Heat-resistant and wear-resistant composite plate and preparation method thereof

By using graphene modified white carbon black and nano-silicon carbide modified polyimide in heat-resistant and wear-resistant composite boards, the heat, wear and impact resistance of the composite board is improved, and the existing composite boards are solved. The problem of insufficient board performance.

CN115816931BActive Publication Date: 2024-12-03GUANGDONG ORIENT GS HOUSING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211523735.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-12-03
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

The heat-resistant and wear-resistant composite panels have insufficient heat-resistant wear resistance and poor impact resistance.

Method used

Using a composite board structure including high-temperature resistant substrate, wear-resistant metal panel, heat-resistant glue layer and wear-resistant coating, the heat-resistant glue layer is modified with graphene white carbon black, and the wear-resistant coating is made of nano silicon carbide modified polyacyl Imines and modified nano-aluminum nitride improve heat, wear and impact resistance through specific mixing and process treatments.

Benefits of technology

The composite panel has significantly improved the heat resistance, wear resistance and impact resistance, making it perform excellently in high temperature and wear conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003972321210000121
    Figure BDA0003972321210000121
Patent Text Reader

Abstract

The invention discloses a heat-resistant and wear-resistant composite plate, which comprises: a high-temperature resistant substrate, a wear-resistant metal panel, a heat-resistant adhesive layer and a wear-resistant coating; the preparation material of the heat-resistant adhesive layer comprises a heat-resistant adhesive layer mixture, and the preparation material of the heat-resistant adhesive layer mixture comprises silicone rubber, graphene-modified white carbon black, ethanol, tri(trimethylsilyl) borate, isopropyl orthosilicate and n-hexane; the preparation material of the wear-resistant coating comprises a wear-resistant coating mixture, and the preparation material of the wear-resistant coating mixture comprises vinyl resin, styrene, calcium stearate, nano-silicon carbide modified polyimide, modified nano-aluminum nitride and acetone. The composite plate of the invention not only has excellent heat resistance and wear resistance, but also has excellent impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite plates, and in particular to a heat-resistant and wear-resistant composite plate and a preparation method thereof. Background Art

[0002] Composite panels are generally divided into: metal composite panels, wood composite panels, color steel composite panels, rock wool composite panels, etc. Composite panels are panels composed of different materials with different functions. For example, the three-in-one panels of concrete, foam insulation layer and surface waterproof layer used for roofing, sandwich panels are also a kind of composite panels. Wear-resistant composite panels, that is, bimetallic composite wear-resistant steel plates, are plate products specially designed for large-area wear conditions. They are formed by surfacing welding on ordinary steel plates or heat-resistant steel plates and stainless steel plates to form an alloy wear-resistant layer with a volume fraction of Cr7C3 carbides of more than 50%. Wear-resistant steel plates have high wear resistance, impact resistance, deformability and weldability. They can be directly processed like steel plates, such as curling, deformation, cutting and punching, and processed into engineering parts to meet the wear and tear of industrial and mining industries.

[0003] CN113292924A discloses a heat-resistant and wear-resistant composite plate and a preparation method thereof, but its wear resistance is not good enough and its impact resistance is poor.

[0004] In summary, after extensive searching by the applicant, it is found that at least the existing heat-resistant and wear-resistant composite plates in this field have problems such as insufficient heat-resistant and wear-resistant performance and poor impact resistance. Therefore, it is necessary to develop or improve a heat-resistant and wear-resistant composite plate and a preparation method thereof. Summary of the invention

[0005] Based on this, in order to solve the problem that the existing heat-resistant and wear-resistant composite plates have poor heat-resistant and wear-resistant properties and poor impact resistance, the present invention provides a heat-resistant and wear-resistant composite plate and a preparation method thereof. The specific technical scheme is as follows:

[0006] A heat-resistant and wear-resistant composite plate, comprising: a high-temperature resistant substrate, a wear-resistant metal panel, a heat-resistant adhesive layer and a wear-resistant coating;

[0007] The preparation material of the heat-resistant adhesive layer includes a heat-resistant adhesive layer mixture, and the preparation material of the heat-resistant adhesive layer mixture includes silicone rubber, graphene-modified white carbon black, ethanol, tri(trimethylsilyl)borate, isopropyl orthosilicate and n-hexane;

[0008] The materials for preparing the wear-resistant coating include a wear-resistant coating mixture, and the materials for preparing the wear-resistant coating mixture include vinyl resin, styrene, calcium stearate, nano-silicon carbide modified polyimide, modified nano-aluminum nitride and acetone.

[0009] Furthermore, the high temperature resistant substrate includes one of a steel plate, a copper plate, a perlite plate, an asbestos plate and a bakelite plate.

[0010] Furthermore, the preparation method of the heat-resistant adhesive layer mixture comprises the following steps:

[0011] By mass, 35 to 45 parts of silicone rubber, 3 to 8 parts of graphene-modified white carbon black, 18 to 22 parts of ethanol, 1 to 3 parts of tris(trimethylsilyl)borate, 2 to 5 parts of isopropyl orthosilicate and 25 to 35 parts of n-hexane are mixed, stirred at 62 to 68° C. at a speed of 700 to 800 r / min for 1.5 to 1.8 hours, and then ultrasonicated for 3 to 5 hours to obtain the heat-resistant adhesive layer mixture.

[0012] Furthermore, the preparation method of the wear-resistant coating mixture comprises the following steps:

[0013] By mass, 45 to 55 parts of vinyl resin, 2 to 5 parts of styrene, 0.5 to 1.5 parts of calcium stearate, 6 to 10 parts of nano-silicon carbide modified polyimide, 2 to 5 parts of modified nano-aluminum nitride and 30 to 40 parts of acetone are mixed evenly, stirred at a speed of 1100 to 1200 r / min for 5 to 7 hours, and then ultrasonicated for 5.1 to 5.5 hours to obtain the wear-resistant coating mixture.

[0014] Furthermore, the preparation method of the graphene-modified white carbon black comprises the following steps:

[0015] The graphene is ultrasonically treated in water for 6 to 8 hours to obtain a graphene aqueous dispersion; white carbon black is ultrasonically treated in water for 5.3 to 5.8 hours to obtain a white carbon black aqueous dispersion; the graphene aqueous dispersion is mixed with the white carbon black aqueous dispersion, and then ammonia water is added to adjust the pH value to 7.5 to 8.5, ultrasonicated for 9 to 11 hours, and then a silane coupling agent is added, stirred at 55 to 58° C. at a speed of 600 to 800 r / min, reacted for 10 to 12 hours, and then filtered, washed and dried to obtain the graphene-modified white carbon black.

[0016] Furthermore, the silicone rubber includes at least one of dimethyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

[0017] Furthermore, the preparation method of the nano-silicon carbide modified polyimide comprises the following steps:

[0018] Add nano-silicon carbide to ethanol, ultrasonicate for 3 to 3.5 hours, then add silane coupling agent, ultrasonicate for 1 to 1.3 hours, reflux at 60 to 80° C. for 3 to 5 hours, then filter, wash and dry to obtain silane coupling agent modified nano-silicon carbide;

[0019] The silane coupling agent modified nano silicon carbide is added to N,N-dimethylacetamide, ultrasonicated for 0.8 to 1.2 hours, then diaminodiphenyl ether is added, stirred evenly at a speed of 550 to 590 r / min, and then benzophenone tetracarboxylic dianhydride is added under the protection of inert gas, and the nano silicon carbide modified polyimide is obtained after reaction.

[0020] Furthermore, the preparation method of the modified nano-aluminum nitride comprises the following steps:

[0021] Nano aluminum nitride, silane coupling agent and ethanol are mixed, stirred at a speed of 900-960 r / min for 5-8 hours, and then styrene and dibenzoyl peroxide are added, stirring is continued, and then heated to 76-79° C. for reaction to obtain the modified nano aluminum nitride.

[0022] Further, the silane coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethylsilane and γ-methacryloxypropyltrimethoxysilane.

[0023] The technical solution also provides a method for preparing a composite plate, wherein a heat-resistant adhesive layer mixture is sprayed in an annular manner from the inside to the outside between a high-temperature resistant substrate and a wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, and then a brazing material is laid in an annular manner between the high-temperature resistant substrate and the wear-resistant metal panel to obtain an annular slab, the annular heat-resistant adhesive layer and the annular slab are arranged alternately, and then the high-temperature resistant substrate and the wear-resistant metal panel are brazed to obtain an original composite plate;

[0024] The wear-resistant coating mixture is evenly coated on the outer surface of the composite board original plate to obtain the composite board.

[0025] The composite plate prepared by the above technical solution has excellent heat resistance and wear resistance because specific graphene-modified white carbon black is used in the preparation material of the heat-resistant adhesive layer, and specific nano-silicon carbide-modified polyimide and modified nano-aluminum nitride are used in the wear-resistant coating. In addition, the heat-resistant and wear-resistant composite plate prepared by the technical solution of the present invention also has excellent impact resistance. Specifically, graphene has very good toughness, and graphene-modified white carbon black can be better dispersed in the heat-resistant adhesive layer, thereby improving the heat resistance of the heat-resistant adhesive layer, and then improving the heat resistance of the composite plate. The polyimide modified by inorganic nanoparticle nanosilicon nitride and the modified nano-aluminum nitride modified by silane and organic matter can both overcome the poor adhesion of inorganic nanoparticles and the insufficient hardness of organic matter, and complement each other, thereby improving the wear resistance and impact resistance of the wear-resistant coating together, so that the heat-resistant and wear-resistant composite plate obtained has excellent impact resistance. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0028] A heat-resistant and wear-resistant composite plate in one embodiment of the present invention comprises: a high-temperature resistant substrate, a wear-resistant metal panel, a heat-resistant adhesive layer and a wear-resistant coating;

[0029] The preparation material of the heat-resistant adhesive layer includes a heat-resistant adhesive layer mixture, and the preparation material of the heat-resistant adhesive layer mixture includes silicone rubber, graphene-modified white carbon black, ethanol, tri(trimethylsilyl)borate, isopropyl orthosilicate and n-hexane;

[0030] The materials for preparing the wear-resistant coating include a wear-resistant coating mixture, and the materials for preparing the wear-resistant coating mixture include vinyl resin, styrene, calcium stearate, nano-silicon carbide modified polyimide, modified nano-aluminum nitride and acetone.

[0031] In one embodiment, the high temperature resistant substrate includes one of a steel plate, a copper plate, a perlite plate, an asbestos plate and a bakelite plate.

[0032] In one embodiment, the method for preparing the heat-resistant adhesive layer mixture comprises the following steps:

[0033] By mass, 35 to 45 parts of silicone rubber, 3 to 8 parts of graphene-modified white carbon black, 18 to 22 parts of ethanol, 1 to 3 parts of tris(trimethylsilyl)borate, 2 to 5 parts of isopropyl orthosilicate and 25 to 35 parts of n-hexane are mixed, stirred at 62 to 68° C. at a speed of 700 to 800 r / min for 1.5 to 1.8 hours, and then ultrasonicated for 3 to 5 hours to obtain the heat-resistant adhesive layer mixture.

[0034] In one embodiment, the method for preparing the wear-resistant coating mixture comprises the following steps:

[0035] By mass, 45 to 55 parts of vinyl resin, 2 to 5 parts of styrene, 0.5 to 1.5 parts of calcium stearate, 6 to 10 parts of nano-silicon carbide modified polyimide, 2 to 5 parts of modified nano-aluminum nitride and 30 to 40 parts of acetone are mixed evenly, stirred at a speed of 1100 to 1200 r / min for 5 to 7 hours, and then ultrasonicated for 5.1 to 5.5 hours to obtain the wear-resistant coating mixture.

[0036] In one embodiment, the method for preparing the graphene-modified white carbon black comprises the following steps:

[0037] The graphene is ultrasonically treated in water for 6 to 8 hours to obtain a graphene aqueous dispersion; white carbon black is ultrasonically treated in water for 5.3 to 5.8 hours to obtain a white carbon black aqueous dispersion; the graphene aqueous dispersion is mixed with the white carbon black aqueous dispersion, and then ammonia water is added to adjust the pH value to 7.5 to 8.5, ultrasonicated for 9 to 11 hours, and then a silane coupling agent is added, stirred at 55 to 58° C. at a speed of 600 to 800 r / min, reacted for 10 to 12 hours, and then filtered, washed and dried to obtain the graphene-modified white carbon black.

[0038] In one embodiment, the silicone rubber includes at least one of dimethyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

[0039] In one embodiment, the preparation method of the nano-silicon carbide modified polyimide comprises the following steps:

[0040] Add nano-silicon carbide to ethanol, ultrasonicate for 3 to 3.5 hours, then add silane coupling agent, ultrasonicate for 1 to 1.3 hours, reflux at 60 to 80° C. for 3 to 5 hours, then filter, wash and dry to obtain silane coupling agent modified nano-silicon carbide;

[0041] The silane coupling agent modified nano silicon carbide is added to N,N-dimethylacetamide, ultrasonicated for 0.8 to 1.2 hours, then diaminodiphenyl ether is added, stirred evenly at a speed of 550 to 590 r / min, and then benzophenone tetracarboxylic dianhydride is added under the protection of inert gas, and the nano silicon carbide modified polyimide is obtained after reaction.

[0042] In one embodiment, the preparation method of the modified nano-aluminum nitride comprises the following steps:

[0043] Nano aluminum nitride, silane coupling agent and ethanol are mixed, stirred at a speed of 900-960 r / min for 5-8 hours, and then styrene and dibenzoyl peroxide are added, stirring is continued, and then heated to 76-79° C. for reaction to obtain the modified nano aluminum nitride.

[0044] In one embodiment, the silane coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethylsilane and γ-methacryloxypropyltrimethoxysilane.

[0045] In one of the embodiments, the technical solution provides a method for preparing a composite plate, wherein a heat-resistant adhesive layer mixture is sprayed in an annular manner from the inside to the outside between a high-temperature resistant substrate and a wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, and then a brazing material is laid in an annular manner between the high-temperature resistant substrate and the wear-resistant metal panel to obtain an annular slab, the annular heat-resistant adhesive layer and the annular slab are arranged alternately, and then the high-temperature resistant substrate and the wear-resistant metal panel are brazed to obtain an original composite plate;

[0046] The wear-resistant coating mixture is evenly coated on the outer surface of the composite board original plate to obtain the composite board.

[0047] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0048] Embodiment 1:

[0049] Preparation of graphene-modified silica: ultrasonically treat graphene in water for 7 hours to obtain a graphene aqueous dispersion; ultrasonically treat silica in water for 5.6 hours to obtain a silica aqueous dispersion; mix the graphene aqueous dispersion with the silica aqueous dispersion, then add ammonia water to adjust the pH value to 8, ultrasonicate for 10 hours, then add γ-aminopropyltriethoxysilane, stir at 57°C at a speed of 700 r / min, react for 11 hours, then filter, wash and dry to obtain graphene-modified silica.

[0050] Preparation of nano-silicon carbide modified polyimide: Add nano-silicon carbide to ethanol, ultrasonicate for 3.3 hours, then add γ-aminopropyltriethoxysilane, ultrasonicate for 1.2 hours, reflux at 70°C for 4 hours, then filter, wash and dry to obtain γ-aminopropyltriethoxysilane modified nano-silicon carbide; add γ-aminopropyltriethoxysilane modified nano-silicon carbide to N,N-dimethylacetamide, ultrasonicate for 1 hour, then add diaminodiphenyl ether, stir evenly at a speed of 570r / min, then add dibenzophenonetetracarboxylic dianhydride under the protection of inert gas, and obtain nano-silicon carbide modified polyimide after reaction.

[0051] Preparation of modified nano-aluminum nitride: Nano-aluminum nitride, γ-aminopropyltriethoxysilane and ethanol were mixed, stirred at a speed of 930 r / min for 6 hours, and then styrene and dibenzoyl peroxide were added, stirring was continued, and then heated to 78°C for reaction to obtain modified nano-aluminum nitride.

[0052] Preparation of heat-resistant adhesive layer mixture: Mix 40 parts of dimethyl silicone rubber, 5 parts of graphene-modified white carbon black, 20 parts of ethanol, 2 parts of tri(trimethylsilyl)borate, 3 parts of isopropyl orthosilicate and 30 parts of n-hexane by mass, stir at 750 r / min at 65°C for 1.7 h, and then ultrasonicate for 4 h to obtain a heat-resistant adhesive layer mixture.

[0053] Preparation of wear-resistant coating mixture: By mass, 50 parts of vinyl resin, 3 parts of styrene, 1 part of calcium stearate, 8 parts of nano-silicon carbide modified polyimide, 3 parts of modified nano-aluminum nitride and 35 parts of acetone were mixed evenly, stirred at a speed of 1150r / min for 6h, and then ultrasonicated for 5.3h to obtain a wear-resistant coating mixture.

[0054] Preparation of composite plate: spray a heat-resistant adhesive layer mixture in an annular manner from inside to outside between a steel plate and a wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, then lay brazing material in an annular manner between a high-temperature resistant substrate and a wear-resistant metal panel to obtain an annular slab, the annular heat-resistant adhesive layer and the annular slab are arranged alternately, then braze the steel plate and the wear-resistant metal panel to obtain a composite plate original plate; evenly coat the wear-resistant coating mixture on the outer surface of the composite plate original plate to obtain a composite plate.

[0055] Embodiment 2:

[0056] The other parts are the same as those in Example 1, except that the dimethyl silicone rubber is replaced by methyl vinyl silicone rubber.

[0057] Embodiment 3:

[0058] The other parts are the same as those in Example 1, except that the dimethyl silicone rubber is replaced by silicon nitrogen rubber.

[0059] Embodiment 4:

[0060] The other parts are the same as those in Example 1, except that γ-aminopropyltriethoxysilane is replaced by γ-(2,3-epoxypropyloxy)propyltrimethoxysilane.

[0061] Embodiment 5:

[0062] The other parts are the same as those in Example 1, except that γ-aminopropyltriethoxysilane is replaced by γ-methacryloxypropyltrimethoxysilane.

[0063] Comparative Example 1:

[0064] Preparation of nano-silicon carbide modified polyimide: Add nano-silicon carbide to ethanol, ultrasonicate for 3.3 hours, then add γ-aminopropyltriethoxysilane, ultrasonicate for 1.2 hours, reflux at 70°C for 4 hours, then filter, wash and dry to obtain γ-aminopropyltriethoxysilane modified nano-silicon carbide; add γ-aminopropyltriethoxysilane modified nano-silicon carbide to N,N-dimethylacetamide, ultrasonicate for 1 hour, then add diaminodiphenyl ether, stir evenly at a speed of 570r / min, then add dibenzophenonetetracarboxylic dianhydride under the protection of inert gas, and obtain nano-silicon carbide modified polyimide after reaction.

[0065] Preparation of modified nano-aluminum nitride: Nano-aluminum nitride, γ-aminopropyltriethoxysilane and ethanol were mixed, stirred at a speed of 930 r / min for 6 hours, and then styrene and dibenzoyl peroxide were added, stirring was continued, and then heated to 78°C for reaction to obtain modified nano-aluminum nitride.

[0066] Preparation of heat-resistant adhesive layer mixture: Mix 40 parts of dimethyl silicone rubber, 5 parts of white carbon black, 20 parts of ethanol, 2 parts of tri(trimethylsilyl)borate, 3 parts of isopropyl orthosilicate and 30 parts of n-hexane by mass, stir at 750 r / min at 65°C for 1.7 hours, and then ultrasonicate for 4 hours to obtain a heat-resistant adhesive layer mixture.

[0067] Preparation of wear-resistant coating mixture: By mass, 50 parts of vinyl resin, 3 parts of styrene, 1 part of calcium stearate, 8 parts of nano-silicon carbide modified polyimide, 3 parts of modified nano-aluminum nitride and 35 parts of acetone were mixed evenly, stirred at a speed of 1150r / min for 6h, and then ultrasonicated for 5.3h to obtain a wear-resistant coating mixture.

[0068] Preparation of composite plate: spray a heat-resistant adhesive layer mixture in an annular manner from inside to outside between a steel plate and a wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, then lay brazing material in an annular manner between a high-temperature resistant substrate and a wear-resistant metal panel to obtain an annular slab, the annular heat-resistant adhesive layer and the annular slab are arranged alternately, then braze the steel plate and the wear-resistant metal panel to obtain a composite plate original plate; evenly coat the wear-resistant coating mixture on the outer surface of the composite plate original plate to obtain a composite plate.

[0069] Comparative Example 2:

[0070] Preparation of graphene-modified silica: ultrasonically treat graphene in water for 7 hours to obtain a graphene aqueous dispersion; ultrasonically treat silica in water for 5.6 hours to obtain a silica aqueous dispersion; mix the graphene aqueous dispersion with the silica aqueous dispersion, then add ammonia water to adjust the pH value to 8, ultrasonicate for 10 hours, then add γ-aminopropyltriethoxysilane, stir at 57°C at a speed of 700 r / min, react for 11 hours, then filter, wash and dry to obtain graphene-modified silica.

[0071] Preparation of modified nano-aluminum nitride: Nano-aluminum nitride, γ-aminopropyltriethoxysilane and ethanol were mixed, stirred at a speed of 930 r / min for 6 hours, and then styrene and dibenzoyl peroxide were added, stirring was continued, and then heated to 78°C for reaction to obtain modified nano-aluminum nitride.

[0072] Preparation of heat-resistant adhesive layer mixture: Mix 40 parts of dimethyl silicone rubber, 5 parts of graphene-modified white carbon black, 20 parts of ethanol, 2 parts of tri(trimethylsilyl)borate, 3 parts of isopropyl orthosilicate and 30 parts of n-hexane by mass, stir at 750 r / min at 65°C for 1.7 h, and then ultrasonicate for 4 h to obtain a heat-resistant adhesive layer mixture.

[0073] Preparation of wear-resistant coating mixture: 50 parts of vinyl resin, 3 parts of styrene, 1 part of calcium stearate, 8 parts of polyimide, 3 parts of modified nano-aluminum nitride and 35 parts of acetone were mixed evenly by mass, stirred at a speed of 1150r / min for 6h, and then ultrasonicated for 5.3h to obtain a wear-resistant coating mixture.

[0074] Preparation of composite plate: spray a heat-resistant adhesive layer mixture in an annular manner from inside to outside between a steel plate and a wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, then lay brazing material in an annular manner between a high-temperature resistant substrate and a wear-resistant metal panel to obtain an annular slab, the annular heat-resistant adhesive layer and the annular slab are arranged alternately, then braze the steel plate and the wear-resistant metal panel to obtain a composite plate original plate; evenly coat the wear-resistant coating mixture on the outer surface of the composite plate original plate to obtain a composite plate.

[0075] Comparative Example 3:

[0076] Preparation of graphene-modified silica: ultrasonically treat graphene in water for 7 hours to obtain a graphene aqueous dispersion; ultrasonically treat silica in water for 5.6 hours to obtain a silica aqueous dispersion; mix the graphene aqueous dispersion with the silica aqueous dispersion, then add ammonia water to adjust the pH value to 8, ultrasonicate for 10 hours, then add γ-aminopropyltriethoxysilane, stir at 57°C at a speed of 700 r / min, react for 11 hours, then filter, wash and dry to obtain graphene-modified silica.

[0077] Preparation of nano-silicon carbide modified polyimide: Add nano-silicon carbide to ethanol, ultrasonicate for 3.3 hours, then add γ-aminopropyltriethoxysilane, ultrasonicate for 1.2 hours, reflux at 70°C for 4 hours, then filter, wash and dry to obtain γ-aminopropyltriethoxysilane modified nano-silicon carbide; add γ-aminopropyltriethoxysilane modified nano-silicon carbide to N,N-dimethylacetamide, ultrasonicate for 1 hour, then add diaminodiphenyl ether, stir evenly at a speed of 570r / min, then add dibenzophenonetetracarboxylic dianhydride under the protection of inert gas, and obtain nano-silicon carbide modified polyimide after reaction.

[0078] Preparation of heat-resistant adhesive layer mixture: Mix 40 parts of dimethyl silicone rubber, 5 parts of graphene-modified white carbon black, 20 parts of ethanol, 2 parts of tri(trimethylsilyl)borate, 3 parts of isopropyl orthosilicate and 30 parts of n-hexane by mass, stir at 750 r / min at 65°C for 1.7 h, and then ultrasonicate for 4 h to obtain a heat-resistant adhesive layer mixture.

[0079] Preparation of wear-resistant coating mixture: By mass, 50 parts of vinyl resin, 3 parts of styrene, 1 part of calcium stearate, 8 parts of nano-silicon carbide modified polyimide, 3 parts of nano-aluminum nitride and 35 parts of acetone were mixed evenly, stirred at a speed of 1150r / min for 6h, and then ultrasonicated for 5.3h to obtain a wear-resistant coating mixture.

[0080] Preparation of composite plate: spray a heat-resistant adhesive layer mixture in an annular manner from inside to outside between a steel plate and a wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, then lay brazing material in an annular manner between a high-temperature resistant substrate and a wear-resistant metal panel to obtain an annular slab, the annular heat-resistant adhesive layer and the annular slab are arranged alternately, then braze the steel plate and the wear-resistant metal panel to obtain a composite plate original plate; evenly coat the wear-resistant coating mixture on the outer surface of the composite plate original plate to obtain a composite plate.

[0081] Test Method

[0082] Heat resistance test: In a high temperature working environment, the internal part of the composite board is tested for flaws.

[0083] Wear resistance test: Tested according to GB / T18102.

[0084] Impact resistance test: Conduct impact toughness test.

[0085] The heat resistance, wear resistance and impact resistance of the composite board were tested. The test results are shown in Table 1.

[0086] Table 1:

[0087]

[0088] As can be seen from the above table, the present invention uses specific graphene-modified white carbon black in the preparation material of the heat-resistant adhesive layer, and uses specific nano-silicon carbide-modified polyimide and modified nano-aluminum nitride in the wear-resistant coating. The obtained composite board has excellent heat resistance and wear resistance. In addition, the heat-resistant and wear-resistant composite board obtained by the present invention also has excellent impact resistance.

[0089] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0090] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A heat-resistant and wear-resistant composite plate, characterized in that: It includes: high temperature resistance Base plates, wear-resistant metal panels, heat-resistant adhesive layers and wear-resistant coatings; The preparation material of the heat-resistant adhesive layer includes a heat-resistant adhesive layer mixture, and the preparation material of the heat-resistant adhesive layer mixture includes silicone rubber, graphene-modified white carbon black, ethanol, tri(trimethylsilyl)borate, isopropyl orthosilicate and n-hexane; The preparation material of the wear-resistant coating includes a wear-resistant coating mixture, and the preparation material of the wear-resistant coating mixture includes vinyl resin, styrene, calcium stearate, nano-silicon carbide modified polyimide, modified nano-aluminum nitride and acetone; The preparation method of the graphene-modified white carbon black comprises the following steps: Ultrasonicate graphene in water for 6 to 8 hours to obtain a graphene aqueous dispersion; ultrasonicate white carbon black in water for 5.3 to 5.8 hours to obtain a white carbon black aqueous dispersion; mix the graphene aqueous dispersion with the white carbon black aqueous dispersion, then add ammonia water to adjust the pH value to 7.5 to 8.5, ultrasonicate for 9 to 11 hours, then add a silane coupling agent, stir at 55 to 58° C. at a speed of 600 to 800 r / min, react for 10 to 12 hours, then filter, wash and dry to obtain the graphene-modified white carbon black; The preparation method of the nano-silicon carbide modified polyimide comprises the following steps: Add nano-silicon carbide to ethanol, ultrasonicate for 3 to 3.5 hours, then add silane coupling agent, ultrasonicate for 1 to 1.3 hours, reflux at 60 to 80° C. for 3 to 5 hours, then filter, wash and dry to obtain silane coupling agent modified nano-silicon carbide; The silane coupling agent modified nano silicon carbide is added to N,N-dimethylacetamide, ultrasonicated for 0.8 to 1.2 hours, then diaminodiphenyl ether is added, stirred evenly at a speed of 550 to 590 r / min, and then benzophenone tetracarboxylic dianhydride is added under the protection of inert gas, and the nano silicon carbide modified polyimide is obtained after reaction; The preparation method of the modified nano aluminum nitride comprises the following steps: Nano aluminum nitride, silane coupling agent and ethanol are mixed, stirred at a speed of 900-960 r / min for 5-8 hours, and then styrene and dibenzoyl peroxide are added, stirring is continued, and then heated to 76-79° C. for reaction to obtain the modified nano aluminum nitride.

2. The composite panel according to claim 1, characterized in that: The high temperature resistant substrate comprises one of a steel plate, a copper plate, a pearlite plate, an asbestos plate and a bakelite plate.

3. The composite panel according to claim 1, characterized in that: The preparation method of the heat-resistant adhesive layer mixture comprises the following steps: By mass, 35 to 45 parts of silicone rubber, 3 to 8 parts of graphene-modified white carbon black, 18 to 22 parts of ethanol, 1 to 3 parts of tris(trimethylsilyl)borate, 2 to 5 parts of isopropyl orthosilicate and 25 to 35 parts of n-hexane are mixed, stirred at 62 to 68° C. at a speed of 700 to 800 r / min for 1.5 to 1.8 hours, and then ultrasonicated for 3 to 5 hours to obtain the heat-resistant adhesive layer mixture.

4. The composite panel according to claim 1, characterized in that: The preparation method of the wear-resistant coating mixture comprises the following steps: By mass, 45 to 55 parts of vinyl resin, 2 to 5 parts of styrene, 0.5 to 1.5 parts of calcium stearate, 6 to 10 parts of nano-silicon carbide modified polyimide, 2 to 5 parts of modified nano-aluminum nitride and 30 to 40 parts of acetone are mixed evenly, stirred at a speed of 1100 to 1200 r / min for 5 to 7 hours, and then ultrasonicated for 5.1 to 5.5 hours to obtain the wear-resistant coating mixture.

5. The composite panel according to claim 1, characterized in that: The silicone rubber includes at least one of dimethyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, fluorosilicone rubber and silicon nitrogen rubber.

6. The composite panel according to claim 1, characterized in that: The silane coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethylsilane and γ-methacryloxypropyltrimethoxysilane.

7. The method for preparing a composite board according to any one of claims 1 to 6, characterized in that: Spraying a heat-resistant adhesive layer mixture in an annular manner from inside to outside between the high-temperature resistant substrate and the wear-resistant metal panel to obtain an annular heat-resistant adhesive layer, and then laying brazing material in an annular manner between the high-temperature resistant substrate and the wear-resistant metal panel to obtain an annular slab, wherein the annular heat-resistant adhesive layer and the annular slab are arranged alternately, and then brazing the high-temperature resistant substrate and the wear-resistant metal panel to obtain a composite board original plate; The wear-resistant coating mixture is evenly coated on the outer surface of the composite board original plate to obtain the composite board.