A lead-poisoning resistant flat-plate denitrification catalyst and preparation method thereof
By modifying mineral materials with organic acids and preparing composite carriers, combined with active components and acidic additives, the problem of deactivation of denitrification catalysts under lead poisoning is solved, and efficient lead-resistant performance and stability are achieved.
Patent Information
- Application Number
- CN202310068733.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-06
AI Technical Summary
Existing denitrification catalysts are deactivated under lead poisoning, resulting in reduced catalyst activity and pore clogging, and lack effective anti-lead poisoning performance.
By modifying mineral materials such as apatite, wollastonite and dolomite with organic acids, a composite carrier is prepared and mixed with TiO2, and active components and acidic additives are added to form a plate-type denitration catalyst that is resistant to lead poisoning and enhance the adsorption capacity of the catalyst. and acidic active sites to improve lead resistance.
It significantly improves the catalyst's resistance to lead poisoning, maintains high denitrification activity and a wide temperature window, and enhances the catalyst's stability and physical and mechanical properties.
Smart Images

Figure GDA0004926190110000101 
Figure GDA0004926190110000111 
Figure GDA0004926190110000112
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of selective catalytic reduction catalysts, and in particular to a lead-poisoning resistant flat plate denitration catalyst and a preparation method thereof. Background Art
[0002] Large-scale emissions of nitrogen oxides will cause problems such as ozone layer depletion, acid rain, and photochemical pollution. The current main denitrification technology is selective catalytic reduction (SCR), among which the denitrification catalyst is the core of this technology.
[0003] Lead, as a heavy metal element, has a high content in most types of coal in my country, and is also rich in flue gas from municipal waste incineration power plants. Most of the lead is released during the fuel combustion process, and then carried by the flue gas and deposited on the surface of the denitrification catalyst, causing the catalyst to be poisoned and deactivated.
[0004] Studies have shown that the mechanism of lead poisoning denitrification catalysts is mainly that Pb-like substances will cover the active sites on the catalyst surface, resulting in a decrease in chemically adsorbed oxygen, which in turn reduces the relative concentration of high-valent vanadium and the acidity of the catalyst surface. The reduction in catalyst reducibility is the main poisoning factor. In addition, PbMoO4 generated by the reaction of Pb and MoO3 will agglomerate on the catalyst surface, covering the acidic sites while blocking the catalyst pores, which in turn leads to catalyst deactivation.
[0005] At present, there are relatively few studies on denitrification catalysts that are resistant to lead poisoning. For example, a Chinese invention patent with application number CN200910114068.1 discloses a catalytic purification method for CO, NO x The rare metal catalyst for HC is a rare transition metal catalyst made of aluminum oxide, cerium oxide, zirconium oxide, lanthanum oxide, yttrium oxide and titanium oxide. It has high activity, good thermal stability, anti-aging, long service life, and is especially resistant to lead poisoning. However, the catalyst has the disadvantages of poor applicability and poor lead resistance.
[0006] In view of this, developing a denitrification catalyst resistant to lead poisoning is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a lead-poisoning resistant flat-plate denitrification catalyst, which has excellent lead-poisoning resistance and has the advantages of high denitrification activity, wide temperature window, high N2 selectivity, etc.
[0008] The present invention provides a method for preparing a lead-poisoning resistant flat-plate denitration catalyst, comprising the following steps:
[0009] S1. Modifying the mineral material using an organic acid to obtain a modified mineral material;
[0010] S2, mixing TiO2 with modified mineral materials to obtain a composite carrier;
[0011] S3, adding active component precursor, auxiliary agent precursor, impregnating agent, glass fiber and water to the composite carrier in sequence, and kneading to obtain a catalyst paste;
[0012] S4, coating the catalyst paste on a stainless steel mesh, and obtaining a lead-poisoning-resistant flat-plate denitrification catalyst after drying and calcining;
[0013] Wherein, the mineral material includes any one or more of apatite, wollastonite and dolomite.
[0014] In the preparation of the lead-poisoning resistant denitrification catalyst of the present invention, first, apatite, wollastonite and dolomite and other mineral materials are modified with organic acids to obtain modified mineral materials with large specific surface area, developed pore structure and stable structure, and the modified mineral materials have high adsorption capacity, ion exchange capacity and immobilization capacity, which improve the adsorption capacity of the catalyst for lead heavy metal elements and reduce its mobility and poisoning effect on the denitrification catalyst; then, the modified mineral material is mixed with a TiO2 carrier to prepare a composite carrier, which significantly increases the specific surface area of the carrier, improves the dispersion of active components and additives on the carrier surface, thereby presenting more oxygen vacancies, so that the denitrification catalyst achieves higher denitrification activity and N2 selectivity, and exhibits more superior catalytic activity; finally, active components and acidic additives are introduced into the composite carrier to increase the acidic active sites on the catalyst surface, enhance the oxidation capacity of the active components, improve the activity of the catalyst, and at the same time increase the ability of the catalyst to capture lead heavy metal elements in situ, thereby inhibiting the reduction effect of lead on chemical oxygen demand, and then improving the lead resistance of the catalyst.
[0015] As a preferred embodiment of the present technical solution, in step S1, during the modification, the mineral material is placed in an organic acid solution and stirred in a water bath at 60-120°C for 1-5 hours to fully improve the acidification effect of the organic acid on the mineral material. When the organic acid treats the mineral material, it can precipitate cations through proton exchange or polarization to activate the mineral material, and can also change the lattice and chemical bonds, ultimately improving the adsorption and immobilization capacity of the mineral material. After filtering, washing, and drying, calcination is performed in an O2 / N2 atmosphere to obtain a modified mineral material mainly composed of CaO;
[0016] The present invention does not strictly limit the specific conditions of drying and calcining. Specifically, during the drying, preferably, the temperature is controlled to be 60-100°C and the time is 3-5h; during the calcining, preferably, the temperature is controlled to be 600-800°C and the time is 3-6h;
[0017] In addition, during the calcination process, the preferred atmosphere is an O2 / N2 atmosphere with a volume fraction and a volume ratio of O2 to N2 of (0.5-5):(99.5-95), because this atmosphere will promote the stability of the structure of the modified mineral material during the calcination process.
[0018] As a preferred embodiment of the present technical solution, the organic acid used in the present invention is preferably any one or more of oxalic acid, citric acid and aminosulfonic acid, and the concentration of the organic acid is 0.5-5 mol / L. When used, the mineral material and the organic acid can be impregnated and modified according to a solid-liquid ratio of 1: (5-15).
[0019] As a preferred embodiment of the present technical solution, the composite carrier used in the present invention still uses TiO2 as the main carrier component, and the mass ratio of TiO2 to the modified mineral material is (1-9):1, wherein the TiO2 is anatase TiO2.
[0020] As a preferred embodiment of the present technical solution, the present invention does not strictly limit the specific types of active components, and oxides such as vanadium, molybdenum, tungsten, cerium, and erbium can be selected. Based on the consideration of composition and denitrification activity, the active components of the present invention include V2O5 and MoO3, wherein the mass fraction of V2O5 in the denitrification catalyst is 0.5-3%, and the mass fraction of MoO3 is 2-6%.
[0021] As a preferred embodiment of the present technical solution, the auxiliary agent includes any one or more of Cr2O3, Nb2O5, Sb2O3 and SnO2, and the auxiliary agent precursor used is any one or more of chromium nitrate, niobium oxalate, antimony acetate and tin tetrachloride, and the mass fraction of the auxiliary agent in the denitration catalyst is 0.5-5%. The addition of the acidic auxiliary agent can increase the acidity of the catalyst, thereby increasing the acidic active sites on the surface of the catalyst, and the increase in the acidic active sites, on the one hand, enhances the oxidation ability of the active components, which helps to improve the catalytic activity, and on the other hand, increases the ability of the catalyst to capture lead heavy metal elements in situ, inhibits the effect of lead on reducing the chemical oxygen demand, and then improves the lead resistance of the catalyst.
[0022] In addition, during the preparation of the denitration catalyst, wetting agents, glass fibers, surfactants and pore-forming agents are also added. The present invention does not strictly limit the specific composition of the wetting agent, surfactant, binder and pore-forming agent, and the wetting agents, surfactants, binders and pore-forming agents commonly used in traditional commercial denitration catalysts can be selected.
[0023] As a preferred embodiment of the present technical solution, the impregnating agent includes any one or more of hydroxypropyl methylcellulose, carboxymethyl cellulose, hydroxypropyl cellulose and methyl cellulose, and the mass ratio of the impregnating agent to the composite carrier is (1-5): 100. The mass ratio of the glass fiber to the composite carrier is (1-5): 100. After all the substances are added, the mixture is kneaded for 1-4 hours to form a uniform catalyst paste, and then the catalyst paste is coated on a stainless steel mesh using a roller.
[0024] As a preferred embodiment of the present technical solution, in step S4, during the drying, the temperature is controlled to be 60-100°C and the time is 5-12h; during the calcination, the temperature is controlled to be 450-550°C and the time is 2-5h.
[0025] In the second aspect, the present invention further discloses a lead-poisoning resistant flat-plate denitrification catalyst prepared by the above-mentioned preparation method, which should also fall within the protection scope of the present invention.
[0026] Compared with the prior art, the lead-poisoning-resistant flat-plate denitration catalyst of the present invention has at least the following technical effects:
[0027] 1. The present invention uses organic acid to modify mineral materials such as apatite, wollastonite and dolomite, and can obtain modified mineral materials with large specific surface area, developed pore structure and stable structure. The modified mineral materials have high adsorption capacity, ion exchange capacity and immobilization capacity, which can not only adjust the carrier binding interface and increase the composite carrier binding force, but also effectively absorb and stabilize the lead heavy metal elements in the flue gas, reduce its mobility and the poisoning effect of the denitrification catalyst, and at the same time, lead can form stable compounds with the elements released by the modified mineral materials, which can also achieve the purpose of stabilizing them;
[0028] 2. The composite carrier used in the present invention is a mixture of TiO2 and modified mineral materials, which can significantly increase the specific surface area of the carrier, improve the dispersion of active components and additives on the carrier surface, thereby presenting more oxygen vacancies, so that the denitration catalyst can achieve higher denitration activity and N2 selectivity, and show more superior catalytic activity; at the same time, the use of the composite carrier also further improves the hydrophobicity, wear resistance, adhesion strength and other physical and mechanical properties of the catalyst;
[0029] 3. The present invention introduces chromium, niobium, antimony and tin as modifying elements, which increase the acidic active sites on the catalyst surface. On the one hand, it enhances the oxidation ability of the active components, which helps to improve the catalytic activity. On the other hand, it increases the ability of the catalyst to capture lead heavy metal elements in situ, inhibits the effect of lead on reducing chemical oxygen demand, and then improves the lead resistance of the catalyst. In addition, the addition of transition metals promotes the expansion of the temperature window, which can make the catalyst show a wide temperature window. DETAILED DESCRIPTION
[0030] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0031] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] S11, firstly weighing apatite and immersing it in a 1 mol / L oxalic acid solution at a solid-liquid ratio of 1:10, stirring it in a water bath at 60°C for 5 hours, filtering and washing it, drying it at 100°C for 3 hours, and then calcining it at 800°C for 3 hours in an atmosphere containing 2 vol% O2 / N2, and grinding it to obtain a modified mineral material;
[0035] S12, mixing TiO2 and modified mineral materials in a mixing tank at a mass ratio of 9:1 to obtain a composite carrier;
[0036] S13, adding ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, chromium nitrate aqueous solution, hydroxypropyl methylcellulose, glass fiber and water to the composite carrier in sequence, and kneading for 4 hours to obtain a catalyst paste;
[0037] S14, using a roller to apply the catalyst paste on a stainless steel mesh, drying at 100° C. for 5 h, and calcining at 450° C. for 2 h to obtain a lead-poisoning resistant flat-plate denitration catalyst;
[0038] The mass fraction of V2O5 in the obtained denitration catalyst is 1%, the mass fraction of MoO3 is 2.7%, and the mass fraction of Cr2O3 is 1%.
[0039] Example 2
[0040] S21, first weighing wollastonite and immersing it in a 2 mol / L citric acid solution at a solid-liquid ratio of 1:10, stirring it in a water bath at 80°C for 4 hours, filtering and washing it, drying it at 90°C for 3 hours, and then calcining it at 700°C for 4 hours in an atmosphere containing 3 vol% O2 / N2, and grinding it to obtain a modified mineral material;
[0041] S22, mixing TiO2 and modified mineral materials in a mixing tank at a mass ratio of 8:2 to obtain a composite carrier;
[0042] S23, adding ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, niobium oxalate aqueous solution, hydroxymethyl cellulose, glass fiber and water to the composite carrier in sequence, and kneading for 3 hours to obtain a catalyst paste;
[0043] S24, using a roller to apply the catalyst paste on a stainless steel mesh, drying at 90° C. for 6 h, and calcining at 500° C. for 3 h to obtain a lead-poisoning resistant flat-plate denitration catalyst;
[0044] The mass fraction of V2O5 in the obtained denitration catalyst is 1.5%, the mass fraction of MoO3 is 3%, and the mass fraction of Nb2O5 is 2%.
[0045] Example 3
[0046] S31, firstly weighing dolomite and immersing it in a 4 mol / L aminosulfonic acid solution at a solid-liquid ratio of 1:10, stirring it in a water bath at 100°C for 3 hours, filtering and washing it, drying it at 80°C for 4 hours, and then calcining it at 600°C for 5 hours in an atmosphere containing 4 vol% O2 / N2, and grinding it to obtain a modified mineral material;
[0047] S32, mixing TiO2 and modified mineral materials in a mixing tank at a mass ratio of 7:3 to obtain a composite carrier;
[0048] S33, adding ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, antimony acetate aqueous solution, hydroxypropyl cellulose, glass fiber and water to the composite carrier in sequence, and kneading for 2 hours to obtain a catalyst paste;
[0049] S34, using a roller to apply the catalyst paste on a stainless steel mesh, drying at 80° C. for 7 h, and calcining at 550° C. for 4 h to obtain a lead-poisoning resistant flat-plate denitration catalyst;
[0050] The mass fraction of V2O5 in the obtained denitration catalyst is 2%, the mass fraction of MoO3 is 3%, and the mass fraction of Sb2O3 is 1%.
[0051] Example 4
[0052] S41, firstly weighing apatite and immersing it in a 1 mol / L citric acid solution at a solid-liquid ratio of 1:10, stirring it in a water bath at 120°C for 2 hours, filtering and washing it, drying it at 70°C for 4 hours, and then calcining it at 600°C for 6 hours in an atmosphere containing 5 vol% O2 / N2, and grinding it to obtain a modified mineral material;
[0053] S42, mixing TiO2 and modified mineral materials in a mixing tank at a mass ratio of 6:4 to obtain a composite carrier;
[0054] S43, adding ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, tin tetrachloride aqueous solution, methyl cellulose, glass fiber and water to the composite carrier in sequence, and kneading for 4 hours to obtain a catalyst paste;
[0055] S44, using a roller to apply the catalyst paste on a stainless steel mesh, drying at 70° C. for 10 h, and calcining at 500° C. for 5 h to obtain a lead-poisoning resistant flat-plate denitration catalyst;
[0056] The mass fraction of V2O5 in the obtained denitration catalyst is 1%, the mass fraction of MoO3 is 2.7%, and the mass fraction of SnO2 is 2%.
[0057] Example 5
[0058] S51, firstly weighing wollastonite, immersing it in a 5 mol / L oxalic acid solution at a solid-liquid ratio of 1:10, stirring it in a water bath at 80°C for 3 hours, filtering and washing it, drying it at 60°C for 5 hours, and then calcining it at 650°C for 4 hours in an atmosphere containing 3 vol% O2 / N2, and grinding it to obtain a modified mineral material;
[0059] S52, mixing TiO2 and modified mineral material in a mixing tank at a mass ratio of 5:5 to obtain a composite carrier;
[0060] S53, adding ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, chromium nitrate aqueous solution, hydroxypropyl methylcellulose, glass fiber and water to the composite carrier in sequence, and kneading for 3 hours to obtain a catalyst paste;
[0061] S54, using a roller to apply the catalyst paste on a stainless steel mesh, drying at 60° C. for 12 h, and calcining at 550° C. for 2 h to obtain a lead-poisoning resistant flat-plate denitration catalyst;
[0062] The mass fraction of V2O5 in the obtained denitration catalyst is 3%, the mass fraction of MoO3 is 5%, and the mass fraction of Cr2O3 is 3%.
[0063] Comparative Example 1
[0064] Place anatase TiO2 in a mixing tank, add ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, hydroxypropyl methylcellulose, glass fiber and water in sequence, and knead for 4 hours to form a uniform catalyst paste;
[0065] The catalyst paste was then coated on a stainless steel mesh using a roller, dried at 80° C. for 7 h, and calcined at 500° C. for 3 h to obtain a denitration catalyst.
[0066] The mass fraction of V2O5 in the obtained denitration catalyst is 1.5%, and the mass fraction of MoO3 is 3%.
[0067] Comparative Example 2
[0068] Firstly, apatite was weighed and immersed in a 2 mol / L oxalic acid solution at a solid-liquid ratio of 1:10, stirred in a water bath at 80°C for 3 h, filtered and washed, dried at 80°C for 4 h, and then calcined at 800°C for 3 h in an atmosphere containing 2 vol% O2 / N2, and ground to obtain a modified mineral material;
[0069] The anatase TiO2 and the modified mineral material are mixed uniformly in a mixing tank at a mass ratio of 8:2 to obtain a composite carrier;
[0070] Adding ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, hydroxypropyl methylcellulose, glass fiber and water to the composite carrier in sequence, and kneading for 4 hours to form a uniform catalyst paste;
[0071] The catalyst paste was coated on a stainless steel mesh using a roller, dried at 80°C for 7 hours, and calcined at 550°C for 5 hours to obtain a denitration catalyst;
[0072] The mass fraction of V2O5 in the obtained denitration catalyst is 1.5%, and the mass fraction of MoO3 is 3%.
[0073] Comparative Example 3
[0074] Place anatase TiO2 in a mixing tank, add ammonium metavanadate aqueous solution, ammonium heptamolybdate aqueous solution, chromium nitrate aqueous solution, hydroxypropyl methylcellulose, glass fiber and water in sequence, and knead for 4 hours to form a uniform catalyst paste;
[0075] The catalyst paste was coated on a stainless steel mesh using a roller, dried at 90°C for 6 hours, and calcined at 500°C for 5 hours to obtain a denitration catalyst;
[0076] The mass fraction of V2O5 in the obtained denitration catalyst is 2%, the mass fraction of MoO3 is 3%, and the mass fraction of Cr2O3 is 2%.
[0077] Comparative Example 4
[0078] Using the TiO2-Al2O3-SiO2 composite carrier disclosed in CN202111095508.0 as the carrier, the specific steps are as follows:
[0079] The low-titanium blast furnace slag was treated with dilute hydrochloric acid of 2 mol / L and 37 wt% by mass, and fully reacted at a constant temperature of 30°C for 2 hours. Subsequently, a solid-liquid separation operation was performed using a centrifuge at 800 r / min, and the solid components were repeatedly washed with pure water until they were neutral, and then dried at 80°C for 12 hours, and ground into powder to obtain an acid leaching slag carrier (a composite carrier mainly composed of TiO2-Al2O3-SiO2);
[0080] The acid leaching residue carrier was used as the denitration catalyst carrier, and the other steps and parameters were basically the same as those in Example 1.
[0081] The mass fraction of V2O5 in the obtained denitration catalyst is 1%, the mass fraction of MoO3 is 2.7%, and the mass fraction of SnO2 is 2%.
[0082] Test Example 1 Denitrification Performance Test
[0083] The denitration performance of the denitration catalysts prepared in Examples 1-5 and Comparative Examples 1-3 was tested under the following conditions: flue gas temperature 365°C, NO x Concentration 500ppm, NH3 / NO x =1, SO2 concentration 400ppm, N2 as balance gas, GHSV = 60000h -1 The test results are shown in Table 1.
[0084] Table 1 Denitrification efficiency of different denitrification catalysts
[0085]
[0086]
[0087] It can be seen from Table 1 that under the test conditions, the flat-plate denitration catalyst with lead poisoning resistance prepared in Examples 1-5 of the present invention has excellent denitration performance compared with Comparative Examples 1-4.
[0088] Test Example 2 Anti-lead poisoning property test
[0089] In order to verify the anti-lead poisoning characteristics of the denitration catalysts prepared in the above examples and comparative examples, the denitration catalysts in the above examples 1-5 and comparative examples 1-4 were subjected to simulated lead poisoning.
[0090] Specifically, a certain amount of sieved catalyst powder was weighed and placed in a precursor solution prepared by lead acetate, and the mixture was stirred continuously in a water bath at 80°C to make it uniformly mixed, and after being impregnated until dry, it was placed in a forced air drying oven at 110°C for 12 hours, and then calcined at 550°C for 2 hours to obtain a denitration catalyst simulating lead poisoning. The lead loading content on the simulated poisoned catalyst was controlled to be 1wt%.
[0091] The denitration performance of the catalyst after simulated lead poisoning was tested under the same conditions as in Experimental Example 1. The test results are shown in Table 2.
[0092] Table 2 Denitrification efficiency of different denitrification catalysts
[0093]
[0094]
[0095] As shown in Table 2, after loading 1 wt% of PbO, the flat-plate denitration catalyst with lead poisoning resistance prepared in Examples 1 to 5 of the present invention has a denitration efficiency significantly better than the denitration catalyst prepared in Comparative Examples 1 to 4. Therefore, the present invention can effectively improve the lead poisoning resistance of the catalyst by adopting the method of composite carrier optimization and additive addition.
[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a lead-poisoning resistant flat-plate denitration catalyst, characterized in that: The following steps are involved: S1. Modifying the mineral material using an organic acid to obtain a modified mineral material; S2, mixing TiO2 with modified mineral materials to obtain a composite carrier; S3, adding active component precursor, auxiliary agent precursor, impregnating agent, glass fiber and water to the composite carrier in sequence, and kneading to obtain a catalyst paste; S4, coating the catalyst paste on a stainless steel mesh, and obtaining a lead-poisoning-resistant flat-plate denitrification catalyst after drying and calcining; Wherein, the mineral material includes any one or more of apatite, wollastonite and dolomite; The organic acid includes any one or more of oxalic acid, citric acid and aminosulfonic acid, and the concentration of the organic acid is 0.5-5 mol / L; The active components include V2O5 and MoO3, wherein the mass fraction of V2O5 in the denitration catalyst is 0.5-3%, and the mass fraction of MoO3 is 2-6%; The auxiliary agent includes any one or more of Cr2O3, Nb2O5, Sb2O3 and SnO2, and the mass fraction of the auxiliary agent in the denitration catalyst is 0.5-5%.
2. The preparation method according to claim 1, characterized in that: In step S1, during the modification, the mineral material is placed in an organic acid solution, stirred in a water bath at 60-120° C. for 1-5 hours, filtered, washed, and dried, and then calcined in an O2 / N2 atmosphere to obtain a modified mineral material; Wherein, during the drying, the temperature is controlled at 60-100°C and the time is 3-5h; During the calcination, the temperature is controlled at 600-800°C and the time is 3-6h; The volume ratio of O2 to N2 in the O2 / N2 atmosphere is 0.5-5:99.5-95.
3. The preparation method according to claim 1, characterized in that: In the composite carrier, the mass ratio of TiO2 to modified mineral material is 1-9:1, wherein the TiO2 is anatase TiO2.
4. The preparation method according to claim 1, characterized in that: The impregnating agent includes any one or more of hydroxypropyl methylcellulose, carboxymethyl cellulose, hydroxypropyl cellulose and methyl cellulose, and the mass ratio of the impregnating agent to the composite carrier is 1-5:
100.
5. The preparation method according to claim 1, characterized in that: The mass ratio of the glass fiber to the composite carrier is 1-5:
100.
6. The preparation method according to claim 1, characterized in that: In step S4, during the drying, the temperature is controlled to be 60-100°C and the time is 5-12h; During the calcination, the temperature is controlled at 450-550° C. and the calcination time is 2-5 hours.
7. A lead-poisoning resistant flat-plate denitrification catalyst, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 6.