A radiation-resistant breathable film and its preparation method and application
By adopting a three-layer structure breathable film, combined with hot pressing and electrospinning technology, the problems of changes in the strength and pore structure of the breathable film in the sterile connector are solved, and a low-cost and high-performance breathable film is achieved. Meets the needs of sterile connectors and improves tolerance to gamma rays.
Patent Information
- Application Number
- CN202211675976.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-26
AI Technical Summary
The breathable film materials in existing sterile connectors have a large change in intensity and pore structure after irradiation after high temperature and high pressure or gamma ray sterilization, which is difficult to meet the requirements of sterile connectors. Polytetrafluoroethylene (PTFE) The material has poor radiation resistance, which makes it difficult to replace the higher cost polyethersulfone (PES) film.
A breathable film with a three-layer structure, including a first micron-thick e-PTFE film layer, a second polymer nonwoven fabric layer and a third PTFE/CNT nanofiber film layer, by hot pressing and electrospinning Technical preparation, the base cloth layer is formed and heat treated to improve radiation resistance.
The strength and pore size of the breathable film are stabilized after 50kGy gamma ray irradiation, meet the performance requirements of sterile connectors, and the cost is lower than that of traditional PES films, with excellent performance, and can effectively intercept bacteria and suspended particles in the air.
Smart Images

Figure BDA0004018276050000051 
Figure BDA0004018276050000071 
Figure BDA0004018276050000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of breathable film materials, and in particular to a radiation-resistant breathable film and a preparation method and application thereof. Background Art
[0002] Aseptic connectors are used for sampling during fermentation tank inoculation, fermentation or cell culture. They connect two independent fluid paths in a dry manner while maintaining the sterile integrity of the two paths. The connector consists of a female end and a male end, each end of which is protected by a layer of removable breathable film. This layer of breathable film can protect the port and maintain the sterility of the sterile fluid path. Since sterile connectors need to be sterile, the breathable film in them usually needs to withstand high temperature and high pressure sterilization above 130°C, or gamma ray sterilization of up to 50kGy.
[0003] The breathable film in sterile connectors is usually polyethersulfone (PES) membrane, which is more expensive. In contrast, polytetrafluoroethylene (PTFE) ) The price is relatively cheap and it has excellent corrosion resistance, making it the most ideal material to replace PES membrane. However, PTFE has poor radiation resistance, and its strength and pore structure will change significantly after irradiation, which limits its application in breathable films in sterile connectors. Summary of the invention
[0004] The object of the present invention is to provide a radiation-resistant breathable film in view of the above problems.
[0005] In order to achieve its purpose, the present invention adopts the following technical solution:
[0006] A radiation-resistant breathable film comprises a first e-PTFE membrane layer, a second non-woven fabric layer, and a third PTFE / CNT nanofiber membrane layer, which are sequentially arranged from top to bottom;
[0007] The second non-woven fabric layer is a polymer non-woven fabric selected from PET, polychlorotrifluoroethylene (PCTFE), polyvinyl formal (PVF), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), polycarbonate (PC) or polyamide (PA);
[0008] The third layer of PTFE / CNT nanofiber membrane has a fiber diameter of 1 to 4 um and a membrane thickness of 0.005 to 0.045 mm.
[0009] The thickness of the e-PTFE membrane is in the micron level, the average pore size is 0.1um to 1.5um, and the air permeability is 68 to 715 L / m2.s.
[0010] Preferably, the average pore size of the e-PTFE membrane is 0.2um to 1.5um or 0.2um to 1.4um or 0.5um to 1.5um, and the air permeability is 87 to 715L / m2.s or 138 to 715L / m2.s or 87 to 663L / m2.s or 324 to 715L / m2.s.
[0011] The second non-woven fabric layer has a thickness of 0.06 to 0.35 mm and a gram weight of 15 to 75 g / m 2 ; The preferred thickness is 0.07-0.3mm or 0.2-0.3mm, and the gram weight is 15-70g / m 2 or 45~70g / m 2 or 45~60g / m 2 ; Preferably use PET non-woven fabric layer.
[0012] The third PTFE / CNT nanofiber membrane layer has a fiber diameter of 1 to 3.8 um, 1.4 to 3.8 um, 2.1 to 3.8 um, or 2.8 to 3.6 um, and a membrane thickness of 0.02 to 0.045 mm, or 0.034 to 0.045 mm.
[0013] In the above technical solution, the first layer is compounded with the second layer by hot pressing to form a base fabric layer; the third layer is prepared by electrostatic spinning, and then the third layer is compounded with the base fabric layer by hot pressing.
[0014] The present invention also provides a method for preparing the breathable film as described in any one of the above, comprising the following steps:
[0015] S1. The first layer of e-PTFE film layer and the second layer of non-woven fabric layer are composited together by hot pressing to obtain a composite base fabric layer;
[0016] S2. placing an aluminum foil on a receiving screen / stick of an electrospinning device, injecting a spinning solution into a spinning solution reservoir, setting operating parameters, and starting the electrospinning device. Under the action of an electric field, a jet of solution is formed at the spinneret, and the jet is accelerated along the direction of the electric field, and finally a third layer of PTFE / CNT nanofiber membrane is obtained on the aluminum foil;
[0017] S3. The PTFE / CNT nanofiber membrane layer obtained in step S2 is removed from the aluminum foil, heat treated at 200-260°C for 2-3h, and then kept at 300-400°C until the spinning carrier solution is completely evaporated;
[0018] S4. The PTFE / CNT nanofiber membrane layer prepared in S3 and the base fabric layer prepared in S1 are composited by hot pressing to obtain a breathable film.
[0019] Preferably, in step S2, the voltage of the electrospinning equipment is 15-35 kV, the spinning solution flow rate is 1.0-2.5 ml / L, the ambient temperature is maintained at 25-30° C., the ambient humidity is maintained at 35-45%, and the receiving distance is 10 cm-20 cm;
[0020] It is further preferred that the voltage of the electrospinning equipment is 15-25 kV or 15-20 kV, the spinning solution flow rate is 1.1-2.3 ml / L or 1.2-2.1 ml / L, the ambient temperature is maintained at 25-28° C., and the receiving distance is 13 cm-20 cm or 15 cm-20 cm.
[0021] In the technical solution of the above preparation method, in step S2, the preparation method of the spinning solution is:
[0022] (1) dissolving polyvinyl alcohol (PVA) in water to prepare a spinning carrier solution with a concentration of 8 to 10 wt %;
[0023] (2) adding a PTFE dispersion emulsion to a spinning carrier solution, wherein the mass ratio of the solid in the PTFE dispersion emulsion to the spinning carrier solution is 8 to 12:1, to obtain a PTFE solution, and stirring the solution uniformly;
[0024] (3) adding a carbon nanotube solution with a concentration of 0.05 to 0.5 g / mL, wherein the volume ratio of the carbon nanotube solution to the PTFE solution is 1:20 to 360;
[0025] (4) Add boric acid to adjust the viscosity of the spinning solution to 250-650 cps.
[0026] In the above method for preparing the spinning solution, the solid content of the PTFE dispersion in step (2) is 45-60 wt %.
[0027] In step (3), the volume ratio of the carbon nanotube solution to the PTFE solution is 1:20-230 or 1:40-230 or 1:50-360 or 1:50-230 or 1:100-230; the concentration of the carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 1.3-11 mg / mL, preferably 1.4-10 mg / mL or 2.0-10 mg / mL or 2.3-8 mg / mL or 3-8 mg / mL or 3-6 mg / mL.
[0028] In step (4), boric acid is added to adjust the viscosity of the spinning solution to 270-630 cps, 270-550 cps, 350-630 cps, or 350-490 cps.
[0029] Finally, the present invention further provides the use of any of the above-mentioned breathable films as a breathable film in a sterile connector, and preferably the breathable film is used to block bacteria and solid particles suspended in the air.
[0030] The beneficial effects of the present invention are:
[0031] The first layer of e-PTFE membrane has a rich microporous structure, which can achieve antibacterial, waterproof, breathable and other properties; it can be composited with the sterile connector frame by heat welding or ultrasonic welding.
[0032] The second non-woven fabric layer provides strength for the overall breathable film, because the e-PTFE and PTFE / CNT nanofiber membrane layers are thin and mechanically weak, requiring additional substrates to provide support strength (perpendicular to the plane of the breathable film) and tensile strength (parallel to the plane of the breathable film). In addition, after the non-woven fabric layer is irradiated with gamma rays, its physical properties are less affected, and the material size and pore structure are relatively stable, so it can be directly sterilized with gamma rays, which is cost-effective.
[0033] The third layer of PTFE / CNT nanofiber membrane is mainly located in the outer layer. Its main function is to intercept bacteria, particulate matter, aerosols and other pollutants from entering the sterile connector. Compared with the membrane material, it has a certain fiber thickness and belongs to the deep filtration material. The main material is PTFE, which has excellent chemical stability. By adding carbon nanotubes for modification, the PTFE material's tolerance to gamma rays is increased, so that the final composite material can meet the requirements of gamma ray sterilization.
[0034] The breathable film prepared by the method of the present invention has a maximum pore size range of 1-5um, and the maximum pore size is ≤28um after 50kGy gamma ray irradiation. After irradiation, its pore size and strength and other indicators still meet the requirements of sterile connectors and can be used in sterile connectors. Compared with traditional polyethersulfone (PES) membranes, it has lower cost and excellent performance.
[0035] When in use, the first e-PTFE film layer of the breathable film is composited with the sterile connector frame by heat welding or ultrasonic welding. The sterile connector frame is usually made of polycarbonate. When in use, the breathable film needs to be torn off after the two interfaces of the sterile connector are connected, and no film residue is required. After the breathable film of the present invention is composited with the sterile connector frame and the film is torn off after flipping 180 degrees, no film residue is left at the sterile connector interface, indicating that the breathable film of the present invention meets the performance requirements of the sterile connector for the breathable film. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with embodiments, but the present invention is not limited thereto.
[0037] The experimental methods in the following examples are conventional methods unless otherwise specified; the materials and reagents used are conventional materials and reagents in the art and are commercially available unless otherwise specified.
[0038] e-PTFE membrane: expanded polytetrafluoroethylene (Expanded PTFE), with a thickness of micrometer level (240-400um), a pore size of 0.1um-1.5um, and an air permeability of 68-715L / m2.s, purchased from Chongqing Baoman New Materials Co., Ltd.
[0039] PET (polyester) non-woven fabric: weight 15-80g / m 2 , thickness 0.07-0.3 mm, commercially available.
[0040] PTFE dispersed emulsion: the brand is D60, the solid content is 60%, and the manufacturer is Hubei Polyfluoride Chemical Technology Co., Ltd. Carbon nanotube (CNT): a commercially available conventional water suspension.
[0041] The breathable film of the present invention has a three-layer structure, comprising a first e-PTFE membrane layer, a second non-woven fabric layer, and a third PTFE / CNT nanofiber membrane layer, which are sequentially arranged from top to bottom.
[0042] The first layer of e-PTFE membrane has a pore size of 0.1um-1.5um and an air permeability of 68-715L / m2.s.
[0043] The second non-woven fabric layer can be made of polymer non-woven fabrics, such as PET, polychlorotrifluoroethylene (PCTFE), polyvinyl formal (PVF), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), polycarbonate (PC), polyamide (PA) and other materials. These non-woven fabric materials have strong support strength and tensile strength, are not easy to deform, have good tolerance to gamma rays, and can have good composite ability with e-PTFE membrane. Considering performance and cost, PET non-woven fabric is used in each embodiment of the present invention.
[0044] The third layer is PTFE / CNT nanofiber membrane layer, with a fiber diameter of 1-4um and a membrane thickness of 0.005-0.045mm.
[0045] The first layer is compounded with the second layer by hot pressing to form a base fabric layer; the third layer is prepared by electrostatic spinning, and then the third layer is compounded with the base fabric layer by hot pressing.
[0046] The method for preparing the breathable film of the present invention is carried out according to the following steps:
[0047] S1. Compounding the first e-PTFE film layer and the second non-woven fabric layer together by hot pressing to obtain a composite base fabric layer.
[0048] S2. Place the aluminum foil on the receiving screen / rod of the electrospinning equipment, inject the spinning solution into the spinning solution reservoir, set the operating parameters, turn on the electrospinning equipment, and under the action of the electric field, the solution at the spinneret forms a jet stream, which accelerates along the direction of the electric field, and finally obtains the third layer of PTFE / CNT nanofiber membrane on the aluminum foil; the voltage of the electrospinning equipment is 15-35kV, the spinning solution flow rate is 1.0-2.5ml / L, the ambient temperature is maintained at 25-30℃, the ambient humidity is maintained at 35-45%, and the receiving distance is 10cm-20cm.
[0049] The preparation method of the spinning solution is:
[0050] (1) dissolving polyvinyl alcohol (PVA) in water to prepare a spinning carrier solution with a concentration of 8 to 10 wt %;
[0051] (2) adding a PTFE dispersion emulsion to a spinning carrier solution, wherein the mass ratio of the solid in the PTFE dispersion emulsion to the spinning carrier solution is 8 to 12:1, to obtain a PTFE solution, and stirring the solution uniformly;
[0052] (3) adding a carbon nanotube solution with a concentration of 0.05 to 0.5 g / mL, wherein the volume ratio of the carbon nanotube solution to the PTFE solution is 1:20 to 360;
[0053] (4) Add boric acid to adjust the viscosity of the spinning solution to 250-650 cps.
[0054] S3. The PTFE / CNT nanofiber membrane layer obtained in step S2 is removed from the aluminum foil, and heat-treated at 200-260° C. for 2-3 hours, and then kept at 300-400° C. until the spinning carrier solution is completely evaporated.
[0055] S4. The PTFE / CNT nanofiber membrane layer prepared in S3 and the base fabric layer prepared in S1 are composited by hot pressing to obtain a breathable film.
[0056] The breathable film in Table 1 was prepared according to the above method, and the relevant parameters of the three-layer material are shown in Table 1.
[0057] The first layer is an e-PTFE membrane layer, the second layer is a non-woven fabric layer, and the third layer is a PTFE / CNT nanofiber membrane layer.
[0058] Table 1
[0059]
[0060] Among them, the specific preparation parameters and spinning parameters of the spinning solution of the third layer are as follows:
[0061] Example 1: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 10wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 8:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.05g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:20 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 2.5mg / mL); add 5wt% boric acid solution to adjust the viscosity of the spinning solution to 270cps, and obtain. The voltage of the electrospinning equipment is 20kV, the spinning solution flow rate is 1.2ml / h, the ambient temperature is maintained at 25℃, the ambient humidity is maintained at 35%, and the receiving distance is 20cm, and an electrospun fiber with a fiber diameter of 1um is obtained.
[0062] Example 2, Comparative Example 1: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 9wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 9:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.3g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:130 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 2.3mg / mL); add 8wt% boric acid solution to adjust the viscosity of the spinning solution to 350cps, and obtain. The voltage of the electrospinning equipment is 20kV, the spinning solution flow rate is 1.2ml / h, the ambient temperature is maintained at 25°C, the ambient humidity is maintained at 35%, and the receiving distance is 20cm, and an electrospun fiber with a fiber diameter of 1.4um is obtained.
[0063] Example 3: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 10wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 10:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.5g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:230 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 2.2mg / mL); add 8wt% boric acid solution to adjust the viscosity of the spinning solution to 410cps, and obtain. The voltage of the electrospinning equipment is 15kV, the spinning solution flow rate is 1.2ml / h, the ambient temperature is maintained at 25℃, the ambient humidity is maintained at 35%, and the receiving distance is 15cm, and an electrospun fiber with a fiber diameter of 2.1um is obtained.
[0064] Example 4: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 10wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 12:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.3g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:100 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 3mg / mL); add 5wt% boric acid solution to adjust the viscosity of the spinning solution to 490cps, and obtain. The voltage of the electrospinning equipment is 20kV, the spinning solution flow rate is 2.1ml / h, the ambient temperature is maintained at 25℃, the ambient humidity is maintained at 35%, and the receiving distance is 15cm, and an electrospun fiber with a fiber diameter of 2.8um is obtained.
[0065] Example 5: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 10wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 12:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.3g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:50 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 6mg / mL); add 8wt% boric acid solution to adjust the viscosity of the spinning solution to 550cps, and obtain. The voltage of the electrospinning equipment is 20kV, the spinning solution flow rate is 2.1ml / h, the ambient temperature is maintained at 25℃, the ambient humidity is maintained at 35%, and the receiving distance is 15cm, and an electrospun fiber with a fiber diameter of 3.6um is obtained.
[0066] Example 6: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 10wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 12:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.4g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:40 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 10mg / mL); add 8wt% boric acid solution to adjust the viscosity of the spinning solution to 630cps, and obtain. The voltage of the electrospinning equipment is 15kV, the spinning solution flow rate is 2.1ml / h, the ambient temperature is maintained at 25℃, the ambient humidity is maintained at 35%, and the receiving distance is 13cm, and an electrospun fiber with a fiber diameter of 3.8um is obtained.
[0067] Example 7: Dissolve polyvinyl alcohol in water to obtain a spinning carrier solution with a concentration of 10wt%; then add polytetrafluoroethylene water dispersion emulsion (solid content 60wt%), with a mass ratio of 12:1 to the spinning carrier solution, and stir and mix evenly; add a carbon nanotube solution with a concentration of 0.5g / mL, and the volume ratio of the carbon nanotube solution to the PTFE solution is 1:360 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 1.4mg / mL); add 8wt% boric acid solution to adjust the viscosity of the spinning solution to 630cps, and obtain. The voltage of the electrospinning equipment is 15kV, the spinning solution flow rate is 2.1ml / h, the ambient temperature is maintained at 25℃, the ambient humidity is maintained at 35%, and the receiving distance is 13cm, and an electrospun fiber with a fiber diameter of 3.8um is obtained.
[0068] The specific preparation parameters and spinning parameters of the spinning solution of the third layer of comparative example 2 are as follows: polyvinyl alcohol is dissolved in water to obtain a spinning carrier solution with a concentration of 10wt%; then polytetrafluoroethylene aqueous dispersion emulsion (solid content 60wt%) is added, and the mass ratio of the polytetrafluoroethylene aqueous dispersion emulsion to the spinning carrier solution is 12:1, and the mixture is stirred and mixed evenly; a carbon nanotube solution with a concentration of 0.5g / mL is added, and the volume ratio of the carbon nanotube solution to the spinning solution is 1:400 (the concentration of carbon nanotubes in the mixed solution of the carbon nanotube solution and the PTFE solution is 1.25mg / mL); 8wt% boric acid solution is added to adjust the viscosity of the spinning solution to 630cps, and the electrostatic spinning fiber with a fiber diameter of 3.8um is obtained. The voltage of the electrostatic spinning equipment is 15kV, the flow rate of the spinning solution is 2.1ml / h, the ambient temperature is maintained at 25°C, the ambient humidity is maintained at 35%, and the receiving distance is 13cm.
[0069] The film obtained in Table 1 was tested for performance:
[0070] The tensile strength and elongation are measured according to GB / T 12914-2008 “Determination of tensile strength and elongation of paper and paperboard”;
[0071] The bursting strength (i.e., the bursting strength in Table 3) is measured using GB / T 454-2020 “Determination of bursting strength of paper”;
[0072] The air permeability of raw materials is measured according to ASTM D737-2018 "Test Method for Air Permeability of Textile Fabrics";
[0073] The pore size is tested using PMI;
[0074] The fiber diameter was tested by SEM;
[0075] The thickness is tested according to GB / T 451.3-2002 "Determination of thickness of paper and paperboard";
[0076] The gram weight is tested according to GBT 451.2-2002 "Determination of Basis Weight of Paper and Paperboard";
[0077] The irradiation test was conducted by exposing the breathable film to 50 kGy of gamma radiation.
[0078] The test results are shown in Table 2:
[0079] Table 2 Performance test results of thin films before and after irradiation
[0080]
[0081]
[0082] From the results of Example 1 and Example 2, it can be seen that compared with Example 1, the gram weight and thickness of the second non-woven fabric layer in Example 2 are increased, so that the strength of the film finally obtained is significantly improved. Compared with Example 6, the proportion of carbon nanotubes in the spinning solution in Example 7 is reduced, so that the strength and radiation resistance of the film are significantly reduced.
[0083] From the comparison between Comparative Example 1 and Example 2, it can be seen that Comparative Example 1 uses a non-woven fabric with a low grammage, and the strength of the obtained film is poor. The choice of the grammage of the non-woven fabric is related to the strength of the composite film and the strength after radiation, and also has a relatively large effect on the change in pore size after irradiation.
[0084] From the comparison between Comparative Example 2 and Example 7, it can be seen that the three-layer materials of the two are the same except for the different amount of carbon nanotubes added to the spinning solution during electrospinning in the third layer. Compared with Example 7, the carbon nanotubes used in the third layer of Comparative Example 2 are less in proportion, and the strength and radiation resistance are significantly reduced, and the pore size after irradiation is unqualified.
[0085] The breathable film prepared by the method of the present invention has a maximum pore size range of 1-5um, and the maximum pore size is ≤28um after being irradiated with 50kGy gamma rays.
[0086] The breathable film prepared by the method of the present invention still meets the performance requirements of the breathable film in the sterile connector in terms of strength and pore structure after being sterilized by 50 kGy gamma-ray irradiation. Applying it to the sterile connector can solve the technical problem in the prior art that the polyethersulfone (PES) breathable film in the sterile connector cannot tolerate irradiation.
Claims
1. A radiation-resistant breathable film, Features: It includes a first e-PTFE membrane layer, a second non-woven fabric layer, and a third PTFE / CNT fiber membrane layer, which are arranged in sequence from top to bottom; The second non-woven fabric layer is made of PET non-woven fabric, and the thickness of the second non-woven fabric layer is 0.06-0.35 mm, and the weight is 15-75 g / m 2 ; The fiber diameter of the third PTFE / CNT fiber membrane layer is 1 to 4 μm, and the membrane thickness is 0.005 to 0.045 mm. The third PTFE / CNT fiber membrane layer is prepared by electrospinning, and the spinning solution is prepared by: (1) dissolving polyvinyl alcohol in water to prepare a spinning carrier solution with a concentration of 8 to 10 wt%; (2) adding PTFE dispersion to the spinning carrier solution, wherein the mass ratio of the solid in the PTFE dispersion to the spinning carrier solution is 8 to 12:1, to obtain a PTFE solution, which is fully stirred; (3) adding a carbon nanotube solution with a concentration of 0.05 to 0.5 g / mL, wherein the volume ratio of the carbon nanotube solution to the PTFE solution is 1:20 to 360; (4) adding boric acid to adjust the viscosity of the spinning solution to 250 to 650 cps, to obtain the obtained solution.
2. The breathable film according to claim 1, Features: The average pore size of the e-PTFE membrane is 0.1um to 1.5um, and the air permeability is 68 to 715 L / m 2 ·s.
3. The breathable film according to claim 1, Features: The first layer is compounded with the second layer by hot pressing to form a base fabric layer; and then the third layer is compounded with the base fabric layer by hot pressing.
4. A method for preparing a breathable film according to any one of claims 1 to 3, It is characterized in that The steps include: S1. The first layer of e-PTFE film layer and the second layer of non-woven fabric layer are composited together by hot pressing to obtain a composite base fabric layer; S2. placing an aluminum foil on a receiving screen or roller of an electrospinning device, injecting a spinning solution into a spinning solution reservoir, setting operating parameters, and starting the electrospinning device. Under the action of an electric field, a jet stream is formed at the spinneret of the solution, which is accelerated along the direction of the electric field, and finally a third layer of PTFE / CNT fiber membrane is obtained on the aluminum foil; S3. The PTFE / CNT fiber membrane layer obtained in step S2 is removed from the aluminum foil, heat treated at 200-260°C for 2-3h, and then kept at 300-400°C until the spinning carrier solution is completely evaporated; S4. The PTFE / CNT fiber membrane layer prepared in S3 and the base fabric layer prepared in S1 are composited by hot pressing to obtain a breathable film.
5. The preparation method according to claim 4, Features: In step S2, the voltage of the electrospinning device is 15-35 kV, the ambient temperature is maintained at 25-30° C., the ambient humidity is maintained at 35-45%, and the receiving distance is 10 cm-20 cm.
6. Use of the breathable film according to any one of claims 1 to 3 as a breathable film in a sterile connector.