A highly stable electroplating additive and preparation method thereof
By adding a specific composition of high-stability electroplating additive to the nickel plating electrolyte, the problem of large workload and insufficient stability caused by polishing and polishing of workpieces in the nickel plating process is solved, and the brightness and stability of the plating layer are achieved. Improve and reduce plating energy consumption and time.
Patent Information
- Application Number
- CN202211455891.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-21
AI Technical Summary
In the decorative nickel plating process, the existing nickel plating electrolyte has the problem of large workload caused by workpiece polishing and polishing, which cannot facilitate continuous processing, and lacks stability and brightness.
A high-stability electroplating additive is adopted, including copper sulfate pentahydrate, sulfuric acid, chloride ion, buffer, primary brightener, emulsifier, secondary brightener, softener, inhibitor, cylinder opening agent, fluorinated glyceryl ether and The carrier brightener is prepared by specific stirring and temperature control methods to form a high-stable electroplating additive to improve the plating performance.
It significantly improves the brightness and uniformity of the surface of the plating, reduces the energy consumption of electroplating, shortens the plating time, improves the stability and pass rate after nickel plating, and the additives are not easy to decompose in the plating solution, avoiding precipitation and discoloration.
Smart Images

Figure CN115787053B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electroplating additives, and in particular to a highly stable electroplating additive and a preparation method thereof. Background Art
[0002] As a surface processing technology for surface modification, electroplating has great flexibility. Different coatings can be applied on the surface of materials according to different requirements to meet different performance requirements, thus expanding the application range of metal materials. Therefore, electroplating has been widely used in various industrial production and scientific research fields. In the machinery manufacturing industry, electroplating is the main means of anti-corrosion and prolonging the service life of metal parts. In the chemical, petroleum industry and coastal, humid and hot areas, the losses caused by corrosion are very large, and the coating has strong corrosion resistance in such an environment. Because the electroplating process is simple and the cost is low, the anti-corrosion effect of electroplating in the petrochemical industry is more obvious. In addition, this makes the application of electroplating more extensive.
[0003] Another advantage of electroplating is that, in general, the coating is only a thin metal layer, ranging from a few microns to tens of microns, which can save a lot of precious metal materials. Compared with other surface treatment methods, electroplating process equipment is simple, operating conditions are easy to control, and it has great economic significance. Therefore, it has gradually developed into a manufacturing method for obtaining surface materials. Electroplating is an important form of deposition, and more than half of the metals in the periodic table can be deposited by electroplating. The electroplating process includes activation, cathode cleaning and plating 2~4. In recent decades, due to the widespread application of electroplating, a practical scientific engineering technology, in various industries, electroplating has developed from a technology to a precise science. Electroplating is an electrodeposition process, that is, the metal ions (or complex ions) in the electrolyte are reduced to metals (or alloys) on the cathode surface under the action of direct current. The metal plated on the substrate is provided by the metal electrolyzed in the electroplating solution. This requires that electroplating must meet two conditions: one is that the plating solution must contain ions of the metal to be plated; the other is that direct current must pass. The electroplating device mainly includes: a DC power supply; a solution that can conduct electric current and has a certain composition; two electrodes in contact with the electroplating solution, the plated part is hung on the cathode, and the anode is generally the metal to be covered.
[0004] The electroplating process is a method of plating a layer of metal on a conductor using the principle of electrolysis. During electroplating, the plating metal or other insoluble materials serve as the anode, and the workpiece to be plated serves as the cathode. The cations of the plating metal are reduced to a plating layer on the cathode surface. Through electroplating, the corrosion resistance, strength, hardness, wear resistance, conductivity, heat resistance and other properties of the cathode can be improved, and the surface can also be decoratively beautified. The multi-layer electroplating process is to perform several layers of electroplating with different materials on the same electroplated product. Multi-layer electroplating can not only reduce the thickness of the plating layer but also improve the performance of the plating layer. Nickel has good physical and chemical properties. It can not only play a role in mechanical protection, but also has electrochemical protection function. In addition, it can also be used as a plating layer for decorative appearance.
[0005] For example, Chinese patent CN109609979B discloses a multi-layer nickel electroplating additive for improving stability. The nickel plating process uses a smaller current density, which reduces energy consumption and shortens the electroplating time. After nickel plating, the brightening effect is good and the stability is high.
[0006] However, compared with other nickel plating systems, such as perchloride, aminosulfonate, citrate, pyrophosphate and fluoroborate type nickel plating electrolytes, there are obvious or certain limitations. The sulfate nickel plating system is the basis of many decorative nickel plating processes. The composition of its nickel plating electrolyte is simple, which cannot reduce the workload of workpiece grinding and polishing, and is not conducive to continuous processing.
[0007] Currently, no effective solution has been proposed for the problems in the related technologies. Summary of the invention
[0008] In view of the problems in the related art, the present invention proposes a highly stable electroplating additive and a preparation method thereof to overcome the above technical problems existing in the existing related art.
[0009] To this end, the specific technical solution adopted by the present invention is as follows:
[0010] According to one aspect of the present invention, a highly stable electroplating additive is provided, the additive comprising the following components in mass fractions:
[0011] 100-200 parts of copper sulfate pentahydrate;
[0012] Sulfuric acid 25-40 parts;
[0013] Chloride ion 40-80 parts;
[0014] Buffer 20-80 parts;
[0015] Primary brightener 6-12 parts;
[0016] Emulsifier 11-44 parts;
[0017] Secondary brightener 20-60 parts;
[0018] 20-25 parts of softener;
[0019] 1-10 parts of inhibitor;
[0020] 5-15 parts of tank opening agent;
[0021] 1-10 parts of fluorinated glyceryl ether;
[0022] Carrier brightener 60-100 parts;
[0023] 1-10 parts of microporous nickel additive.
[0024] Furthermore, the buffer includes boric acid, phosphoric acid, citric acid, carbonic acid, acetic acid and barbituric acid.
[0025] Furthermore, the primary brightener is an organic compound containing a =C-SO2- structure.
[0026] Furthermore, the emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0027] Furthermore, the secondary brightener includes 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener includes the following steps:
[0028] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0029] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0030] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0031] Furthermore, the softener includes ester quaternary ammonium salt, dialkyl quaternary ammonium salt, alkyl acyl quaternary ammonium salt, pyridinium quaternary ammonium salt type and imidazole type softener.
[0032] Furthermore, the cylinder opening agent includes an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0033] Wherein, the aldehyde compounds include acetaldehyde propylene glycol acetal, phenylpropyne aldehyde diacetaldehyde, - diketone compounds, dimethoxymethane, p-anisaldehyde, 2-furanoxyaldehyde, 2-methylpropanal and p-dimethylaminobenzaldehyde;
[0034] The manganese-containing compounds include manganese naphthenate, manganous anhydride, manganese anhydride, basic manganese oxide, manganese carbonate and permanganic anhydride.
[0035] Furthermore, the fluorinated glyceryl ethers include perfluorononene polyglyceryl ether, octafluorobiphenyl diglycidyl ether and hexafluorononyl glycidyl ether.
[0036] Furthermore, the carrier brightener is a non-ionic polyether compound.
[0037] According to another aspect of the present invention, a method for preparing a highly stable electroplating additive is also provided, the preparation method comprising the following steps:
[0038] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0039] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0040] S3, adding a buffer, a primary brightener, an emulsifier, and a secondary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0041] S4. Regulate the reaction temperature of the reactor to control the temperature at room temperature, and add softener, inhibitor, cylinder opening agent, fluorinated glyceryl ether and carrier brightener in sequence, and stir evenly to obtain a highly stable electroplating additive.
[0042] Boric acid: It is a white powdery crystal or a triclinic flaky shiny crystal with a smooth feel and no odor. It is soluble in water, alcohol, glycerin, ether and essential oils. The aqueous solution is weakly acidic. It is used in glass, enamel, ceramics, medicine, metallurgy, leather, dyes, pesticides, fertilizers, textiles and other industries.
[0043] Sodium alkylbenzene sulfonate: solid, soluble in water, active matter content 30%~40%, unsaponifiable matter content 3% (based on 100% active matter), pH value about 8, with surface activity of cleaning, wetting, foaming, emulsifying and dispersing.
[0044] Sodium allyl sulfonate: the third monomer of acrylic fiber, improves the dyeing performance of fiber, and makes the coloring firm. It is used as brightener for electroplating nickel, improves metal distribution ability and ductility, water treatment agent, and oilfield drilling mud additive.
[0045] Polyoxyethylene ether, also known as polyethylene oxide or polyethylene oxide, is a crystalline, thermoplastic water-soluble polymer. It is both a new type of water-soluble resin and a non-ionic surfactant. The demand for it in various industries is increasing. From the perspective of the developed fields, the production and application prospects of polyoxyethylene ether are broad.
[0046] Sodium propargyl sulfonate, electroplating brightener, can improve the brightness of the current density area, enhance the positioning force, leveling ability, and impurity tolerance;
[0047] 1,4-Butynediol: white or light yellow crystals, white rhombic crystals (light yellow after moisture absorption), solubility: soluble in water, acidic solution, ethanol and acetone, slightly soluble in chloroform, insoluble in benzene and ether, other properties: solid butynediol is easily deliquescent in air at 25 degrees, is toxic, has the chemical properties of dihydric primary alcohols, and can also undergo addition reactions.
[0048] Diethoxybutynediol: Amber viscous liquid with an alcohol-like odor.
[0049] Ester-based quaternary ammonium salt is a new type of cationic surfactant with excellent softening, antistatic and anti-yellowing properties. It does not contain APEO or formaldehyde, is easily biodegradable and environmentally friendly. It has a small dosage, good effect, convenient preparation, low overall cost and extremely high cost performance. It is the best substitute for dioctadecyl dimethyl ammonium chloride (D1821), film, softener, etc.
[0050] Dimethoxymethane: also known as dimethyl ether and methylal, is a colorless liquid with a chloroform-like odor. It is mainly used as a solvent and analytical reagent. It is irritating to the mucous membranes and has an anesthetic effect. Inhalation of vapor can cause irritation of the nose and throat. Inhalation of high concentrations can cause dizziness, etc. It is harmful to the eyes and the damage can last for several days. Long-term skin contact can cause dry skin.
[0051] p-Anisaldehyde: It is a colorless to light yellow liquid at room temperature, with a hawthorn-like odor. It is used to prepare the main fragrance of hawthorn flower fragrance. It can also be used in flower fragrances such as lilac, orchid, sunflower, acacia, mimosa, locust, magnolia, vanilla, sweet bean flower, and non-flower fragrances such as freshly cut grass, fragrant myrtle, and aldehyde fragrance. It can also be used in heavy wood fragrances such as sandalwood. It is also used in soap fragrances. It is used in food to sweeten and blend fragrances.
[0052] p-Dimethylaminobenzaldehyde: used as a dye intermediate, also used as a reagent for the determination of urobilin, indole, alkaloids, etc. and as a chromatographic analysis reagent.
[0053] Manganese carbonate: It is a raw material for manufacturing soft ferrites for telecommunication equipment, synthesizing manganese dioxide and manufacturing other manganese salts. It is used as a catalyst for desulfurization, a pigment for enamels, coatings and varnishes. It is also used as a fertilizer and feed additive. It is used in medicine, welding rod auxiliary materials, etc., and as a raw material for producing electrolytic manganese metal.
[0054] The beneficial effects of the present invention are:
[0055] 1. The present invention improves the performance of the plating solution and the coating to a great extent by adding emulsifiers, secondary brighteners, primary brighteners, carrier brighteners, etc., and the additives of the present invention will not produce inclusions in the coating, which can significantly improve the surface brightness of the coating and ensure the uniformity of the coating.
[0056] 2. The nickel plating process provided by the present invention containing the above-mentioned multi-layer nickel electroplating additive adopts a smaller current density, reduces energy consumption, and has a short electroplating time. After nickel plating, the brightening effect is good and the stability is high.
[0057] 3. The electroplating additive used in the present invention has extremely high stability, does not decompose in the plating solution, does not precipitate or discolor after multiple electroplatings and long-term storage, and ensures the brightness of the PCB board and the qualified rate of the PCB board after electroplating. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0059] Figure 1 is a flow chart of a method for preparing a highly stable electroplating additive according to an embodiment of the present invention;
[0060] Figure 2 It is a comparison chart of the hardness of PCB boards treated with electroplating additives prepared in Example 1, Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 in the experimental group;
[0061] Figure 3 It is a comparison chart of the current efficiency of PCB boards treated with electroplating additives prepared in Example 1, Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 in the experimental group;
[0062] Figure 4 It is a structural diagram of the primary brightener. DETAILED DESCRIPTION
[0063] To further illustrate each embodiment, the present invention provides drawings, which are part of the disclosure of the present invention and are mainly used to illustrate the embodiments and can be used in conjunction with the relevant descriptions in the specification to explain the operating principles of the embodiments. With reference to these contents, ordinary technicians in the field should be able to understand other possible implementations and advantages of the present invention. The components in the figures are not drawn to scale, and similar component symbols are generally used to represent similar components.
[0064] According to an embodiment of the present invention, a highly stable electroplating additive and a preparation method thereof are provided.
[0065] Embodiment 1
[0066] A highly stable electroplating additive, comprising the following components in mass fractions:
[0067] Copper sulfate pentahydrate 100g;
[0068] Sulfuric acid 25g;
[0069] Chloride ion 40g;
[0070] Buffer 20g;
[0071] Primary brightener 6g;
[0072] Emulsifier 11g;
[0073] Secondary brightener 20g;
[0074] Softener 20g;
[0075] Inhibitor 1g;
[0076] 5g of tank opening agent;
[0077] Fluorinated glyceryl ether 1g;
[0078] Carrier brightener 60g;
[0079] Microporous nickel additive 1g.
[0080] The buffer is boric acid.
[0081] The primary brightener is Figure 4 shown.
[0082] The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0083] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0084] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0085] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0086] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0087] The softener is an imidazole softener.
[0088] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0089] Wherein, the aldehyde compound is - diketone compounds;
[0090] The manganese-containing compound is permanganese anhydride.
[0091] The fluorine-containing glyceryl ether is perfluorononene polyglyceryl ether.
[0092] The carrier brightener is a non-ionic polyether compound.
[0093] Select the above raw materials with the mass fraction, and prepare the electroplating additive according to a preparation method of a highly stable electroplating additive, such as Figure 1 As shown, the preparation method comprises the following steps:
[0094] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0095] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0096] S3, adding a buffer, a primary brightener, an emulsifier, and a secondary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0097] S4. Regulate the reaction temperature of the reactor to control the temperature at room temperature, and add softener, inhibitor, cylinder opening agent, fluorinated glyceryl ether and carrier brightener in sequence, and stir evenly to obtain a highly stable electroplating additive.
[0098] Embodiment 2
[0099] A highly stable electroplating additive, comprising the following components in mass fractions:
[0100] Copper sulfate pentahydrate 150g;
[0101] Sulfuric acid 32.5 g;
[0102] Chloride ion 60g;
[0103] Buffer 50g;
[0104] Primary brightener 9g;
[0105] Emulsifier 27.5g;
[0106] Secondary brightener 40g;
[0107] Softener 22.5g;
[0108] Inhibitor 5.5 g;
[0109] 10g of tank opening agent;
[0110] Fluorinated glyceryl ether 5.5 g;
[0111] Carrier brightener 80g;
[0112] Microporous nickel additive 5.5g.
[0113] The buffer is boric acid.
[0114] The primary brightener is Figure 4 shown.
[0115] The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0116] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0117] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0118] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0119] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0120] The softener is an imidazole softener.
[0121] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0122] Wherein, the aldehyde compound is - diketone compounds;
[0123] The manganese-containing compound is manganese anhydride.
[0124] The fluorine-containing glyceryl ether is perfluorononene polyglyceryl ether.
[0125] The carrier brightener is a non-ionic polyether compound.
[0126] The raw materials with the above mass fractions are selected, and the electroplating additive is prepared according to a preparation method of a highly stable electroplating additive, which comprises the following steps:
[0127] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0128] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0129] S3, adding a buffer, a primary brightener, an emulsifier, and a secondary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0130] S4. Regulate the reaction temperature of the reactor to control the temperature at room temperature, and add softener, inhibitor, cylinder opening agent, fluorinated glyceryl ether and carrier brightener in sequence, and stir evenly to obtain a highly stable electroplating additive.
[0131] Embodiment 3
[0132] A highly stable electroplating additive, comprising the following components in mass fractions:
[0133] Copper sulfate pentahydrate 200g;
[0134] Sulfuric acid 40g;
[0135] Chloride ion 80g;
[0136] Buffer 80g;
[0137] Primary brightener 12g;
[0138] Emulsifier 44g;
[0139] Secondary brightener 60g;
[0140] Softener 25g;
[0141] Inhibitor 10g;
[0142] 15g of tank opening agent;
[0143] Fluorinated glyceryl ether 10g;
[0144] Carrier brightener 100g.
[0145] Microporous Nickel Additive 10g
[0146] The buffer is boric acid.
[0147] The primary brightener is Figure 4 shown.
[0148] The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0149] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0150] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0151] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0152] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0153] The softener is an ester-based quaternary ammonium salt.
[0154] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0155] Wherein, the aldehyde compound is acetaldehyde propylene glycol acetal;
[0156] The manganese-containing compound is manganese naphthenate.
[0157] The fluorine-containing glyceryl ether is octafluorobiphenyl diglycidyl ether.
[0158] The carrier brightener is fatty alcohol polyoxyethylene ether.
[0159] The raw materials with the above mass fractions are selected, and the electroplating additive is prepared according to a preparation method of a highly stable electroplating additive, which comprises the following steps:
[0160] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0161] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0162] S3, adding a buffer, a primary brightener, an emulsifier, and a secondary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0163] S4. Regulate the reaction temperature of the reactor to control the temperature at room temperature, and add softener, inhibitor, cylinder opening agent, fluorinated glyceryl ether and carrier brightener in sequence, and stir evenly to obtain a highly stable electroplating additive.
[0164] Comparative Example 1
[0165] A highly stable electroplating additive, comprising the following components in mass fractions:
[0166] Copper sulfate pentahydrate 100g;
[0167] Sulfuric acid 25g;
[0168] Chloride ion 40g;
[0169] Buffer 20g;
[0170] Primary brightener 6g;
[0171] Emulsifier 11g;
[0172] Secondary brightener 20g;
[0173] 5g of tank opening agent;
[0174] Fluorinated glyceryl ether 1g;
[0175] Carrier brightener 60g;
[0176] Microporous nickel additive 1g.
[0177] The buffer is boric acid.
[0178] The primary brightener is Figure 4 shown.
[0179] The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0180] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0181] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0182] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0183] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0184] The softener is a dialkyl quaternary ammonium salt.
[0185] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0186] Wherein, the aldehyde compound is dimethoxymethane;
[0187] The manganese-containing compound is manganese carbonate.
[0188] The fluorine-containing glyceryl ether is hexafluorononyl glycidyl ether.
[0189] The carrier brightener is a non-ionic polyether compound.
[0190] The raw materials with the above mass fractions are selected, and the electroplating additive is prepared according to a preparation method of a highly stable electroplating additive, which comprises the following steps:
[0191] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0192] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0193] S3′, adding a buffer, a primary brightener, and an emulsifier to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0194] S4′, regulating the reaction temperature of the reactor to control the temperature at room temperature, and sequentially adding inhibitors, cylinder opening agents, fluorinated glyceryl ethers and carrier brighteners, and stirring evenly to obtain a highly stable electroplating additive.
[0195] Comparative Example 2
[0196] A highly stable electroplating additive, comprising the following components in mass fractions:
[0197] Copper sulfate pentahydrate 100g;
[0198] Sulfuric acid 25g;
[0199] Chloride ion 40g;
[0200] Buffer 20g;
[0201] Secondary brightener 20g;
[0202] Emulsifier 11g;
[0203] Inhibitor 1g;
[0204] 5g of tank opening agent;
[0205] Fluorinated glyceryl ether 1g;
[0206] Microporous nickel additive 1g.
[0207] The buffer is boric acid.
[0208] The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0209] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0210] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0211] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0212] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0213] The softener is an imidazole softener.
[0214] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0215] Wherein, the aldehyde compound is 2-methylpropanal;
[0216] The manganese-containing compound is basic manganese oxide.
[0217] The fluorine-containing glyceryl ether is perfluorononene polyglyceryl ether.
[0218] The carrier brightener is a non-ionic polyether compound.
[0219] The raw materials with the above mass fractions are selected, and the electroplating additive is prepared according to a preparation method of a highly stable electroplating additive, which comprises the following steps:
[0220] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0221] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0222] S3′, adding a buffer, a primary brightener, and an emulsifier to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0223] S4′′, regulating the reaction temperature of the reactor to control the temperature at room temperature, and sequentially adding inhibitors, cylinder opening agents, and fluorinated glyceryl ether, and stirring evenly to obtain a highly stable electroplating additive.
[0224] Comparative Example 3
[0225] A highly stable electroplating additive, comprising the following components in mass fractions:
[0226] Copper sulfate pentahydrate 100g;
[0227] Sulfuric acid 25g;
[0228] Chloride ion 40g;
[0229] Buffer 20g;
[0230] Secondary brightener 20g;
[0231] Inhibitor 1g;
[0232] 5g of tank opening agent;
[0233] Fluorinated glyceryl ether 1g;
[0234] Microporous nickel additive 1g.
[0235] The buffer is boric acid.
[0236] The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1.
[0237] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0238] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0239] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0240] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0241] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0242] Wherein, the aldehyde compound is - diketone compounds;
[0243] The manganese-containing compound is permanganese anhydride.
[0244] The fluorine-containing glyceryl ether is perfluorononene polyglyceryl ether.
[0245] The raw materials with the above mass fractions are selected, and the electroplating additive is prepared according to a preparation method of a highly stable electroplating additive, which comprises the following steps:
[0246] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0247] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0248] S3′′, adding a buffer and a primary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min;
[0249] S4′′, regulating the reaction temperature of the reactor to control the temperature at room temperature, and sequentially adding inhibitors, cylinder opening agents, and fluorinated glyceryl ether, and stirring evenly to obtain a highly stable electroplating additive.
[0250] Comparative Example 4
[0251] The secondary brightener comprises 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate, and the preparation method of the secondary brightener comprises the following steps:
[0252] 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate are sequentially added into the reactor;
[0253] The mixed liquid is stirred by adjusting the number of injection ports and the stirring rate under the reactor blades;
[0254] By adding an appropriate amount of acid into the reactor and lowering the pH value, the pH value of the mixed solution is controlled to be around 7 to obtain a secondary brightener.
[0255] The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1;
[0256] Wherein, the aldehyde compound is - diketone compounds;
[0257] The manganese-containing compound is permanganese anhydride.
[0258] The carrier brightener is a non-ionic polyether compound.
[0259] The raw materials with the above mass fractions are selected, and the electroplating additive is prepared according to a preparation method of a highly stable electroplating additive, which comprises the following steps:
[0260] S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution;
[0261] S2, placing the base liquid into the reactor and setting the plating conditions of the reactor;
[0262] S3′′, adding a buffer and a secondary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to be 2000 rpm / min;
[0263] S4′′′, regulating the reaction temperature of the reactor, controlling the temperature at room temperature, and adding the cylinder agents in sequence, stirring evenly to obtain a highly stable electroplating additive.
[0264] Experimental Group
[0265] The electroplating additives prepared in Example 1, Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 were selected and placed in a container. PCB boards of the same specification were added to perform electroplating reactions, and the experimental phenomena were observed and the experimental data were recorded. The experimental results are shown in Table 1 and Figure 2 , Figure 3 As shown;
[0266] Table 1: Electroplating performance comparison table of various embodiments and comparative examples
[0267] Hardness (HV) Current efficiency (%) Brightness (level) PCB board qualification rate (%) Embodiment 1 260 99.2 4 98.4 Embodiment 2 254 99.4 4 98.6 Embodiment 3 240 99.2 4 98.4 Comparative Example 1 210 98 4 97.1 Comparative Example 2 220 97.5 3 95.2 Comparative Example 3 200 97.4 2 94.4 Comparative Example 4 190 98.1 2 86
[0268] As can be seen from Table 1, the electroplating additive prepared by the present invention has the functional advantages of high stability and high brightness, and significantly improves the processing quantity and qualified rate of PCBs.
[0269] In summary, with the aid of the above technical scheme of the present invention, the present invention improves the performance of the plating solution and the coating to a great extent by adding an emulsifier, a secondary brightener, a primary brightener, a carrier brightener, etc., and the additive of the present invention will not produce inclusions in the coating, and can significantly improve the surface brightness of the coating, thereby ensuring the uniformity of the coating; the nickel plating process provided by the present invention containing the above multi-layer nickel electroplating additive adopts a smaller current density, reduces energy consumption, and has a short electroplating time, and has a good brightening effect and high stability after nickel plating. The electroplating additive used in the present invention has extremely high stability, will not decompose in the plating solution, will not precipitate or discolor after multiple electroplatings and long-term storage, and ensures the brightness of the PCB board and the qualified rate of the PCB board after electroplating.
[0270] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly stable electroplating additive for use in a nickel plating process of a multi-layer nickel electroplating additive, characterized in that: The additive includes the following components by mass fraction: 100-200 parts of copper sulfate pentahydrate; Sulfuric acid 25-40 parts; Chloride ion 40-80 parts; Buffer 20-80 parts; Primary brightener 6-12 parts; Emulsifier 11-44 parts; Secondary brightener 20-60 parts; 20-25 parts of softener; 1-10 parts of inhibitor; 5-15 parts of tank opening agent; 1-10 parts of fluorinated glyceryl ether; Carrier brightener 60-100 parts; 1-10 parts of microporous nickel additive; The primary brightener is of organic compounds; The emulsifier includes sodium allyl sulfonate, polyoxyethylene ether and sodium propargyl sulfonate, and the mass fraction ratio is 6:4:1; The secondary brightener includes 1,4-butynediol, diethoxybutynediol, ethoxypropynyl alcohol, diethylpropargylamine and propanepyridine sulfate; The carrier brightener is fatty alcohol polyoxyethylene ether.
2. A highly stable electroplating additive according to claim 1, characterized in that: The buffering agent includes boric acid.
3. A highly stable electroplating additive according to claim 1, characterized in that: The softener includes one of an ester-based quaternary ammonium salt, a dialkyl quaternary ammonium salt, and an imidazole-type softener.
4. A highly stable electroplating additive according to claim 1, characterized in that: The cylinder opening agent comprises an aldehyde compound and a manganese-containing compound in a mass fraction of 1:1; Wherein, the aldehyde compound includes acetaldehyde propylene glycol acetal, - one of a diketone compound, dimethoxymethane and 2-methylpropanal; The manganese-containing compound includes one of manganese naphthenate, manganese anhydride, basic manganese oxide, manganese carbonate and permanganese anhydride.
5. A highly stable electroplating additive according to claim 1, characterized in that: The fluorine-containing glyceryl ether includes one of perfluorononene polyglyceryl ether, octafluorobiphenyl diglycidyl ether and hexadecanoyl glycidyl ether.
6. A method for preparing a highly stable electroplating additive, for realizing the preparation of the highly stable electroplating additive according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1. Weigh an appropriate amount of copper sulfate pentahydrate solution, add the copper sulfate pentahydrate solution to deionized water, stir and dissolve, then add the required amount of sulfuric acid and chloride ions, stir evenly, and obtain a base solution; S2, placing the base liquid into the reactor and setting the plating conditions of the reactor; S3, adding a buffer, a primary brightener, an emulsifier, and a secondary brightener to the base liquid in sequence, stirring while adding, and controlling the stirring rate to 2000 rpm / min; S4. Regulate the reaction temperature of the reactor to control the temperature at room temperature, and add softener, inhibitor, cylinder opening agent, fluorinated glycerol ether, carrier brightener and microporous nickel additive in sequence, and stir evenly to obtain a highly stable electroplating additive.
Citation Information
Patent Citations
A multilayer nickel plating additive to improve stability
CN109609979B
Multi-frequency narrow beam antenna
CN210984971U
Zinc-nickel alloy electroplating system
CN101273157A
Multi-layer nickel electroplating additive for improving stability
CN109609979A
Improvements in or relating to high-rate electrolytic nickel-plating methods, and installations
GB1213267A