensitive resin composition is heated at a temperature of about 70 to 90°C for about 10 to 20 minutes, and a drying treatment (pre-drying) is performed to dry the coating film to form a second coating film.
[0083] The second photosensitive resin composition is applied in such a manner that the total thickness of the first coating layer after drying and the second coating layer after drying is greater than the thickness of the conductor of the wiring board. The thickness of the second coating layer after drying is not particularly limited as long as the total thickness of the first coating layer after drying and the second coating layer after drying is greater than the thickness of the conductor of the wiring board. For example, when the thickness of the conductor is 150 μm or more and 350 μm or less, from the perspective of preventing sagging in the protective film and improving the covering property of the protective film on the etching portion of the conductor, the lower limit is preferably 20 μm, and particularly preferably 25 μm. On the other hand, from the perspective of reliably photocuring the first coating layer, the upper limit of the thickness of the second coating layer after drying is preferably 50 μm, and particularly preferably 45 μm. It should be noted that, as needed, the coating film forming step by applying the second photosensitive resin composition and the step of drying the formed coating film can be repeated multiple times to form a second coating film having a specified thickness. When the cycle of the coating film forming step and the step of drying the formed coating film is performed a plurality of times, the second coating film has a structure in which a plurality of dried coating films of the second photosensitive resin composition are stacked.
[0084] The ratio of the thickness of the second coating film after drying: the thickness of the first coating film after drying is not particularly limited, and can be appropriately selected according to the thickness of the conductor, for example, and is preferably 1:1 to 10, and particularly preferably 1:2 to 5.
[0085] On a coating film having a laminated structure of a first coating film and a second coating film formed by forming a second coating film on a first coating film, a negative film is closely attached and irradiated with ultraviolet rays (e.g., a wavelength range of 300 to 400 nm) from above, wherein the negative film has a pattern that is all light-transmissive except for the pads of the circuit pattern. Then, the non-exposed area corresponding to the above-mentioned pads is removed with a dilute alkali aqueous solution, thereby developing the coating film having a laminated structure. As a developing method, a spray method, a shower method, etc. are used, and as the dilute alkali aqueous solution used, for example, a 0.5 to 5% by mass sodium carbonate aqueous solution can be cited. Then, a heat curing treatment (post-curing) is performed at 130 to 170° C. for 20 to 80 minutes using a hot air circulation dryer or the like, thereby obtaining a wiring board formed with a protective film having a target pattern.
[0086] [Example]
[0087] Next, embodiments of the present invention will be described, but the present invention is not limited to these examples unless exceeding the gist of the present invention.
[0088] Examples 1 to 5, Comparative Examples 1 to 3
[0089] The components shown in Table 1 below were mixed in the proportions shown in Table 1 below, and mixed and dispersed at room temperature using a triple roll to prepare the first photosensitive resin composition and the second photosensitive resin composition used in Examples 1 to 5 and Comparative Examples 1 to 3. Regarding the viscosity measurement of the first photosensitive resin composition and the second photosensitive resin composition, when the viscosity was measured using an Iwata cup (in Table 1 below, the unit of viscosity is "s"), when the rotational viscosity was measured using NK-2 (ANEST IWATA Corporation) (in Table 1 below, the unit of viscosity is "dPa·s"), a Brookfield B-type viscometer (sample temperature 25°C, rotation speed 50 rpm, Brookfield Corporation) was used. Then, the prepared first photosensitive resin composition and the second photosensitive resin composition were applied as follows to prepare a test body. The numbers in Table 1 below represent parts by mass. In addition, the blank column in Table 1 below indicates that no compounding was performed.
[0090] It should be noted that the details of the components in Table 1 are as follows.
[0091] (A) Photosensitive resin containing carboxyl group
[0092] SP-4621 (solid content 60% by mass, diethylene glycol monoethyl ether acetate 20% by mass, naphtha 20% by mass), SP-4785 (solid content 60% by mass, diethylene glycol monoethyl ether acetate 20% by mass, naphtha 20% by mass): Showa Denko K.K.
[0093] (B) Photopolymerization initiator
[0094] ·Irgacure 907: DKSH Japan Co., Ltd.
[0095] ·KAYACURE JETX: Nippon Kayaku Co., Ltd.
[0096] (C) Reactive diluent
[0097] ·Aronix M-400: Toa Gosei Co., Ltd.
[0098] (D) Epoxy compounds
[0099] ·N695: DIC Co., Ltd.
[0100] ·Epicoat 828, YX-4000K: Mitsubishi Chemical Corporation.
[0101] (E) Non-reactive diluent
[0102] ·ARCOSOLV PM: SANYO CHEMICALS CO., LTD.
[0103] Colorants
[0104] ·FASTOGEN GREEN: DIC Co., Ltd.
[0105] additive
[0106] Melamine: Nissan Chemical Industries, Ltd.
[0107] DICY-7: Japan Epoxy Resin Co., Ltd.
[0108] ·Antage MB: Kawaguchi Chemical Industry Co., Ltd.
[0109] filler
[0110] ·Barium sulfate B-30: Sakai Chemical Industry Co., Ltd.
[0111] ·R-974: Japan AEROSIL Co., Ltd.
[0112] Test body production process
[0113] Substrate: Glass epoxy substrate "FR-4"
[0114] Substrate surface treatment: polishing and grinding
[0115] Application of the first photosensitive resin composition: Spraying (horizontal air jet, nozzle opening diameter 0.5 mm)
[0116] Application of the second photosensitive resin composition: spray coating (horizontal air jet, nozzle opening diameter 0.5 mm) or screen printing (T-100 screen)
[0117] Drying (pre-drying): For the coating of the first photosensitive resin composition, dry at 80°C for 10 minutes each time the coating is applied, and for the coating of the second photosensitive resin composition, dry at 80°C for 20 minutes
[0118] Exposure: 200-300 mJ / cm 2 Exposure (wavelength 300-400nm, ADTEC Engineering Co., Ltd. "SAC")
[0119] Alkali development: 1 mass% Na2CO3 aqueous solution, liquid temperature 30°C, spray pressure 0.2MPa, development time 90 seconds
[0120] Post-curing: 150°C, 60 minutes
[0121] The evaluation items are as follows.
[0122] (1) Embedment of wires
[0123] A substrate having a circuit pattern in which the conductor line width is 400 μm and the spacing of the gaps between the lines is 400 μm was used. The conductor had a conductor thickness as shown in the following Table 1. A test body was prepared according to the above-mentioned test body preparation process. The post-cured protective film filled between the lines was observed from the top surface using an optical microscope (magnification 200 times) to observe the presence or absence of gaps, and evaluation was performed according to the following criteria.
[0124] ○: It was confirmed that no voids were generated in the post-cured protective film that filled the lines.
[0125] △: Some voids were observed in the post-cured protective film that filled the lines.
[0126] ×: It was confirmed that a large number of voids were generated in the post-cured protective film that filled the spaces between the wires, or the photosensitive composition was not filled in the spaces between the wires.
[0127] (2) Heat resistance
[0128] The samples obtained in the test body preparation step were subjected to a peeling test using a transparent tape after being immersed in a solder bath at 260°C for 30 seconds according to the test method of JIS C-6481. This was repeated 1 to 3 times as one cycle, and the state of the coating was visually observed and evaluated according to the following criteria.
[0129] ◎: No change was observed in the coating film even after 3 cycles were repeated.
[0130] ○: Slight change was observed in the coating film after 3 cycles were repeated.
[0131] △: Changes were observed in the coating film after repeating 2 cycles.
[0132] ×: Peeling was observed in the coating film after one cycle was repeated.
[0133] (3) Clarity (minimum development line width)
[0134] According to the test body preparation process described above, exposure was performed from above a negative film designed to have a line width of 100 to 800 μm, and the width of the line that could be formed (remaining) after alkali development was observed and evaluated as the resolution.
[0135] It should be noted that, in the case of spray coating, the viscosity of the first photosensitive resin composition and the second photosensitive resin composition is a value measured using an Iwata cup at 25°C. In addition, in the case of screen printing coating, the viscosity of the second photosensitive resin composition is a value measured using a Brookfield B-type viscometer at 25°C. In addition, to the first photosensitive resin composition and the second photosensitive resin composition having the formulation of Table 1 below, a small amount of a reactive diluent in Table 1 below was further added immediately before the test body was prepared, thereby adjusting the viscosity of the first photosensitive resin composition and the second photosensitive resin composition shown in Table 1 below. For the viscosity adjustment immediately before the test body was prepared, NK-2 (ANEST IWATA Corporation) was used when measuring the viscosity using an Iwata cup, and a Brookfield B-type viscometer (sample temperature 25°C, rotation speed 50 rpm, Brookfield Corporation) was used when measuring the rotational viscosity.
[0136] The evaluation results are shown in Table 1 below.
[0137] [Table 1]
[0138]
[0139] According to Table 1, in Examples 1 to 5, a first photosensitive resin composition having a viscosity of 20 seconds when measured by an Iwata cup is sprayed on a substrate having a conductor with a thickness of 200 μm to 300 μm to form a first coating film having a film thickness after drying that is less than or equal to the thickness of the conductor (in the example, a thickness that is 20 μm less than the thickness of the conductor), and then a second photosensitive resin composition having a higher viscosity than the first photosensitive resin composition is applied on the surface of the first coating film in such a manner that the total film thickness after drying of the first coating film and the film thickness after drying of the second coating film is greater than the thickness of the conductor to form a second coating film. Thus, a protective film having excellent embedding properties and heat resistance between lines can be formed. In addition, in Examples 1 to 5, the clarity is also excellent.
[0140] In particular, it can be seen from Examples 1 and 2 that when the second photosensitive resin composition having a viscosity of 90 seconds when measured by an Iwata cup is sprayed, the embedding property between lines is further improved. In addition, it can be seen from Examples 1 and 4 that if a colorant is not added to the first coating film, the heat resistance and clarity of the protective film are further improved. In addition, according to Examples 1 and 3, if a polyacid-modified free radical polymerizable unsaturated monocarboxylic acid epoxy resin to which a free radical polymerizable unsaturated group is further added is used as the carboxyl group-containing photosensitive resin of the first photosensitive resin composition, the photocurability of the first coating film is improved, and the heat resistance and clarity of the protective film are further improved.
[0141] On the other hand, in Comparative Example 1 in which the first photosensitive resin composition having a viscosity of 60 seconds when measured by an Iwata cup was sprayed, the protective film did not obtain heat resistance. In Comparative Example 2 in which a first coating film was formed by screen printing a photosensitive resin composition of 180 dPa·s, the photosensitive composition did not fill the spaces between the lines, and heat resistance was not obtained. In Comparative Example 3 in which a protective film was formed by spraying a photosensitive resin composition having a viscosity of 20 seconds when measured by an Iwata cup, sagging occurred, and the photosensitive composition did not fill the spaces between the lines.
[0142] Industrial Applicability
[0143] The method for manufacturing a wiring board with a protective film of the present invention can prevent the generation of gaps in the protective film even if the protective film is filled between thick conductors formed on the wiring board, and can impart excellent heat resistance even if the protective film is formed on the thick conductor. Therefore, it has high utilization value, for example, in the field of providing an insulating film such as a solder resist film on a printed wiring board having a thick conductor with a thickness of 150 μm or more.
Claims
1. A method for manufacturing a wiring board having a protective film, wherein include: A first coating film forming step, wherein a first coating film is formed by spraying a first photosensitive resin composition on a wiring board having a substrate and a conductor provided on the substrate, wherein the viscosity of the first photosensitive resin composition is 10 seconds or more and 50 seconds or less when measured by an Iwata cup, the thickness of the first coating film after drying is less than or equal to the thickness of the conductor, and in the first coating film forming step, the step of spraying the first photosensitive resin composition and then drying is performed multiple times, so that the first coating film is formed into a structure in which multiple layers of the first photosensitive resin composition are stacked. A second coating film forming step, wherein a second photosensitive resin composition having a high viscosity of 80 seconds or more and 100 seconds or less when measured by an Iwata cup is applied on the surface of the first coating film to form the second coating film, wherein the total thickness of the first coating film after drying and the thickness of the second coating film after drying is greater than the thickness of the conductor, The conductor is a thick conductor having a thickness of 150 μm or more.
2. The method for manufacturing a wiring board having a protective film according to claim 1, in, The second coating film is formed by spraying the second photosensitive resin composition.
3. The method for manufacturing a wiring board having a protective film according to claim 1 or 2, in, The viscosity of the first photosensitive resin composition is 10 seconds or more and 30 seconds or less when measured with an Iwata cup.
4. The method for manufacturing a wiring board having a protective film according to any one of claims 1 to 3, in, The first coating film does not contain a colorant.
5. The method for manufacturing a wiring board having a protective film according to any one of claims 1 to 4, in, In the first coating film forming step, a film thickness of the first coating film after drying is smaller than a thickness of the conductor by 5.0 μm or more and 30 μm or less.
6. The method for manufacturing a wiring board having a protective film according to any one of claims 1 to 5, in, The protective film is composed of the first coating film and the second coating film.
7. The method for manufacturing a wiring board having a protective film according to any one of claims 1 to 6, in, The first coating film has a thickness of 100 μm or more and 250 μm or less after drying, and the second coating film has a thickness of 20 μm or more after drying.
8. The method for manufacturing a wiring board having a protective film according to any one of claims 1 to 7, in, The first photosensitive resin composition and the second photosensitive resin composition include (A) a photosensitive resin containing a carboxyl group, (B) a photopolymerization initiator, (C) a reactive diluent, (D) an epoxy compound, and (E) a non-reactive diluent.
Citation Information
Patent Citations
Printed circuit board with thick wiring circuit, and its production
JP2008078595A
Printed circuit board and method of manufacturing printed circuit board
CN107801316A
Method for formation of solder resist film
JP1998244206A