A high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material and preparation method thereof
By using a composite structure of graphene-coated styrene-butadiene rubber microspheres, the problems of toughening and damping of epoxy resin materials have been solved, achieving efficient energy dissipation and performance improvement, and making it suitable for various resin processing molding processes and industrial production.
Patent Information
- Application Number
- CN202111482901.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-12-07
AI Technical Summary
Existing epoxy resin materials have shortcomings in terms of toughening and damping performance. In particular, the direct addition of graphene leads to increased viscosity and agglomeration problems, and the energy dissipation mechanism is simple, making it difficult to significantly improve toughness and damping performance.
By constructing a composite structure of graphene-coated styrene-butadiene rubber microspheres, a graphene/styrene-butadiene rubber/epoxy resin composite material was prepared by spray drying. Graphene was enriched at the interface between the rubber and the resin, forming a constrained damping microstructure, which combined multiple energy dissipation mechanisms of graphene and rubber.
The toughness and damping properties of epoxy resin-based composite materials are significantly improved. The synergistic effect of graphene and rubber particles effectively enhances the energy dissipation capacity of the material, achieving high toughness and high damping effect.
Smart Images

Figure HDA0003396080420000011 
Figure HDA0003396080420000012
Abstract
Description
Technical Field
[0001] The invention relates to the field of nano-carbon composite materials, in particular to a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material and a preparation method thereof. Background Art
[0002] Epoxy resin and epoxy-based composite materials are widely used in chemical, aviation, aerospace, military and other high-tech fields due to their excellent physical and chemical properties and good processing properties. Epoxy resin has high mechanical strength due to its high density of cured crosslinking, but it also has poor impact toughness and damping and vibration reduction performance due to its high crosslinking density, which makes it difficult to meet the requirements of modern technological development, limiting its wide application. Therefore, the research on toughening and damping performance improvement of epoxy resin has always been a hot topic in the fields of industry and scientific research at home and abroad.
[0003] The key to controlling the toughness and damping properties of materials lies in the regulation and conversion of the energy of the system under the action of external loads. Adding rubber elastic particles to epoxy resin to increase energy dissipation is currently the most commonly used and effective method. Rubber elastic particles are highly flexible in their molecular chains and are prone to interchain slippage, which leads to energy dissipation. In addition, they can dissipate a large amount of energy in the resin matrix by inducing silver streaks and shear bands, thereby making the epoxy resin exhibit excellent impact toughness and viscoelastic damping properties. However, the introduction of rubber particles leads to a significant decrease in the tensile strength and shear modulus of epoxy resin. In order to avoid the problem of significant decrease in resin strength, people have tried to toughen epoxy resin with inorganic rigid particles. In recent years, graphene has become the most promising reinforcing and toughening filler with its significant advantages such as high strength, high specific surface area and nanoscale characteristics. Studies have shown that graphene squeezes and slides each other during deformation, and a large amount of energy dissipation is generated due to friction. In addition, the introduction of graphene brings richer interfaces to the polymer matrix, allowing the material to generate high energy dissipation through relative sliding friction at the interface, opening up important ideas for the preparation and development of high-toughness and high-damping materials. However, the direct addition of graphene powder usually significantly increases the viscosity of the resin, leading to many problems such as graphene filler agglomeration and poor dispersibility. More importantly, the current enhancement of polymer toughness and damping performance by graphene mostly relies on friction and slip between the graphene and polymer interfaces, which leads to energy dissipation. The energy consumption mechanism is single, and the effect of improving the toughness and damping performance of epoxy resin is not significant. Therefore, how to give full play to the energy consumption mechanism of graphene and rubber particles so that the two can work together is the key to obtaining high-toughness, high-damping epoxy resin materials with excellent comprehensive performance. Summary of the invention
[0004] The object of the present invention is to provide a graphene / styrene-butadiene rubber / epoxy resin composite material with high toughness and high damping characteristics and a preparation method thereof. The preparation method constructs a composite structure of graphene-coated styrene-butadiene rubber microspheres, effectively regulates the enrichment of graphene at the interface between rubber and resin, and forms a constrained damping microstructure between the graphene sheet and the rubber microspheres, fully utilizes the friction and sliding energy consumption of graphene at the modulus mismatch interface, the constraining effect of graphene on the rubber elastomer, and the high damping and high toughness of the rubber material itself, so that the energy consumption mechanism of graphene and rubber particles can be fully utilized and effectively coordinated, thereby significantly improving the toughness and damping performance of the epoxy resin-based composite material.
[0005] The technical solution of the present invention is:
[0006] A high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises, by weight, 50-80 parts of epoxy resin, 15-40 parts of curing agent, and 0.1-5 parts of composite microspheres of styrene-butadiene rubber wrapped with graphene.
[0007] The high-toughness and high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises composite microspheres of styrene-butadiene rubber wrapped with graphene, wherein the graphene is reduced graphene oxide, the diameter of the flakes of which is 100nm-5μm, and the atomic percentage of oxygen is 2%-30%; the raw material used for the reduced graphene oxide is graphene oxide prepared by chemical oxidation or electrolytic graphite oxidation, the atomic percentage of oxygen is 30%-60%, the diameter of the flakes is 100nm-5μm, and the number of flakes is 1-10.
[0008] The high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises composite microspheres of styrene-butadiene rubber wrapped with graphene, wherein the styrene-butadiene rubber is styrene-butadiene rubber microspheres with a diameter of 1 to 5 μm obtained by spray drying using styrene-butadiene rubber latex as a raw material.
[0009] The high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises composite microspheres of graphene wrapped in styrene-butadiene rubber, graphene being coated on the surface of the styrene-butadiene rubber microspheres, the weight of the graphene accounting for 0.5% to 30% of the total weight of the composite microspheres, and the diameter of the composite microspheres being 1 to 5 μm.
[0010] The high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material has an amine curing agent as the curing agent, including one or more of ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, and diethylaminopropylamine.
[0011] The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises the following steps:
[0012] (1) Preparation of graphene-wrapped styrene-butadiene rubber composite microspheres
[0013] a. After diluting the styrene-butadiene rubber latex, adding the vulcanization accelerator, stirring for 0.5 to 2 hours, and then obtaining styrene-butadiene rubber microspheres with a particle size distribution of 1 to 5 μm by spray drying;
[0014] b. Using graphene oxide as a raw material, dispersing graphene oxide in deionized water, and obtaining a stably dispersed graphene oxide aqueous dispersion by ultrasonic treatment; dropping hydrazine hydrate and ammonia water into the dispersion, placing the dispersion in an oil bath at 70 to 110° C. for reaction for 0.5 to 2 hours; after the reaction, adding a surfactant, and ultrasonically dispersing for 20 to 50 minutes to obtain a uniform and stable reduced graphene oxide aqueous dispersion;
[0015] c. adding the styrene-butadiene rubber microspheres prepared in step a to the reduced graphene oxide aqueous dispersion prepared in step b, wherein the mass ratio of the styrene-butadiene rubber microspheres to the reduced graphene oxide aqueous dispersion is 1:100 to 1:1000 (preferably 1:150 to 1:600), ultrasonically dispersing until uniform, and obtaining graphene-wrapped styrene-butadiene rubber composite microspheres by spray drying;
[0016] (2) Weigh 50 to 80 parts by weight of epoxy resin, add 0.1 to 5 parts of the composite microspheres of graphene wrapped in styrene-butadiene rubber obtained in step (1), and perform ultrasonic treatment until the microspheres are uniformly dispersed; add 15 to 40 parts of a curing agent, and stir evenly; vacuumize to remove bubbles, and perform curing to obtain a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material.
[0017] The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises the following steps: in step (1) a, the styrene-butadiene rubber emulsion is diluted with water to make its solid content 0.5wt% to 20wt%; based on 100 parts of the styrene-butadiene rubber mass, the vulcanization aids are: 0.5 to 5 parts of sulfur powder, 1 to 10 parts of zinc oxide, 0.3 to 3 parts of stearic acid, and 0.5 to 5 parts of dibenzothiazole disulfide.
[0018] The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises the following steps: in step (1) b, the solid content of the graphene oxide aqueous dispersion is 0.01-0.1wt%; hydrazine hydrate and ammonia water are added dropwise to the dispersion, wherein the hydrazine hydrate accounts for 0.01-0.03wt% of the dispersion, and the ammonia water accounts for 0.05-0.3wt% of the dispersion; after the reaction is completed, the surfactant added is sodium dodecylbenzene sulfonate, and the surfactant accounts for 0.02-0.2wt% of the aqueous dispersion obtained by the reaction.
[0019] The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material, in step (1) a and step (1) c, the spray drying parameters are: adjusting the inlet temperature to 70-200° C., the annular air volume to 25-45 m 3 / h, the feed rate is 10~1000mL / h, and the compressed air flow rate is 300~1200L / h.
[0020] The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises the following steps: curing is performed according to corresponding conditions: first curing at room temperature for 24 to 48 hours, and then curing at 50 to 70° C. for 5 to 10 hours.
[0021] The design concept of the present invention is:
[0022] Focusing on the key issues of epoxy resin's poor impact toughness and damping vibration reduction performance. The present invention proposes a novel method for preparing a graphene / styrene-butadiene rubber / epoxy resin composite material with high toughness and high damping characteristics. The present invention uses secondary spray drying technology to obtain a composite microsphere structure of styrene-butadiene rubber wrapped with graphene, and the composite microsphere is used as an additive to compound with an epoxy resin matrix. The obtained epoxy resin composite material has the remarkable characteristics of high toughness and high damping performance, which is mainly attributed to the following points: On the one hand, graphene is enriched in large quantities at the interface between rubber elastomer and epoxy resin, and deformation is easily generated at the interface with modulus mismatch, resulting in interlayer slippage and thus dissipating a large amount of energy; on the other hand, the graphene layer is coated on the surface of the rubber elastomer microsphere to form a constrained damping microstructure, so that graphene can restrain the movement of rubber molecular chains while enhancing the mechanical properties of rubber particles, thereby increasing friction energy consumption. In addition, the high damping and high toughness of the rubber elastic particles themselves are effectively utilized. The functional and structural properties of graphene and rubber particles are fully utilized, and multiple energy dissipation mechanisms work synergistically to achieve a significant improvement in the toughness and damping properties of epoxy resin-based composites.
[0023] Significantly different from the traditional modification methods such as introducing rubber particles, inorganic rigid particles, polymer core-shell particles, etc., the present invention designs composite microspheres with graphene rigid sheets as the shell and rubber elastic particles as the core through a secondary spray drying method, fully combining the unique advantages of traditional rubber and new inorganic nanomaterials, and constructing a constrained microstructure of graphene / rubber elastomer. The presence of graphene nanosheets not only helps the system dissipate a large amount of energy, but also can maintain the excellent mechanical properties of the resin itself. In addition, graphene has an isolating effect on rubber particles, and the obtained composite microspheres have uniform particle size and excellent dispersibility in epoxy resin. The toughness and damping performance of the resin can be effectively improved at a relatively low addition amount, providing a new idea for the design of high-toughness and high-damping epoxy resin materials. The preparation method is simple and efficient, has good repeatability, strong universality, and is suitable for industrial production.
[0024] The advantages and beneficial effects of the present invention are:
[0025] 1. The present invention utilizes a spray drying method to mix reduced graphene oxide and rubber microspheres uniformly dispersed in an aqueous solution and then directly dry them into powder, thereby effectively avoiding the problem of graphene being easily agglomerated when directly dispersed into epoxy resin, and accurately controlling the distribution of graphene at the interface between rubber and resin, thereby effectively utilizing the large amount of energy consumption caused by sliding friction of graphene sheets.
[0026] 2. The present invention designs composite microspheres with graphene rigid sheets as the outer shell and rubber particles as the inner core by a secondary spray drying method, which fully combines the unique energy consumption advantages of traditional rubber and new graphene two-dimensional nanomaterials. In addition to its own friction and sliding energy consumption, the graphene sheets are also coated on the surface of the rubber microspheres to form a constrained damping microstructure, so that while the graphene enhances the mechanical properties of the rubber particles, it can restrain the movement of the rubber molecular chain and thus increase the friction energy consumption. In addition, the high damping and high toughness of the rubber elastic particles themselves are effectively utilized. The functional and structural characteristics of graphene and rubber particles are fully utilized, and multiple energy consumption mechanisms work synergistically to achieve a significant improvement in the toughness and damping performance of epoxy resin-based composite materials.
[0027] 3. The composite microspheres obtained by the spray drying method of the present invention have uniform particle sizes, concentrated in 1 to 3 μm, and have excellent dispersibility in epoxy resin. The toughness and damping performance of the resin can be effectively improved at a relatively low addition amount.
[0028] 4. The present invention utilizes mature spray drying technology, which is simple, efficient, and has good repeatability. In addition, the epoxy resin always maintains good processing fluidity during the processing. Therefore, the present invention is generally applicable to a variety of resin processing and molding processes, as well as large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The SEM photograph of the styrene-butadiene rubber microspheres prepared in Example 1. The right picture is a further enlarged picture of the left picture.
[0030] Figure 2 This is a SEM photo of the composite microspheres of styrene-butadiene rubber wrapped by secondary spraying graphene prepared in Example 1. The right picture is a further enlarged picture of the left picture. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. The above are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
[0032] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the present invention in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.
[0033] In the specific implementation process, the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material and its preparation method of the present invention first use styrene-butadiene rubber emulsion as raw material to prepare styrene-butadiene rubber microspheres by spray drying; then the styrene-butadiene rubber microspheres are mixed with graphene dispersion and spray dried for a second time to obtain graphene-wrapped styrene-butadiene rubber composite microspheres; finally, the composite microsphere powder is directly dispersed in an epoxy resin matrix, and the graphene / styrene-butadiene rubber / epoxy resin composite material is obtained after curing. By regulating the interaction between the components of the composite material and coordinating the restraining effect of graphene on the rubber elastomer, not only the impact toughness of the epoxy resin composite material can be significantly enhanced, but also the damping vibration performance of the composite material can be significantly increased.
[0034] The high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises, by weight, 50-80 parts of epoxy resin, 15-40 parts of curing agent, and 0.1-5 parts of composite microspheres of styrene-butadiene rubber wrapped with graphene. Preferably, 60-70 parts of epoxy resin, 25-35 parts of curing agent, and 0.1-2 parts of composite microspheres of styrene-butadiene rubber wrapped with graphene. In the composite microspheres of styrene-butadiene rubber wrapped with graphene, the graphene is reduced graphene oxide, the diameter of the lamellae is 100nm-5μm, and the atomic percentage of oxygen is 2%-30%; preferably, the diameter of the lamellae is 1μm-3μm, and the atomic percentage of oxygen is 10%-25%. The raw material used for the reduced graphene oxide is graphene oxide obtained by chemical oxidation or electrolytic graphite oxidation, the atomic percentage of oxygen element is 30% to 60%, the diameter of the sheet is 100nm to 5μm, and the number of sheets is 1 to 10; preferably, the atomic percentage of oxygen element is 40% to 50%, the diameter of the sheet is 1μm to 3μm, and the number of sheets is 1 to 3. Styrene butadiene rubber is a styrene butadiene rubber microsphere with a diameter of 1 to 5μm obtained by spray drying with styrene butadiene rubber latex as raw material; graphene is coated on the surface of the styrene butadiene rubber microsphere, the weight of graphene accounts for 0.5% to 30% (preferably 5% to 10%) of the total weight of the composite microsphere, and the size of the composite microsphere is 1 to 5μm.
[0035] The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises the following steps:
[0036] (1) Preparation of graphene-wrapped styrene-butadiene rubber composite microspheres
[0037] a. Add vulcanization aids to the diluted styrene-butadiene rubber latex, stir thoroughly for 0.5 to 2 hours, and then obtain styrene-butadiene rubber microspheres with a particle size distribution of 1 to 5 μm by spray drying. The solid content of the styrene-butadiene rubber latex is 0.5wt% to 20wt%; based on 100 parts of styrene-butadiene rubber, the vulcanization aids are: 0.5 to 5 parts of sulfur powder, 1 to 10 parts of zinc oxide, 0.3 to 3 parts of stearic acid, and 0.5 to 5 parts of dibenzothiazole disulfide. The parameters of spray drying are: adjust the inlet temperature to 70 to 200°C, the circulating air volume to 25 to 45m 3 / h, the feed rate is 10~1000mL / h, and the compressed air flow rate is 300~1200L / h.
[0038] b. Using graphene oxide (GO) as raw material, GO is dispersed in deionized water, and a stable GO aqueous dispersion is obtained by ultrasonication, wherein the solid content of the GO aqueous dispersion is 0.01-0.1wt%; hydrazine hydrate and ammonia water are added dropwise to the GO aqueous dispersion, wherein the hydrazine hydrate accounts for 0.01-0.03wt% of the GO aqueous dispersion, and the ammonia water accounts for 0.05-0.3wt% of the GO aqueous dispersion, and the dispersion is placed in an oil bath at 70-110°C for reaction for 0.5-2h. After the reaction is completed, a surfactant is added to the dispersion, wherein the surfactant is sodium dodecylbenzene sulfonate, and the surfactant accounts for 0.02-0.2wt% of the aqueous dispersion obtained by the reaction, and after ultrasonic dispersion for 20-50 minutes, a uniform and stable aqueous dispersion of reduced graphene oxide is obtained.
[0039] c. Add a certain amount of the reduced graphene oxide aqueous dispersion prepared in step b to the styrene butadiene rubber microspheres prepared in step a, perform ultrasonic treatment until the dispersion is uniform, and then spray dry the microspheres to obtain the graphene-wrapped styrene butadiene rubber composite microspheres. The spray drying parameters are: adjust the inlet temperature to 70-200°C, the circulating air volume to 25-45m 3 / h, the feed rate is 10~1000mL / h, and the compressed air flow rate is 300~1200L / h.
[0040] (2) Weigh 50 to 80 parts by weight of epoxy resin, add 0.1 to 5 parts of the composite microspheres of graphene wrapped in styrene-butadiene rubber obtained in step (1), and perform ultrasonic treatment until the microspheres are uniformly dispersed; add 15 to 40 parts of a curing agent, and stir evenly; vacuumize to remove bubbles, and perform curing according to corresponding conditions to obtain a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material.
[0041] The present invention is further described below with reference to the embodiments, but the invention is not limited to the embodiments:
[0042] Example 1
[0043] In this embodiment, the preparation method of the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material is as follows:
[0044] (1) Preparation of graphene-wrapped styrene-butadiene rubber composite microspheres
[0045] a. Dilute the styrene-butadiene rubber latex with deionized water to a solid content of 2wt% and a volume of 500mL. Weigh 3g of sulfur powder, 5g of zinc oxide, 1.5g of stearic acid, and 3g of dibenzothiazole disulfide, disperse them in the styrene-butadiene rubber latex, and stir thoroughly for 1h. Use a spray drying device, adjust the inlet temperature to 120℃, and the circulating air volume to 35m 3 / h, feed rate is 200mL / h, compressed air flow rate is 900L / h. Figure 1The particle size distribution of styrene-butadiene rubber microspheres is 1 to 5 μm.
[0046] b. Using graphene oxide (GO) as raw material, weigh 10g of GO slurry (commercially available product, i.e., a GO aqueous solution with a certain concentration) with a concentration of 10mg / mL and disperse it in 300mL of deionized water, and obtain a stably dispersed GO aqueous dispersion by ultrasonication; add 60μL of hydrazine hydrate and 1mL of ammonia water to the GO aqueous dispersion, and place it in an oil bath at 100℃ for 1h. After the reaction is completed, add 200mg of sodium dodecylbenzene sulfonate to the obtained dispersion, and after ultrasonic dispersion for 30 minutes, a uniform and stable aqueous dispersion of reduced graphene oxide is obtained.
[0047] c. Weigh 3 g of styrene-butadiene rubber microspheres prepared in step a, add them to the reduced graphene oxide aqueous dispersion prepared in step b, and perform ultrasonic treatment until the dispersion is uniform. Use a spray drying device and adjust the inlet temperature to 120°C and the circulating air volume to 35 m 3 / h, feed rate is 200mL / h, compressed air flow rate is 900L / h. Spray drying can be used again to obtain Figure 2 The composite microspheres of styrene-butadiene rubber wrapped with graphene have a particle size distribution of 1 to 5 μm, wherein the weight of the graphene accounts for 3.2% of the total weight of the composite microspheres.
[0048] (2) Weigh 30 g of epoxy resin, add 130 mg of the graphene-wrapped styrene-butadiene rubber composite microspheres obtained in step (1), and perform ultrasonic treatment until uniform dispersion; add 12 g of triethylenetetramine, a curing agent, and stir evenly; evacuate to remove bubbles, cure at room temperature for 36 h, and then cure at 60° C. for 6 h, to finally obtain a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material with a composite microsphere addition amount of 0.3 wt %.
[0049] (3) The prepared graphene / styrene-butadiene rubber / epoxy resin composite material was subjected to notch impact toughness test according to ASTM D 6110-10, and the impact strength can reach 18 kJ / m 2 , which is 50% higher than pure epoxy. The dynamic thermomechanical properties of the prepared graphene / styrene-butadiene rubber / epoxy resin composite material were tested. At room temperature of 27°C, the tanδ of the composite material increased by 27% compared with pure epoxy. The cantilever beam vibration damping performance test of the prepared graphene / styrene-butadiene rubber / epoxy resin composite material was carried out. The damping ratio of the composite material increased by 35% compared with pure epoxy.
[0050] Example 2
[0051] In this embodiment, the preparation method of the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material is as follows:
[0052] (1) Preparation of graphene-wrapped styrene-butadiene rubber composite microspheres
[0053] a. Dilute the styrene-butadiene rubber latex with deionized water to a solid content of 5wt% and a volume of 200mL. Weigh 1.5g sulfur powder, 5g zinc oxide, 2g stearic acid, and 4g dibenzothiazole disulfide, disperse them in the styrene-butadiene rubber latex, and stir thoroughly for 1.5h. Use a spray drying device, adjust the inlet temperature to 150℃, and the circulating air volume to 42m 3 / h, the feed rate is 100mL / h, and the compressed air flow rate is 1000L / h. The styrene-butadiene rubber microspheres with a particle size distribution of 1 to 5μm are obtained by spray drying.
[0054] b. Using graphene oxide (GO) as raw material, weigh 20g of GO slurry (commercially available product, i.e., GO aqueous solution with a certain concentration) with a concentration of 10mg / mL and disperse it in 300mL of deionized water, and obtain a stably dispersed GO aqueous dispersion by ultrasonication; add 100μL of hydrazine hydrate and 1.8mL of ammonia water to the GO aqueous dispersion, and place it in an oil bath at 110℃ for 1.5h. After the reaction is completed, add 400mg of sodium dodecylbenzene sulfonate to the obtained dispersion, and after ultrasonic dispersion for 40 minutes, a uniform and stable aqueous dispersion of reduced graphene oxide is obtained.
[0055] c. Weigh 1 g of the styrene-butadiene rubber microspheres prepared in step a, add them to the reduced graphene oxide aqueous dispersion prepared in step b, and perform ultrasonic treatment until the dispersion is uniform. Use a spray drying device and adjust the inlet temperature to 150°C and the circulating air volume to 42 m 3 / h, feed rate is 100mL / h, compressed air flow rate is 1000L / h. Spray drying can be used again to obtain Figure 2 The composite microspheres of styrene-butadiene rubber wrapped with graphene have a particle size distribution of 1 to 5 μm, wherein the weight of the graphene accounts for 16.7% of the total weight of the composite microspheres.
[0056] (2) Weigh 10 g of epoxy resin, add 100 mg of the graphene-wrapped styrene-butadiene rubber composite microspheres obtained in step (1), and ultrasonicate until uniformly dispersed; add 4 g of curing agent triethylenetetramine, and stir evenly; vacuumize to remove bubbles, cure at room temperature for 48 hours, and then place at 60° C. to cure for 6 hours, and finally obtain a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material with a composite microsphere addition amount of 0.7 wt%.
[0057] (3) The prepared graphene / styrene-butadiene rubber / epoxy resin composite material was subjected to notch impact toughness test according to ASTM D 6110-10, and the impact strength can reach 20 kJ / m 2, which is 67% higher than pure epoxy. The dynamic thermomechanical properties of the prepared graphene / styrene-butadiene rubber / epoxy resin composite material were tested. At room temperature of 27°C, the tanδ of the composite material increased by 22% compared with pure epoxy. The cantilever beam vibration damping performance of the prepared graphene / styrene-butadiene rubber / epoxy resin composite material was tested. The damping ratio of the composite material increased by 31% compared with pure epoxy.
[0058] The results of the examples show that the present invention uses secondary spray drying technology to obtain a composite microsphere structure with graphene wrapped in styrene-butadiene rubber, and the composite microsphere is compounded with an epoxy resin matrix as an additive, and the prepared graphene / styrene-butadiene rubber / epoxy resin composite material has significantly improved impact toughness and damping performance, and is only accompanied by a slight loss of mechanical modulus. The present invention fully combines the unique energy consumption advantages of traditional rubber and new graphene two-dimensional nanomaterials, and the obtained composite microspheres have uniform particle size, excellent dispersibility, and can effectively improve the toughness and damping performance of the resin at a relatively low addition, providing a new idea for the design of high-toughness and high-damping epoxy resin materials. In addition, the preparation method provided by the present invention is simple and efficient, has good repeatability, and strong universality, is suitable for large-scale production, and has important application prospects in the field of high-performance resin materials.
[0059] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material, characterized in that: The invention comprises, by weight, 50 to 80 parts of epoxy resin, 15 to 40 parts of curing agent, and 0.1 to 5 parts of composite microspheres of styrene-butadiene rubber wrapped with graphene; The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material comprises the following steps: (1) Preparation of graphene-wrapped styrene-butadiene rubber composite microspheres a. After diluting the styrene-butadiene rubber latex, adding the vulcanization accelerator, stirring for 0.5 to 2 hours, and then obtaining styrene-butadiene rubber microspheres with a particle size distribution of 1 to 5 μm by spray drying; b. Using graphene oxide as a raw material, dispersing graphene oxide in deionized water, and obtaining a stably dispersed graphene oxide aqueous dispersion by ultrasonic treatment; dropping hydrazine hydrate and ammonia water into the dispersion, placing the dispersion in an oil bath at 70 to 110° C. for reaction for 0.5 to 2 hours; after the reaction, adding a surfactant, and ultrasonically dispersing for 20 to 50 minutes to obtain a uniform and stable reduced graphene oxide aqueous dispersion; c. adding the styrene-butadiene rubber microspheres prepared in step a to the reduced graphene oxide aqueous dispersion prepared in step b, wherein the mass ratio of the styrene-butadiene rubber microspheres to the reduced graphene oxide aqueous dispersion is 1:100 to 1:1000, performing ultrasonic treatment until the dispersion is uniform, and obtaining graphene-wrapped styrene-butadiene rubber composite microspheres by spray drying; (2) Weigh 50 to 80 parts by weight of epoxy resin, add 0.1 to 5 parts of the composite microspheres of graphene wrapped in styrene-butadiene rubber obtained in step (1), and perform ultrasonic treatment until the microspheres are uniformly dispersed; add 15 to 40 parts of a curing agent, and stir evenly; vacuumize to remove bubbles, and perform curing to obtain a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material.
2. The high toughness, high damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 1, characterized in that: In the composite microspheres of graphene wrapped with styrene-butadiene rubber, the graphene is reduced graphene oxide, the diameter of its flakes is 100nm-5μm, and the atomic percentage of oxygen is 2%-30%; the raw material used for the reduced graphene oxide is graphene oxide prepared by chemical oxidation or electrolytic graphite oxidation, the atomic percentage of oxygen is 30%-60%, the diameter of its flakes is 100nm-5μm, and the number of flakes is 1-10.
3. The high toughness, high damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 1, characterized in that: In the graphene-wrapped styrene-butadiene rubber composite microspheres, the styrene-butadiene rubber is styrene-butadiene rubber microspheres with a diameter of 1 to 5 μm obtained by using styrene-butadiene rubber latex as a raw material through a spray drying method.
4. The high toughness, high damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 1, characterized in that: In the composite microspheres of styrene-butadiene rubber wrapped with graphene, the graphene is coated on the surface of the styrene-butadiene rubber microspheres, the weight of the graphene accounts for 0.5% to 30% of the total weight of the composite microspheres, and the diameter of the composite microspheres is 1 to 5 μm.
5. The high toughness, high damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 1, characterized in that: The curing agent is an amine curing agent, including one or more of ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, and diethylaminopropylamine.
6. A method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material according to any one of claims 1 to 5, characterized in that: The steps include: (1) Preparation of graphene-wrapped styrene-butadiene rubber composite microspheres a. After diluting the styrene-butadiene rubber latex, adding the vulcanization accelerator, stirring for 0.5 to 2 hours, and then obtaining styrene-butadiene rubber microspheres with a particle size distribution of 1 to 5 μm by spray drying; b. Using graphene oxide as a raw material, dispersing graphene oxide in deionized water, and obtaining a stably dispersed graphene oxide aqueous dispersion by ultrasonic treatment; dropping hydrazine hydrate and ammonia water into the dispersion, placing the dispersion in an oil bath at 70 to 110° C. for reaction for 0.5 to 2 hours; after the reaction, adding a surfactant, and ultrasonically dispersing for 20 to 50 minutes to obtain a uniform and stable reduced graphene oxide aqueous dispersion; c. adding the styrene-butadiene rubber microspheres prepared in step a to the reduced graphene oxide aqueous dispersion prepared in step b, wherein the mass ratio of the styrene-butadiene rubber microspheres to the reduced graphene oxide aqueous dispersion is 1:100 to 1:1000, performing ultrasonic treatment until the dispersion is uniform, and obtaining graphene-wrapped styrene-butadiene rubber composite microspheres by spray drying; (2) Weigh 50 to 80 parts by weight of epoxy resin, add 0.1 to 5 parts of the composite microspheres of graphene wrapped in styrene-butadiene rubber obtained in step (1), and perform ultrasonic treatment until the microspheres are uniformly dispersed; add 15 to 40 parts of a curing agent, and stir evenly; vacuumize to remove bubbles, and perform curing to obtain a high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material.
7. The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 6, characterized in that: In step (1) a, the styrene-butadiene rubber emulsion is diluted with water to make its solid content 0.5wt% to 20wt%; based on 100 parts of the styrene-butadiene rubber, the vulcanization aids are: 0.5 to 5 parts of sulfur powder, 1 to 10 parts of zinc oxide, 0.3 to 3 parts of stearic acid, and 0.5 to 5 parts of dibenzothiazole disulfide.
8. The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 6, characterized in that: In step (1) b, the solid content of the graphene oxide aqueous dispersion is 0.01-0.1wt%; hydrazine hydrate and ammonia water are added dropwise to the dispersion, hydrazine hydrate accounts for 0.01-0.03wt% of the dispersion, and ammonia water accounts for 0.05-0.3wt% of the dispersion; after the reaction is completed, the added surfactant is sodium dodecylbenzene sulfonate, and the surfactant accounts for 0.02-0.2wt% of the aqueous dispersion obtained by the reaction.
9. The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 6, characterized in that: In step (1) a and step (1) c, the spray drying parameters are: adjusting the inlet temperature to 70-200°C, the circulating air volume to 25-45m 3 / h, the feed rate is 10~1000mL / h, and the compressed air flow rate is 300~1200L / h.
10. The method for preparing the high-toughness, high-damping graphene / styrene-butadiene rubber / epoxy resin composite material according to claim 6, characterized in that: In step (2), curing is performed according to corresponding conditions: first curing at room temperature for 24 to 48 hours, and then curing at 50 to 70° C. for 5 to 10 hours.
Citation Information
Cited By
Modified brominated butyl rubber composite damping material and preparation method thereof