A 550MPa grade extra-thick steel plate and a manufacturing method thereof
Through specific chemical composition and smelting processes, excellent martensite and bainite structures are formed, which solves the production problems of high-strength and high-toughness extra-thick steel plates in the existing technology, and realizes high-strength and excellent low-temperature toughness 550MPa grade steel plates. Meet the requirements of large hydropower generator sets and mechanical steel structures in high-altitude areas.
Patent Information
- Application Number
- CN202310077258.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-02-08
AI Technical Summary
It is difficult to produce high-strength and high-toughness extra-thick steel plates in the prior art, especially in large hydropower generator sets and mechanical steel structure manufacturing in high-altitude areas, the internal quality and processing performance of the steel plates are difficult to meet the high requirements.
Using specific chemical composition and smelting processes, including reasonable proportions of C, Si, Mn, Cr, Ni, Mo, V, Ti, Nb, B and other elements, through initial refining, refining, continuous casting, heating, and rolling , cooling, quenching and tempering process steps to form excellent martensite and bainite structures, and improve the strength and toughness of the steel plate.
The production of 550MPa grade high-strength extra-thick steel plates is achieved, ensuring the internal quality of the steel plates, ultrasonic flaw detection level and low-temperature toughness, and meeting the manufacturing needs of large hydropower generator sets and mechanical steel structures in high-altitude areas.
Smart Images

Figure CN116179950B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a particularly thick 550MPa grade steel plate used for manufacturing hydroelectric generator sets and mechanical steel structures, and also relates to a manufacturing method of the steel plate. Background Art
[0002] Hydropower has become one of the important clean energy sources in the contemporary world with its renewable and pollution-free advantages. With the rapid development of my country's industrial technology, hydropower projects have gradually developed towards large-scale development. The thickness and strength of steel plates used in the manufacture of structural components such as seat rings, guide vanes, flanges, etc. of large hydropower generators are getting thicker and thicker. As the thickness increases and the strength increases, the requirements for internal quality such as ultrasonic flaw detection level and steel plate toughness are also getting higher and higher. In addition, with the development of steel structure machinery manufacturing technology, the demand for thick, high-strength, and high-toughness steel plates is also increasing year by year, especially for some steel structure machinery used in high-cold areas, which have high requirements for low-temperature toughness and internal quality of steel plates. Generally, flat steel ingots, electroslag ingots and water-cooled steel ingots are used to manufacture these thick steel plates, but their yield rate is low and the cost is high; although continuous casting billets have the advantages of high yield rate and low cost, they are limited by compression ratio, and the internal quality and strength and toughness of steel plates are difficult to guarantee, resulting in the thickness and strength and toughness level of steel plates that can be produced being greatly limited.
[0003] Publication No. CN111826585 A discloses a thick and high-toughness S500QL1 steel plate and its production method. The steel plate has a thickness of 200mm to 300mm, is made of steel ingot or electroslag ingot, and is subjected to high-temperature quenching, sub-temperature quenching and tempering heat treatment. The structure of the steel plate is bainite and undissolved ferrite, the yield strength is 490Mpa to 540Mpa, the tensile strength is 630Mpa to 680Mpa, the average impact energy at -60℃ at 1 / 4 of the plate thickness is ≥100J, and the average impact energy at -80℃ at 1 / 4 of the plate thickness is ≥70J. The thickness of the steel plate is greater than that of the present invention, but the disadvantage is that the yield rate of steel ingot or electroslag ingot production is low, and when the electroslag ingot is made, hydrogen expansion annealing and AL content are required, the production cycle of two quenching and tempering heat treatment is long, the process is complicated, and the strength level of the steel plate is also lower than that of the present invention.
[0004] Publication No. CN111020384 A discloses a quenched and tempered high-strength SM570 steel plate for large mirror plates of hydro-turbine generators and a production method thereof, with a steel plate thickness of 160 mm to 200 mm, strict purity control during smelting, water-cooled steel ingot production, a heating process using a method of simmering steel - heating up - heat preservation - steel turning - heat preservation, two-stage rolling of rough rolling + finishing rolling, offline external mechanized furnace quenching of the steel plate + trolley furnace tempering heat treatment, a steel plate microstructure of 30% to 40% ferrite + 30% to 40% bainite + pearlite, a yield strength of ≥450Mpa, a tensile strength of ≥630Mpa, a low-temperature longitudinal impact energy of -50°C of ≥100J, and a Brinell hardness of ≥190HB. The disadvantages are that the yield rate of water-cooled steel ingot production is low, the process is complex, and the strength level of the steel plate is much lower than that of the present invention.
[0005] Publication No. CN 103725959 A discloses a method for producing a 130mm low alloy low temperature toughness thick steel plate, which is produced by continuous casting of 400mm thickness, with a steel plate thickness of 130mm, and heat treated by normalizing + accelerated cooling heat treatment process, with a steel plate yield strength of 360Mpa-420MPa, a tensile strength of 520Mpa-600MPa, -40℃ impact ≥150J, -60℃ impact ≥75J. The strength level of the steel plate is only 355Mpa, which is far lower than the present invention, and the thickness of the steel plate is also less than the present invention. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a 550MPa grade high-strength, high-toughness extra-thick steel plate with excellent internal quality and processing performance for the above-mentioned prior art, which is used to manufacture large hydroelectric generating sets and mechanical steel structures in high-cold areas.
[0007] The technical solution adopted by the present invention to solve the above problems is: a 550MPa grade high-strength extra-thick steel plate, characterized in that the steel plate is smelted from the following components in mass percentage: C: 0.06% to 0.16%, Si: ≤0.35%, Mn: 1.10% to 1.70%, P≤0.012%, S≤0.002%, Cr: 0.40% to 0.80%, Cu: ≤0.50%, Ni: 0.35% to 1.00%, Als: 0.025% to 0.050%, Nb: 0.015% to 0.050%, V: 0.020% to 0.080%, Ti: 0.010% to 0.025%, Mo: 0.25% to 0.60%, B: 0.0001% to 0.0025%, and the balance is Fe and unavoidable impurities.
[0008] The functions of the components and contents in the steel plate in the present invention are:
[0009] ⑴, Carbon (C)
[0010] Improve the hardenability of steel. With the increase of carbon content in steel, the Ms-Mf martensitic phase transformation temperature range expands, the phase transformation temperature range moves down, and the isothermal transformation C curve moves to the right, which promotes the martensitic phase transformation and the lower bainitic phase transformation, and promotes the steel to have sufficient strength and excellent toughness after quenching and tempering; it combines with strong carbide forming elements such as Nb and Ti to play the effect of controlled rolling and controlled cooling to refine grains. However, if the content is too high, the amount in the form of interstitial atoms is too large, which seriously affects the toughness of the steel. Therefore, the present invention controls the carbon content to 0.06% to 0.16%.
[0011] ⑵、Silicon (Si)
[0012] It is an economical deoxidizer commonly used in the steelmaking process. If the residual amount is too low, the steelmaking cost will increase. When the steel contains alloys such as Cu and Ni, it will increase the adhesion of the oxide scale during the heating process, increase the descaling burden during the rolling process, and may even affect the surface quality of the steel plate. The present invention controls the Si content in the steel to ≤0.35%.
[0013] ⑶. Manganese (Mn)
[0014] Improve the hardenability of steel, increase the depth of the martensite layer in the steel plate after quenching, reduce the phase transition point of martensite and bainite, promote the bainite phase transition in the lower bainite phase transition area, ensure the strength of steel and improve the low temperature toughness. However, there is a tendency to promote the growth of austenite grains. Therefore, the manganese content used in the present invention is 1.10% to 1.70%.
[0015] ⑷. Phosphorus (P)
[0016] It is a harmful element in steel, which reduces the low-temperature toughness of steel plates and increases the toughness-brittleness transition temperature of steel. It increases the temper brittleness of steel. It is very easy to segregate. Try to reduce its content.
[0017] ⑸. Sulfur (S)
[0018] It is a harmful element in steel, which seriously reduces the toughness and plasticity of steel, causes the directionality of steel performance, increases the temper brittleness of steel, and is very easy to segregate. Try to reduce its content.
[0019] ⑹、Chromium (Cr)
[0020] Dissolved in austenite, it shifts the austenite isothermal transformation curve to the right, reduces the phase transition point of steel, reduces the critical transformation cooling rate of austenite, improves the hardenability of steel, promotes the formation of martensite after rapid cooling, is beneficial to the control of bainite morphology, and improves the strength and toughness of steel. During high-temperature tempering, it can form special carbides with fine particles, which significantly delay the recovery and recrystallization of the α phase, thus making the steel have higher tempering stability. Medium-strong carbide-forming elements hinder the diffusion of carbon in martensite, thereby slowing down the decomposition rate of martensite, reducing the diffusion coefficient of carbon in austenite, significantly slowing down the formation rate of austenite during heating, and prolonging the insulation time required for austenitization. The present invention controls chromium to 0.40% to 0.80%.
[0021] ⑺. Nickel (Ni)
[0022] Ni reduces the A1 phase transformation temperature, accelerates the formation of austenite during heating, and increases the diffusion coefficient of carbon in austenite; strongly reduces the Ms and Mf points of martensitic phase transformation, improves hardenability, significantly delays the formation of bainite, and can promote the formation of lower bainite-like bainite with good phase transformation toughness in the lower temperature zone, which can effectively improve the impact toughness of steel and reduce its brittle transition temperature; in addition, nickel can effectively prevent the cracking caused by copper hot brittleness. However, the price is relatively expensive, and the nickel content of the present invention is controlled at 0.35% to 1.00%.
[0023] ⑻, Molybdenum (Mo)
[0024] The Ms and Mf points are reduced, the hardenability of the steel is improved, and the depth of the martensite layer is increased; the C curve of the austenite phase transformation is shifted to the right, the pearlite transformation and bainite transformation curves are separated, and the cooling conditions are controlled to form fine lower bainite type low-carbon bainite with good strength and toughness; when tempered after quenching, the steel has a strong tempering stability and has a very significant effect of reducing temper brittleness. Medium-strong carbide forming elements increase the diffusion activation energy of carbon in martensite, hinder the diffusion of carbon in martensite, thereby slowing down the decomposition rate of martensite, and are expensive. The present invention controls the molybdenum content to 0.25-0.60%.
[0025] ⑼、Aluminum (AL)
[0026] Aluminum is a strong deoxidizing element, used for final deoxidation of molten steel, and used in combination with Si for molten steel refining. The heating process has a certain effect of hindering the growth of austenite grains, but when the residual Al content in the steel reaches a certain limit, it may cause the coarsening of austenite grains. The present invention controls the acid-soluble aluminum (ALs) to 0.025% to 0.050%.
[0027] ⑽、Vanadium (V)
[0028] Solid solution in austenite can improve the hardenability of steel. When tempered at high temperature, it makes the steel have higher tempering stability and has the effect of inhibiting the second type of temper brittleness. However, when precipitated in steel, it is not good for toughness. The present invention controls it within 0.020% to 0.080%.
[0029] ⑾. Titanium (Ti)
[0030] It is a strong carbon and nitride forming element, forming TiC particles with high melting point, strong stability, and not easy to aggregate and grow. It is dispersed in the austenite matrix, hindering the growth of grains and thus refining the austenite grains. When the content is too high, it is not good for toughness. The present invention controls it within 0.010% to 0.025%.
[0031] ⑿. Niobium (Nb)
[0032] The particles of NbC, NbN, Nb(C, N) with high melting point, strong stability and not easy to aggregate and grow are formed and dispersed in the austenite matrix, which hinders the growth of grains and refines the austenite grains; increases the austenite recrystallization temperature, promotes the enrichment of nucleation of γ / α phase transformation, and refines the structure after phase transformation. The secondary hardening phenomenon can be suppressed during tempering after quenching, thereby improving the impact toughness of the steel plate. The present invention controls it at 0.015% to 0.050%.
[0033] ⒀, Boron (B)
[0034] It segregates at the grain boundaries, greatly improving the hardenability of the steel; but at the same time it is easy to cause temper brittleness, which has a very harmful effect on the impact toughness of the steel. The thicker the steel plate, the more obvious the effect. Therefore, the present invention limits the boron content to 0.0001% to 0.0025%.
[0035] ⒁. Copper (Cu)
[0036] It can improve the tempering resistance of steel. It is easy to produce hot brittleness during heating or hot rolling, which deteriorates the surface quality of the steel plate. The copper content of the present invention is controlled to ≤0.50%.
[0037] The manufacturing method of the 550MPa grade high-strength extra-thick steel plate with the above chemical composition for manufacturing large hydroelectric generator sets and mechanical steel structures in high-cold areas of the present invention comprises the following specific steps:
[0038] The first step is primary refining, which selects scrap steel and molten iron to reduce the harmful elements such as As, Sb, Sn, and Pb that cause temper brittleness in the steel, ensuring that the content of each element in the final molten steel is ≤0.004%. KR pretreatment removes the [S] content in the molten iron to ≤0.005%, and at the end of the BOF converter primary refining, the molten steel [P] is controlled to ≤0.008% to ensure that the final molten steel [P] is ≤0.012%. In addition to adversely affecting the toughness of the steel plate, S and P are also factors that cause temper brittleness, so their residual content is reduced from the beginning of primary refining.
[0039] Step 2: Refining
[0040] Including LF refining and RH vacuum treatment, precise control of chemical composition and temperature, and ensuring that the [O] content of the molten steel is no more than 11ppm, the [H] content is no more than 1.0ppm, and the [S] content is no more than 0.002% at the end of refining. Residual oxygen [O] in the steel exists in the form of inclusions and segregates at the center of the continuous casting billet. A high content may cause crack defects in the center of the steel plate, resulting in failure of ultrasonic flaw detection; if the residual hydrogen [H] in the steel is too high, white spot defects will occur, and the steel must be scrapped. Even if the hydrogen content is low and not enough to produce white spot defects, it may cause the steel plate to fail ultrasonic flaw detection or the steel plate to fail impact toughness.
[0041] The third step is continuous steel casting
[0042] The molten steel is cast into continuous casting slabs on a straight arc continuous casting machine. The thickness of the slab is 370mm to 450mm. The superheat of the molten steel is controlled during the casting process. The width, thickness and pulling speed of the continuous casting slab are matched and controlled. When the solid phase fraction of the continuous casting slab is 0.59 to 0.73, the continuous casting slab is subjected to light pressure, and finally the low-multiple structure center segregation of the continuous casting slab is ≤C1.0 level, the center looseness is ≤0.5 level, and there are no internal defects such as middle cracks and triangular cracks. This center segregation and center looseness can be guaranteed by the subsequent rolling effect. It does not affect the internal quality of the final steel plate (i.e., the quality of ultrasonic flaw detection). The continuous casting slab is removed from the casting machine and cut into sections, and then quickly hoisted into the slow cooling pit for slow cooling. After slow cooling to the temperature of the continuous casting slab ≤300℃, it is removed from the pit for rolling. Slow cooling mainly plays the role of hydrogen expansion annealing, further reducing the hydrogen content in the continuous casting slab.
[0043] Step 4: Heating
[0044] The continuous casting slab is heated in a continuous heating furnace. According to the relevant calculation of micro-alloying element solid solution and practical exploration, the temperature of the heating section is determined to be 1000℃~1290℃, and the temperature of the soaking section is controlled at 1230℃~1270℃. At this time, the deformation resistance of the steel is reduced by heating at the highest possible temperature, creating excellent conditions for the deformation of the continuous casting slab during steel rolling. At the same time, the carbides of Ti and part of the carbonitrides of Nb are still in an undissolved state, dispersed and evenly distributed in the matrix of the continuous casting slab, which plays a role in preventing the growth of austenite grains. The other alloying elements have reached complete solid solution, but the heating temperature is below the austenite coarsening temperature of this steel grade to avoid the coarsening of austenite grains. The total heating time of the heating section plus the soaking section is 8min / cm~15min / cm of billet thickness, so that the core of the continuous casting billet reaches 1210℃~1250℃ to meet the requirements of the reduction system in the steel rolling process, so that the steel rolling deformation penetrates into the core of the continuous casting billet, improves the internal deformation of the continuous casting billet until the core reaches a large deformation, breaks the coarse cast grains, welds the loose center of the continuous casting billet, and further improves the segregation of carbon in the center of the continuous casting billet. If the heating time is further extended, the carbonitrides of Ti and Nb will decompose and dissolve in large quantities, causing the austenite grains to grow rapidly, which is not conducive to refining the organization and ensuring the performance of the steel plate. The core temperature of the continuous casting billet is automatically calculated by the heating system according to the heat transfer characteristics of the steel grade and the test results.
[0045] Step 5: Rolling
[0046] After the continuous casting billet leaves the heating furnace, the surface oxide scale is removed by a high-pressure water descaling box, and the initial rolling is immediately carried out on a 4300mm four-roll reversible thick plate rolling mill to 1.2 to 1.6 times the thickness of the finished steel plate. This thickness must meet the requirements of the reduction rate of breaking the inner part of the continuous casting billet until the core cast grains and the looseness of the welding center at this stage; the widening pass in the initial rolling stage is not counted, and the number of rolling passes with a single pass reduction rate of 9% to 27% is controlled at 5 to 8. Continuously increasing the single pass reduction rate can increase the effect of breaking the cast coarse structure and recrystallization in a single pass, but it is limited by the total thickness of the continuous casting billet. Increasing the reduction rate of a single pass will definitely reduce the total number of passes, which in turn reduces the overall welding porosity, crushing of cast coarse structure and recrystallization effects, and cannot meet the internal quality requirements of the steel plate. A single-pass reduction rate of less than 9% cannot meet the requirements of crushing cast coarse structure and recrystallization. During the rolling process, the four-roll cooling water is frequently turned on to reduce the surface temperature of the steel plate, so that during deformation, a certain temperature gradient is formed from the surface to the core of the steel plate, forming a certain deformation resistance gradient, achieving strong pressure at the center, maximizing the internal deformation of the steel plate, welding the center of the continuous casting billet loose, and on the other hand removing the secondary iron oxide scale on the surface of the steel plate. The widening pass is placed at the front pass after the start of rolling, so that the thickness of the continuous casting billet is relatively thinned, and the deformation is more easily affected by the core, so as to improve the density of the steel plate and ensure that the ultrasonic flaw detection of the steel plate meets the requirements; the final rolling temperature at this stage should be at T R(i.e., the complete recrystallization temperature of austenite) and above. At the same time, in order to give full play to the role of high temperature rolling in facilitating deformation and penetration, the final rolling temperature is controlled at T R +50℃ and above, according to the specific test, the final rolling temperature is controlled at ≥990℃, and the high temperature section is broken by rolling mechanical force and repeated recrystallization to refine the coarse cast structure and refine the grains. After the initial rolling, the core austenite grains should be at or above 5.0. After the initial rolling, the steel plate is cooled by auxiliary water spraying to avoid too much mixed crystals caused by long waiting time in the partial recrystallization zone (the temperature drop of thick steel plate is slow), and then the finishing rolling is carried out on a 4300mm four-roll reversible finishing mill. The finishing rolling is carried out in the austenite non-recrystallization zone, so that the non-recrystallized austenite reaches a cumulative deformation rate of 18% to 35%. In addition, the finishing rolling adjusts the plate shape and finely controls the size. According to the measurement, the finishing rolling start temperature is 910℃~840℃, and the final rolling temperature is 900℃~840℃.
[0047] Step 6: Accelerate Cooling
[0048] After finishing rolling, the steel plate is water-cooled by the DQ+ACC system. The cooling start temperature is Ar3+110~170℃, where Ar3 is the temperature at which ferrite begins to precipitate in austenite. The total flow rate of DQ cooling water is 5500Nm 3 / h~8000Nm 3 / h, ACC cooling water total flow 9500Nm 3 / h~12000Nm 3 / h, ACC cooling water 16 groups are fully open, roller running speed is 0.3m / s~0.9m / s, the thicker the steel plate, the slower the roller speed, the surface temperature of the steel plate out of the water cooling system is controlled to be ≤350℃, the average cooling rate of the steel plate is 8℃ / s~21℃ / s, due to the excessive thickness of the steel plate, the core cooling rate is 4℃ / s~12℃ / s, and the metallographic structure of the steel plate after cooling is martensite + bainite. After the steel plate is finished rolling, it starts cooling, and starts cooling in the austenite zone. High supercooling and high cooling rate increase the phase deformation nucleation rate, inhibit grain growth, and promote austenite intracrystalline nucleation in combination with the deformation band brought by the finish rolling, and refine the organization to the maximum extent. Through DQ rapid cooling to the lower area of the austenite to bainite transformation phase zone, the phase transformation produces fine bainite organization. This bainite grain is fine and easy to decompose during heat treatment heating. With the appropriate roller speed, the cooling penetrates into the core of the steel plate and the core also reaches the necessary cooling rate. The final cooling temperature is controlled at Mf-40℃~100℃. At this time, the entire section has completed the phase transformation. In the continuous cooling process, some areas of the steel plate have reached the martensitic phase transformation starting point (Ms) and its critical cooling rate, and martensitic phase transformation occurs. Therefore, the steel plate organization after cooling is bainite plus martensite, with fine grains. After the phase transformation is completed, the final cooling is mainly to prevent the subsequent phase transformation from causing coarse phase transformation organization, large internal stress of the steel plate, and deterioration of the plate shape. After the steel plate leaves the ACC water cooling system, it is quickly removed from the production line and enters the slow cooling cover for 72h to 96h to reduce the internal stress of the steel plate and avoid defects inside the steel plate during the cooling process that may cause the steel plate to fail ultrasonic flaw detection. After such controlled rolling and accelerated cooling, the steel plate grains will not affect the quality of ultrasonic flaw detection due to coarse grain reflection, and at the same time, the microstructure is prepared for heat treatment of the steel plate.
[0049] Step 7: Quenching
[0050] The steel plate is heated again to 760℃~830℃ in the heating furnace, and is taken out of the furnace after the core of the steel plate reaches the target temperature and is kept warm for 0.4min / mm~0.75min / mm according to the plate thickness. The surface temperature drop of the steel plate from the time of taking out of the furnace to the start of quenching is controlled within 40℃, otherwise the quenching degree and cooling rate may be reduced due to the lowering of the quenching temperature. The cooling water temperature is guaranteed to be ≤26℃ during the quenching process, and the cooling water volume reaches 9000Nm 3 / h~12000Nm 3 / h. If a quenching tank is used, the cooling water in the tank must be circulated and stirred to ensure that the quenching cooling rate of the core of the steel plate is ≥6℃ / s. The water can be discharged and quenching can be stopped only after the temperature of the core of the steel plate is ≤210℃. This is the requirement for the full cross-section of the steel plate to complete the phase transformation. To ensure that the temperature of the core of the steel plate is ≤210℃, the surface temperature of the steel plate when the quenching water is stopped must be ≤100℃. The heating process ensures that the microstructure completes the reverse transformation of martensite to austenite, bainite decomposes into ferrite and carbide, part of the ferrite is transformed into austenite, and the diffusion and homogenization of carbon and alloy elements are completed. The volume percentage of the retained ferrite is 11% to 24%, and the average diameter is 15 to 25μm. The ferrite is basically evenly distributed between the austenite, dividing the austenite and preventing the austenite grains from growing. At the same time, the martensite and bainite grains are refined during the quenching cooling process. During the quenching process, the temperature of the steel plate is rapidly cooled to the middle and lower temperature of the bainite transformation phase zone, which is below 500°C for the steel plate of the present invention. Since the steel plate is relatively thick, the cooling rate and temperature from the surface of the steel plate to the core are different. However, by controlling the cooling conditions and ensuring that the cooling rate of the core of the steel plate is ≥6°C / s, the austenite phase transformation of the entire section of the steel plate can be achieved to martensite and bainite. Bainite is a lower bainite ferrite matrix and fine carbides and M / A islands are evenly distributed in the laths. This bainite has good toughness. If the cooling rate or temperature is not well controlled, it may be transformed into upper bainite bainite, and the carbides and M / A islands are coarse, which greatly reduces the low-temperature toughness of the steel plate and increases the toughness-brittle transition temperature of the steel plate. After quenching, the metallographic structure of the steel plate is 55% to 31% martensite + 34% to 45% lower bainite bainite + 11% to 24% ferrite.
[0051] Step 8: Tempering
[0052] The tempering temperature Ac1-50~120℃, Ac1 is the temperature at which bainite or martensite begins to transform into austenite during heating, and the specific temperature for this steel grade is 610℃~680℃. The holding time after reaching the temperature is 1.3min / mm plate thickness~2.5min / mm plate thickness, martensite decomposes, bainite undergoes crystal transformation, M / A island decomposes, carbides spheroidize and maintain uniform dispersion distribution, and the final steel plate structure is tempered troostite + tempered bainite + a small amount of polygonal ferrite, of which the volume percentage is 55%~31% tempered troostite + 34%~45% bainite + 11%~24% ferrite, the average grain size of ferrite is 6μm~15μm, the average grain length of martensite and bainite is 10μm~35μm, and the width is 10μm~25μm. The target performance requirements of the steel plate are achieved. In addition, the internal stress of the steel plate is reduced by tempering to ensure that the steel plate has excellent processing and use performance.
[0053] Compared with the prior art, the advantages of the present invention are:
[0054] The present invention improves the density of continuous casting billets through unique smelting and continuous casting processes, reduces the central segregation and central porosity of continuous casting billets, avoids the generation of internal defects such as middle cracks, further improves the central segregation of continuous casting billets and welds the central porosity defects through continuous casting billet reheating and controlled rolling processes, avoids coarse steel plate organization, and solves the problem that the compression ratio of continuous casting billet rolling thick steel plate is low, which makes it difficult to ensure the quality of ultrasonic flaw detection; the chemical composition reduces the temper brittleness, adopts appropriate amount of C and Cr, Ni, Mo, V, Nb and other alloy components to control the hardenability and phase change characteristics of the steel plate, refines the grains through controlled rolling, controlled cooling, quenching and tempering processes, obtains a mixed organization of martensite, bainite and polygonal ferrite with ideal size and morphology, ensures that the extra-thick steel plate obtains high strength, high toughness and uniform performance, solves the problem that the strength and toughness are difficult to ensure due to excessive thickness of the steel plate, and improves the processing and use performance of the steel plate. Ensure that the internal quality, mechanical properties and processing and use performance of the steel plate meet the requirements of large hydropower generating units and large mechanical steel structure manufacturing in high-cold areas.
[0055] The extra thick steel plate manufactured by the present invention specifically includes the following advantages:
[0056] ⑴. The continuous casting billet is formed into a steel plate with a thickness of 100 to 180 mm.
[0057] ⑵. The steel plate has excellent internal quality, and the ultrasonic flaw detection meets GB / T 2970 Grade I;
[0058] ⑶. High strength steel plate, yield strength (Rp0.2) ≥ 550MPa, tensile strength (Rm) ≥ 660MPa ~ 770MPa, elongation after fracture (A) ≥ 18%;
[0059] ⑷. Excellent low temperature toughness of steel plate, -20℃ longitudinal and transverse KV2≥120J, -60℃ longitudinal and transverse KV2≥100J;
[0060] ⑸. The steel plate is produced by quenching + tempering heat treatment process to ensure excellent processing and performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 Microstructure of 100mm thick 550MPa grade extra thick steel plate.
[0062] Figure 2 Microstructure of 150mm thick 550MPa grade extra thick steel plate.
[0063] Figure 3 Microstructure of 180mm thick 550MPa grade extra thick steel plate. DETAILED DESCRIPTION
[0064] The present invention will be further described below with reference to examples.
[0065] The embodiments of the present invention are smelted by the components in mass percentage in the following Table 1, with the remainder being Fe and unavoidable impurities.
[0066] Table 1 Melting components of the present invention (mass percentage %)
[0067]
[0068]
[0069] The production steps of the 550MPa grade extra thick steel plate of the present invention are as follows:
[0070] The first step is primary refining, which selects scrap steel and molten iron, and the content of harmful elements such as As, Sb, Sn, and Pb in the steel is ≤0.004%. KR pretreatment removes the [S] content in the molten iron to ≤0.005%, and the molten steel [P] is controlled to ≤0.008% at the end of the BOF converter primary refining.
[0071] The second step is refining, including LF refining and RH vacuum treatment, to precisely control the chemical composition and temperature, and ensure that the [O] content of the molten steel is no more than 11ppm, the [H] content is no more than 1.0ppm, and the [S] content is no more than 0.002% at the end of refining. The specific refining process parameters and effects of each embodiment are shown in Table 2 below.
[0072] Table 2 Refining effect of each embodiment
[0073]
[0074] The third step is continuous steel casting, with a slab thickness of 370 mm to 450 mm. During the casting process, the superheat of the molten steel is controlled, and the width, thickness and casting speed of the continuous casting slab are matched and controlled, and a light reduction is applied to the continuous casting slab. The final continuous casting slab has a low-magnification center segregation of ≤C1.0 level, a center porosity of ≤0.5 level, and no internal defects such as middle cracks and triangular cracks. The specific continuous casting process parameters and continuous casting slab quality effects of each embodiment are shown in Table 3 below.
[0075] Table 3 Continuous casting process parameters and continuous casting billet quality effects of various embodiments
[0076]
[0077] In the fourth step, the continuous casting slab is heated in a continuous heating furnace, the temperature of the heating section is 1000°C to 1290°C, the temperature of the soaking section is controlled at 1230°C to 1270°C, the total heating time of the heating section plus the soaking section is 8min / cm billet thickness to 15min / cm billet thickness, and the core temperature of the continuous casting slab is 1210°C to 1250°C. The specific heating process parameters of each embodiment are shown in Table 4 below.
[0078] Table 4 Heating process parameters of each embodiment
[0079]
[0080] The fifth step is rolling, which is carried out on a 4300mm four-roll reversible thick plate mill, with the initial rolling being 1.2 to 1.6 times the thickness of the finished steel plate, the number of rolling passes with a single pass reduction rate of 9% to 27% being controlled at 5 to 8 passes, the widening pass being placed at the front pass after the start rolling, the initial rolling and final rolling temperatures being ≥ 990°C; the finish rolling makes the non-recrystallized austenite reach a cumulative deformation rate of 18% to 35%, the start rolling temperature is 910°C to 840°C, and the final rolling temperature is 900°C to 840°C. The rolling process parameters of each embodiment are shown in Table 5 below.
[0081] Table 5 Rolling process parameters of each embodiment
[0082]
[0083] The sixth step is to accelerate cooling, control the cooling start temperature, water volume, cooling water group, roller speed, final cooling temperature, average cooling of steel plate and other parameters. After cooling, the metallographic structure of the steel plate is martensite + bainite.
[0084] The rapid offline process is put into the slow cooling cover for slow cooling for 72 hours to 96 hours. The specific accelerated cooling process parameters of each embodiment are shown in Table 6 below.
[0085] Table 6 Accelerated cooling process parameters of various embodiments
[0086]
[0087]
[0088] The seventh step is quenching. The steel plate is heated to 760℃~830℃ again in the heating furnace, and taken out of the furnace after the core of the steel plate reaches the target temperature and is kept warm for 0.4min / mm~0.75min / mm according to the plate thickness. The surface temperature drop of the steel plate from the time of taking out of the furnace to the start of quenching is controlled within 40℃. The cooling water temperature is guaranteed to be ≤26℃ during the quenching process, and the cooling water volume reaches 9000Nm3 / h~12000Nm3 / h. If a quenching tank is used, the cooling water in the tank must be circulated and stirred to ensure that the quenching cooling rate of the core of the steel plate is ≥6℃ / s. The surface temperature of the steel plate should be ≤100℃ when the quenching water is stopped. The quenching process parameters of each embodiment are shown in Table 7 below.
[0089] Step 8: Tempering. The tempering temperature is Ac1-50~120℃, and the specific temperature for this steel is 610℃~680℃. The holding time after reaching the temperature is 1.3min / mm plate thickness~2.5min / mm plate thickness. The final steel plate structure is tempered troostite+tempered bainite+a small amount of polygonal ferrite. The tempering process parameters of each embodiment are shown in Table 7 below.
[0090] Table 7 Quenching and tempering process parameters of each embodiment
[0091]
[0092] The properties of the 550MPa grade extra thick steel plates of various embodiments of the present invention are shown in Tables 8 and 9 below:
[0093] Table 8 Tensile properties of 550MPa grade extra thick steel plate
[0094]
[0095]
[0096] Table 9 Impact toughness of 550MPa grade extra thick steel plate
[0097]
[0098] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a 550MPa grade extra thick steel plate, It is characterized in that The steel plate is smelted from the following components in mass percentage: C: 0.06% to 0.16%, Si: ≤0.35%, Mn: 1.10% to 1.70%, P≤0.012%, S≤0.002%, Cr: 0.40% to 0.80%, Cu: ≤0.50%, Ni: 0.35% to 1.00%, Als: 0.025% to 0.050%, Nb: 0.015% to 0.050%, V: 0.020% to 0.080%, Ti: 0.010%~0.025%, Mo: 0.25%~0.60%, B: 0.0001%~0.0025%, the balance is Fe and inevitable impurities; continuous casting billet material, steel plate thickness 100mm~180mm; the microstructure of the steel plate is tempered troostite + tempered bainite + a small amount of polygonal ferrite, wherein the volume percentage is 55%~31% tempered troostite + 34%~45% bainite + 11%~24% ferrite, the average ferrite grain size is 6µm~15µm, the average martensite and bainite grain length is 10µm~35µm, and the width is 10µm~25µm; the process steps of the method are: The first step, initial refining Scrap steel and molten iron are selected to ensure that the content of harmful elements in the final molten steel is ≤0.004%. KR pretreatment removes the [S] content in the molten iron to ≤0.005%. At the end of the BOF converter primary refining, the molten steel [P] is controlled to ≤0.008% to ensure that the final molten steel [P] is ≤0.012%; Step 2: Refining Including LF refining and RH vacuum treatment, after refining, the [O] content of the molten steel is guaranteed to be no more than 11ppm, the [H] content is no more than 1.0ppm, and the [S] content is no more than 0.002%; The third step is continuous steel casting The molten steel is cast into continuous casting slabs on a straight arc continuous casting machine. The slab thickness is 370mm-450mm. The continuous casting slabs are removed from the casting machine and cut into sections before being quickly hoisted into a slow cooling pit for slow cooling. After the temperature of the continuous casting slabs is cooled to ≤300℃, they are removed from the pit for rolling. Step 4: Heating The continuous casting slab is heated in a continuous heating furnace, the temperature of the heating section is 1000℃~1290℃, the temperature of the soaking section is controlled at 1230℃~1270℃, and the total heating time of the heating section plus the soaking section is 8min / cm slab thickness~15min / cm slab thickness, so that the core temperature of the continuous casting slab reaches 1210℃~1250℃; Step 5: Rolling After the continuous casting billet leaves the heating furnace, the surface oxide scale is removed by a high-pressure water descaling box, and then the initial rolling is immediately carried out. The initial rolling is 1.2 to 1.6 times the thickness of the finished steel plate. The final rolling temperature in this stage is controlled at ≥990℃. After the initial rolling, the temperature is lowered by auxiliary water spraying, and then the finishing rolling is carried out. The starting rolling temperature of the finishing rolling is 910℃ to 840℃, and the final rolling temperature is 900℃ to 840℃. Step 6: Accelerate Cooling After finishing rolling, the steel plate is water-cooled by the DQ+ACC system, and the cooling start temperature is Ar3+110~170℃. The surface temperature of the steel plate is controlled to be ≤350℃ when it leaves the water cooling system. The average cooling rate of the steel plate is 8℃ / s~21℃ / s, the core cooling rate is 4℃ / s~12℃ / s, and the final cooling temperature is controlled at Mf-40℃~100℃. After cooling, the metallographic structure of the steel plate is martensite+bainite. The steel plate is quickly offline after leaving the ACC water cooling system and enters the slow cooling cover for slow cooling for 72h~96h. Step 7: Quenching The steel plate is heated again to 760℃~830℃ in the heating furnace, and taken out of the furnace after the core of the steel plate reaches the target temperature and is kept warm for 0.4min / mm~0.75min / mm according to the plate thickness. The surface temperature drop of the steel plate is controlled within 40℃ from the time of taking out of the furnace to the start of quenching. The cooling water temperature is guaranteed to be ≤26℃ during the quenching process, and the cooling water volume reaches 9000Nm 3 / h~12000 Nm 3 / h, the surface temperature of the steel plate is ≤100℃ when the quenching water stops; Step 8: Tempering The tempering temperature Ac1-50~120℃, Ac1 is the temperature at which bainite or martensite begins to transform into austenite when heated, the holding time after reaching the temperature is 1.3min / mm plate thickness~2.5min / mm plate thickness, martensite decomposes, bainite undergoes crystal transformation, M / A islands decompose, carbides spheroidize and maintain dispersed and uniform distribution, and the final steel plate structure is tempered troostite + tempered bainite + a small amount of polygonal ferrite.
2. The method for manufacturing a 550MPa grade extra thick steel plate according to claim 1, Features: The steel plate has a yield strength (Rp0.2) ≥ 550MPa, a tensile strength (Rm) ≥ 660MPa-770MPa, and an elongation after fracture (A) ≥ 18%; high toughness, longitudinal and transverse KV2 ≥ 120J at -20°C, and longitudinal and transverse KV2 ≥ 100J at -60°C.
3. A method for manufacturing a 550MPa grade extra thick steel plate according to claim 1, Features In step three, the superheat of the molten steel is controlled during the casting process, and the width, thickness and drawing speed of the continuous casting billet are matched and controlled. When the solid phase fraction of the continuous casting billet is 0.59-0.73, light pressure is applied to the continuous casting billet, and finally the low-magnification center segregation of the continuous casting billet is ≤C1.0 and the center porosity is ≤0.
5.
4. A method for manufacturing a 550MPa grade extra thick steel plate according to claim 1, Features In step 5, the widening passes in the initial rolling stage are not recorded, and the number of rolling passes with a single-pass reduction rate of 9% to 27% is controlled at 5 to 8 passes. After the initial rolling, the core austenite grains are at level 5.0 or above; the finishing rolling is carried out in the non-recrystallized zone of austenite, so that the non-recrystallized austenite reaches a cumulative deformation rate of 18% to 35%.
5. A method for manufacturing a 550MPa grade extra thick steel plate according to claim 1, Features The total flow rate of DQ cooling water in step 6 is 5500Nm 3 / h~8000 Nm 3 / h, ACC cooling water total flow 9500 Nm 3 / h~12000 Nm 3 / h, roller running speed 0.3m / s~0.9m / s.
6. A method for manufacturing a 550MPa grade extra thick steel plate according to claim 1, Features If a quenching tank is used in step seven, the cooling water in the tank must be circulated and stirred to ensure that the quenching cooling rate of the core of the steel plate is ≥6°C / s, and the quenching is stopped after the core temperature of the steel plate is ≤210°C.
7. A method for manufacturing a 550MPa grade extra thick steel plate according to claim 1, Features The tempering temperature in step eight is 610°C to 680°C.
Citation Information
Patent Citations
130mm low-alloy low-temperature-toughness thick plate and production method thereof
CN103725959A
Hardened and tempered ultra-thick high-strength SM570 steel plate and production method thereof
CN111020384A
Large-thickness high-toughness S500QL1 steel plate and production method thereof
CN111826585A
Steel plate with thickness of larger than 60mm and yield strength of 690MPa and preparation method of steel plate
CN104278216A
Super-thick high-strength and high-toughness lamellar tearing resistant Q550 steel plate and manufacturing method thereof
CN107904488A