Silicon-oxygen composite material for lithium-ion battery and preparation method and application thereof
By using a three-layer silicon-oxygen composite material in lithium-ion batteries, combining prelithiation of distorted silicon-oxygen materials with lithium carbon compounds and silicone coating technology, the first Coulomb efficiency and cycling performance of silicon-oxygen negative electrode materials are solved. The problem of low results in high efficiency and stability of the battery.
Patent Information
- Application Number
- CN202211080202.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-09-05
AI Technical Summary
The first Coulomb efficiency and cycling performance of silicon oxygen negative electrode materials in existing lithium-ion batteries are low, and the residual alkalinity and gas production problems are easily generated during prelithiation, which affects the long-term stability of the battery.
Silicon-oxygen composite materials for lithium-ion batteries with three-layer structure, including silicon-based material cores, conductive carbon layers and silicone cladding layers, are prelithiated by secondary baking of disproportionated silicon oxygen materials and lithium carbon compounds, and use The silicone source is coated and the pH value is controlled within the range of 6 to 10 to form a stable material structure.
It significantly improves the structural stability and battery capacity of silicon oxygen composite materials, combines excellent first-time Coulomb efficiency, first-time reversible capacity and high cycle stability, avoiding the problems of increased alkalinity and gas production.
Smart Images

Figure CN115911294B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials for lithium-ion batteries, and in particular to a silicon-oxygen composite material for lithium-ion batteries, a preparation method thereof and an application thereof. Background Art
[0002] In recent years, with the continuous development of new energy technologies, lithium-ion batteries have been widely used. However, the theoretical capacity of traditional graphite-based negative electrode materials is low and cannot meet the market demand for high energy density of lithium-ion batteries. Studies have shown that single silicon has a high theoretical capacity. However, in practice, it is found that when silicon is used as a negative electrode material, its volume expansion rate reaches 300%, the slurry particles are easy to break and fall off, and the battery's first coulombic efficiency is low and the cycle stability is poor. Silicon-oxygen materials have attracted widespread attention as high-specific capacity negative electrode materials, but the resulting low first efficiency and poor cyclability limit the widespread application of this material. Therefore, improving the first coulombic efficiency and cycle performance of silicon-oxygen negative electrode materials has become an urgent problem to be solved.
[0003] Based on this problem, many material researchers have proposed the idea of pre-supplementing lithium after continuous attempts, that is, doping some metallic lithium while synthesizing the negative electrode material to compensate for the irreversible lithium element consumed in the battery reaction and improve the battery's first coulombic efficiency. The first coulombic efficiency of silicon oxide materials can be significantly improved by pre-lithiation. However, pre-lithiated silicon oxide materials often encounter some problems in the preparation of battery electrodes, such as increased pH value when preparing aqueous slurry, easy gas production, easy generation of particles and pores when slurry is coated, etc., resulting in poor electronic conductivity of lithium-containing silicon oxide materials, low first coulombic efficiency and cycle performance.
[0004] For example, a Chinese document with application publication number CN 111710845 A discloses a silicon-oxygen composite negative electrode material, a preparation method thereof, and a lithium-ion battery. The composite negative electrode material includes composite particles, a carbon layer formed on the surface of the composite particles, and a hydrophobic layer formed on the surface of the carbon layer. The composite particles include lithium silicate and a non-metallic silicon-containing material, the lithium silicate is Li4SiO4, and the non-metallic silicon-containing material includes at least one of nano-silicon and silicon oxide. The preparation method includes calcining a mixture containing a silicon source and a lithium-containing compound under a protective atmosphere to obtain a silicon-oxygen composite negative electrode material. It is further disclosed that the silicon source is silicon monoxide, and the lithium-containing compound is a reducing lithium-containing compound, specifically including lithium hydride, alkyl lithium, metallic lithium, lithium aluminum hydride, lithium amide or lithium borohydride; the calcination temperature is 300-600°C.
[0005] However, according to the records in its embodiments, it only discloses embodiments using lithium hydride, metallic lithium, and lithium borohydride as lithium-containing compounds. It is well known to those skilled in the art that lithium hydride, metallic lithium, and lithium borohydride are all highly reactive substances. If the above raw materials are used to supplement lithium, the residual raw materials will cause reactions with moisture and / or carbon dioxide in the air. Taking lithium hydride as an example, if it is used to supplement lithium, the residual lithium hydride will react with moisture and carbon dioxide in the air to generate lithium hydroxide and lithium carbonate, resulting in increased alkalinity, corroding the binder, thereby affecting its long-term cycle performance. This is why only 50 weeks of power-on cycle data are provided in this technical solution.
[0006] In addition, the technical solution controls the molar ratio of silicon source to lithium-containing compound and the calcination temperature to ensure that the prepared silicon-oxygen negative electrode material contains only lithium silicate Li4SiO4, so that it has an initial reversible capacity of up to 1540mAh / g. However, the Li4SiO4 phase is more soluble in water, resulting in rapid cycle decay. In addition, too much pre-lithium reagent needs to be added to generate this phase, and the initial efficiency is lower than that of other phases.
[0007] A Chinese document with application publication number CN 111326721 A discloses a method for preparing a composite negative electrode pre-embedded lithium material, comprising: a M b Dry or wet mix with organic carbon source, and calcine to obtain coated product Li a M b / C; then the coated product Li a M b / C and SiO x After mixed ball milling, a composite negative electrode pre-embedded lithium material is obtained; and further disclosed is Li a M b One or more selected from Li3N, Li3P, Li2Si2O5, Li4SiO4, Li2C2, Li4C, Li6C2, Li8C3, Li6C3, Li4C3, Li4C5. According to its preparation process, it can be confirmed that Li a M b With SiO x It is just a simple ball milling mixing, no chemical reaction occurs, and lithium silicate is not generated. Therefore, it is equivalent to no pre-lithiation. Summary of the invention
[0008] In view of the above-mentioned problems existing in the prior art, the present invention discloses a silicon-oxygen composite material for lithium-ion batteries, which solves the problems of high residual alkali content in conventional pre-lithiation silicon-oxygen materials during use and gas generation during processing. The structural stability and battery capacity of the prepared silicon-oxygen composite material are greatly improved, and the assembled lithium-ion battery has excellent first coulombic efficiency, first reversible capacity and cycle stability.
[0009] The specific technical solutions are as follows:
[0010] A silicon-oxygen composite material for lithium-ion batteries, comprising a three-layer structure, which comprises a silicon-based material core, a conductive carbon layer and an organic silicon coating layer from the inside to the outside;
[0011] The silicon-based material core comprises single crystal silicon and lithium metasilicate (Li2SiO3);
[0012] The organic silicon in the organic silicon coating layer comes from one or more of silane coupling agent, silicone oil, high temperature vulcanized silicone rubber, liquid silicone rubber and silicone resin.
[0013] Preferred:
[0014] The pH value of the silicon-oxygen composite material for lithium-ion batteries is 6-10; more preferably 8-10, and even more preferably 8-9.
[0015] The median particle size (D50) of the silicon-based material core is 1.0 to 10.0 μm;
[0016] The thickness of the conductive carbon layer is 0.1 to 100 nm, and more preferably 5 to 40 nm;
[0017] The thickness of the organic silicon coating layer is 0.1 to 100 nm, and more preferably 1 to 20 nm.
[0018] The present invention also discloses a method for preparing the silicon-oxygen composite material for lithium-ion batteries, comprising the following steps:
[0019] (1) Silicon oxide material SiO x Carry out a calcination to obtain a disproportionate silicon-oxygen material, wherein 0.8≤x≤1.5;
[0020] (2) in an inert atmosphere or under vacuum conditions, mixing the disproportionated silicon-oxygen material and the lithium-carbon compound uniformly, and then performing secondary calcination to obtain a pre-lithiated silicon-oxygen material;
[0021] (3) The pre-lithiation silicon-oxygen material is coated with an organic silicon source, and then the pre-lithiation silicon-oxygen material is broken up and sieved to obtain the silicon-oxygen composite material for lithium-ion batteries.
[0022] In the preparation process disclosed in the present invention, the silicon oxide material SiO xAs raw materials, a disproportionate silicon-oxygen material is first calcined once, and then a special lithium-carbon compound is selected as a pre-lithiation agent to be calcined twice with the disproportionate silicon-oxygen material to fully carry out pre-lithiation. At the same time, a continuous carbon coating layer is formed in situ on the surface of the silicon-based material core formed; finally, a hydrophobic organic silicon source is used for coating again to reduce alkalinity and side reactions, and finally a silicon-oxygen composite material for lithium-ion batteries is obtained.
[0023] Step (1) is specifically:
[0024] Silicon oxide material SiO x Put it into an atmosphere furnace and carry out a roasting process under an inert atmosphere or vacuum conditions;
[0025] After a calcination, the SiO x The conversion of SiO2 into crystalline Si and crystalline SiO2 is more conducive to the pre-lithiation reaction of lithium-carbon compounds. x When mixed with lithium-carbon compounds for calcination, the pre-lithiation reaction is incomplete, a large amount of pre-lithiation reagent remains, the first cycle efficiency of the material is low, and the cycle performance is poor.
[0026] If the temperature of the primary calcination is too low or the time is too short, the disproportionation effect cannot be achieved and the reaction rate with the pre-lithiation reagent cannot be increased; if the temperature is too high or the time is too long, the grain size of the generated crystalline Si and crystalline SiO2 will be too large, affecting the cycle performance of the final product.
[0027] The primary calcination temperature is 600-1000°C, and the time is 0.5-50 hours, preferably 600-900°C, and the time is 2-15 hours. As long as the expected pre-lithium effect can be achieved, there is no particular limitation. Within the above preferred range, if the temperature is high, the corresponding reaction time is shorter, and conversely, if the temperature is low, the corresponding reaction time is longer.
[0028] The grain sizes of the crystalline Si and crystalline SiO2 prepared within the above preferred range are moderate, both less than 20 nm. The reaction rate of the crystalline SiO2 at this particle size and the pre-lithiation reagent is moderate, and the silicon dioxide is reacted as completely as possible. The crystalline Si at this particle size can also ensure that the finally prepared silicon-oxygen composite material has excellent cycle stability.
[0029] More preferably, the primary calcination is carried out at a temperature of 700 to 900° C. and for a time of 2 to 6 hours.
[0030] The silicon oxide material SiO x The median particle size D50 is 1.0 to 10.0 μm, preferably 4.0 to 6.0 μm; the purity is 99.99%.
[0031] The inert atmosphere is selected from one or more of argon, nitrogen, helium and neon.
[0032] In step (2), a special pre-lithiation reagent, a lithium carbon compound, is used to pre-lithiate the silicon oxide compound through secondary calcination, so that the silicon dioxide in the disproportionate silicon oxide material is converted into lithium metasilicate, thereby improving the initial efficiency of the negative electrode material; at the same time, due to the use of the disproportionate silicon oxide material, the pre-lithiation reaction is more thorough, the residual lithium carbide is low, and it is more stable in the air than conventional pre-lithiation reagents such as metallic lithium and lithium hydride, and it is not easy to generate residual alkali, thereby avoiding the problem of high residual alkali; and the use of this raw material can leave a layer of carbon on the surface during pre-lithiation, thereby achieving the effect of in-situ carbon coating, realizing simultaneous pre-lithiation and carbon coating, and solving the disadvantages of traditional pre-lithiation and carbon coating being carried out in steps.
[0033] Experiments have found that when using other highly active pre-lithiation reagents such as lithium hydride, the residual alkali content is relatively high, whether the method is to coat the carbon before pre-lithiation or to coat the carbon after pre-lithiation. Test results show that the pH value of the materials made by both methods is around 12, which greatly affects the cycle performance of the material.
[0034] Preferably, the lithium carbon compound is selected from Li2C2, Li6C2, Li8C3, Li6C3, Li4C3, Li4C5, Li4C, LiC6, LiC 12 ,LiC 18 One or more of; further preferably, one or more selected from Li6C2, Li8C3, Li4C.
[0035] It has been found through experiments that the use of the above further preferred lithium-carbon compound can obtain a carbon coating layer of suitable thickness while achieving excellent pre-lithiation effect.
[0036] In step (2), when the amount of lithium-carbon compound used is too much, a lot of carbon will remain, which will easily lead to a decrease in the overall capacity of the negative electrode material and an increase in the specific surface area, which is not conducive to the stability of the slurry. The lithium-carbon compound is likely to remain and react with water to cause excessive alkalinity. When the amount of lithium-carbon compound used is too little, the lithium replenishment effect cannot be achieved, the coating is poor, and the first efficiency of the finally assembled battery is reduced and the conductivity is poor.
[0037] Preferably, the mass ratio of the disproportionate silicon-oxygen material to the lithium-carbon compound is 1:0.1-1.0.
[0038] More preferably, the mass ratio of the disproportionated silicon-oxygen material to the lithium-carbon compound is 1:0.1-0.3, and more preferably 1:0.13-0.22.
[0039] It has been found through experiments that the above further preferred mass ratio can ensure that the residual carbon content in the pre-lithiation silicon oxide material is 3-6wt% by mass, which is conducive to forming a carbon coating layer of suitable thickness, so that the first efficiency of the final assembled battery is higher than 90%.
[0040] Regarding the mixing of the disproportionate silicon-oxygen material and the lithium-carbon compound, stirring or ball milling can be used to fully mix them so that the lithium-carbon compound uniformly and comprehensively covers the disproportionate silicon-oxygen material.
[0041] The secondary calcination temperature is 500-900° C. and the time is 0.5-8 hours. The calcination temperature can ensure that the disproportionated silicon-oxygen material and the lithium-carbon compound react fully and form a carbon coating layer on the surface of the silicon-oxygen material.
[0042] The test found that if the secondary calcination temperature is too low, such as 400°C, the silicon oxide material and lithium carbide will basically not react, and the pre-lithium effect cannot be achieved; no carbon layer remains on the surface of the disproportionate silicon oxide material, and the conductivity of the material is poor. If the secondary calcination temperature is too high, it is easy to cause silicon grain growth.
[0043] More preferably, the secondary calcination temperature is 650-800°C.
[0044] The inert atmosphere is selected from one or more of argon, nitrogen, helium and neon.
[0045] In step (3), the use of an organic silicon source for coating can isolate the water in the aqueous slurry to avoid initiating reaction gas production, and can also coat the remaining very small amount of lithium carbon compound, while inhibiting the dissolution of lithium silicate salts, thereby reducing the pH value of the material to a certain extent; more importantly, the organic silicon source has a higher affinity with the silicon-oxygen material, which is more conducive to improving the tightness of the coating. Further breaking up and screening can solve the adhesion between particles generated during high-temperature roasting.
[0046] Experiments have found that if the organic silicon source coating is replaced by carbon coating, gas production cannot be effectively avoided; if the organic silicon source coating is replaced by other hydrophobic materials, such as lauric acid, stearic acid, etc., the coating effect of the hydrophobic layer is poor, gas production is easy, and it may react with the lithium metasilicate in the material to destroy the material structure.
[0047] The organic silicon source is selected from one or more of silane coupling agent, silicone oil, high temperature vulcanized silicone rubber, liquid silicone rubber and silicone resin.
[0048] The silane coupling agent is selected from any one or two or more of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, vinyl tributoxysilane, acryl trimethoxysilane, acryl triethoxysilane, acryl tripropoxysilane, acryl tributoxysilane, butenyl trimethoxysilane, butenyl triethoxysilane, butenyl tripropoxysilane, butenyl tributoxysilane, vinyl tri(β-methoxyethoxy)silane, γ-aminopropyl triethoxysilane, γ-chloropropyl trimethoxysilane, and vinyl trichlorosilane; preferably, one or more of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, vinyl tri(β-methoxyethoxy)silane, and γ-aminopropyl triethoxysilane.
[0049] The silicone oil refers to a linear polysiloxane product that remains in a liquid state at room temperature. Specifically, it can be selected from one or more of methyl silicone oil, ethyl silicone oil, phenyl silicone oil, methyl hydrogen silicone oil, methyl phenyl silicone oil, and methyl chlorophenyl silicone oil. The methyl silicone oil is, for example, dimethyl silicone oil, and the ethyl silicone oil is, for example, diethyl silicone oil.
[0050] The high temperature vulcanized silicone rubber refers to an elastomer which is vulcanized under heating and pressure with a high molar mass linear polydimethyl (or methyl vinyl, methylphenylvinyl, methyltrifluoropropyl, etc.) siloxane as the base polymer, mixed with reinforcing fillers and vulcanizers (organic silicon oxides), etc.
[0051] The liquid silicone rubber refers to a base material with self-leveling or thixotropic properties, which is prepared from linear polyorganosiloxane with a medium degree of polymerization as a basic polymer, fillers, various auxiliary agents and additives.
[0052] The silicone resin is a thermosetting polysiloxane polymer with a highly cross-linked structure, which is generally prepared from an organic chlorosilane mixture or an organic ethoxysilane through hydrolysis and polycondensation reactions in a mixed solvent.
[0053] Preferably, the organic silicon source is selected from silane coupling agent and / or silicone oil.
[0054] When the amount of the organosilicon source is too much, the coating amount may be too much, the coating layer is too thick, the conductivity is poor, the cycle is poor, the material performance cannot be exerted, and the capacity is reduced; when the amount of the organosilicon source is too little, the coating effect cannot be achieved, the hydrophobic effect cannot be obtained, the processing performance is poor, the silicon grains are prone to side reactions and gas production. Preferably, the mass ratio of the pre-lithiation silicon oxygen material to the organosilicon source is 1:0.001-0.1; more preferably 1:0.005-0.05.
[0055] The coating includes liquid phase coating or gas phase coating;
[0056] When the coating is selected from liquid phase coating, it specifically includes:
[0057] Mixing an organic silicon source with an organic solvent to obtain an organic silicon source solution, uniformly mixing the pre-lithiation silicon-oxygen material with the organic silicon source solution, and removing the organic solvent by drying;
[0058] The organic silicon source is selected from one or more of silane coupling agent, silicone oil, high temperature vulcanized silicone rubber, liquid silicone rubber, and silicone resin;
[0059] The organic solvent is selected from one or more of ethanol, ether, acetone, acetaldehyde and tetrahydrofuran.
[0060] Preferably, the concentration of the organic silicon source solution is 1 to 40 wt %, more preferably 1 to 8 wt %.
[0061] The mixing process is accompanied by stirring at a speed of 100 to 600 rpm; the mixing time is the coating time, preferably 0.5 to 10 h.
[0062] The drying is carried out at 40-80° C., and the organic solvent is fully removed after drying; if the organic silicon source is selected from a silane coupling agent, the small molecular substances produced by hydrolysis are simultaneously dried and removed.
[0063] When the coating is selected from gas phase coating, it specifically includes:
[0064] The organic silicon source is evaporated into gas by heating, and then adsorbed on the surface layer of the pre-lithiated silicon-oxygen material;
[0065] The organic silicon source is selected from silicone oil and / or silicone resin.
[0066] The organic silicon source has a higher affinity with the silicon-oxygen material, which is beneficial to improve the tightness of the coating. After high-temperature evaporation, the small molecular compounds produced by the reaction of the organic silicon source with the silicon-oxygen material will be evaporated and removed at high temperature.
[0067] The invention also discloses a lithium ion battery, which adopts the silicon-oxygen composite material for lithium ion batteries.
[0068] According to tests, the lithium-ion battery assembled with the silicon-oxygen composite material for lithium-ion batteries prepared by the present invention has excellent first coulombic efficiency, first reversible capacity and cycle stability.
[0069] Compared with the prior art, the present invention has the following advantages:
[0070] The preparation method of the silicon-oxygen composite material for lithium-ion batteries disclosed in the present invention is to disproportionate the silicon-oxygen material, use a lithium-carbon compound for pre-lithiation, and then use organic silicon for coating, and precisely control the reaction conditions and parameter ranges of each step, so as to give play to the synergistic effect of each step, and obtain unexpected pre-lithiation effect and pH reduction effect. By using lithium carbide as a pre-lithiation reagent, it is not easy to generate residual alkali, and it is not easy to cause alkalinity to increase. In addition, the carbon produced as a by-product of the pre-lithiation reaction can be coated on the surface of the silicon material, which is conducive to promoting the coating of the silicon material by the carbon material. Furthermore, the coating organic silicon layer is used to improve the hydrophobicity of the material, inhibit gas production, and at the same time, it can inhibit the dissolution of lithium silicate and reduce the pH value of the material to a certain extent, solve the gas production problem of the negative electrode slurry during the processing, and make the material more suitable for the existing negative electrode slurry system.
[0071] The silicon-oxygen composite material prepared by the above method has a multi-layer core-shell structure, and the assembled lithium-ion battery has excellent first coulombic efficiency, first reversible capacity and high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 The XRD pattern of the disproportionate silicon-oxygen material prepared in step (1) of the embodiment;
[0073] Figure 2 This is a TEM photo of the silicon-oxygen composite material for lithium-ion batteries prepared in Example 1. DETAILED DESCRIPTION
[0074] In this specification, unless otherwise specified, symbols, units, abbreviations, and terms have ordinary meanings. For example, when "-" or "-" is used to express a numerical range, both endpoints are included and the unit is common.
[0075] The raw materials or reagents used in the present invention are all purchased from mainstream manufacturers in the market. Those without indicating the manufacturer or the concentration are all analytically pure raw materials or reagents that can be routinely obtained, as long as the expected effect can be played, there is no particular restriction. The homogenizer, stirrer, coating machine, drying equipment, thickness gauge and other instruments and equipment used in the present embodiment are all purchased from major manufacturers in the market, as long as the expected effect can be played, there is no particular restriction. In the present embodiment, if specific techniques or conditions are not indicated, the techniques or conditions described in the literature in this area or according to the product specification are carried out.
[0076] In order to better understand the above technical solution, the present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. It should be noted that, unless otherwise specifically stated, all percentages, parts, and ratios used in the present invention are based on mass.
[0077] Example 1
[0078] (1) 2.0 kg of SiO (purchased from Yunnan Lichen New Material Technology Co., Ltd., D50 = 5 μm, purity 99.99%) was put into an atmosphere furnace, calcined at 800 ° C for 4 h under an argon atmosphere, and then taken out after cooling to room temperature to obtain a disproportionate silicon oxide material. The reaction equation of this step is shown in the following formula (I):
[0079] 2SiO=Si+SiO2 (Ⅰ).
[0080] (2) Under an argon atmosphere, 1.0 kg of the above-mentioned disproportionated silicon oxide material and 0.16 kg of Li6C2 were put into a mixer and mixed for 1 hour to obtain a mixed powder material, which was put into an atmosphere furnace and calcined at 700° C. for 4 hours under an argon atmosphere, and then cooled to room temperature to obtain a pre-lithiated silicon oxide material. The reaction equation of this step is shown in the following formula (II):
[0081] 2Li6C2+9SiO2=6Li2SiO3+3Si+4C (II).
[0082] (3) 1.0 kg of the above-mentioned pre-lithiated silicon-oxygen material was added to 0.67 kg of an acetone solution of vinyltrimethoxysilane (concentration of 3.0 wt %, mass of solute of 0.02 kg), stirred at 600 rpm for 0.5 h, filtered and dried at 80 ° C, and then fully dispersed using a disperser, and sieved with a 1000 mesh sieve to obtain a silicon-oxygen composite material for lithium-ion batteries.
[0083] After testing, the median particle size D50 was 5.4 μm and the pH value was 8.2.
[0084] Figure 1 This is the XRD pattern of the disproportionate silicon-oxygen material prepared in step (1) of this embodiment. By observing the pattern, it can be confirmed that after high-temperature calcination for disproportionation reaction, SiO is successfully converted into crystalline silicon and crystalline silicon dioxide.
[0085] Figure 2 This is a TEM image of the silicon-oxygen composite material for lithium-ion batteries prepared in this example. A three-layer structure can be found in the image.
[0086] Example 2
[0087] (1) 2.0 kg of SiO 0.8 (purchased from Yunnan Lichen New Material Technology Co., Ltd., D50 = 6 μm, purity 99.99%) was put into an atmosphere furnace, calcined at 700 ° C for 6 hours under an argon atmosphere, and then taken out after cooling to room temperature to obtain a disproportionate silicon oxide material. The reaction equation of this step is shown in the following formula (I):
[0088] 5SiO 0.8 =3Si+2SiO2 (III).
[0089] (2) Under an argon atmosphere, 1.0 kg of the above-mentioned disproportionated silicon oxide material and 0.13 kg of Li4C were put into a mixer and mixed for 1 hour to obtain a mixed powder material, which was put into an atmosphere furnace and calcined at 650° C. for 5 hours under an argon atmosphere, and then cooled to room temperature to obtain a pre-lithiated silicon oxide material. The reaction equation of this step is shown in the following formula (II):
[0090] Li4C+3SiO2=2Li2SiO3+Si+C (IV).
[0091] (3) 1.0 kg of the above-mentioned pre-lithiated silicon-oxygen material was added to 0.167 kg of an acetone solution of vinyltrimethoxysilane (concentration of 3.0 wt %, mass of solute of 0.005 kg), stirred at 600 rpm for 0.5 h, filtered and dried at 80 ° C, and then fully dispersed using a disperser, and sieved with a 1000 mesh sieve to obtain a silicon-oxygen composite material for lithium-ion batteries.
[0092] After testing, the median particle size D50 was 6.2 μm and the pH value was 8.9.
[0093] Example 3
[0094] (1) 2.0 kg of SiO 1.5 (purchased from Yunnan Lichen New Material Technology Co., Ltd., D50 = 4 μm, purity 99.99%) was put into an atmosphere furnace, calcined at 900 ° C for 2 h under an argon atmosphere, and then taken out after cooling to room temperature to obtain a disproportionate silicon oxide material. The reaction equation of this step is shown in the following formula (I):
[0095] 4SiO 1.5 =Si+3SiO2 (V).
[0096] (2) Under an argon atmosphere, 1.0 kg of the above-mentioned disproportionated silicon oxide material and 0.22 kg of Li8C3 were put into a mixer and mixed for 1 hour to obtain a mixed powder material, which was put into an atmosphere furnace and calcined at 800°C for 3 hours under an argon atmosphere, and then cooled to room temperature to obtain a pre-lithiated silicon oxide material.
[0097] Li8C3+6SiO2=4Li2SiO3+2Si+3C (VI).
[0098] (3) 1.0 kg of the above-mentioned pre-lithiated silicon-oxygen material was added to 1.67 kg of an acetone solution of vinyltrimethoxysilane (concentration of 3.0 wt %, mass of solute of 0.05 kg), stirred at 600 rpm for 0.5 h, filtered and dried at 80 ° C, and then fully dispersed using a disperser, and sieved with a 1000 mesh sieve to obtain a silicon-oxygen composite material for lithium-ion batteries.
[0099] After testing, the median particle size D50 was 4.6 μm and the pH value was 8.7.
[0100] Example 4
[0101] The preparation process is basically the same as that of Example 1, except that the temperature of high-temperature calcination in step (1) is replaced with 600° C. and the time is replaced with 5 h.
[0102] Example 5
[0103] The preparation process is basically the same as that of Example 1, except that the temperature of the secondary calcination in step (2) is replaced with 500°C.
[0104] Example 6
[0105] The preparation process is basically the same as that of Example 1, except that the mass of Li6C2 added in step (2) is replaced by 0.1 kg.
[0106] Example 7
[0107] The preparation process is basically the same as that of Example 1, except that the mass of Li6C2 added in step (2) is replaced by 0.3 kg.
[0108] Example 8
[0109] The preparation process is basically the same as that of Example 1, except that the 0.16 kg of Li6C2 added in step (2) is replaced by 0.29 kg of Li2C2.
[0110] Example 9
[0111] The preparation process is basically the same as that of Example 1, except that the vinyltrimethoxysilane in step (3) is replaced by an equal mass of vinyltri(β-methoxyethoxy)silane.
[0112] Example 10
[0113] Steps (1) and (2) are exactly the same as those in Example 1.
[0114] (3) 1.0 kg of the above-mentioned pre-lithiated silicon-oxygen material and 0.02 kg of dimethyl silicone oil (purchased from Gaide Chemical Network, boiling point 180° C.) were put into an evaporator, heated to 250° C., rotated at 5 rpm, and kept warm for 2 h. After gradually cooling, the mixture was fully dispersed using a disperser and sieved with a 1000-mesh sieve to obtain a silicon-oxygen composite material for lithium-ion batteries.
[0115] Comparative Example 1
[0116] The preparation process is substantially the same as that of Example 1, except that step (1) is not used, and the silicon oxide material SiO is directly subjected to pre-lithiation in step (2).
[0117] Comparative Example 2
[0118] The preparation process is basically the same as that of Example 1, except that step (2) is not used, and the disproportionated silicon oxide material is directly subjected to the coating step (3).
[0119] Comparative Example 3
[0120] The preparation process is basically the same as that of Example 1, except that step (3) is not adopted, and the pre-lithiated silicon-oxygen material is directly dispersed and sieved with a 1000-mesh sieve.
[0121] Comparative Example 4
[0122] The preparation process is basically the same as that of Example 1, except that 0.16 kg of Li6C2 in step (2) is replaced by 0.1 kg of lithium hydride.
[0123] Comparative Example 5
[0124] Steps (1) and (2) are exactly the same as those in Example 1.
[0125] (3) The pre-lithiated silicon-oxygen material prepared as above is placed in a chemical vapor deposition furnace, and after argon replacement, methane gas is introduced, and the temperature of the chemical vapor deposition furnace is raised to 700°C and kept warm for 4 hours to perform chemical vapor phase cracking deposition. After the deposition is completed, the introduction of methane gas is stopped, and the carbon-coated pre-lithiated silicon-oxygen material is obtained after natural cooling.
[0126] After testing, the median particle size D50 was 5.7 μm and the pH value was 11.1.
[0127] Comparative Example 6
[0128] The preparation process is basically the same as that of Example 1, except that the temperature of high temperature calcination in step (1) is replaced with 1000°C.
[0129] Comparative Example 7
[0130] The preparation process is basically the same as that of Example 1, except that the temperature of the secondary calcination in step (2) is replaced with 1000°C.
[0131] Comparative Example 8
[0132] The preparation process is basically the same as that of Example 3, except that the temperature of the secondary calcination in step (2) is replaced with 400°C.
[0133] Comparative Example 9
[0134] The preparation process is basically the same as that of Example 1, except that the mass of Li6C2 added in step (2) is replaced by 0.05.
[0135] Comparative Example 10
[0136] The preparation process is basically the same as that of Example 1, except that the mass of Li6C2 added in step (2) is replaced by 0.5.
[0137] Comparative Example 11
[0138] The preparation process is basically the same as that of Example 1, except that the 0.67 kg acetone solution of vinyltrimethoxysilane (concentration of 3.0 wt %, mass of solute of 0.02 kg) added in step (3) is replaced by 0.67 kg ethanol solution of lauric acid (concentration of 3.0 wt %, mass of solute of 0.02 kg).
[0139] The silicon-oxygen composite materials prepared in the above-mentioned embodiments and comparative examples were assembled into batteries and subjected to electrochemical performance tests. The specific assembly and testing processes are as follows.
[0140] 1. Preparation of liquid lithium-ion batteries
[0141] (1) Preparation of positive electrode
[0142] The positive electrode active material lithium nickel cobalt manganese oxide (NCM811), conductive agent SuperP, carbon nanotubes, binder polyvinylidene fluoride (PVDF) are mixed with N-methylpyrrolidone (NMP) in a mass ratio of 97:1:0.5:1.5 to form a positive electrode slurry (solid content of 70%), coated on the current collector aluminum foil, dried at 70°C, cold pressed at 4MPa at room temperature, and then trimmed, cut, and striped, and the pole ears are welded to make positive electrode sheets.
[0143] (2) Preparation of negative electrode
[0144] Under an inert protective atmosphere, the silicon-oxygen composite material for lithium-ion batteries of the embodiment of the present invention or the comparative material of the comparative example is fully mixed with natural graphite (particle size D50 = 15 μm, purchased from B&T Company) in a ratio of 1:9 to obtain a negative electrode active material, and the negative electrode active material, conductive agent SuperP, adhesive PVDF are mixed with NMP in a mass ratio of 97.5:1.0:1.5 to form a negative electrode slurry (solid content of 50%), which is coated on the current collector copper foil, dried at 100°C, cold pressed at room temperature at 4 MPa, and then trimmed, cut, and stripped, and the pole ears are welded to make a negative electrode sheet.
[0145] (3) Assembly of lithium-ion batteries
[0146] Using a PE porous polymer film as a separator, the prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets, and the bare battery cell is wound; the bare battery cell is placed in an aluminum plastic shell package, and dried at 100°C to a moisture content of less than 100 ppm under a relative vacuum pressure of -0.95×105Pa. The electrolyte is injected into the dried bare battery cell, wherein the electrolyte is composed of ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) (EC:EMC:DEC volume ratio = 1:1:1) and LiPF6 (concentration 1.0M), and the battery is packaged and left to stand to make a soft-pack lithium-ion battery.
[0147] 2. Testing of lithium-ion batteries
[0148] 2.1 First Coulomb efficiency test:
[0149] The battery prepared above was formed and divided into different capacities using a battery test cabinet. The formation process was to charge at a constant current of 0.05C for 2.0h, and then at a constant current of 0.15C for 2.5h; the division process was to charge at a constant current of 0.33C to 4.2V, and then at a voltage of 4.2V, constant voltage charge to a cutoff current of 0.02C, and discharge at 0.33C to 2.5V; the sum of the above charge capacity and the discharge capacity were recorded as the first charge capacity and the first discharge capacity, and the first reversible specific capacity (mAh / g) was calculated, and the first charge specific capacity, the first discharge specific capacity and the first coulombic efficiency were calculated.
[0150] 2.2 Normal temperature cycle performance test:
[0151] At 25°C, charge the battery to 4.2V at 0.5C constant current and constant voltage, cut off current 0.02C, leave for 5 minutes, then discharge to 2.5V at 1C constant current, leave for 5 minutes. Repeat this cycle, calculate the capacity retention rate of the 500th cycle after 500 cycles of charge / discharge, and the calculation formula is as follows:
[0152] Capacity retention rate at the 500th cycle at room temperature (%)=(discharge capacity at the 500th cycle / discharge capacity at the 1st cycle)×100%.
[0153] The pH test of the silicon-oxygen composite materials prepared in the above embodiments and comparative examples is carried out as follows:
[0154] 5 g of the prepared silicon-oxygen composite material and 45 g of deionized water were stirred and mixed thoroughly, and solid-liquid separation was performed using a suction filtration device. The pH value of the liquid phase was tested using a potentiometric pH meter, and recorded as the pH value of the silicon-oxygen composite material.
[0155] The pH values of the silicon-oxygen composite materials prepared in the above embodiments and comparative examples, as well as the data of the assembled batteries and the electrochemical performance tests are all listed in the following Table 1.
[0156] Table 1
[0157]
[0158]
[0159] According to the data in Table 1, by comparing Examples 1 to 3, it can be found that by using Li6C2, Li4C or Li8C3 as the pre-lithiation agent and using appropriate temperatures for the two calcinations, the pH values of the prepared silicon-oxygen composite materials are all lower than 9, and the assembled batteries have excellent first coulombic efficiency, first reversible capacity and cycle stability.
[0160] By comparing Example 1 with Examples 4 to 5, it can be found that whether the primary calcination temperature is slightly lower (Example 4) or the secondary calcination temperature is slightly lower, the pH value of the prepared silicon-oxygen composite material will increase to more than 9, and the first coulombic efficiency, first reversible capacity and cycle capacity retention rate data of the assembled battery will decrease.
[0161] By comparing Example 1 with Examples 6 to 7, it can be found that when the amount of pre-lithiation reagent added is too much (Example 7), the pH value of the prepared silicon-oxygen composite material increases, and the first reversible capacity and cycle capacity retention rate data of the assembled battery are significantly reduced.
[0162] By comparing Example 1 and Example 8, it can be found that when Li2C2 is used as the pre-lithiation agent, the first reversible capacity and cycle stability of the battery assembled from the prepared silicon-oxygen composite material both show a significant decrease.
[0163] By comparing Example 1 with Examples 9 to 10, it can be found that replacing the type of the organosilicon source in step (3) or replacing the liquid phase coating with the gas phase coating does not affect the performance of the final assembled battery.
[0164] By comparing Example 1 with Comparative Examples 1 to 3, it can be found that compared with Example 1, the electrochemical performance of the batteries finally assembled in Comparative Examples 1 to 3 is poor. The reason may be that the disproportionation reaction of step 1 was not carried out in Comparative Example 1, resulting in incomplete pre-lithiation reaction in step 2, too much pre-lithiation reagent remaining, resulting in poor performance; no pre-lithiation treatment was used in Comparative Example 2, and the silicon oxide in the material generated irreversible lithium silicate salts during the first charge and discharge process, which irreversibly consumed the lithium ions of the positive electrode, resulting in low first efficiency; the pre-lithiation silicon oxygen material in Comparative Example 3 was not coated with an organic silicon hydrophobic layer, and the residual pre-lithiation reagents in the pre-lithiation process and the lithium silicate salts in the material reacted with water during the slurrying process, resulting in a high pH value and poor cycle performance. It can be proved that the preparation method of the silicon oxygen composite material disclosed in the present invention, the three steps affect each other and are indispensable, otherwise the final assembled battery cannot have excellent first coulomb efficiency, first reversible capacity and cycle stability.
[0165] By comparing Example 1 and Comparative Example 4, it can be found that if the lithium carbon compound disclosed in the present invention is replaced with a common pre-lithiation reagent in the art - lithium hydride, the pH value of the prepared silicon-oxygen composite material is as high as 12.3, and the first coulombic efficiency, first reversible capacity and cycle capacity retention rate of the assembled battery are significantly lower than those in Example 1. Analysis shows that the reason may be that the pre-lithiation reagent uses conventional lithium hydride to replace lithium carbide, and there is no conductive material layer on the surface of the silicon-oxygen material after pre-lithiation, and the material has poor conductivity. In addition, lithium hydride is very active and easily generates residual alkali with moisture and carbon dioxide in the environment, resulting in a significant increase in alkalinity, easy gas production, and poor cycle performance.
[0166] By comparing Example 1 and Comparative Example 5, it can be found that if the coated organic silicon layer in step (3) is replaced by a carbon layer, the pH value of the prepared silicon-oxygen composite material will still increase significantly, up to 11.1, and the first coulombic efficiency and the first reversible capacity of the assembled battery will decrease, especially the cycle capacity retention rate will decrease significantly. Analysis shows that the reason may be that the method of coating the organic silicon layer after the pre-lithium reaction is used instead of the coated carbon layer, but the coating carbon layer causes the capacity of the material to decrease, and it is impossible to prevent the residual pre-lithium reagent and the acid lithium salt from reacting with water, and the pH of the material is high and the cycle performance is poor.
[0167] By comparing Example 1 and Comparative Example 11, it can be found that if the coated organic silicon layer in step (3) is replaced with an organic layer of lauric acid, although the pH value of the prepared silicon-oxygen composite material does not change, the first coulombic efficiency and cycle capacity retention rate of the assembled battery both show a significant decrease, especially the cycle capacity retention rate. The reason for this may be that lauric acid has poor hydrophobicity and is easy to react with lithium metasilicate in the pre-lithiation silicon-oxygen material, which may regenerate silicon dioxide or silicic acid substances, resulting in a decrease in the first efficiency, while the structural stability of the material is destroyed and the cycle performance deteriorates.
[0168] By comparing Example 1 with Comparative Examples 6 to 8, it can be found that whether the temperature of the two calcinations is too low or too high, it is not conducive to the preparation of a battery with excellent first coulombic efficiency, first reversible capacity and cycle capacity retention rate. The reason may be that the disproportionation reaction temperature in Comparative Example 6 is too high, resulting in excessive growth of silicon grains in the silicon-oxygen material, affecting the cycle performance of the material; the reaction temperature in Comparative Example 7 is too high, resulting in excessive growth of silicon grains in the silicon-oxygen material, affecting the cycle performance of the material; the reaction temperature in Comparative Example 8 is too low, resulting in a low degree of pre-lithiation, more pre-lithium reagents remain, resulting in too high pH value of the material, poor capacity and first efficiency and cycle performance of the material.
[0169] By comparing Example 1 with Comparative Examples 9 to 10, it can be found that if the amount of the pre-lithiation reagent added is too low, the first coulombic efficiency of the assembled battery is low. The reason may be that the amount of the pre-lithiation reagent added is small, and part of the silica does not react, which leads to the easy consumption of active lithium ions during the charge and discharge cycle, resulting in a decrease in the first efficiency; if the amount of the pre-lithiation reagent added is too high, the pH value of the prepared silicon-oxygen composite material increases significantly, and the cycle stability decreases significantly. The reason may be that the content of the pre-lithiation reagent added is too much, the reaction is not complete, and the residual amount is large, resulting in an increase in alkalinity.
[0170] The applicant declares that the above is only a specific implementation of the present invention, but the protection scope of the present invention is not limited thereto. The above specific examples are used to illustrate the present invention, which is only used to help understand the present invention and is not used to limit the present invention. A technician in the technical field to which the present invention belongs can also make several simple deductions, deformations, substitutions or combinations based on the concept of the present invention. These deductions, deformations, substitutions or combinations also fall within the scope of the claims of the present invention.
Claims
1. A silicon-oxygen composite material for lithium-ion batteries, It is characterized in that It includes a three-layer structure, which is a silicon-based material core, a conductive carbon layer and an organic silicon coating layer from the inside to the outside; The silicon-based material core comprises single crystal silicon and lithium metasilicate; The organic silicon in the organic silicon coating layer comes from one or more of silane coupling agent, silicone oil, high temperature vulcanized silicone rubber, liquid silicone rubber, and silicone resin; The method for preparing the silicon-oxygen composite material for lithium-ion batteries comprises the following steps: (1) Silicon oxide material SiO x Carry out a calcination to obtain a disproportionate silicon-oxygen material, wherein 0.8≤x≤1.5; The primary calcination temperature is 700-900°C; (2) in an inert atmosphere or under vacuum conditions, the disproportionated silicon-oxygen material is uniformly mixed with a lithium-carbon compound, and then subjected to secondary calcination to obtain a pre-lithiated silicon-oxygen material; The mass ratio of disproportionate silicon-oxygen material to lithium-carbon compound is 1:0.1~0.3; The secondary calcination temperature is 650-800°C; (3) The pre-lithiation silicon-oxygen material is coated with an organic silicon source, and then the pre-lithiation silicon-oxygen material is broken up and sieved to obtain the silicon-oxygen composite material for lithium-ion batteries.
2. The silicon-oxygen composite material for lithium-ion batteries according to claim 1, Features: The pH value of the silicon-oxygen composite material for lithium-ion batteries is 6-10; or, The median particle size of the silicon-based material core is 1.0-10.0 μm; or, The thickness of the conductive carbon layer is 0.1-100 nm; or, The thickness of the organic silicon coating layer is 0.1-100 nm.
3. The silicon-oxygen composite material for lithium-ion batteries according to claim 1, It is characterized in that Step (1) is as follows: Silicon oxide material SiO x Put it into an atmosphere furnace and carry out a roasting process under an inert atmosphere or vacuum conditions; The time of the primary calcination is 0.5 to 50 hours; The inert atmosphere is selected from one or more of argon, nitrogen, helium and neon.
4. The silicon-oxygen composite material for lithium-ion batteries according to claim 1, It is characterized in that In step (2): The lithium carbon compound is selected from Li 2 C 2 , Li 6 C 2 , Li 8 C 3 , Li 6 C 3 , Li 4 C 3 , Li 4 C 5 , Li 4 C. LiC 6 ,LiC 12 ,LiC 18 One or more of; The inert atmosphere is selected from one or more of argon, nitrogen, helium and neon; The secondary calcination time is 0.5 to 8 hours.
5. The silicon-oxygen composite material for lithium-ion batteries according to claim 1, It is characterized in that In step (3): The organic silicon source is selected from one or more of silane coupling agent, silicone oil, high temperature vulcanized silicone rubber, liquid silicone rubber, and silicone resin; The mass ratio of the pre-lithiation silicon-oxygen material to the organic silicon source is 1:0.001-0.
1.
6. The silicon-oxygen composite material for lithium-ion batteries according to claim 5, It is characterized in that The coating includes liquid phase coating or gas phase coating; When the coating is selected from liquid phase coating, it specifically includes: Mixing an organic silicon source with an organic solvent to obtain an organic silicon source solution, uniformly mixing the pre-lithiation silicon-oxygen material with the organic silicon source solution, and removing the organic solvent by drying; The organic silicon source is selected from one or more of silane coupling agent, silicone oil, high temperature vulcanized silicone rubber, liquid silicone rubber, and silicone resin; The organic solvent is selected from one or more of ethanol, ether, acetone, acetaldehyde, and tetrahydrofuran; or, When the coating is selected from gas phase coating, it specifically includes: The organic silicon source is evaporated into gas by heating, and then adsorbed on the surface layer of the pre-lithiated silicon-oxygen material; The organic silicon source is selected from silicone oil and / or silicone resin.
7. The silicon-oxygen composite material for lithium-ion batteries according to claim 1, It is characterized in that The organosilicon source is selected from silane coupling agent and / or silicone oil; The silane coupling agent is selected from any one or more of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tripropoxysilane, vinyl tributoxysilane, acryl trimethoxysilane, acryl triethoxysilane, acryl tripropoxysilane, acryl tributoxysilane, butenyl trimethoxysilane, butenyl triethoxysilane, butenyl tripropoxysilane, butenyl tributoxysilane, vinyl tris (β-methoxyethoxy) silane, γ-aminopropyl triethoxysilane, γ-chloropropyl trimethoxysilane, and vinyl trichlorosilane; The silicone oil is selected from one or more of methyl silicone oil, ethyl silicone oil, phenyl silicone oil, methyl hydrogen silicone oil, methyl phenyl silicone oil, and methyl chlorophenyl silicone oil.
8. The silicon-oxygen composite material for lithium-ion batteries according to claim 7, It is characterized in that The silane coupling agent is selected from one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl tripropoxy silane, vinyl tri(β-methoxyethoxy) silane, and γ-aminopropyl triethoxy silane.
9. A lithium ion battery, It is characterized in that The silicon-oxygen composite material for lithium-ion batteries according to any one of claims 1 to 8 is used.