A catalyst for preparing higher alcohols by hydrogenating CO2 and its preparation method and application
By introducing Fe and Cs additives into Cu-Co-based catalysts, the catalyst composition and preparation method are optimized, and the problem of low selectivity and conversion of Cu-Co catalysts for higher alcohols is solved, and efficient CO2 conversion into higher alcohols is achieved. Have industrial potential.
Patent Information
- Application Number
- CN202211540960.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-02
AI Technical Summary
The existing Cu-Co-based catalysts have low selectivity for C2+ alcohols, and the CO2 conversion rate is not ideal, making it difficult to effectively promote the conversion of CO2 into higher alcohols. The cost of precious metal catalysts is high, which limits industrial applications.
By introducing transition metal additives Fe and alkali metal additives Cs, the composition and preparation method of Cu-Co-based catalysts are optimized, and the preparation method of combining co-precipitation method and equal volume impregnation method is used to form a CuxCo1My-zA catalyst to enhance the activation of the catalyst CO2 and promote C-C coupling capacity.
It significantly improves CO2 conversion and selectivity of higher alcohols, the catalyst has excellent stability and reactivity, a simple preparation method, and has industrial application prospects.
Smart Images

Figure BDA0003977607810000061 
Figure BDA0003977607810000062 
Figure BDA0003977607810000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a catalyst for preparing higher alcohols by hydrogenating CO2, and a preparation method and application thereof. Background Art
[0002] CO2 is an abundant carbon resource. By coupling the green hydrogen obtained by electrolysis of water with new energy, CO2 can be catalytically converted into clean fuels and high-value-added chemicals. This can not only alleviate the global warming problem caused by greenhouse gas emissions, but also reduce the over-reliance on fossil-based energy. It is a very promising way to utilize CO2 resources. Among them, the alcohol products synthesized by CO2 hydrogenation can be used as alternative fuels, fuel additives, solvents and chemical intermediates. The synthesis of methanol does not require carbon chain growth. The excellent CuZnAl methanol synthesis catalyst has been commercialized, but the more attractive higher alcohols (C 2+ The synthesis of 2-hydroxy-2-nitropropene (2-hydroxy-2-nitropropene) faces severe challenges due to the difficult-to-control CC coupling.
[0003] The chemical inertness of CO2 usually requires a high temperature for its catalytic conversion. In the process of CO2 hydrogenation, the endothermic reverse water gas shift reaction (CO2+H2→CO+H2O) is inevitable, and the CO produced can be used to obtain rich hydrocarbon products through Fischer-Tropsch synthesis. Therefore, the CO* produced by the enhanced reverse water gas shift reaction and the CH produced by the Fischer-Tropsch process are x * The efficient coupling of species is the synthesis of C 2+ The active sites used for the hydrogenation of CO2 to produce higher alcohols need to have the ability to activate CO2, dissociate CO to form CH x * species and the ability to non-dissociatively adsorb CO, therefore, the development of multifunctional active sites is extremely critical.
[0004] The key to the preparation of higher alcohols by hydrogenation of CO2 lies in the catalyst. The catalysts currently used for the preparation of higher alcohols by hydrogenation of CO2 are mainly divided into two categories: precious metal catalysts and non-precious metal catalysts. Precious metal catalysts mainly include Rh, Pt, Pd and Au, etc. Patent CN 111185160 A discloses a catalyst with precious metal Au as an active component. Au is fixed on an oxide carrier by a colloid method. The catalyst can improve the dispersion of precious metals and the interaction between the precious metal and the carrier, and reduce metal agglomeration. The catalyst prepared by this method has good catalytic reaction activity and selectivity in the carbon dioxide hydrogenation reaction. However, its industrial application is limited due to the small reserves of precious metals and the high price.
[0005] Non-precious metal catalysts are mainly developed based on catalysts for preparing higher alcohols from synthesis gas. Existing patents have reported various catalytic systems for preparing higher alcohols from CO2 hydrogenation, including Cu-based (CN113751062 A, CN110465302A), Mo-based (CN109201096B), and Fe-based (CN 111659432 A). Among them, Cu-based catalysts have great development potential due to their high catalytic activity and relatively low cost advantages, and have milder operating conditions than Mo-based catalysts.
[0006] The modified Fischer-Tropsch synthesis catalyst is mainly based on Cu-Fe and Cu-Co based catalysts. Cu-based catalysts have high reverse water gas shift activity and can convert CO2 into CO. Co-based catalysts show excellent activity and selectivity for higher alcohols in the Fischer-Tropsch reaction. Therefore, Cu-Co based catalysts are considered to be very promising catalysts for synthesizing higher alcohols. Patent CN 102489301B discloses a structured Cu-Co based catalyst and a preparation method thereof. An in-situ synthesis method is used to obtain a copper-cobalt-aluminum hydrotalcite film precursor on a treated aluminum substrate, which is perpendicular to the substrate, has uniformly dispersed wafers, and has strong adhesion to the substrate. After calcination and reduction under certain conditions, a uniformly dispersed nanoparticle catalyst is obtained. It is applied to the preparation of higher alcohols from synthesis gas with good results.
[0007] However, the data show that only Cu-Co based catalysts have a 2+ The alcohol selectivity is still low, and the conversion rate of CO2 is not ideal. Therefore, it is particularly important to increase the interaction between the components and improve their ability to activate carbon dioxide by screening and adding various metal additives and alkali metal additives. This patent combines the two, and then introduces the preferred metal additives and alkali metal additives to modify the obtained Cu-Co-based catalyst, which can synergistically catalyze the reverse water gas shift reaction and the Fischer-Tropsch reaction, enrich the content of C1 intermediate species, effectively promote CC coupling, and efficiently convert CO2 into higher alcohols in one step. Summary of the invention
[0008] The purpose of the present invention is to provide a catalyst for preparing higher alcohols by hydrogenation of CO2, which mainly strengthens the CC coupling in the process of CO2 hydrogenation so as to have higher reaction activity and selectivity of target product higher alcohols.
[0009] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0010] In one aspect, the present invention provides a catalyst for preparing higher alcohols by hydrogenation of CO2, wherein the catalyst has the molecular formula Cu x Co1M y-zA, where M is a metal promoter, A is an alkali metal promoter, x and y are the molar ratios of metal Cu and metal promoter M to metal Co, respectively, and the value ranges of x and y are 0.5-2 and 0.5-1.5, respectively. z is the mass fraction of the alkali metal promoter in the catalyst, and the value range of z is 0.5-5%.
[0011] Preferably, M is selected from any one of transition metal elements, alkaline earth metal elements and third main group elements. Further preferably, the transition metal element is selected from any one of Fe, Zn, Mn, Cu, Zr and Ce, the alkaline earth metal element is selected from any one of Ca, Mg and Ba, and the third main group element is selected from any one of Al, Ga and In. Further preferably, M is selected from any one of transition metal elements Fe and Zn. Most preferably, M is Fe.
[0012] Preferably, A is selected from any one of Li, Na, K, Rb and Cs, more preferably, A is selected from any one of Na, K and Cs, and most preferably, A is Cs.
[0013] Preferably, the value range of z is 0.5-5%, more preferably, the value range of z is 0.5%, 3%, 5%, and most preferably, the value of z is 3%.
[0014] Preferably, the value range of x is 0.5-2, more preferably, the value range of x is 0.5, 1, 2, and most preferably, x is 1.
[0015] Preferably, the value range of y is 0.5-1.5, and further preferably, the value range of y is 1.5.
[0016] The present invention provides a method for preparing the above catalyst, wherein the preparation method is selected from one of the following methods:
[0017] Preparation method 1: co-precipitation method, comprising the following steps:
[0018] (1a) dissolving Cu salt, Co salt and M salt in water to obtain solution L1;
[0019] (1b) dissolving a precipitant containing A in water to obtain a solution L2;
[0020] (1c) Solution L1 and solution L2 are added dropwise at the same time, and after the addition is completed, Cu is obtained by aging, separation, washing, drying and roasting. x Co1M y-z A.
[0021] Preparation method 2: Combination of coprecipitation method and equal volume impregnation method, including the following steps:
[0022] (2a) dissolving Cu salt, Co salt and M salt in water to obtain solution L1;
[0023] (2b) dissolving the precipitant without A in water to obtain solution L3;
[0024] (2c) Solution L1 and solution L3 are added dropwise at the same time, and after the addition is completed, Cu is obtained by aging, separation, washing, drying and roasting. x Co1M y ;
[0025] (2d) Dissolving a precipitant containing A or a salt of A in water to obtain a solution L4, and loading the solution L4 onto Cu using an equal volume impregnation method. x Co1M y After aging, drying and calcination, Cu x Co1M y-z A.
[0026] Preferably, the Cu salt, Co salt, and M salt are selected from any one of their corresponding nitrates, chlorides, sulfates, carbonates, and acetates, and the A salt is selected from its corresponding nitrate or chloride. Most preferably, the Cu salt, Co salt, and M salt are selected from their corresponding nitrates, and the A salt is selected from its corresponding nitrate.
[0027] Preferably, the precipitant containing A is selected from any one of Na2CO3, K2CO3, Rb2CO3, Cs2CO3, Na2HCO3, K2HCO3, LiOH, NaOH, KOH, RbOH and CsOH; further preferably, the precipitant containing A is selected from K2CO3 or Cs2CO3; most preferably, the precipitant containing A is Cs2CO3.
[0028] Preferably, the precipitant not containing an alkali metal auxiliary agent A is selected from any one of (NH4)2CO3, NH4HCO3 and NH3·H2O, and most preferably, the precipitant not containing an alkali metal auxiliary agent A is (NH4)2CO3.
[0029] Preferably, the salt of the alkali metal auxiliary agent A is selected from any one of NaCl, KCl, NaNO3, and KNO3; more preferably, the salt of the alkali metal auxiliary agent A is selected from NaNO3 and KNO3; most preferably, the salt of the alkali metal auxiliary agent A is KNO3.
[0030] Preferably, the separation is a conventional separation method in the art, including but not limited to liquid separation, extraction, distillation, fractionation, filtration and centrifugation; most preferably, the separation is centrifugation.
[0031] Preferably, the water is selected from distilled water, double distilled water, and deionized water; most preferably, the water is deionized water.
[0032] Preferably, in step 1a) and step 2a), the total molar concentration of metal ions in the solution L1 is 0.5-2 mol / L;
[0033] Preferably, in step 1b) and step 2b), the molar concentration of the precipitant in the solutions L2 and L3 is 0.5-2 mol / L;
[0034] Preferably, in step (1c) and step 2c), the dropping temperature is 20-80°C, more preferably 25-60°C, the dropping time is 0.5-48h, more preferably 2-12h, the pH of the mixed solution of L1 and L3 is 6-12, more preferably 8-10, the stirring speed during dropwise addition is 300-800r / min, more preferably 400-700r / min; centrifugation and washing are 0-10 times, more preferably 2-8 times; the drying temperature is 60-150°C, more preferably 80-120°C, the time is 6-48h, more preferably 8-24h; the calcination temperature is 300-500°C, more preferably 350-450°C, the time is 2-10h, more preferably 3-8h, and the drying and calcination atmosphere is selected from at least one of air, nitrogen and argon.
[0035] Preferably, in step 2d), the aging temperature is 20-30°C, the aging time is 2-48h, more preferably, 4-12h, the drying temperature is 60-150°C, more preferably, 80-120°C, the drying time is 6-48h, more preferably, 8-24h, the calcination temperature is 300-500°C, more preferably, 350-450°C, the calcination time is 2-10h, more preferably, 3-8h, and the aging, drying and calcination atmospheres are selected from at least one of air, nitrogen and argon.
[0036] The catalyst provided by the present invention is preferably used for the production of higher alcohols by fixed-bed CO2 hydrogenation.
[0037] Preferably, the method comprises the following steps:
[0038] 1) tabletting the catalyst, selecting a 40-60 mesh catalyst and mixing it with 40-60 mesh quartz sand particles, and then loading the mixture into a fixed bed reactor;
[0039] 2) before the reaction, the catalyst is reduced at 0.1-0.5 MPa, the reducing atmosphere is selected from at least one of pure H2, pure CO, 10% H2 / Ar, and 10% CO / Ar; the reduction temperature is 300-350°C, and the reduction time is 0.5-10h;
[0040] 3) After the reduction is completed, the temperature is lowered to 250-280°C, more preferably 250°C, at least one of pure CO and 10% CO / Ar is introduced, activated at 0.1-0.5 MPa for 2-24 hours, and raw gas is introduced for reaction.
[0041] Preferably, the catalyst is used with a raw gas composition of H2 / CO2 / N2=72 / 24 / 4 and a space velocity of 3000-6000 mL / min. cat -1 h -1 , the reaction temperature is 250-320°C, the reaction pressure is 3-5MPa, the higher alcohol is C 2+ alcohol.
[0042] The catalyst for preparing higher alcohols by hydrogenating CO2 provided by the present invention has excellent CO2 conversion rate, higher alcohol selectivity and stability, and its preparation method is simple, easy to operate, easy to repeat and scale up production, and has potential industrial application prospects. DETAILED DESCRIPTION
[0043] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0044] The technical details of the present invention are described in detail by the following examples. It should be noted that the examples are only used to further illustrate the technical features of the present invention, rather than to limit the protection scope of the present invention.
[0045] Example 1
[0046] According to the metal molar ratio of Cu / Co=1 and Zn / Co=1.5, 7.2g of copper nitrate trihydrate, 8.7g of cobalt nitrate hexahydrate and 13.4g of zinc nitrate hexahydrate were weighed and dissolved in deionized water to prepare 1mol / L solution L1, and 29.0g of anhydrous potassium carbonate was weighed and dissolved in deionized water to prepare 2mol / L solution L2. At 25°C and a stirring speed of 500r / min, solution L1 and solution L2 were dripped into a 500mL beaker at the same time, and the pH was controlled to be 8. After the dripping was completed, it was aged at 25°C for 2h, then centrifuged and washed 6 times, then placed in a 100°C oven to dry for 12h, and then calcined in a muffle furnace at 400°C for 3h to obtain an oxide catalyst. The K content was measured by inductively coupled plasma emission spectrometer (ICP-OES, Optima 8000, PerkinElmer) to be 0.5%, and the obtained catalyst was named Cu1Co1Zn 1.5 -0.5%K.
[0047] The performance of the above catalyst in the fixed bed for the preparation of higher alcohols by CO2 hydrogenation was evaluated. 1g of the above catalyst was weighed and mixed with 2g of quartz sand particles, and the catalyst and quartz sand were both 40-60 mesh. The catalyst was reduced at 350℃ for 2h in 10% H2 / Ar at 0.1MPa. After reduction, the temperature was lowered to 250℃ and then switched to 10% CO / Ar and activated for 10h. After the activation, the raw gas of H2 / CO2 / N2=72 / 24 / 4 was introduced, and the space velocity was 4000mLg cat -1 h -1 , reaction temperature is 300℃, reaction pressure is 3MPa. The performance results are shown in Table 1.
[0048] Example 2
[0049] The catalyst preparation method and evaluation process were the same as in Example 1, except that the catalyst was washed once. The K content was measured by ICP-OES to be 5%, and the obtained catalyst was named Cu1Co1Zn 1.5 -5% K. The performance results are shown in Table 1.
[0050] Example 3
[0051] The catalyst preparation method and evaluation process were the same as in Example 1, except that the catalyst was washed three times. The K content was measured by ICP-OES to be 3%, and the obtained catalyst was named Cu1Co1Zn 1.5 -3% K. The performance results are shown in Table 1.
[0052] Table 1. Catalytic performance results of various examples
[0053]
[0054] From the data in Table 1, it can be seen that the K content has a significant effect on the conversion rate and selectivity of higher alcohols in the Cu-Co based CO2 hydrogenation reaction, among which there is a significant promoting effect when the K content is 3%.
[0055] Example 4
[0056] The catalyst preparation method and evaluation process were the same as in Example 1, except that the precipitant was changed from anhydrous potassium carbonate to 41.1 g of cesium carbonate. The Cs content was measured by ICP-OES to be 3%, and the obtained catalyst was named Cu1Co1Zn 1.5 -3% Cs. The performance results are shown in Table 2.
[0057] Table 2. Catalytic performance results of various examples
[0058]
[0059] It can be seen from the data in Table 2 that the alkali metal additive Cs has a significant promoting effect on the Cu-Co based CO2 hydrogenation to produce higher alcohols.
[0060] Example 5
[0061] The catalyst preparation method and evaluation process were the same as those in Example 4, except that zinc nitrate hexahydrate was replaced with 18.2 g of ferric nitrate nonahydrate (Fe / Co=1.5). The resulting catalyst was named Cu1Co1Fe 1.5 -3% Cs. The performance results are shown in Table 3.
[0062] Table 3. Catalytic performance results of various examples
[0063]
[0064] It can be seen from the data in Table 3 that the metal additive Fe has a significant promoting effect on the Cu-Co based CO2 hydrogenation to produce higher alcohols.
[0065] Example 6
[0066] The catalyst preparation method and evaluation process are the same as those in Example 4. The catalyst is Cu1Co1Zn 1.5 -3% Cs. Only by extending the aging time of the catalyst to 48h and the activation time of the catalyst to 24h during the preparation process, the reaction space velocity was increased to 6000mLg cat -1 h -1 The performance results are shown in Table 4.
[0067] Example 7
[0068] The catalyst preparation method and evaluation process are the same as those in Example 4. The catalyst is Cu1Co1Zn 1.5-3% Cs. The catalyst reduction condition was changed to 300°C for 10 hours, the reaction temperature was changed to 320°C, and the reaction pressure was changed to 5MPa. The performance results are shown in Table 4.
[0069] Example 8
[0070] The catalyst preparation method and evaluation process were the same as those in Example 7, except that zinc nitrate hexahydrate was replaced with 18.2 g of ferric nitrate nonahydrate (Fe / Co=1.5). The resulting catalyst was named Cu1Co1Fe 1.5 -3% Cs.
[0071] Example 9
[0072] The catalyst preparation method and evaluation process are the same as those in Example 4. The catalyst is Cu1Co1Zn 1.5 -3% Cs. Only the catalyst activation pressure was changed to 0.5 MPa and the reaction temperature was changed to 250°C. The performance results are shown in Table 4.
[0073] Example 10
[0074] The catalyst preparation method and evaluation process are the same as those in Example 4. The catalyst is Cu1Co1Zn 1.5 -3% Cs. The catalyst drying condition was changed to 80°C for 24 hours, the calcination condition was changed to 350°C for 8 hours, and the activation time was changed to 2 hours. The performance results are shown in Table 4.
[0075] Embodiment 11
[0076] The catalyst preparation method and evaluation process are the same as those in Example 4. The catalyst is Cu1Co1Zn 1.5 -3% Cs. The catalyst drying condition was changed to 120°C for 12 hours and the calcination condition was changed to 450°C for 3 hours. The performance results are shown in Table 4.
[0077] Table 4. Catalytic performance results of various examples
[0078]
[0079] It can be seen from the data in Table 4 that the preparation method and the condition parameters in the evaluation process have a significant impact on the preparation of higher alcohols by Cu-Co based CO2 hydrogenation.
[0080] Example 12
[0081] According to the metal molar ratio of Cu / Co=1 and Fe / Co=1.5, 7.2g of copper nitrate trihydrate, 8.7g of cobalt nitrate hexahydrate and 18.2g of ferric nitrate nonahydrate were weighed and dissolved in deionized water to prepare a 0.5mol / L solution L1, and 20.2g of ammonium carbonate was weighed and dissolved in deionized water to prepare a 1mol / L solution L3. At 25°C and a stirring speed of 500r / min, solution L1 and solution L3 were dripped into a 500mL beaker at the same time, and the pH was controlled to 8. After the dripping was completed, it was aged at 25°C for 2h, then centrifuged and washed 6 times, then placed in a 100°C oven to dry for 12h, and then calcined at 400°C in a muffle furnace for 3h. The oxide was named Cu1Co1Fe 1.5 0.41 g of KNO3 was weighed and dissolved in deionized water to obtain solution L4, based on the metal K accounting for 3% of the total mass of the oxide catalyst. Solution L4 was loaded on 5 g of Cu1Co1Fe 1.5 The catalyst was aged at 25 °C for 12 h, dried in an oven at 100 °C for 12 h, and then calcined in a muffle furnace at 400 °C for 3 h. The resulting catalyst was named Cu1Co1Fe 1.5 -3%K.
[0082] The performance of the above catalyst in the fixed bed for the preparation of higher alcohols by CO2 hydrogenation was evaluated. 1g of the above catalyst was weighed and mixed with 2g of quartz sand particles, and the catalyst and quartz sand were both 40-60 mesh. The catalyst was reduced at 350℃ for 2h in 10% H2 / Ar at 0.1MPa. After reduction, the temperature was lowered to 250℃ and then switched to 10% CO / Ar and activated for 10h. After the activation, the raw gas of H2 / CO2 / N2=72 / 24 / 4 was introduced, and the space velocity was 4000mLg cat -1 h -1 , reaction temperature is 300℃, reaction pressure is 3MPa. The performance results are shown in Table 5.
[0083] Table 5. Catalytic performance results of various examples
[0084]
[0085] It can be seen from the data in Table 5 that the preparation method has an impact on the performance of Cu-Co based CO2 hydrogenation to prepare higher alcohols.
[0086] Embodiment 13
[0087] The catalyst preparation method and evaluation process were the same as those in Example 12, except that the KNO3 used in the equal volume impregnation was replaced with 0.58 g of NaNO3. The resulting catalyst was named Cu1Co1Fe 1.5 -3%Na. The performance results are shown in Table 6.
[0088] Table 6. Catalytic performance results of various examples
[0089]
[0090] It can be seen from the data in Table 6 that the type of alkali metal additive has an impact on the performance of Cu-Co based CO2 hydrogenation to prepare higher alcohols.
[0091] Embodiment 14
[0092] The catalyst preparation method and evaluation process were the same as those in Example 12, except that the Cu / Co molar ratio was changed to 0.5, the mass of copper nitrate trihydrate was 3.6 g, and the mass of ammonium carbonate was changed to 17.3 g accordingly. The obtained catalyst was named Cu 0.5 Co1Fe 1.5 -3% K. The performance results are shown in Table 1.
[0093] Embodiment 15
[0094] The catalyst preparation method and evaluation process were the same as those in Example 12, except that the Cu / Co molar ratio was changed to 2, the mass of copper nitrate trihydrate was 14.5 g, and the mass of ammonium carbonate was changed to 25.9 g accordingly. The obtained catalyst was named Cu2Co1Fe 1.5 -3% K. The performance results are shown in Table 7.
[0095] Table 7. Catalytic performance results of various examples
[0096]
[0097] Example 16
[0098] The catalyst preparation method and evaluation process were the same as those in Example 12, except that the Fe / Co molar ratio was changed to 0.5 and the mass of ferric nitrate nonahydrate was 6.1 g. The resulting catalyst was named Cu2Co1Fe 0.5 -3% K. The performance results are shown in Table 8.
[0099] Table 8. Catalytic performance results of various examples
[0100]
[0101] It can be seen from the data in Tables 7 and 8 that changes in the x and y values significantly affect the performance of Cu-Co based CO2 hydrogenation to prepare higher alcohols.
[0102] Based on the performance results of the above examples, the metal promoter Fe and the alkali metal promoter Cs have a significant promoting effect on the Cu-Co based CO2 hydrogenation to produce higher alcohols, and the content of various components, catalyst preparation method and reaction conditions all have an impact on the catalytic performance. Among them, the CO2 conversion rate can reach up to 32.7%, and the C 2+The highest alcohol selectivity can reach 17.9%, and the total alcohol selectivity exceeds 20%. In addition, the catalysts in the examples have good stability.
[0103] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can further make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any equivalent changes, modifications and evolutions made by technicians familiar with this profession without departing from the spirit and scope of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention and are within the protection scope of the present invention.
Claims
1. A method for preparing C from CO2 by hydrogenation 2+ A catalyst for alcohols, characterized in that The molecular formula of the catalyst is Cu x Co1M y -zA, wherein M is a metal additive, A is an alkali metal additive, x is in the range of 1-2, y is in the range of 1.5, z is the mass fraction of the alkali metal additive in the catalyst, and z is in the range of 3%; M is selected from any one of the transition metal elements Fe and Zn; A is selected from any one of Na, K and Cs; The method for preparing the catalyst comprises the following steps: (1) Dissolve Cu salt, Co salt and M salt in water to obtain solution L1; (2) dissolving the precipitant containing A in water to obtain solution L2; (3) Solution L1 and solution L2 are added dropwise at the same time. After the addition is completed, Cu is obtained after aging, separation, washing, drying and roasting. x Co1M y -zA; The aging temperature is 25°C and the aging time is 2h; The drying temperature is 100°C and the drying time is 12h; The calcination temperature is 400° C. and the calcination time is 3 hours.
2. The catalyst according to claim 1, characterized in that The Cu salt, Co salt, and M salt are selected from any one of their corresponding nitrates, chlorides, sulfates, carbonates, and acetates; and the precipitant containing A is selected from any one of Na2CO3, K2CO3, Cs2CO3, Na2HCO3, K2HCO3, NaOH, KOH, and CsOH.
3. The method for preparing the catalyst according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Dissolve Cu salt, Co salt and M salt in water to obtain solution L1; (2) dissolving the precipitant containing A in water to obtain solution L2; (3) Solution L1 and solution L2 are added dropwise at the same time. After the addition is completed, Cu is obtained after aging, separation, washing, drying and roasting. x Co1M y -zA; The aging temperature is 25°C and the aging time is 2h; The drying temperature is 100°C and the drying time is 12h; The calcination temperature is 400° C. and the calcination time is 3 hours.
4. The catalyst as claimed in claim 1 is used for fixed bed CO2 hydrogenation to produce C 2+ Application in alcohol.
5. The use according to claim 4, characterized in that The fixed bed CO2 hydrogenation preparation method 2+ The process parameters of alcohol are as follows: the particle size of the catalyst and quartz sand particles used for loading is 40-60 mesh; the reduction pressure is 0.1-0.5MPa, the reducing gas is selected from at least one of pure H2, pure CO, 10% H2 / Ar, and 10% CO / Ar, the reduction temperature is 300-350℃, and the reduction time is 0.5-10h; the temperature is lowered to 250-280℃, the activation pressure is 0.1-0.5MPa, and the activation time is 2-24h; the raw gas composition is H2 / CO2 / N2=72 / 24 / 4, and the space velocity is 3000-6000 mLg cat -1 h -1 , reaction temperature 250-320℃, reaction pressure 3-5MPa.