A modified amine chain extender, polyurethane coating and preparation method thereof
The reaction of the active cyclic carbonate with the amino chain extender to generate a modified amine chain extender, which solves the problems of short operating time and large viscosity of the amine chain extender, and realizes the low viscosity and excellent mechanical properties of the polyurethane coating, simplifying the The process and reduce costs.
Patent Information
- Application Number
- CN202211702588.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The existing amine chain extenders have short operating time, high viscosity, easy precipitation during storage and high reactivity, which limit their application and process operation difficulty in polyurethane materials.
By reacting the active cyclic carbonate compound with an amino chain extender, the amino group is converted into a hydroxyl group, and a modified amine chain extender is formed, and introduced into the polyurethane backbone, reducing viscosity and prolonging the reaction time.
The low viscosity and excellent mechanical properties of polyurethane coatings are achieved, the scope of use of amine chain extenders is expanded, the process is simplified and the cost is reduced.
Smart Images

Figure CN116217442B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of elastomer materials, and specifically relates to a modified amine chain extender, a polyurethane coating and a preparation method thereof. Background Art
[0002] Polyurethane, also known as polyurethane, is a type of polymer containing a large number of repeating units of carbamate bonds in the macromolecular chain. The repeating units are mainly obtained by the addition reaction of isocyanate groups (-NCO) and hydroxyl groups (-OH). Since Otto Bayer and others developed the isocyanate and polyol addition route in 1937, polyurethane has begun to develop with industrial practical value. After decades of development, it has become an important member of the polymer material family and has been widely used in various engineering fields, including chemical, electronics, construction, textile, automobile, medical, national defense, aerospace and other fields.
[0003] The carbamate bond is a characteristic functional group of polyurethane materials. The characteristic of this bond is that it is both a donor and an acceptor of hydrogen bonds. Under the action of hydrogen bonds, multiple carbamate bonds aggregate to form hard segment micro-regions. The existence of hard segment micro-regions makes the material macroscopically manifest in physical properties such as high strength and wear resistance. On the other hand, polyol components usually refer to oligomers with different molecular weights and hydroxyl groups at the end. Except for the hydroxyl functional group that participates in hydrogen bonds after chemical reactions, the remaining chain segments exist in a "loose" state and are called soft segments. The soft segment parts of polymer molecules are aggregated together and are called soft segment micro-regions. The existence of soft segment micro-regions makes the material macroscopically have high elasticity, high elongation and other properties. Due to the existence of soft and hard segment micro-regions, polyurethane materials integrate excellent properties such as elasticity, strength, wear resistance, and hardness.
[0004] On the other hand, due to the wide range of raw materials available, different materials with different properties can be developed through different combinations. For example, the performance of polyurethane materials can be adjusted to a large extent by selecting different isocyanates, polyols (polyethers, polyesters, etc.), catalysts, additives, or different molding and post-processing methods, such as elastomers, adhesives, plastics, etc. At present, polyurethane is the only synthetic polymer material with significant application value in seven major fields: coatings, foams, plastics, rubbers, fibers, adhesives, and functional polymers. It has become the most diverse, widely used, and fastest-growing special organic synthetic material.
[0005] Chain extender is one of the important materials in the composition of polyurethane materials, and contributes to the hard segment content in polyurethane molecules. It is also called chain extender, which is a substance that can extend the molecular chain and increase the molecular weight through functional group reaction. Chain extenders usually have the characteristics of low molecular weight, active reaction, and strong reaction competition probability for isocyanate and polyol systems. It can not only effectively adjust the reaction speed of the reaction system, adjust the process parameters such as the viscosity growth of the reactants, but also introduce certain characteristic groups in the chain extender into the polyurethane main chain through chain extension reaction, giving the polyurethane molecule certain properties.
[0006] Polyurethane chain extenders contain two or more functional groups, including diols (fatty alcohols, aromatic alcohols), diamines, alcohol amines, polyols, etc. Chain extenders are used in various types of polyurethane products, including foams, adhesives, coatings, cast polyurethanes (CPUs), thermoplastic polyurethanes (TPUs), etc. Different types or structures of chain extenders are selected according to different terminal applications or processing technologies. Among them, compared with diol chain extenders, polyurethane materials prepared using amine chain extenders have better tensile strength, tear strength, and wear resistance. This is because: 1) amino groups react with isocyanates to form urea bonds, and the hard segment / hard region formed by urea bonds has higher cohesive energy; 2) amino groups have higher reactivity with isocyanates, which reduces the probability of isocyanates reacting with water, thereby reducing the generation of defects; 3) amino groups have higher activity, which reduces the probability of side reactions and has a more efficient chain extension effect. Typical side reactions include: cross-linking of active hydrogen between isocyanates and carbamate bonds, self-polymerization of isocyanates, and other reactions. In academia and industry, different types of amine chain extenders are widely used. The most representative one is MOCA (4,4'-methylenebis(2-chloroaniline)). Because the presence of chlorine atoms adjacent to the amino group reduces the reactivity of the amino group, it has been widely used in two-component polyurethane coatings and cast elastomers. However, it is a solid, and after being dissolved in the coating system, the system viscosity is relatively high. E300 (dimethylthiotoluenediamine) and E100 (diethyltoluenediamine) are also commonly used chain extenders in the industry. They have low viscosity at room temperature but high reactivity and are usually used in spray polyurea systems.
[0007] In summary, although amino chain extenders are widely used, there are still difficulties that cannot be ignored: 1) The operation time is short; 2) Commonly used aromatic ring structure chain extenders are usually solid (crystalline), such as MOCA. Solid chain extenders need to be dissolved or melted to participate in the reaction, and the system viscosity is high. There is a risk of precipitation (crystallization) during the storage process, which poses great process operation difficulties for the manufacture of downstream terminal products; 3) Aromatic amine chain extenders are liquid at room temperature, have high reaction activity, and can usually only be used by spraying; 4) Most amine chain extenders are defined as hazardous chemicals.
[0008] Taking all the above factors into consideration, it is an urgent need of the industry to develop a new type of modified amine chain extender technology that can introduce the chain segments of amine chain extenders into the polyurethane polymer chain while bringing convenience to the production and manufacturing process. Summary of the invention
[0009] In order to solve the above problems, the present invention provides a modified amine chain extender technology, wherein the modified amine chain extender reacts an active cyclic carbonate compound with an amino chain extender to convert the more active amino group in the amino chain extender into a hydroxyl group, and the active cyclic carbonate compound reacts with the amino chain extender to generate a compound containing a carbamate bond, thereby introducing the carbamate in the modified amine chain extender into the polyurethane main chain and converting it into a part of the polyurethane molecular chain, so that the final product polyurethane coating has low viscosity and better mechanical properties.
[0010] The technical solution of the present invention is as follows:
[0011] The present invention provides a modified amine chain extender, wherein the modified amine chain extender is obtained by reacting a cyclic carbonate compound with an amino chain extender through the following reaction formula (I):
[0012]
[0013] Where R1 is C2-C n One or more molecular segments selected from alkyl (n is greater than or equal to 2), halogenated aromatic hydrocarbons or halogenated alkyl, ether bonds, ester bonds, carbonyl groups, and siloxanes;
[0014] R2 and R3 are each independently a hydrogen atom, a C1-C n Alkyl (n is greater than or equal to 1), halogenated group, unsaturated hydrocarbon group.
[0015] Furthermore, R2 and R3 are each independently any one of H, CH3, CH2-CH3, Cl, Br, I, alkenyl, and alkynyl.
[0016] Furthermore, the amino chain extender is one or more of aromatic, fatty, and silicone-based.
[0017] Furthermore, the amino chain extender is one or more of aromatic amines, fatty amines, and siloxane amines such as ethanolamine, methyldiethanolamine, 3,3'-dichloro-4,4'-diphenylmethane, 3,5-dimethylthiotoluenediamine, 4,4'-diaminodiphenylmethane, m-phenylenediamine, diethyltoluenediamine, methylcyclohexanediamine, isophoronediamine, 1,6-hexanediamine, 4,4'-diethylenedicyclohexylamine, propylenediamine, pentamethylenediamine, octanediamine, 1,3-bis(aminomethyl)cyclohexane, 1,3-bis(aminopropyl)tetramethyldisiloxane, and polyetheramine.
[0018] Furthermore, the cyclic carbonate is one or more of ethylene carbonate, fluoroethylene carbonate, vinylene carbonate, propylene carbonate, chloropropylene carbonate, butylene carbonate, cyclohexene carbonate, vinyl cyclohexene carbonate, styrene cyclic carbonate and the like.
[0019] The present invention also provides a polyurethane coating prepared by using the modified amine chain extender. The polyurethane coating comprises the following main raw materials in parts by weight:
[0020] Isocyanate: 3-17 parts by weight;
[0021] Polyol: 10-45 parts by weight;
[0022] Amino chain extender: 1-15 parts by weight;
[0023] Cyclic carbonate: 0.1-10 parts by weight
[0024] Plasticizer: 10-30 parts by weight;
[0025] Dispersant: 0.05-0.5 parts by weight;
[0026] Inorganic powder: 20-60 parts by weight;
[0027] Defoaming agent: 0-1 parts by weight;
[0028] Adhesion promoter: 0-2 parts by weight;
[0029] Catalyst: 0-0.5 parts by weight;
[0030] Solvent: 0-10 parts by weight.
[0031] Furthermore, the polyol is a polyether polyol having a molecular weight of 2000 to 5000.
[0032] Furthermore, the amino chain extender is an aromatic amine, such as aromatic amine MOCA.
[0033] Furthermore, the plasticizer is one or more of phthalates and chlorinated paraffins, for example, one or two of diisononyl phthalate (DINP) and No. 52 chlorinated paraffin.
[0034] Furthermore, the dispersant is a polycarboxylic acid, such as an alkylammonium salt solution of a polycarboxylic acid BYK-AT203.
[0035] Furthermore, the inorganic powder is one or more of organic bentonite, calcium carbonate, talc and the like.
[0036] Furthermore, the pigment is iron brown.
[0037] Furthermore, the defoamer is a polysiloxane oily defoamer, such as BYK065.
[0038] Furthermore, the adhesion promoter is one or more siloxane oligomers, such as siloxane oligomer silok-6654.
[0039] Furthermore, the catalyst is an organotin catalyst, such as organotin T-12.
[0040] Furthermore, the solvent is No. 150 solvent oil.
[0041] The present invention also provides a method for preparing the aforementioned polyurethane coating, the method comprising:
[0042] Step S1: Preparation of component A
[0043] Add polyether polyol to the reactor, open the vacuum environment in the reactor, stir and heat to 110-120°C, and keep the temperature at this temperature for 2-3 hours; then cool to 65-70°C, add stoichiometric isocyanate under high-speed stirring, react for 0.5 hours, heat to 80-85°C, continue to react at this temperature for 3-4 hours, then cool to below 50°C, vacuum degas for 0.5-1 hour, discharge, and obtain isocyanate prepolymer for standby use;
[0044] Step S2: Preparation of component B
[0045] S2-1: Add amino chain extender, cyclic carbonate, polyol, plasticizer and dispersant into the reactor and start mechanical stirring until uniform. This process is to dehydrate the raw materials and synthesize the modified amine chain extender in situ at the same time;
[0046] S2-2: gradually raise the temperature of the reactor to 90-100°C, add pigment, calcium carbonate, talcum powder and other inorganic powders, and stir mechanically;
[0047] S2-3: Turn on the vacuum to at least -0.095MPa, and continue to heat the reactor to 110-120°C. After reaching the set temperature, a dehydration reaction occurs for 2-3h. This process is for dehydration of raw materials and in-situ synthesis of modified amine chain extenders;
[0048] S2-4: After the dehydration is completed, the temperature of the reactor is lowered to 50-55°C, and the catalyst, defoamer, adhesion promoter, and solvent are added under stirring conditions, and stirred for 1-2 hours; then the temperature is lowered to below 50°C, and the material is discharged after degassing for 30 minutes to 1 hour under a vacuum degree of -0.095MPa for standby use;
[0049] Step S3: Polyurethane coating preparation
[0050] Component A and component B are mixed in a weight ratio of A:B=1:(0.5-4).
[0051] Furthermore, in step S1, the isocyanate prepolymer is obtained by polyaddition reaction of isocyanate and polyether polyol, wherein the R value of the polyether polyol is 1.9-2.1.
[0052] Furthermore, in step S2-1, the mechanical stirring rate is 300 rpm.
[0053] The present invention also provides a method for preparing the aforementioned polyurethane coating, the method comprising:
[0054] Step T1: Dehydration of raw materials, including in-situ synthesis of modified amine chain extenders
[0055] T1-1: Add amino chain extender, cyclic carbonate, polyol, plasticizer and dispersant into the reactor and start mechanical stirring until uniform;
[0056] T1-2: Gradually heat the reactor to 90-100°C, add pigments, calcium carbonate, talcum powder and other inorganic powders, and stir evenly;
[0057] T1-3: Turn on the vacuum to at least -0.095 MPa, and continue to heat the reactor to 110-120°C. After reaching the set temperature, the dehydration reaction occurs for 2-3 hours, which is marked as mixture M;
[0058] Step T2: Polyurethane coating preparation
[0059] The obtained mixture M is cooled to 65-70°C, and then a stoichiometric amount of isocyanate is added. After reacting for 0.5h, the temperature is raised to 80-85°C. After reaching the set temperature, the reaction is continued for more than 3h, and then the temperature is lowered to 50-55°C. A defoamer, an adhesion promoter, a catalyst, a solvent and other additives are added. After stirring evenly, the mixture is vacuum degassed for 0.5h and discharged.
[0060] Furthermore, in step T1-1, the rate of mechanical stirring is 300 rpm.
[0061] Furthermore, in step T1-2, the mechanical stirring rate is 500 rpm.
[0062] The present invention has the following beneficial effects:
[0063] 1. The present invention synthesizes a novel modified amine chain extender. The modified amine chain extender is a compound that converts the more active amino group in the amino chain extender into a hydroxyl group by reacting an active cyclic carbonate compound with an amino chain extender. On the one hand, the active cyclic carbonate compound reacts with the amino chain extender to generate a compound with a carbamate bond, and after further reaction, the compound is introduced into the polyurethane main chain and converted into a part of the polyurethane molecular chain, i.e., a resin. On the other hand, the modified amine chain extender obtained after the easily crystallized amino chain extender reacts with the cyclic carbonate is a liquefied product, which reduces the viscosity of the polyurethane reaction system and prolongs the operation time of the reaction with isocyanate. In summary, the use of amino chain extender synthesis and modification technology not only reduces the amount of resin added (cyclic carbonate becomes a resin segment fixed on the molecular chain), but also expands the scope of use of the amino chain extender.
[0064] 2. The present invention aims to solve the problems that the amino chain extender has high reaction activity and short operation time, and some solid amino chain extenders are difficult to dissolve in the system and are easy to precipitate during storage. The present invention adopts a cyclic carbonate compound as a reactant and utilizes the ring-opening reaction mechanism between the cyclic carbonate compound and the amino group in the amino chain extender / amino compound to prepare a modified chain extender / oligomer containing a carbamate bond. Although the amino group of the amino chain extender is not converted into a urea bond with isocyanate, one amino group is first converted into a carbamate bond, and the hydroxyl group generated after the ring opening further reacts with isocyanate to form a carbamate bond, that is, one amino group is finally converted into two carbamate bonds. Compared with the amino group directly reacting with isocyanate to form a urea bond, the polyurethane polymer generated by this technical route has a larger molecular weight and a higher hard segment content.
[0065] 3. The modification method of the chain extender / amino compound of the present invention has the outstanding advantages of simple process, easy implementation, low cost, etc., and the product has low viscosity and better performance, and is particularly suitable for the preparation of materials in the fields of coatings, elastomers, adhesives, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 This is the Fourier transform infrared (FI-IR) spectrum of the modified amine chain extender.
[0067] The amine chain extender is a modified amine chain extender product obtained by reacting MOCA with propylene carbonate (PC) at 110°C for 7-10 hours under a nitrogen atmosphere. A sample of the modified amine chain extender product is evenly spread on the transmission panel glass, pressed with a rotating upper arm, and scanned. The scanning range is set to 4000-400cm -1 , the number of scans is 32 times, the resolution is 4cm -1 .
[0068] The names of the labels in the figure are as follows:
[0069] 1. Propylene carbonate; 2. Modified amine chain extender product; 3. MOCA. DETAILED DESCRIPTION
[0070] The invention is described in detail below with reference to the embodiments, but the invention is not limited thereto.
[0071] The experimental methods described in the following examples are conventional methods unless otherwise specified.
[0072] The reagents and materials are well-known materials and can be prepared by those skilled in the art or obtained from commercial sources.
[0073] The polyether polyol, isocyanate and cyclic carbonate used in the examples were provided by Wanhua Chemical; MOCA (4,4'-methylenebis(2-chloroaniline)) was provided by Jiangsu Xiangyuan; E300 was provided by Zhangjiagang Yarui Chemical Co., Ltd.; calcium carbonate, talc and the like were provided by Jiangxi Guangyuan.
[0074] In order to more clearly and intuitively illustrate the characteristics of the modification technology route, the following examples and comparative examples all use the same formulation system, and the mass ratio of component A to component B is 1:1.
[0075] Embodiment 1:
[0076] A polyurethane coating comprises the following raw materials in parts by weight:
[0077] Calculated by weight of component A, component A includes:
[0078] Isocyanate (MDI): 27.5 parts by weight
[0079] Polyether diol (molecular weight 2000): 63.5 parts by weight
[0080] Polyether triol (molecular weight 5000): 9 parts by weight:
[0081] Calculated by weight of component B, component B includes:
[0082] Polyether polyol (molecular weight 5000): 5 parts by weight;
[0083] MOCA chain extender: 13.8 parts by weight;
[0084] Propylene carbonate: 5.3 parts by weight;
[0085] Diisononyl phthalate plasticizer: 8.4 parts by weight;
[0086] BYK-AT203 dispersant: 0.5 parts by weight;
[0087] No. 52 chlorinated paraffin: 24.3 parts by weight;
[0088] Inorganic powder: including 1 part iron brown, 33 parts calcium carbonate, 6.5 parts talc;
[0089] BYK065 defoamer: 0.3 parts by weight;
[0090] Adhesion promoter Silok-6654: 0.1 parts by weight;
[0091] T-12 catalyst: 0.05 parts by weight;
[0092] No. 150 solvent oil: 2 parts by weight;
[0093] The preparation method is as follows:
[0094] Preparation of component A: Add 63.5 parts of polyether diol (molecular weight 2000) and 9 parts of polyether triol (molecular weight 5000) into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under vacuum degree -0.095MPa. Cool down to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h. Cool down to below 50°C, degas for 0.5h under vacuum degree -0.095MPa, and discharge for standby use.
[0095] Preparation of component B: Add 5 parts of polyether triol (molecular weight 5000), 5.3 parts of propylene carbonate (PC), 8.4 parts of diisononyl phthalate (DINP), 24.3 parts of 52 chlorinated paraffin, 0.5 parts of dispersant BYK-AT203 to a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talcum powder, 13.8 parts of MOCA. After stirring evenly, heat to 110-115°C, open the vacuum to -0.095MPa at the same time, and dehydrate for 2-3h. Lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of defoamer BYK065, 0.1 parts of adhesion promoter Silok-6654, 2 parts of 150 solvent oil under high-speed stirring, and stir for 1.5h. Cool down to below 50°C, degas for 0.5h under vacuum degree of -0.095MPa, then discharge the material for later use.
[0096] Coating preparation: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
[0097] Embodiment 2:
[0098] A polyurethane coating comprises the following raw materials in parts by weight:
[0099] Calculated by weight of component A, component A includes:
[0100] Isocyanate (MDI): 27.5 parts by weight
[0101] Polyether diol (molecular weight 2000): 63.5 parts by weight
[0102] Polyether triol (molecular weight 5000): 9 parts by weight:
[0103] Calculated by weight of component B, component B includes:
[0104] Polyether triol (molecular weight 5000): 5 parts by weight;
[0105] MOCA chain extender: 13.8 parts by weight;
[0106] Propylene carbonate: 2.7 parts by weight;
[0107] Diisononyl phthalate plasticizer: 8.4 parts by weight;
[0108] BYK-AT203 dispersant: 0.5 parts by weight;
[0109] No. 52 chlorinated paraffin: 26.9 parts by weight;
[0110] Inorganic powder: including 1 part iron brown, 33 parts calcium carbonate, 6.5 parts talc;
[0111] BYK065 defoamer: 0.3 parts by weight;
[0112] Adhesion promoter Silok-6654: 0.1 parts by weight;
[0113] T-12 catalyst: 0.05 parts by weight;
[0114] No. 150 solvent oil: 2 parts by weight;
[0115] The preparation method is as follows:
[0116] Preparation of component A: Add 63.5 parts of polyether diol (molecular weight 2000) and 9 parts of polyether triol (molecular weight 5000) into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under vacuum degree -0.095MPa. Cool down to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h. Cool down to below 50°C, degas for 0.5h under vacuum degree -0.095MPa, and discharge for standby use.
[0117] Preparation of component B: Add 5 parts of polyether triol (molecular weight 5000), 2.7 parts of propylene carbonate (PC), 8.4 parts of diisononyl phthalate (DINP), 26.9 parts of 52 chlorinated paraffin, 0.5 parts of dispersant BYK-AT203 to a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talcum powder, 13.8 parts of MOCA. After stirring evenly, heat to 110-115°C, open the vacuum to -0.095MPa at the same time, and dehydrate for 2-3h. Lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of defoamer BYK065, 0.1 parts of adhesion promoter Silok-6654, 2 parts of 150 solvent oil under high-speed stirring, and stir for 1.5h. Cool down to below 50°C, degas for 0.5h under vacuum degree of -0.095MPa, then discharge the material for later use.
[0118] Coating preparation: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
[0119] Embodiment 3:
[0120] A polyurethane coating comprises the following raw materials in parts by weight:
[0121] Calculated by weight of component A, component A includes:
[0122] Isocyanate (MDI): 27.5 parts by weight
[0123] Polyether diol (molecular weight 2000): 63.5 parts by weight
[0124] Polyether triol (molecular weight 5000): 9 parts by weight:
[0125] Calculated by weight of component B, component B includes:
[0126] Polyether triol (molecular weight 5000): 7.2 parts by weight;
[0127] E00 chain extender: 7.5 parts by weight;
[0128] Propylene carbonate: 3.5 parts by weight;
[0129] Diisononyl phthalate plasticizer: 8.4 parts by weight;
[0130] BYK-AT203 dispersant: 0.5 parts by weight;
[0131] No. 52 chlorinated paraffin: 26.9 parts by weight;
[0132] Inorganic powder: including 1 part iron brown, 33 parts calcium carbonate, 6.5 parts talc;
[0133] BYK065 defoamer: 0.3 parts by weight;
[0134] Adhesion promoter Silok-6654: 0.1 parts by weight;
[0135] T-12 catalyst: 0.05 parts by weight;
[0136] No. 150 solvent oil: 2 parts by weight;
[0137] The preparation method is as follows:
[0138] Preparation of component A: Add 63.5 parts of polyether diol (molecular weight 2000) and 9 parts of polyether triol (molecular weight 5000) into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under vacuum degree -0.095MPa. Cool down to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h. Cool down to below 50°C, degas for 0.5h under vacuum degree -0.095MPa, and discharge for standby use.
[0139] Preparation of component B: Add 7.2 parts of polyether triol (molecular weight 5000), 3.5 parts of propylene carbonate (PC), 9 parts of diisononyl phthalate (DINP), 29.6 parts of 52-chlorinated paraffin, 0.5 parts of dispersant BYK-AT203 to a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talcum powder, 7.5 parts of E300. After stirring evenly, heat to 110-115°C, open the vacuum to -0.095MPa at the same time, and dehydrate for 2-3h. Lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of defoamer BYK065, 0.1 parts of adhesion promoter Silok-6654, 2 parts of 150 solvent oil under high-speed stirring, and stir for 1.5h. Cool down to below 50°C, degas for 0.5h under vacuum degree of -0.095MPa, then discharge the material for later use.
[0140] Coating preparation: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
[0141] Comparative Example 1:
[0142] Preparation of component A: Add 63.5 parts of polyether diol (molecular weight 2000) and 9 parts of polyether triol (molecular weight 5000) into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under vacuum degree -0.095MPa. Cool down to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h. Cool down to below 50°C, degas for 0.5h under vacuum degree -0.095MPa, and discharge for standby use.
[0143] Preparation of component B: Add 5 parts of polyether triol (molecular weight 5000), 9 parts of diisononyl phthalate (DINP), 29 parts of 52 chlorinated paraffin, 0.5 parts of dispersant BYK-AT203 to a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talcum powder, and 13.8 parts of MOCA. After stirring evenly, heat to 110-115°C, turn on the vacuum to -0.095MPa, and dehydrate for 2-3h. Lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of defoamer BYK065, 0.1 parts of adhesion promoter Silok-6654, and 2 parts of 150 solvent oil under high-speed stirring, and stir for 1.5h. Cool down to below 50°C, degas for 0.5h under vacuum degree of -0.095MPa, and then discharge for standby use.
[0144] Coating preparation: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
[0145] Comparative Example 2:
[0146] Preparation of component A: Add 63.5 parts of polyether diol (molecular weight 2000) and 9 parts of polyether triol (molecular weight 5000) into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under vacuum degree -0.095MPa. Cool down to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h. Cool down to below 50°C, degas for 0.5h under vacuum degree -0.095MPa, and discharge for standby use.
[0147] Preparation of component B: Add 7.2 parts of polyether triol (molecular weight 5000), 9 parts of diisononyl phthalate (DINP), 33 parts of 52 chlorinated paraffin, 0.5 parts of dispersant BYK-AT203 into a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talcum powder, 7.5 parts of E300. After stirring evenly, heat to 110-115°C, open the vacuum to -0.095MPa at the same time, and dehydrate for 2-3h. Lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of defoamer BYK065, 0.1 parts of adhesion promoter Silok-6654, 2 parts of 150 solvent oil under high-speed stirring, and stir for 1.5h. Cool down to below 50°C, degas for 0.5h under vacuum degree of -0.095MPa, then discharge the material for later use.
[0148] Coating preparation: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
[0149] Table 1 Performance test results of polyurethane coatings of Examples 1-3 and Comparative Examples 1-3
[0150]
[0151] In Table 1, by comparing Comparative Example 1, Example 1, and Example 2, it is found that the viscosity of component B is significantly reduced by the modification of solid MOCA by PC, and the elongation at break of polyurethane is significantly increased after the reaction of MOCA and PC, indicating that the molecular weight of the polyurethane molecular chain becomes larger. It is further found through Comparative Example 2 and Example 3 that the modification of liquid E300 by PC does not increase the viscosity of component B, but the elongation at break is significantly increased. It can be found from Examples 1-3 that no matter whether PC is modified on MOCA or E300, the physical and mechanical properties of the waterproof coating can still meet the requirements of polyurethane waterproof coating directly used for waterproof layer in TB / T2965-2018.
[0152] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. A polyurethane coating, characterized in that: The invention comprises the following raw materials in parts by weight: Calculated by weight of component A, component A includes: Isocyanate MDI: 27.5 parts by weight; Polyether diol with a molecular weight of 2000: 63.5 parts by weight; Polyether triol with a molecular weight of 5000: 9 parts by weight; Calculated by weight of component B, component B includes: Polyether triol with a molecular weight of 5000: 5 parts by weight; MOCA chain extender: 13.8 parts by weight; Propylene carbonate: 5.3 parts by weight; Diisononyl phthalate plasticizer: 8.4 parts by weight; BYK-AT203 dispersant: 0.5 parts by weight; No. 52 chlorinated paraffin: 24.3 parts by weight; Inorganic powder: including 1 part iron brown, 33 parts calcium carbonate, 6.5 parts talc; BYK065 defoamer: 0.3 parts by weight; Adhesion promoter Silok-6654: 0.1 parts by weight; T-12 catalyst: 0.05 parts by weight; No. 150 solvent oil: 2 parts by weight; The preparation method is as follows: Preparation of component A: add 63.5 parts of polyether diol with a molecular weight of 2000 and 9 parts of polyether triol with a molecular weight of 5000 into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under a vacuum degree of -0.095MPa, cool to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h; cool to below 50°C, degas for 0.5h under a vacuum degree of -0.095MPa, and discharge for standby use; Preparation of component B: Add 5 parts of polyether triol with a molecular weight of 5000, 5.3 parts of propylene carbonate, 8.4 parts of diisononyl phthalate plasticizer, 24.3 parts of No. 52 chlorinated paraffin, and 0.5 parts of BYK-AT203 dispersant into a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talc, and 13.8 parts of MOCA; after stirring evenly, heat to 110-115°C and Open the vacuum to -0.095MPa and dehydrate for 2-3h; lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of BYK065 defoamer, 0.1 parts of adhesion promoter Silok-6654, and 2 parts of No. 150 solvent oil under high-speed stirring, and stir for 1.5h; lower the temperature to below 50°C, degas for 0.5h under the condition of vacuum degree of -0.095MPa, and then discharge the material for standby use; Preparation of polyurethane coating: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
2. A polyurethane coating, characterized in that: The invention comprises the following raw materials in parts by weight: Calculated by weight of component A, component A includes: Isocyanate MDI: 27.5 parts by weight; Polyether diol with a molecular weight of 2000: 63.5 parts by weight; Polyether triol with a molecular weight of 5000: 9 parts by weight; Calculated by weight of component B, component B includes: Polyether triol with a molecular weight of 5000: 5 parts by weight; MOCA chain extender: 13.8 parts by weight; Propylene carbonate: 2.7 parts by weight; Diisononyl phthalate plasticizer: 8.4 parts by weight; BYK-AT203 dispersant: 0.5 parts by weight; No. 52 chlorinated paraffin: 26.9 parts by weight; Inorganic powder: including 1 part iron brown, 33 parts calcium carbonate, 6.5 parts talc; BYK065 defoamer: 0.3 parts by weight; Adhesion promoter Silok-6654: 0.1 parts by weight; T-12 catalyst: 0.05 parts by weight; No. 150 solvent oil: 2 parts by weight; The preparation method is as follows: Preparation of component A: add 63.5 parts of polyether diol with a molecular weight of 2000 and 9 parts of polyether triol with a molecular weight of 5000 into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under a vacuum degree of -0.095MPa, cool to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h; cool to below 50°C, degas for 0.5h under a vacuum degree of -0.095MPa, and discharge for standby use; Preparation of component B: Add 5 parts of polyether triol with a molecular weight of 5000, 2.7 parts of propylene carbonate, 8.4 parts of diisononyl phthalate plasticizer, 26.9 parts of No. 52 chlorinated paraffin, and 0.5 parts of BYK-AT203 dispersant into a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talc, and 13.8 parts of MOCA; after stirring evenly, heat to 110-115°C and Open the vacuum to -0.095MPa and dehydrate for 2-3h; lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of BYK065 defoamer, 0.1 parts of adhesion promoter Silok-6654, and 2 parts of No. 150 solvent oil under high-speed stirring, and stir for 1.5h; lower the temperature to below 50°C, degas for 0.5h under the condition of vacuum degree of -0.095MPa, and then discharge the material for standby use; Preparation of polyurethane coating: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.
3. A polyurethane coating, characterized in that: The invention comprises the following raw materials in parts by weight: Calculated by weight of component A, component A includes: Isocyanate MDI: 27.5 parts by weight; Polyether diol with a molecular weight of 2000: 63.5 parts by weight; Polyether triol with a molecular weight of 5000: 9 parts by weight; Calculated by weight of component B, component B includes: Polyether triol with a molecular weight of 5000: 7.2 parts by weight; E300 chain extender: 7.5 parts by weight; Propylene carbonate: 3.5 parts by weight; Diisononyl phthalate plasticizer: 8.4 parts by weight; BYK-AT203 dispersant: 0.5 parts by weight; No. 52 chlorinated paraffin: 26.9 parts by weight; Inorganic powder: including 1 part iron brown, 33 parts calcium carbonate, 6.5 parts talc; BYK065 defoamer: 0.3 parts by weight; Adhesion promoter Silok-6654: 0.1 parts by weight; T-12 catalyst: 0.05 parts by weight; No. 150 solvent oil: 2 parts by weight; The preparation method is as follows: Preparation of component A: add 63.5 parts of polyether diol with a molecular weight of 2000 and 9 parts of polyether triol with a molecular weight of 5000 into a four-necked flask, stir and heat to 110°C, dehydrate for 2-3 hours under a vacuum degree of -0.095MPa, cool to 65°C, add 27.5 parts of isocyanate MDI under high-speed stirring, react for 0.5h, then heat to 85°C and continue to react for 3h; cool to below 50°C, degas for 0.5h under a vacuum degree of -0.095MPa, and discharge for standby use; Preparation of component B: Add 7.2 parts of polyether triol with a molecular weight of 5000, 3.5 parts of propylene carbonate, 9 parts of diisononyl phthalate plasticizer, 26.9 parts of No. 52 chlorinated paraffin, and 0.5 parts of BYK-AT203 dispersant into a four-necked flask, stir and heat to 90°C, add 1 part of iron brown, 33 parts of calcium carbonate, 6.5 parts of talc, and 7.5 parts of E300; after stirring evenly, heat to 110-115°C and Open the vacuum to -0.095MPa and dehydrate for 2-3h; lower the temperature to below 55°C, add 0.05 parts of catalyst T-12, 0.3 parts of BYK065 defoamer, 0.1 parts of adhesion promoter Silok-6654, and 2 parts of No. 150 solvent oil under high-speed stirring, and stir for 1.5h; lower the temperature to below 50°C, degas for 0.5h under the condition of vacuum degree of -0.095MPa, and then discharge the material for standby use; Preparation of polyurethane coating: Stir component B evenly before mixing, and mix component A and component B accurately according to the weight ratio required by the product, stir for 3-4 minutes to obtain a uniformly mixed coating, prepare samples, and cure for 7 days under standard conditions and test.