A SnSe / SnO2@C composite and its preparation method and application
Through the preparation of SnSe/SnO2@C composite, the problems of low migration rate and large irreversible capacity of tin selenide-based anode materials in potassium ion batteries are solved, and the transmission rate and electrochemical performance of potassium ions are improved, which is suitable for large-scale production .
Patent Information
- Application Number
- CN202211526439.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The existing tin selenide-based anode materials have problems such as low ion/electron migration and deintercalation rates, large irreversible capacity and low Coulomb efficiency in potassium ion batteries, which limit their application.
Using the preparation method of SnSe/SnO2@C composite, SnSe is reacted with inorganic tin salt and selenium powder in a reducing solvent to form SnSe, and is compounded with SnO2 under hydrothermal conditions, followed by heat treatment and carbon coating to form a heterostructure To accelerate ion/electron migration and improve conductivity.
It significantly improves the transfer rate of potassium ions and the electrochemical properties of the electrode materials, enhances structural stability and conductivity, alleviates volume expansion, and is suitable for large-scale production.
Smart Images

Figure CN115893331B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy storage material preparation, and in particular relates to a SnSe / SnO2@C composite and a preparation method and application thereof. Background Art
[0002] In recent years, the frequent and excessive use of fossil energy by humans has led to energy, resource and environmental crises, which has had a serious impact on the sustainable development of human society. Traditional fossil energy such as coal, oil, and natural gas provide the most important energy resources for human society, but the scarcity of fossil energy and the ecological and environmental problems caused by its combustion have driven the growth of renewable resources, and the instability of renewable resources has further promoted the development of large-scale energy storage equipment. Therefore, it is extremely necessary to develop a new type of energy storage material with high reserves, high energy efficiency and less environmental pollution. It is understood that the current energy storage technology mainly includes two types: physical energy storage and electrochemical energy storage. Compared with physical energy storage, electrochemical energy storage has the advantages of high application efficiency, flexible and simple application, and good safety performance. Today's popular energy sources include supercapacitors, primary batteries, and secondary ion batteries, especially lithium-ion batteries and potassium-ion batteries, which have the greatest potential for exploration and application.
[0003] In the current environment of rapid development and application of portable electronic devices and new energy vehicles, we humans have higher application requirements for the working power supply of electronic devices and energy storage batteries for mobile devices. They must meet the requirements of repeated charging and discharging, high compaction density, high energy density, high working voltage, long cycle life, safety and high efficiency. Lithium-ion batteries are widely used due to the above advantages. However, the storage of lithium in the earth's crust is insufficient and the price is high, which is not conducive to large-scale production and application. Potassium and lithium are in the same main group and have similar chemical properties. Potassium is abundant in the strata and easy to obtain. In addition, it is friendly to the natural environment. Therefore, potassium-ion batteries are considered to have great potential. However, in potassium-ion batteries, the low theoretical specific capacity of potassium metal negative electrode and potassium dendrites will cause safety hazards, which greatly limits the commercial application of potassium metal as negative electrode material. Commercial graphite materials are generally selected in lithium-ion batteries, but because of their small interlayer spacing, they are not suitable for use in the negative electrode materials of potassium-ion batteries. Therefore, it is particularly important to develop a high-performance potassium storage negative electrode material. Selenide nanomaterials have gradually come into the public eye due to their good photoelectric properties and excellent structural stability. As a type of alloy negative electrode material, tin selenide has great development potential. However, there are relatively few studies on SnSe as a negative electrode material for potassium ion batteries. Therefore, it is extremely necessary to conduct research on SnSe as a negative electrode material for potassium ion batteries.
[0004] However, there are some problems with tin selenide-based negative electrode materials: (I) the electrode undergoes a huge volume change during the process of potassium ion insertion and extraction; (II) as the negative electrode of potassium ion batteries, tin selenide undergoes an irreversible first electrochemical reaction with potassium ions, resulting in a relatively large irreversible capacity, which reduces the coulombic efficiency of this type of material, greatly affecting its practical application. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a SnSe / SnO2@C composite and a preparation method and application thereof, so as to solve the technical problems of low ion / electron migration and deintercalation rate, large irreversible capacity and low coulombic efficiency existing in the prior art when tin selenide-based negative electrode materials are used in potassium ion batteries.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention discloses a method for preparing a SnSe / SnO2@C composite, comprising the following steps:
[0008] 1) adding an inorganic tin salt to ethylene glycol or glycerol, and after ultrasonic dispersion, adding a surfactant until it is completely dissolved to obtain a solution A; then adding selenium powder to a reducing solvent, stirring until it is completely dissolved to obtain a solution B; adding the solution B dropwise to the solution A, stirring evenly, to obtain a mixed solution C;
[0009] 2) After ultrasonic dispersion of the mixed solution C, hydrothermal reaction is first performed, cooled to room temperature, centrifuged, washed, and freeze-dried to obtain SnSe / SnO2 composite powder, the SnSe / SnO2 composite powder is mixed and ground evenly with 2-methylimidazole, and then heat-treated and cooled to room temperature to obtain a SnSe / SnO2@C composite.
[0010] Optimally, in step 1), the mass ratio of the inorganic tin salt: surfactant: selenium powder is (1.1-3.26): (0.092-0.92): (0.083-0.972).
[0011] Optimally, in step 2), the mixing ratio of the SnSe / SnO2 composite powder and 2-methylimidazole is (10:1 to 1:1).
[0012] Optimally, in step 2), the hydrothermal reaction is carried out at 120-200° C. for 10-20 hours.
[0013] Optimally, in step 2), the freeze-drying temperature is -30°C to -40°C, and the time is 10h to 12h; the heat treatment condition is 300 to 800°C for 2 to 5h.
[0014] Optimally, in step 2), the heat treatment is carried out in an argon atmosphere, and the heat treatment conditions are firstly heating to 300-800°C, then keeping at 300-800°C for 2-5h, and then cooling to 100-300°C after 10-40min.
[0015] Optimally, in step 1), the stirring speed is 200-500 r / min.
[0016] Optimally, in step 1), the inorganic tin salt is SnCl2·2H2O or SnCl4·5H2O; the surfactant is any one of polyvinylpyrrolidone, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid and oleic acid; and the reducing solvent is any one of ethylenediamine, triethanolamine, hydrazine hydrate and potassium borohydride aqueous solution.
[0017] The invention also discloses a SnSe / SnO2@C complex prepared by the above preparation method.
[0018] The invention also discloses the application of the SnSe / SnO2@C complex in preparing anode materials for potassium ion batteries.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention discloses a method for preparing a SnSe / SnO2@C composite, wherein an inorganic tin salt is used as Sn 2+ Source; Use reducing solvent to reduce selenium powder to Se 2- , Sn 2+ with Se 2- The reaction generates SnSe, which is a narrow bandgap semiconductor material with a double atomic layer crystal structure. Its bandgap is close to that of traditional semiconductor material Si. Its energy gap is about 0.9eV, and it has strong absorption in the ultraviolet, visible and near-infrared regions. By adding excess Sn 2+ Source, in Sn 2+ with Se 2- While the reaction generates SnSe, the excess Sn 2+SnO2 will also be generated. SnO2 is a potential energy material with high chemical stability, thermal stability, high photocatalytic activity, gas sensitivity, high luminescence properties and low charge transfer impedance. A simple solvothermal method is used to compound SnSe and SnO2 to form a heterostructure. The interface of the heterostructure can provide a short and straight charge path and abundant active sites, thereby accelerating the migration and deintercalation of ions / electrons, greatly improving the conductivity of SnSe. The large work function difference between SnSe and SnO2 enables the lattice of the SnSe / SnO2 composite material to form a relatively large internal electric field, effectively enhancing the electron transport inside SnSe / SnO2. The SnSe / SnO2 composite structure can effectively enhance the transmission rate of potassium ions in potassium ion batteries, which is of great significance to the performance improvement of potassium ion batteries. The SnSe and SnO2 are combined to improve the electrochemical performance of the electrode material. By adding 2-methylimidazole, mixing and heat treating, and coating SnSe / SnO2 with carbon, the prepared SnSe / SnO2@C composite has stronger structural stability, conductivity and electrochemical performance, and can effectively alleviate volume expansion. The preparation process is simple, with high repeatability, short preparation cycle, low reaction temperature, reduced energy consumption and production cost, and is suitable for large-scale production.
[0021] Furthermore, by controlling the content of each precursor, the content of additives, the reaction temperature, the reaction time, etc., the morphology and size of the product can be well controlled, and the SnSe / SnO2@C composite material was successfully prepared, which showed good electrochemical performance in potassium ion batteries.
[0022] The present invention also discloses a SnSe / SnO2@C composite prepared by the above-mentioned preparation method, wherein SnSe nanoparticles and SnO2 nanoparticles are uniformly mixed, the size of the particles is about 10-20nm, and the SnSe / SnO2 particles grow on lamellar graphene. The SnSe / SnO2 lattice can form a relatively large internal electric field, effectively enhancing the electron transport inside the SnSe / SnO2@C composite, and SnSe / SnO2 can effectively enhance the transmission rate of potassium ions in potassium ion batteries; the coated carbon material makes the SnSe / SnO2@C composite have stronger structural stability, conductivity and electrochemical performance.
[0023] The present invention also discloses the application of the SnSe / SnO2@C composite in a negative electrode material of a battery. When used as a negative electrode of a potassium ion battery, the SnSe / SnO2@C composite is mixed with a binder and a conductive agent at a mass ratio of 8:1.5:1.5 to prepare a negative electrode sheet, wherein the binder is carboxymethyl cellulose CMC and the conductive agent is Super P. The SnSe / SnO2@C composite can effectively enhance the transmission rate of potassium ions in potassium ion batteries, and is of great significance to improving the performance of potassium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The X-ray diffraction (XRD) pattern of the SnSe / SnO2@C composite prepared in Example 1 of the present invention;
[0025] Figure 2 The scanning electron microscope (SEM) photographs of the SnSe / SnO2@C composite prepared in Example 1 of the present invention, wherein (a) is a SEM image at a low magnification; and (b) is a SEM image at a high magnification. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0028] The present invention is further described in detail below in conjunction with specific embodiments and accompanying drawings:
[0029] A method for preparing a SnSe / SnO2@C composite comprises the following steps:
[0030] 1) First, 1.1-3.26 g of SnCl2·2H2O or SnCl4·5H2O is added to 35-65 mL of ethylene glycol or glycerol, and after ultrasonic dispersion for 30-120 min, 0.092-0.92 g of PVP (polyvinyl pyrrolidone), CTAB (hexadecyltrimethylammonium bromide), EDTA (ethylenediaminetetraacetic acid) or oleic acid is added and stirred for 20-50 min until completely dissolved to obtain solution A; then 0.083-0.972 g of selenium powder is added to 3-9 mL of ethylenediamine, triethanolamine, hydrazine hydrate or potassium borohydride aqueous solution, and stirred with a magnetic stirrer for 30-80 min until completely dissolved to obtain solution B; solution B is added dropwise to solution A and stirred for 60-120 min until uniform, to obtain a mixed solution C;
[0031] 2) The mixed solution C was ultrasonically dispersed for 30 to 180 minutes until uniform, and then transferred to a reactor. The filling degree of the hydrothermal reactor was controlled at 50% to 80%, and the reaction was carried out at 120 to 200°C for 10 to 20 hours. After the reaction was completed, the product D was cooled to room temperature with the furnace, and was repeatedly washed with deionized water and ethanol and centrifuged several times. Freeze-dried at -30°C to -40°C for 10 hours, powder E was collected, and SnSe / SnO2 composite powder was obtained; the obtained SnSe / SnO2 composite powder was mixed and ground with 2-methylimidazole at a mass ratio of (10:1 to 1:1) to obtain powder F, and then powder F was heat-treated under the conditions of first heating to 300 to 800°C, then keeping at 300 to 800°C for 2 to 5 hours, then cooling to 100 to 300°C after 10 to 40 minutes, and finally cooling to room temperature to obtain SnSe / SnO2@C composite.
[0032] Embodiment 1:
[0033] A method for preparing a SnSe / SnO2@C composite comprises the following steps:
[0034] 1) Add 1.1 g of SnCl2·2H2O to 35 mL of ethylene glycol, and after ultrasonic dispersion for 30 min, add 0.092 g of PVP and stir for 20 min until completely dissolved to form solution A; add 0.083 g of selenium powder to 3 mL of ethylenediamine and stir with a magnetic stirrer for 30 min until completely dissolved to obtain solution B; then add solution B dropwise to solution A and stir for 60 min until uniform, to form a mixed solution C;
[0035] 2) The mixed solution C was ultrasonically dispersed for 30 minutes until uniform, and then transferred to a reactor, reacted at 120°C for 10 hours, and cooled to room temperature with the furnace after the reaction was completed. The product D was repeatedly washed with deionized water and ethanol and centrifuged several times. After that, the product was freeze-dried at -30°C for 10 hours, and the powder E was collected to obtain the SnSe / SnO2 composite powder; the obtained SnSe / SnO2 composite powder was mixed with 2-methylimidazole at a mass ratio of 10:1 and ground uniformly to obtain powder F, and then the sample was heat-treated, first heated to 300°C, then kept at 300°C for 2 hours, and then cooled to room temperature to obtain the SnSe / SnO2@C complex.
[0036] See also Figure 1 The X-ray diffraction pattern of the SnSe / SnO2@C complex prepared in Example 1 of the present invention. The SnSe / SnO2@C complex was analyzed using a Rigaku D / max2000PC X-ray diffractometer. It can be seen from the figure that the SnSe / SnO2@C complex has the same structure as SnSe with a JCPDS number of 89-0232 and SnO2 with a JCPDS number of 46-1008, indicating that SnSe nanoparticles and SnO2 nanoparticles were successfully prepared.
[0037] See also Figure 2 The following is a scanning electron microscope photo of the SnSe / SnO2@C composite prepared in Example 1 of the present invention. (a) is a SEM image at a low magnification; (b) is a SEM image at a high magnification. Field emission scanning electron microscopy (FESEM) was used for observation. It can be seen from the figure that the SnSe nanoparticles and the SnO2 nanoparticles are uniformly mixed, forming a nano-sized structure, and are coated with uniform pyrolytic carbon.
[0038] Embodiment 2:
[0039] A method for preparing a SnSe / SnO2@C composite comprises the following steps:
[0040] 1) Add 1.5 g of SnCl4·5H2O to 45 mL of glycerol, and after ultrasonic dispersion for 50 min, add 0.37 g of CTAB and stir for 30 min until completely dissolved to form solution A; add 0.36 g of selenium powder to 5 mL of hydrazine hydrate and stir with a magnetic stirrer for 50 min until completely dissolved to obtain solution B; then add solution B dropwise to solution A and stir for 80 min until uniform, to form a mixed solution C;
[0041] 2) The mixed solution C was ultrasonically dispersed for 50 minutes until uniform, and then transferred to a reactor, reacted at 150°C for 12 hours, and cooled to room temperature with the furnace after the reaction was completed. The product D was repeatedly washed with deionized water and ethanol and centrifuged several times. After that, the product was freeze-dried at -30°C for 12 hours, and the powder E was collected to obtain the SnSe / SnO2 composite powder; the obtained SnSe / SnO2 composite powder was mixed and ground with 2-methylimidazole at a mass ratio of 5:1 to obtain powder F, and then the sample was heat-treated, first heated to 500°C, then kept at 500°C for 3 hours, then cooled to 300°C, and then cooled to room temperature to obtain the SnSe / SnO2@C complex.
[0042] Embodiment 3:
[0043] The preparation method comprises:
[0044] 1) Add 2.13 g of SnCl2·2H2O to 55 mL of ethylene glycol, and after ultrasonic dispersion for 100 min, add 0.68 g of oleic acid and stir for 40 min until completely dissolved to form solution A; add 0.674 g of selenium powder to 6 mL of potassium borohydride aqueous solution, and stir with a magnetic stirrer for 60 min until completely dissolved to obtain solution B; then add solution B dropwise to solution A and stir for 100 min until uniform, to form a mixed solution C;
[0045] 2) The mixed solution C was ultrasonically dispersed for 150 minutes until uniform, and then transferred to a reactor, reacted at 180°C for 16 hours, and cooled to room temperature with the furnace after the reaction was completed. It was repeatedly washed with deionized water and ethanol and centrifuged several times to obtain product D. After that, it was freeze-dried at -40°C for 10 hours, and powder E was collected to obtain SnSe / SnO2 composite powder; the obtained SnSe / SnO2 composite powder was mixed and ground with 2-methylimidazole at a mass ratio of 3:1 to obtain powder F, and then the sample was heat-treated, first heated to 600°C, then kept at 600°C for 4 hours, then cooled to 300°C, and then cooled to room temperature to obtain SnSe / SnO2@C composite.
[0046] Embodiment 4:
[0047] The preparation method comprises:
[0048] 1) Add 3.26 g of SnCl4·5H2O to 60 mL of ethylene glycol, and after ultrasonic dispersion for 120 min, add 0.92 g of CTAB and stir for 50 min until completely dissolved to form solution A; add 0.972 g of selenium powder to 9 mL of triethanolamine and stir with a magnetic stirrer for 80 min until completely dissolved to obtain solution B; then add solution B dropwise to solution A and stir for 120 min until uniform, to form a mixed solution C;
[0049] 2) The mixed solution C was ultrasonically dispersed for 180 minutes until uniform, and then transferred to a reactor, reacted at 200°C for 20 hours, cooled to room temperature with the furnace after the reaction, and washed repeatedly with deionized water and ethanol, and centrifuged several times to obtain product D. Then, freeze-dried at -40°C for 12 hours, powder E was collected to obtain SnSe / SnO2 composite powder; the obtained SnSe / SnO2 composite powder was mixed and ground with 2-methylimidazole at a mass ratio of 1:1 to obtain powder F, and then the sample was heat-treated, first heated to 800°C, then kept at 800°C for 5 hours, then cooled to 300°C, and then cooled to room temperature to obtain SnSe / SnO2@C composite.
[0050] The present invention uses ethylene glycol or glycerol as a solvent and adopts a simple solvothermal method to prepare a SnSe / SnO2@C composite. SnSe nanoparticles are uniformly mixed with SnO2 nanoparticles and coated with a complete pyrolytic carbon material. The preparation method of the present invention is simple, has a short cycle, and has good sample dispersibility. Mixing SnSe with SnO2 further improves the conductivity of SnSe, and then coating it with pyrolytic carbon improves the structural stability of the composite material. The composite has good potassium storage performance as a negative electrode material for potassium ion batteries. Studies have found that the SnSe / SnO2@C composite electrode has a pseudocapacitive effect in the potassium storage process, which has great research value. The composite material has good photocatalytic and electrochemical properties as a photocatalytic material and an electrode material.
[0051] Tin dioxide (SnO2) has attracted widespread attention due to its abundant reserves and high theoretical capacity. SnO2 is a potential energy material with high chemical stability, thermal stability, high photocatalytic activity, gas sensitivity, high luminescence properties and low charge transfer impedance. It has potential application prospects in the fields of photocatalysts, gas sensors, light-emitting devices and batteries.
[0052] In addition, SnSe is a narrow bandgap semiconductor material with a double atomic layer crystal structure. Its bandgap is close to that of traditional semiconductor material Si. Its energy gap is about 0.9eV. It has strong absorption in the ultraviolet, visible and near-infrared regions, and has great application potential in the fields of batteries and photovoltaics. However, there are relatively few studies on SnSe as anode materials for potassium ion batteries. Therefore, it is extremely necessary to conduct research on SnSe as anode materials for potassium ion batteries.
[0053] More importantly, the large work function difference between tin dioxide (5.24 eV) and tin selenide (4.19 eV) enables the lattice of the SnSe / SnO2 composite material to form a relatively large internal electric field, effectively enhancing the electron transport within SnSe / SnO2. The SnSe / SnO2 composite structure is of great significance to the performance improvement of potassium ion batteries. The interface of SnSe / SnO2 can provide short and straight charge paths and abundant active sites, thereby accelerating the migration and deintercalation of ions / electrons. Mixing SnSe with SnO2, the two can synergistically improve the electrochemical performance of the electrode material. In order to enhance its structural stability, we coated it with carbon, which further improved its electrochemical performance.
[0054] The SnSe / SnO2@C composite prepared by the preparation method of the present invention comprises SnSe nanoparticles and SnO2 nanoparticles uniformly mixed, the size of the particles is about 10-20 nm, and the SnSe / SnO2 particles grow on lamellar graphene.
[0055] When the SnSe / SnO2@C composite prepared by the preparation method is used as a negative electrode of a potassium ion battery, the SnSe / SnO2@C composite is mixed with a binder and a conductive agent in a mass ratio of 8:1.5:1.5 to prepare a negative electrode sheet, the binder is carboxymethyl cellulose CMC, and the conductive agent is Super P.
[0056] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A SnSe / SnO 2 @C complex preparation method, It is characterized in that The following steps are involved: 1) Add inorganic tin salt to ethylene glycol or glycerol, disperse uniformly by ultrasonication, and then add surfactant until completely dissolved to obtain solution A; then add selenium powder to reducing solvent, stir until completely dissolved to obtain solution B; add solution B dropwise to solution A, stir uniformly to obtain mixed solution C; 2) After ultrasonic dispersion of the mixed solution C, hydrothermal reaction was performed, cooled to room temperature, centrifuged, washed, and freeze-dried to obtain SnSe / SnO 2 Composite powder, SnSe / SnO 2 The composite powder was mixed and ground evenly with 2-methylimidazole, and then heat treated and cooled to room temperature to obtain SnSe / SnO 2 @C complex; In step 1), the inorganic tin salt is SnCl 2 ·2H 2 O or SnCl 4 ·5H 2 O; the surfactant is any one of polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, ethylenediaminetetraacetic acid and oleic acid; the reducing solvent is any one of ethylenediamine, triethanolamine, hydrazine hydrate and potassium borohydride aqueous solution; In step 1), the mass ratio of the inorganic tin salt: surfactant: selenium powder is (1.1-3.26): (0.092-0.92): (0.083-0.972); In step 2), the SnSe / SnO 2 The mixing ratio of the composite powder and 2-methylimidazole is (10:1~1:1).
2. SnSe / SnO according to claim 1 2 @C complex preparation method, It is characterized in that In step 2), the hydrothermal reaction is carried out at 120-200 °C for 10-20 h.
3. SnSe / SnO according to claim 1 2 @C complex preparation method, It is characterized in that In step 2), the freeze-drying temperature is -30°C to -40°C, and the time is 10 h to 12 h; the heat treatment condition is 300 to 800°C for 2 to 5 h.
4. SnSe / SnO according to claim 1 2 @C complex preparation method, It is characterized in that In step 2), the heat treatment is carried out in an argon atmosphere, and the heat treatment conditions are firstly raised to 300-800°C, then kept at 300-800°C for 2-5 hours, and then cooled to 100-300°C after 10-40 minutes.
5. SnSe / SnO according to claim 1 2 @C complex preparation method, It is characterized in that In step 1), the stirring speed is 200-500 r / min.
6. SnSe / SnO prepared by the preparation method according to any one of claims 1 to 5 2 @C complex.
7. SnSe / SnO according to claim 6 2 Application of @C complex in the preparation of negative electrode materials for potassium ion batteries.