A method for preparing ductile iron casting and ductile iron casting

By using high-quality scrap steel and special spheroidizing agent for subcontracted spheroidization treatment in the production of ductile cast iron parts, the problems of spheroidization and mechanical properties when the wall thickness is greater than 1000mm are solved, and high spheroidization and excellent mechanical properties are achieved. , simplifies the process and reduces costs.

CN116179931BActive Publication Date: 2024-11-26GUANGDONG ZHONGTIAN CHUANGZHAN DUCTILE IRON CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310171262.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-11-26
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a spheroidization rate of more than 95% and excellent mechanical properties without using forced cooling measures, and there is difficulty in structural defects when the wall thickness of the ductile iron parts is greater than 1000 mm.

Method used

By using high-quality scrap steel, special spheroidizing agents and incubators, subcontract spheroidizing treatment is carried out, element content and additive ratio are adjusted, high spheroidizing rate and excellent mechanical properties are achieved, and the need for forced cooling is avoided.

Benefits of technology

The spheroidization rate and excellent mechanical properties of ductile iron parts with a wall thickness of more than 1000mm are achieved, which simplifies the production process, reduces costs, and ensures that the internal structure of the product is defect-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179931B_ABST
    Figure CN116179931B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of ductile iron technology and discloses a method for preparing ductile iron parts with a wall thickness ≥1000mm. The process is as follows: (1) The raw materials and high-quality carbon raiser are melted together to form molten iron. Samples are taken for analysis and the element content is adjusted to be within the required range; (2) After the element content is adjusted, the molten iron is heated to 1460-1500℃ and poured into a tundish; (3) A spheroidizing agent is placed on one side of the spheroidizing ladle, and a low-silicon inoculant is placed on the spheroidizing agent. The molten iron in the tundish is poured into the spheroidizing ladle through a water tank for spheroidizing inoculation treatment; (4) After the spheroidizing inoculation treatment is completed, the slag is removed, and then the casting is poured into the mold to obtain the casting. A special inoculant is added during the pouring. The preparation method of this invention does not use accelerated cooling process measures to prepare ductile iron parts with a wall thickness of more than 1000mm. The casting body has excellent mechanical properties, the spheroidization rate can reach more than 95% or even 98%, and the number of graphite spheres reaches 500 / mm. 2 above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ductile iron, and in particular relates to a preparation method of a ductile iron part and a ductile iron part. Background Art

[0002] Cast iron is an iron-carbon alloy with a carbon content greater than 2.11%. It is obtained by high-temperature melting and casting of industrial pig iron, scrap steel and other steel and their alloy materials. In addition to Fe, it also contains other carbon in cast iron precipitated in the form of graphite. If the precipitated graphite is in the form of strips, the cast iron is called gray cast iron or gray cast iron; if it is in the form of worms, it is called vermicular cast iron; if it is in the form of flocs, it is called malleable cast iron or code iron; and if it is in the form of balls, it is called ductile cast iron.

[0003] The chemical composition of ductile iron other than iron is usually: carbon content 3.0-4.0%, silicon content 1.8-3.2%, manganese, phosphorus, sulfur total not exceeding 3.0% and appropriate amounts of rare earth, magnesium and other spheroidizing elements.

[0004] Ductile iron has high mechanical properties, which is based on the excellent graphite spheroidization condition. The standards for measuring the graphite spheroidization condition are the spheroidization rate, graphite nodule diameter and graphite nodule roundness. As one of the important indicators of the intrinsic quality of ductile iron, the spheroidization rate can directly affect the mechanical properties of ductile iron parts. In the national standard GB / T9441-2021 "Metallographic Inspection of Ductile Iron", the spheroidization rate ≥95% in Table 1 of the spheroidization grade on page 3 is defined as: spheroidization grade 1.

[0005] In the article "Factors Affecting the Quality of Thick and Large Section Ductile Iron Castings and Control Measures" published in the 507th issue of "Mechanical Industry Standardization and Quality" in August 2015, it is recorded that "For extra-large thick-walled ductile iron castings, forced cooling control is a necessary means. Forced cooling generally includes air cooling, mist cooling, water cooling, etc. For some container castings, in order to enhance the chilling effect of the inner cavity, liquid nitrogen cooling can also be used to accelerate the solidification speed of the casting."

[0006] In the existing technology, when the wall thickness of ductile iron castings is more than 1000mm, it is impossible to achieve a spheroidization rate of 95% or more without the assistance of process assurance, such as using cast iron chillers, graphite, etc. to speed up the chilling speed.

[0007] Patent CN 108866427 A discloses a method for manufacturing an ultra-large cross-section low-temperature high-toughness ferrite ductile iron casting. The ductile iron casting weighs more than 50 tons and has a wall thickness of more than 400 mm. Its composition is: C: 3.6-3.7%; Si original: 0.9-1.0%; Si final: 1.9-2.0%; Mn: ≤0.1%; P: ≤0.03%; S≤0.01%; Mg: 0.03-0.08%; RE: 0.01-0.02%; Ni: 0.6-0.8%; Sb: 0.003-0.005%. During manufacturing, technical measures such as "high-temperature pure base iron liquid + water-cooled metal mold + cold iron + spheroidizer 5800 + composite strengthening inoculation + alloying + low-temperature boxing" are adopted. The obtained ultra-large cross-section low-temperature and high-toughness ferrite ductile iron parts can meet the quality standards of grade QT400-18 ductile iron. The spheroidization rate of the finished castings reaches 88%, and the spheroidization level is 2-3.

[0008] Patent CN 111074145 A discloses a thick and large end-face ferrite-based ductile iron casting and a preparation method thereof, wherein the thick and large end-face ferrite-based ductile iron casting has a maximum thickness of not less than 800 mm, and its chemical composition is as follows (calculated by the weight percentage of the cast iron): C: 3.5-3.7wt%; Si: 1.8-2.0wt%; Ni: 0.5-1.0wt%; Mn≤0.15wt%; P≤0.03wt%; S: 0.006-0.012wt%; Mg: 0.035-0.045wt%; Sb: 0.003-0.006wt%; the remainder is Fe and impurities introduced during the preparation process. The casting mold is designed based on MAGMA simulation software; furan resin self-hardening sand molding is adopted; wherein, when casting, a layer of universal chill with a thickness of 80-200mm is covered on the outer layer of the casting mold.

[0009] It can be seen from the above two patent documents that when the wall thickness of ductile iron castings is more than 400 mm, even if a forced cooling process is adopted, it is very difficult to achieve a spheroidization rate of more than 95%, that is, spheroidization grade 1, for the obtained product.

[0010] Therefore, if a preparation method can be developed that can obtain large thick-walled ductile iron castings with high spheroidization rate, excellent mechanical properties and no structural defects without forced cooling measures, it will not only simplify the existing production process but also reduce costs, which is an important improvement with great production practice significance and commercial use. Summary of the invention

[0011] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing super-large ductile iron castings without forced cooling measures. The present invention provides a method for preparing ductile iron castings, which can achieve a spheroidization rate of more than 95%, even 98%, and a graphite ball number of 500 / mm without using accelerated cooling process measures. 2 The above significantly simplifies the production process and improves product performance.

[0012] The second object of the present invention is to provide a ductile iron casting obtained by the above-mentioned preparation method.

[0013] In order to achieve the first invention object, the present invention adopts the following technical solutions:

[0014] A method for preparing a ductile iron casting, wherein the wall thickness of the ductile iron casting is ≥1000 mm, and the specific process is:

[0015] (1) Melting the raw materials and high-quality carburizer into raw iron liquid, sampling and analyzing, and adjusting the following element contents within the required range: C: 3.70-3.88wt%; Si: 1.2-1.80wt%; Mn: ≤0.60wt%; P: ≤0.020wt%; S: ≤0.015wt%; Ti: ≤0.001wt%;

[0016] Furthermore, the raw material in step (1) is high-quality scrap steel.

[0017] The high-quality scrap steel referred to in the present invention has trace elements satisfying the following requirements: Ti: ≤0.001wt%, Pb: ≤0.008wt%, Zn: ≤0.005wt%, V: ≤0.001wt%, Cr: ≤0.03wt%, and Bi: ≤0.006wt%.

[0018] Furthermore, the amount of the high-quality recarburizer added in step (1) is 4.06-4.27wt% of the raw material, and its components meet the following requirements: C≥98.5wt%, S<0.03wt%, N<200PPM, and particle size: 2-5mm.

[0019] The high-quality recarburizer referred to in the present invention is a recarburizer that has been graphitized at high temperature. Under high temperature conditions, the arrangement of carbon atoms is in the microscopic form of graphite, so it is called graphitization. In one embodiment of the present invention, its specific components can be: C: 99.2wt%, ash content 0.42wt%, volatile content 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm.

[0020] Regarding the selection and limitation of element types and contents, some scholars have analyzed the chemical composition of ductile iron and concluded that the alloy elements and trace elements in ductile iron have a significant impact on the microstructure and properties of ductile iron.

[0021] In the prior art, castings with a wall thickness greater than 100 mm are called thick-walled ductile iron castings. The alloying elements in such ductile iron castings mainly include magnesium (Mg), silicon (Si), manganese (Mn), sulfur (S), phosphorus (P) and rare earth elements (Re). Among them, magnesium is the key element for the spheroidization of ductile iron. If the amount of magnesium is insufficient, it will lead to poor spheroidization. If it is too high, it will cause spheroidal distortion and affect the overall performance. Too high silicon content will cause graphite to be shaped and affect the chemical properties of ductile iron. Therefore, the silicon content should be low. The presence of an appropriate amount of manganese in cast iron can increase the content of pearlite and strengthen the matrix structure. Sulfur and phosphorus are surfactants in ductile iron. If the content increases, it will have a bad effect on the casting performance and mechanical properties of ductile iron. Rare earth elements have two main functions in ductile iron. One is desulfurization and degassing, and the other is to form high melting point compounds with trace elements to neutralize the adverse effects of trace elements.

[0022] In addition, thick-walled ductile iron also contains trace elements such as Sb, Sn, Cu, Ni, and Bi. For the above trace elements, if the content is not well controlled, it will have an adverse effect on the performance of ductile iron. For example, through the analysis of the Cu content, it can be seen that Cu can increase the amount of pearlite, refine the eutectic group, and make it easier to obtain pearlite structure during normalizing of cast iron. Therefore, Cu has the effect of promoting the formation of pearlite from austenite and hindering graphitization in the eutectoid transformation.

[0023] The content of alloy elements and trace elements in thick-walled ductile iron should be controlled within a reasonable range in order to minimize their impact on ductile iron.

[0024] To this end, it is necessary to control the element composition and its content at the molten iron smelting stage, while taking into account some inevitable trace losses in the production process and the changes in element types and contents brought about by the addition of new reagents, and designing the content of each element in the molten iron smelting stage required to achieve the ideal chemical composition of ductile iron parts.

[0025] After long-term experiments and improvements, the applicant finally obtained the content range of important elements in the original iron liquid suitable for the ductile iron casting of the present invention, specifically: C: 3.70-3.88wt%; Si: 1.2-1.80wt%; Mn: ≤0.60wt%; P: ≤0.020wt%; S: ≤0.015wt%; Ti: ≤0.001wt%. The content of Ti must be strictly controlled at ≤0.001wt%, the purpose of which is to prevent the anti-spheroidization effect of Ti, because Ti is a grain boundary segregation type anti-spheroidizing element. When the casting is thicker and the cooling speed is slower, the destructive effect of the anti-spheroidizing element is stronger, which is easy to cause graphite to distort and form waterweed-like graphite.

[0026] (2) After the element content is adjusted, the raw iron liquid is heated to 1460-1500°C and poured into the tundish;

[0027] (3) placing a spheroidizing agent on one side of the spheroidizing bag, and pressing a low-silicon inoculant on the spheroidizing agent, that is, the low-silicon inoculant is pressed on the spheroidizing agent, and pouring the raw iron liquid in the tundish into the spheroidizing bag through a water trough for spheroidizing inoculation treatment; the components of the spheroidizing agent meet the following requirements: Mg: 5.0-5.5wt%, Si: 45-50wt%, Ca: 2.5-2.6wt%, La: 0.5-0.6wt%, Ce: 0.3-0.4wt%, Al: 0.7-0.9wt%, and particle size: 3-20mm.

[0028] The spheroidizing agent provided by the present invention has the advantage that it does not contain the heavy rare earth yttrium (Y) element, because the source of yttrium is scarce and expensive, and the spheroidizing agent of the present invention achieves the same effect as the yttrium-containing spheroidizing agent and reduces the cost through component selection and optimization. In the spheroidizing agent, the La element content is controlled in the range of 0.5-0.6wt%, the purpose of which is to reduce the shrinkage tendency of the molten iron after spheroidization treatment.

[0029] The components of the low-silicon inoculant meet the following requirements: Si: 40-45wt%, Ca: 1.0-2.0wt%, Ba: 2.0-3.0wt%, Al: 0.6-0.8wt%, particle size: 3-8mm.

[0030] The low-silicon inoculant provided by the present invention has an improvement in its components in that it avoids the generation of oxidized slag inclusions during inoculation due to high Si content.

[0031] (4) After the spheroidizing inoculation treatment is completed, the slag is removed, and then the casting is poured into the mold to obtain the casting, and a special inoculant is added during the pouring;

[0032] The components of the special-effect inoculant meet the following requirements: Si: 50-55wt%, Ce: 0.8-1.0wt%, Ca: 0.5-1.0wt%, Al: 0.7-0.8wt%, and particle size 0.2-0.7mm.

[0033] The improvement of the special-effect inoculant provided by the present invention lies in that the appropriate amount of Ce element contained therein can effectively promote the formation of graphite nucleation core and refine graphite.

[0034] The casting mold used in the present invention can be made of furan resin sand or clay sand. In some prior art, thick-walled ductile iron is prepared by covering a layer of cold iron on the outer layer of the casting mold, such as patent CN 111074145 A, or the casting mold is provided with a water cooling device and metal mold hanging sand, such as patent CN 108866427 A, the purpose of which is to accelerate the cooling of the casting, shorten the solidification time, and improve the quality of the casting. Generally speaking, for extra-large thick-walled ductile iron castings (wall thickness is more than 400mm), forced cooling control is an essential means, but such forced cooling control technical means increase the cost and make the process more complicated, and the appropriate cooling rate needs to be determined according to the chemical composition, organizational characteristics, cross-sectional dimensions and forging deformation of the casting, and there is a problem of high technical difficulty and repeated multiple tests, and improper cooling may cause cracks inside the casting. The unique process provided by the present invention enables the preparation of extra-large ductile iron castings with excellent performance and no structural defects even without adopting forced cooling control technology such as adding cold iron to the casting mold, self-contained water cooling device or metal mold sand hanging.

[0035] In the technical field of preparing ductile iron castings, the thicker the wall of the casting, the higher the technical difficulty. The technical solution of the present invention can obtain cast iron parts with excellent performance and no structural defects without forced cooling control technology when preparing ductile iron castings with a wall thickness of more than 1000mm. Its mechanism is to use high-quality raw materials to melt into raw iron liquid with an element content within the specified range of the present invention, add corresponding amounts of special spheroidizing agent and inoculant, and use a transfer bag spheroidization method to obtain iron liquid with a high spheroidization rate. The special effect inoculant is added to the iron liquid during pouring to obtain a casting.

[0036] Furthermore, in the above-mentioned method for preparing ductile iron castings, the amount of the spheroidizing agent added in step (3) is 1.0wt% of the raw material, and the amount of the low-silicon inoculant added is 0.6wt% of the raw material.

[0037] Furthermore, in the above-mentioned method for preparing ductile iron castings, the addition amount of the special effect inoculant in step (4) is 0.2wt% of the raw material.

[0038] Furthermore, in the above-mentioned method for preparing ductile iron castings, the castings in step (4) are classified into QT400-18, QT500-7 or QT600-3 according to the material grade.

[0039] Furthermore, in the above-mentioned method for preparing ductile iron castings, in order to obtain castings of a specific material grade, the contents of Si and Mn elements in the raw iron liquid are adjusted in step (1), and the required content of Cu is added during the spheroidizing treatment in step (3).

[0040] The specific adjustment method is: if the Si content is lower than the required content, add 75% ferrosilicon in block form; if the Si content is higher than the required content, add raw materials; if the Mn content is lower than the required content, add 55% ferromanganese in broken blocks; if the Mn content is higher than the required content, add raw materials; and if the Cu element is added, 99.9% electrolytic copper in block form is used. Among them, the Si and Mn content are adjusted when the original iron liquid is sampled and analyzed, and the Cu element is added after the spheroidizer and low-silicon inoculant are placed and pressed on top.

[0041] To achieve the second purpose of the present invention, the technical solution adopted is:

[0042] A ductile iron casting with a wall thickness of ≥1000mm and a spheroidization rate of ≥95% is prepared by the preparation method as described above.

[0043] The applicant tested the chemical composition of as-cast castings of different material grades produced by the method of the present invention, and obtained the following data after a large number of tests:

[0044] The QT400-18 casting made of high-quality scrap steel includes the following element components: C: 3.60-3.78wt%, Si: 1.9-2.2wt%, Mn: ≤0.25wt%, P: ≤0.02wt%, S: ≤0.01wt%, RE: 0.003-0.005wt%, Mg: 0.035-0.045wt%, Ti: ≤0.001wt%;

[0045] The QT500-7 casting made of high-quality scrap steel includes the following element components: C: 3.60-3.78wt%, Si: 2.3-2.5wt%, Mn: 0.25-0.45wt%, P: ≤0.02wt%, S: ≤0.01wt%, Cu: 0.32-0.45wt%, RE: 0.003-0.005wt%, Mg: 0.035-0.045wt%, Ti: ≤0.001wt%;

[0046] The QT600-3 casting made of high-quality scrap steel includes the following element components: C: 3.60-3.78wt%, Si: 2.0-2.3wt%, Mn: 0.5-0.6wt%, P: ≤0.02wt%, S: ≤0.01wt%, Cu: 0.5-0.6wt%, RE: 0.003-0.005wt%, Mg: 0.035-0.045wt%, Ti: ≤0.001wt%;

[0047] The detection adopts the bulk sampling method, the sampling position is the core of the casting, and the sample diameter is 40mm.

[0048] The RE element refers to a rare earth element, and in the present invention, is a general term for lanthanum (La) and cerium (Ce).

[0049] As mentioned above, the content of Si, Mn and Cu elements is adjusted to obtain castings of specific material grades. The adjustment can be made based on the chemical composition of the castings of the above grades and the content added and lost in the process. The lost content refers to the trace elements that inevitably remain in the equipment or splash into the environment.

[0050] The raw material is QT400-18 casting made of high-quality scrap steel. The reason for not containing Cu is to prevent the formation of pearlite.

[0051] In the ductile iron material grade, "QT" is the pinyin initials of "ductile iron", and the latter two groups of numbers represent the tensile strength value and elongation value of the cast iron, respectively, and have nothing to do with the specific chemical composition. The mechanical properties of the castings of different material grades of the present invention and their naming are derived from the combined effect of the types and contents of all elements and the internal structure of the castings, rather than being determined by the presence or absence and content of certain elements. The preparation process provided by the present invention enables the castings to have an excellent internal structure without obvious defects, so the chemical composition will be different from the existing cast iron of the same grade.

[0052] The mechanical properties of the castings of various material grades of the present invention are tested by sampling the body and the results are as follows:

[0053] The tensile strength of QT400-18 castings made of high-quality scrap steel is R m 400-480MPa, yield strength R p0.2 The hardness is 242-295MPa, the elongation after fracture A is 15-18%, and the hardness is 140-155HB;

[0054] The tensile strength of QT500-7 castings made of high-quality scrap steel is R m 450-540MPa, yield strength R p0.2The hardness is 286-324MPa, the elongation after fracture A is 7-10%, and the hardness is 160-175HB;

[0055] The tensile strength of QT600-3 castings made of high-quality scrap steel is R m 560-610MPa, yield strength R p0.2 The hardness is 329-366MPa, the elongation after fracture A is 4.5-7.5%, and the hardness is 182-208HB;

[0056] In the above performance test, the tensile strength R m The test method is carried out according to GB / T228-2010 Metal Material Room Temperature Tensile Test Method, the yield strength R p0.2 The test method is carried out according to the room temperature tensile test method for metal materials in GB / T228-2010, the elongation after fracture A test method is carried out according to the room temperature tensile test method for metal materials in GB / T228-2010, and the hardness test method is carried out according to the metal Brinell hardness test method in GB / T231.2-2002.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] (1) The preparation method provided by the present invention does not use accelerated cooling process measures to prepare ductile iron castings with a wall thickness greater than 1000 mm, and the spheroidization rate is above 95%, even reaching 98%, and the number of graphite balls is 500 / mm 2 and above, and there are no internal structural defects.

[0059] (2) The preparation method provided by the present invention only needs to adjust the contents of Si, Mn and Cu elements during the preparation process to obtain three different grades of ductile iron with excellent performance, namely QT400-18, QT500-7 and QT600-3, which meets the needs of minimum changes in production conditions and equipment to replace the preparation of the above three grades of ductile iron in actual production, avoids many complicated adjustment and replacement operations on raw materials and equipment, and these three grades of ductile iron have the high spheroidization rate and excellent internal structure described in (1) while having the performance required by their respective grades.

[0060] (3) In the preparation method provided by the present invention, the raw materials, various additives, element content ranges and other substances and various parameters defined are determined by the inventors through long-term creative work and repeated experiments. When the same material grade of ductile iron is prepared by using the same transfer bag spheroidization method and without forced cooling, the comprehensive performance of the ductile iron parts obtained by using the substances and parameters defined by the present invention is the best. That is, the present invention provides the raw materials, various additives, element content ranges and other substances and various parameters required for preparing ductile iron with excellent performance by using the transfer bag spheroidization method and without forced cooling.

[0061] (4) The castings manufactured by the preparation method of the present invention have excellent mechanical properties. The ultrasonic flaw detection reaches level 01 of EN12680-3:2012, and the sound speed reaches 6000-6200m / s, indicating that its internal structure is excellent and defect-free. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 Schematic diagram of sampling samples of the base casting and body of the product in Example 1

[0063] Figure 2-4 Metallographic images of the base casting bodies of different grades of products in Examples 1-3

[0064] Figure 5-15 Metallographic image of the base casting body sample of comparative example 1-11 DETAILED DESCRIPTION

[0065] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0066] Example 1

[0067] The raw material is QT400-18 casting made of high-quality scrap steel

[0068] (Base: weight 18495Kg, wall thickness 1108mm, such as Figure 1 (shown in 1, the same below)

[0069] The element composition of the product includes: C: 3.65wt%, Si: 2.07wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0070] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0071] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0072] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0073] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0074] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0075] A method for preparing ductile iron castings, the specific process is:

[0076] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0077] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0078] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0079] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0080] The prepared ductile iron casting was named casting A1.

[0081] The spheroidization rate of the casting A1 body sample is 96%, and the number of graphite balls is 600 / mm 2 ,like Figure 2 The sampling position is the core of the casting, and the sample diameter is 40 mm, the same below.

[0082] Example 2

[0083] The raw material is QT500-7 casting made of high-quality scrap steel

[0084] The element composition of the product includes: C: 3.78wt%, Si: 2.5wt%, Mn: 0.40wt%, P: 0.017wt%, S: 0.009wt%, Cu: 0.45wt%, RE: 0.0047wt%, Mg: 0.045wt%, Ti: ≤0.001wt%;

[0085] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0086] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0087] Spheroidizing agent components: Mg: 5.5wt%, Si: 50wt%, Ca: 2.5wt%, La: 0.6wt%, Ce: 0.35wt%, Al: 0.9wt%, particle size: 10mm;

[0088] Low silicon inoculant composition: Si: 45wt%, Ca: 1.0wt%, Ba: 2.0wt%, Al: 0.8wt%, particle size: 3mm;

[0089] Special inoculant composition: Si: 55wt%, Ce: 0.9wt%, Ca: 1.0wt%, Al: 0.8wt%, particle size 0.7mm;

[0090] A method for preparing ductile iron castings, the specific process is:

[0091] (1) 20000 kg of raw materials and 854 kg of high-quality carburizer were melted into raw iron liquid, 446 kg of block 75% ferrosilicon and 76 kg of broken block 55% ferromanganese were added, and the following element contents were sampled and analyzed and adjusted to: C: 3.88 wt%; Si: 1.52 wt%; Mn: 0.40 wt%; P: 0.017 wt%; S: 0.010 wt%; Ti: 0.0008 wt%;

[0092] (2) After the element content is adjusted, the raw iron liquid is heated to 1500°C and poured into the tundish;

[0093] (3) 200 kg of spheroidizing agent is placed on one side of the spheroidizing bag, 120 kg of low-silicon inoculant is placed on the spheroidizing agent, 90 kg of block 99.9% electrolytic copper is added, and the raw iron liquid in the tundish is poured into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0094] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0095] The prepared ductile iron casting was named casting A2.

[0096] The spheroidization rate of the casting A2 body sample is 98%, and the number of graphite balls is 600 / mm 2 ,like Figure 3 .

[0097] Example 3

[0098] The raw material is QT600-3 casting made of high-quality scrap steel

[0099] The element composition of the product includes: C: 3.67wt%, Si: 2.10wt%, Mn: 0.60wt%, P: 0.017wt%, S: 0.009wt%, Cu: 0.55wt%, RE: 0.0039wt%, Mg: 0.035wt%, Ti: ≤0.001wt%;

[0100] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0101] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0102] Spheroidizing agent composition: Mg: 5.3wt%, Si: 45wt%, Ca: 2.5wt%, La: 0.5wt%, Ce: 0.3wt%, Al: 0.8wt%, particle size: 20mm;

[0103] Low silicon inoculant composition: Si: 40wt%, Ca: 2.0wt%, Ba: 2.5wt%, Al: 0.6wt%, particle size: 8mm;

[0104] Special inoculant composition: Si: 53wt%, Ce: 0.8wt%, Ca: 0.8wt%, Al: 0.8wt%, particle size 0.5mm;

[0105] A method for preparing ductile iron castings, the specific process is:

[0106] (1) 20000 kg of raw materials and 840 kg of high-quality carburizer were melted into raw iron liquid, 408 kg of block 75% ferrosilicon and 157.6 kg of broken block 55% ferromanganese were added, and the following element contents were sampled and analyzed and adjusted to: C: 3.78 wt%; Si: 1.38 wt%; Mn: 0.60 wt%; P: 0.017 wt%; S: 0.015 wt%; Ti: 0.0005 wt%;

[0107] (2) After the element content is adjusted, the raw iron liquid is heated to 1480°C and poured into the tundish;

[0108] (3) 200 kg of spheroidizing agent is placed on one side of the spheroidizing bag, 120 kg of low-silicon inoculant is placed on the spheroidizing agent, 112 kg of block 99.9% electrolytic copper is added, and the raw iron liquid in the tundish is poured into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0109] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0110] The prepared ductile iron casting was named casting A3.

[0111] Sampling rate of casting A3 body: 95%, number of graphite balls: 600 / mm 2 ,like Figure 4 .

[0112] Comparative Example 1

[0113] The raw material is QT400-18 casting made of high-quality scrap steel

[0114] The element composition of the product includes: C: 3.30wt%, Si: 2.07wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.019wt%, RE: 0.0044wt%, Mg: 0.019wt%, Ti: ≤0.001wt%;

[0115] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0116] Conventional recarburizer components include: C: 90.5wt%, ash: 4.65wt%, volatile matter: 4.85wt%, S: 0.055wt%, N: 400PPM, particle size: 2-5mm;

[0117] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0118] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0119] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0120] A method for preparing ductile iron castings, the specific process is:

[0121] (1) 20000 kg of raw materials and 812 kg of conventional carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.38 wt%; Si: 1.3 wt%; Mn: 0.25 wt%; P: 0.017 wt%; S: 0.026 wt%; Ti: 0.001 wt%;

[0122] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0123] (3) Place 100 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0124] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0125] The prepared ductile iron casting was named casting D1.

[0126] The spheroidization rate of the casting D1 body sample is 84%, and the number of graphite balls is 125 / mm 2 ,like Figure 5 .

[0127] Comparative Example 2

[0128] The raw material is QT400-18 casting made of conventional scrap steel

[0129] The elemental composition of the product includes: C: 3.65wt%, Si: 2.07wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: 0.032wt%;

[0130] Conventional scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti: 0.032wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0131] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0132] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0133] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0134] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0135] A method for preparing ductile iron castings, the specific process is:

[0136] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.032 wt%;

[0137] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0138] (3) Place 100 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0139] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0140] The prepared ductile iron casting was named casting D2.

[0141] The spheroidization rate of the casting D2 body sample is 84%, and there is waterweed-like graphite. The number of graphite balls is 100 / mm 2 ,like Figure 6 .

[0142] Comparative Example 3

[0143] The raw material is QT400-18 casting made of high-quality scrap steel

[0144] The element composition of the product includes: C: 4.18wt%, Si: 2.95wt%, Mn: 0.80wt%, P: 0.017wt%, S: 0.018wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0145] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0146] High-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.040wt%, N: 150PPM, particle size: 2-5mm;

[0147] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0148] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0149] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0150] A method for preparing ductile iron castings, the specific process is:

[0151] (1) 20000 kg of raw materials and 959 kg of high-quality carburizer were melted into raw iron liquid, 647 kg of block 75% ferrosilicon and 238 kg of broken block 55% ferromanganese were added, and the following element contents were sampled and analyzed and adjusted to: C: 4.35 wt%; Si: 2.2 wt%; Mn: 0.80 wt%; P: 0.017 wt%; S: 0.024 wt%; Ti: 0.001 wt%;

[0152] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0153] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0154] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0155] The prepared ductile iron casting was named casting D3.

[0156] The spheroidization rate of the casting D3 body sample is 80%, and graphite floating appears. The number of graphite balls is 100 / mm 2 ,like Figure 7 .

[0157] Comparative Example 4

[0158] The raw material is QT400-18 casting made of high-quality scrap steel

[0159] The element composition of the product includes: C: 3.65wt%, Si: 2.07wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0020wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0160] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0161] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0162] Spheroidizing agent components: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0163] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0164] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0165] A method for preparing ductile iron castings, the specific process is:

[0166] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0167] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0168] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0169] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0170] The prepared ductile iron casting was named casting D4.

[0171] Sampling rate of casting D4 body: 80%, number of graphite balls: 100 / mm 2 ,like Figure 8 .

[0172] Comparative Example 5

[0173] The raw material is QT400-18 casting made of high-quality scrap steel

[0174] The element composition of the product includes: C: 3.65wt%, Si: 2.07wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0035wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0175] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0176] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0177] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.45wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0178] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0179] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0180] A method for preparing ductile iron castings, the specific process is:

[0181] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0182] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0183] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0184] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0185] The prepared ductile iron casting was named casting D5.

[0186] The spheroidization rate of the casting D5 body sample is 85%, and the number of graphite balls is 150 / mm 2 ,like Fig. 9 .

[0187] Comparative Example 6

[0188] The raw material is QT400-18 casting made of high-quality scrap steel

[0189] The element composition of the product includes: C: 3.65wt%, Si: 2.07wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0055wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0190] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0191] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0192] The spheroidizing agent components include: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.65wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0193] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0194] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0195] A method for preparing ductile iron castings, the specific process is:

[0196] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0197] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0198] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0199] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0200] The prepared ductile iron casting was named casting D6.

[0201] The spheroidization rate of the casting D6 body sample is 85%, and the number of graphite balls is 150 / mm 2 ,like Fig.10 .

[0202] Comparative Example 7

[0203] The raw material is QT400-18 casting made of high-quality scrap steel

[0204] The element composition of the product includes: C: 3.65wt%, Si: 2.19wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0205] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0206] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0207] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0208] Inoculant composition: Si: 73wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0209] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0210] A method for preparing a ductile iron casting, wherein the wall thickness of the ductile iron casting is ≥400 mm, and the specific process is:

[0211] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 369 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.26 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0212] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0213] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0214] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0215] The prepared ductile iron casting was named casting D7.

[0216] The spheroidization rate of the casting D7 body sample is 87%, and the number of graphite balls is 175 / mm 2 ,like Fig.11 .

[0217] Comparative Example 8

[0218] The raw material is QT400-18 casting made of high-quality scrap steel

[0219] The element composition of the product includes: C: 3.65wt%, Si: 2.03wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0220] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0221] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0222] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0223] Inoculant composition: Si: 35wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0224] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0225] A method for preparing ductile iron castings, the specific process is:

[0226] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0227] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0228] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0229] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0230] The prepared ductile iron casting was named casting D8.

[0231] The spheroidization rate of the casting D8 body sample is 82%, and the number of graphite balls is 75 / mm 2 ,like Fig.12 .

[0232] Comparative Example 9

[0233] The raw material is QT400-18 casting made of high-quality scrap steel

[0234] The element composition of the product includes: C: 3.65wt%, Si: 2.05wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0235] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0236] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0237] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0238] Special inoculant composition: Si: 50wt%, Ce: 1.0wt%, Ca: 0.5wt%, Al: 0.75wt%, particle size 0.2mm;

[0239] A method for preparing ductile iron castings, the specific process is:

[0240] (1) (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, and 446 kg of block 75% ferrosilicon was added. Samples were taken for analysis and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.52 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0241] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0242] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing treatment;

[0243] (4) After the spheroidization treatment is completed, the slag is removed and then poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during pouring.

[0244] The prepared ductile iron casting was named casting D9.

[0245] The spheroidization rate of the casting D9 body sample is 79%, the graphite is coarse, and the number of graphite balls is 25 / mm 2 ,like Fig.13 .

[0246] Comparative Example 10

[0247] The raw material is QT400-18 casting made of high-quality scrap steel

[0248] The element composition of the product includes: C: 3.65wt%, Si: 2.09wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0249] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0250] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0251] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0252] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0253] Special inoculant composition: Si: 60wt%, Ce: 0.5wt%, Ca: 1.5wt%, Al: 1.5wt%, particle size 0.2mm;

[0254] A method for preparing ductile iron castings, the specific process is:

[0255] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 380 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.3 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0256] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0257] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0258] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into a mold to obtain a casting. 40 kg of special-effect inoculant is added during the pouring.

[0259] The prepared ductile iron casting was named casting D10.

[0260] The spheroidization rate of the casting D10 body sample is 90%, and the number of graphite balls is 250 / mm 2 ,like Fig.14 .

[0261] Comparative Example 11

[0262] The raw material is QT400-18 casting made of high-quality scrap steel

[0263] The element composition of the product includes: C: 3.65wt%, Si: 2.05wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.008wt%, RE: 0.0044wt%, Mg: 0.039wt%, Ti: ≤0.001wt%;

[0264] The high-quality scrap steel components include: C: 0.07wt%, Si: 0.016wt%, Mn: 0.21wt%, P: 0.017wt%, S: 0.006wt%, Ti≤0.001wt%, Pb≤0.008wt%, Zn≤0.005wt%, V≤0.001wt%, Cr≤0.03wt%, Bi≤0.006wt%;

[0265] The high-quality recarburizer components include: C: 99.2wt%, ash: 0.42wt%, volatile matter: 0.38wt%, S: 0.015wt%, N: 150PPM, particle size: 2-5mm;

[0266] Spheroidizing agent composition: Mg: 5.0wt%, Si: 47wt%, Ca: 2.6wt%, La: 0.55wt%, Ce: 0.4wt%, Al: 0.7wt%, particle size: 3mm;

[0267] Low silicon inoculant composition: Si: 43wt%, Ca: 1.5wt%, Ba: 3.0wt%, Al: 0.7wt%, particle size: 6mm;

[0268] A method for preparing ductile iron castings, the specific process is:

[0269] (1) 20000 kg of raw materials and 812 kg of high-quality carburizer were melted into raw iron liquid, 401 kg of block 75% ferrosilicon was added, and the following element contents were adjusted to: C: 3.70 wt%; Si: 1.37 wt%; Mn: 0.21 wt%; P: 0.017 wt%; S: 0.014 wt%; Ti: 0.001 wt%;

[0270] (2) After the element content is adjusted, the raw iron liquid is heated to 1460°C and poured into the tundish;

[0271] (3) Place 200 kg of spheroidizing agent on one side of the spheroidizing bag, and press 120 kg of low-silicon inoculant on the spheroidizing agent. Pour the raw iron liquid in the tundish into the spheroidizing bag through the water trough for spheroidizing inoculation treatment;

[0272] (4) After the spheroidizing inoculation treatment is completed, the slag is removed and then the casting is poured into the mold to obtain the casting.

[0273] The prepared ductile iron casting was named casting D11.

[0274] The spheroidization rate of the casting D11 body sample is 78, the graphite is coarse, and the number of graphite balls is 25 / mm 2 ,like Fig.15 .

[0275] Performance Testing

[0276] 1. Metallographic structure inspection of castings

[0277] The casting body is used for sampling, the sampling position is the core of the casting, and the sample diameter is 40mm (such as Figure 1 The sample metallographic structure inspection specification refers to GB / T9441-2021 "Metallographic Inspection of Ductile Iron". The inspection results are shown in Table 1.

[0278] The metallographic diagrams of castings A1 to A3 are as follows: Figures 2 to 4 As shown, the metallographic diagrams of castings D1 to D11 are as follows: Figures 5 to 15 shown.

[0279] Table 1

[0280]

[0281]

[0282] 2. Testing of various mechanical properties of castings

[0283] Tensile strength R m The test method is based on the room temperature tensile test method for metal materials in GB / T228-2010. A static tensile load is applied uniformly along the axial direction of the specimen until the elongation at which the specimen breaks. During the entire process, the load applied to the specimen is measured and the tensile strength value can be calculated.

[0284] Yield Strength R p0.2 The test method is based on the room temperature tensile test method for metal materials in GB / T228-2010. During the process of applying a static tensile load at a uniform speed along the axial direction of the specimen, the yield strength can be calculated based on the stress when 0.2% plastic deformation occurs.

[0285] The test method for the elongation after fracture A is carried out according to the room temperature tensile test method for metal materials GB / T228-2010. A static tensile load is uniformly applied along the axial direction of the sample until the elongation of the sample breaks. During the whole process, the elongation value of the sample gauge length is measured, and the elongation after fracture can be calculated, that is, the percentage of the residual elongation of the gauge length after fracture to the original gauge length.

[0286] The hardness test method is based on the metal Brinell hardness test method of GB / T231.2-2002.

[0287] The test results are shown in Table 2.

[0288] 3. Ultrasonic flaw detection test

[0289] Test standard: EN12680-3:2012 (EN12680-3:2012 "Casting - Ultrasonic Testing - Part 3 - Ductile Iron Castings")

[0290] The test results are shown in Table 2.

[0291] Table 2

[0292]

[0293]

[0294] It can be seen from the data in Table 2 that the castings A1 to A3 prepared in the embodiment of the present invention have excellent mechanical properties, and the ultrasonic flaw detection reaches level 01 of EN12680-3:2012, and the sound speed reaches 6000-6200m / s, indicating that the internal structure is excellent and defect-free.

[0295] Although the castings prepared in comparative examples D1 to D11 belong to the same QT400-18 ductile iron castings as casting A1 prepared in Example 1, it can be clearly seen that the mechanical properties of the castings of comparative examples 1 to 11 are inferior to those of the castings of Example 1, and the presence of internal defects leads to a low ultrasonic flaw detection level.

[0296] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing ductile iron castings, characterized in that: The wall thickness of the ductile iron casting is ≥1000mm, and the specific process is: (1) Melt the raw materials and high-quality carburizer into raw iron liquid, take samples for analysis and adjust the following element contents to the required range: C: 3.70-3.88wt%; Si: 1.2-1.80wt%; Mn: ≤0.60wt%; P: ≤0.020wt%; S: ≤0.015wt%; Ti: ≤0.001wt%; (2) After the element content is adjusted, the raw iron liquid is heated to 1460-1500℃ and poured into the tundish; (3) Place a spheroidizing agent on one side of the spheroidizing bag, press a low-silicon inoculant on the spheroidizing agent, and pour the raw iron liquid in the tundish into the spheroidizing bag through a water trough for spheroidizing inoculation treatment; The components of the spheroidizing agent meet the following requirements: Mg: 5.0-5.5wt%, Si: 45-50wt%, Ca: 2.5-2.6wt%, La: 0.5-0.6wt%, Ce: 0.3-0.4wt%, Al: 0.7-0.9wt%, particle size: 3-20mm; The components of the low-silicon inoculant meet the following requirements: Si: 40-45wt%, Ca: 1.0-2.0wt%, Ba: 2.0-3.0wt%, Al: 0.6-0.8wt%, particle size: 3-8mm; (4) After the spheroidizing inoculation treatment is completed, the slag is removed, and then the casting is poured into the mold to obtain the casting, and a special inoculant is added during the pouring; The components of the special effect inoculant meet the following requirements: Si: 50-55wt%, Ce: 0.8-1.0wt%, Ca: 0.5-1.0wt%, Al: 0.7-0.8wt%, particle size 0.2-0.7mm; The raw material in step (1) is high-quality scrap steel, and the composition of the high-quality scrap steel meets the following requirements: Ti: ≤0.001wt%, Pb: ≤0.008wt%, Zn: ≤0.005wt%, V: ≤0.001wt%, Cr: ≤0.03wt%, Bi: ≤0.006wt%; In step (3), the amount of the spheroidizing agent added is 1.0wt% of the raw material, and the amount of the low-silicon inoculant added is 0.6wt% of the raw material; The amount of the special effect inoculant added in step (4) is 0.2wt% of the raw material; The addition amount of the high-quality recarburizer is 4.06-4.27wt% of the raw material, and the components meet the following requirements: C≥98.5wt%, S<0.03wt%, N<200PPM, and particle size: 2-5mm.

2. A ductile iron casting with a wall thickness of ≥1000 mm and a spheroidization rate of ≥95% prepared by the preparation method as claimed in claim 1.

Citation Information

Cited By

  • High strength and high thermal conductivity gray cast iron and manufacturing method thereof

    TWI941463B