Ceramic tile powder and preparation method thereof, ceramic tile
Through spray drying and vibration fluidization drying processes, combined with the waste heat and hot air of the ceramic tile kiln, the problems of high energy consumption and poor powder performance in the preparation of ceramic tile powder were solved, and powder with good fluidity was obtained and effectively utilized. The waste heat of the kiln reduces production costs and pollution.
Patent Information
- Application Number
- CN202310521426.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-09
AI Technical Summary
The existing ceramic tile powder preparation process has problems of high energy consumption and poor powder performance, especially the uniformity and energy consumption in the wet powder making process, and the powder particles are fine and flowable in the dry powder making process, making it difficult to Suitable for the production of ceramic tiles with low water absorption rate. In addition, the waste heat and hot air of the ceramic tile kiln has not been effectively utilized, causing pollution and heat waste.
Using a process of combining spray drying and vibration fluidization device, the comprehensive slurry is first spray-dried to a moisture content of 12 to 18 wt%, and then the waste heat and hot air of the ceramic tile kiln is used for vibration fluidization and drying to a moisture content of 5.5 to 5.5 to 5. 7.5 wt% to obtain a powder with good fluidity. This process optimizes the particle grading and fluidity of the powder by controlling parameters such as hot air temperature, pressure in the drying tower, atomization nozzle aperture and spray nozzle aperture.
It has achieved the reduction of energy consumption in the preparation of ceramic tile powder, obtained powder with reasonable particle grade and good fluidity, met the production needs of various ceramic tiles, and reduced equipment costs and pollution through the utilization of waste heat and hot air, and improved production efficiency.
Smart Images

Figure CN116693304B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic tiles, and in particular to a ceramic tile powder and a preparation method thereof, and a ceramic tile. Background Art
[0002] In the prior art, there are generally several types of methods for preparing ceramic tile powder. One type is the traditional, widely used wet powder making process, which is to ball-mill various raw materials to obtain a slurry with a moisture content of 30-37wt%, homogenize, sieve and remove iron, and then spray dry to obtain a powder with a moisture content of 5.5-7%. This powder making process is the most mature, with good powder performance, but high energy consumption. The other type is the dry powder making process, which generally refers to grinding various raw materials (generally using a vertical mill) and then adding water to granulate into a powder with a certain particle size distribution. For example, a roller granulator, a disc granulator, a tower granulator, etc. are used for granulation. This type of powder making process has the advantage of low energy consumption and has also been industrialized on a large scale. However, the powder particles prepared by it are fine, have poor fluidity, and poor air exhaust, and are difficult to be used in the production of some ceramic tiles with low water absorption. Another type is a new type of wet powder making process, which is to ball-mill various raw materials to obtain a slurry with a moisture content of 30-37wt%, and then use a process of filter pressing-mud block cutting-drying-crushing granulation after homogenization and iron removal. This process has not yet been applied on a large scale in industry. Since ceramic slurry is a composite formula of plastic raw materials and ridge raw materials, and the sedimentation behavior of different raw materials is different, the use of filter pressing will cause the slurry homogenization to deteriorate and the formula volatility to be large. In addition, the powder particles obtained by crushing and granulation are mostly irregular, and the powder fluidity is poor. In the process of crushing and granulation, fine plastic materials (such as clay, true particle size of about 2μm) will separate from the powder, resulting in changes in the formula, and resulting in more recovery of fine materials and low granulation efficiency. In addition, there is also a method of dividing the ball-milled slurry into two parts, one part is filtered and dehydrated, and then mixed with the other part, and then spray-dried. This process still has problems with uniformity and excessive energy consumption. Therefore, the powder making process in the prior art either has the problem of high energy consumption or has the problem of poor powder performance and poor stability.
[0003] On the other hand, the waste heat hot air generated by the ceramic brick firing kiln has a high temperature (100-300℃), and direct discharge not only causes pollution, but also wastes heat. At present, one technology for recovering waste heat is to use the waste heat hot air as combustion air for the hot air furnace of the spray drying tower, but this usage is limited and it is difficult to achieve large-scale utilization of kiln waste heat. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a ceramic tile powder and a preparation method thereof, which can reduce the energy consumption of powder making and the prepared powder has good fluidity.
[0005] Another technical problem to be solved by the present invention is to provide a ceramic tile.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing ceramic tile powder, which comprises the following steps:
[0007] (1) ball milling the raw materials according to the proportions to obtain a comprehensive slurry;
[0008] (2) drying the comprehensive slurry by a spray drying device to obtain a first powder having a moisture content of 12 to 18 wt %; wherein the spray drying device comprises a drying tower, an atomizing device and a first heating device, wherein the atomizing device is arranged in the drying tower and is used to atomize the comprehensive slurry into droplets; the first heating device is used to provide a first hot air to the drying tower so that the droplets are dried to form a first powder; the temperature of the first hot air is 400 to 600° C.;
[0009] (3) Drying the first powder by a vibrating fluidized bed device to obtain a second powder with a moisture content of 5.5 to 7.5 wt %. The second hot air used for drying by the vibrating fluidized bed device is waste heat from a ceramic brick kiln, and the temperature thereof is 150 to 300° C.
[0010] As an improvement of the above technical solution, the temperature of the first hot air is 400-450° C., and the pressure in the drying tower is 300-500 Pa.
[0011] As an improvement of the above technical solution, the temperature of the first hot air is 400-450°C, the atomizing device includes an atomizing nozzle, the aperture of the spray plate of the atomizing nozzle is 1.5-5 mm, and the atomizing pressure of the comprehensive slurry is 1.5-2.2 MPa.
[0012] As an improvement of the above technical solution, the water content of the comprehensive slurry is 33-37wt%.
[0013] As an improvement of the above technical solution, the temperature of the first hot air is 400-500°C;
[0014] The atomizing device comprises a spray gun arranged along the circumference of the drying tower, the spray gun outlet is connected to an atomizing nozzle, the spray gun has an inclination angle of 120° to 140°, and the atomizing angle of the atomizing nozzle is 120° to 160°, so that the droplets sprayed from multiple spray guns overlap in a preset area.
[0015] As an improvement of the above technical solution, the aperture of the spray plate of the atomizing nozzle is 1-3 mm, and the atomizing pressure of the comprehensive slurry is 2-2.5 MPa, so that the atomizing angle of the atomizing nozzle is 120°-160°.
[0016] As an improvement of the above technical solution, the kiln waste heat hot air includes kiln flue gas waste heat hot air and tail cooling waste heat hot air, the temperature of the kiln flue gas waste heat hot air is 200-220°C, and the temperature of the tail cooling waste heat hot air is 150-180°C;
[0017] The hot air from the tail cooling waste heat is introduced into the first hot air outlet of the vibrating fluidizing device, and the hot air from the kiln flue gas waste heat is introduced into the second hot air outlet of the vibrating fluidizing device. The first hot air outlet is arranged close to the inlet of the vibrating fluidizing device, and the second hot air outlet is arranged close to the outlet of the vibrating fluidizing device.
[0018] As an improvement of the above technical solution, the water content of the comprehensive slurry is 37.5-39 wt %. Accordingly, the present invention also discloses a ceramic tile powder, which is prepared by the above preparation method.
[0019] Correspondingly, the present invention also discloses a ceramic tile, which is made of the above ceramic tile powder.
[0020] The implementation of the present invention has the following beneficial effects:
[0021] 1. The preparation method of ceramic tile powder of the present invention comprises the following steps: firstly drying the comprehensive slurry to a moisture content of 12-18 wt% by using a spray drying device, and then drying the slurry to a moisture content of 5.5-7.5 wt% by using a vibrating fluidizing device, thereby obtaining ceramic tile powder. Based on the preparation method, the obtained ceramic tile powder has a reasonable particle size distribution and good fluidity, and can meet the production requirements of various types of ceramic tiles. In addition, the vibrating fluidizing device uses waste heat hot air from the kiln, which effectively reduces the overall energy consumption.
[0022] 2. The method for preparing ceramic tile powder of the present invention controls the temperature of the hot air entering the drying tower, the pressure inside the drying tower, or controls the aperture of the spray piece of the atomizing nozzle and the atomizing pressure, so that the process of the present invention can be implemented without significantly changing the structure of the original drying tower of the ceramic factory, thereby reducing equipment costs.
[0023] 3. The preparation method of ceramic tile powder of the present invention controls the spray gun setting position, tilt angle, atomization angle, and temperature of hot air entering the drying tower, so that the droplets sprayed from the spray gun overlap in a preset area, thereby obtaining weakly connected twin particles. Such twin particles will be broken under the action of the absolutely dry tail cold waste heat hot air at the inlet of the vibrating fluidizing device during the subsequent drying process of the vibrating fluidizing device, thereby optimizing the particle grading of the powder. Furthermore, kiln flue gas waste heat hot air with a certain humidity is used for cooling near the outlet of the vibrating fluidizing device, which ensures a good drying effect while also avoiding the powder from breaking and producing too much fine powder, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart of a method for preparing ceramic tile powder in one embodiment of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. It is hereby stated that the directional terms such as up, down, left, right, front, back, inside, outside, etc. that appear or will appear in the text of the present invention are only based on the accompanying drawings of the present invention, and are not specific limitations of the present invention.
[0026] The present invention provides a method for preparing ceramic tile powder, which comprises the following steps:
[0027] S1: ball milling the raw materials according to the proportion to obtain a comprehensive slurry;
[0028] The preparation method of the present invention can be applied to ceramic tiles with a water absorption rate of 0.01% to 20%. Those skilled in the art can select relevant raw materials according to specific formulation requirements. For example, the raw materials may include clay raw materials commonly used in the art (such as black mud, white mud, plaster, kaolin, bentonite, magnesia soil, etc.), flux raw materials (such as feldspar, heavy calcium, light calcium, talc, diopside, etc.), aggregates (such as quartz, bauxite, etc.), additives (such as water glass, lignin, etc.), but are not limited thereto.
[0029] The ball milling can be performed by a common single ball mill in the art, or by a continuous ball mill. In one embodiment of the present invention, after the ball milling is completed, the obtained comprehensive slurry is aged, screened, and iron removed.
[0030] The water content of the comprehensive slurry is 33-39 wt %. The preparation method of the present invention is suitable for comprehensive slurry with a higher water content. The formula with a high water content is suitable for production by a continuous ball mill, which effectively improves the efficiency of continuous ball milling.
[0031] It should be noted that in the traditional wet powder making process (ball milling-spray drying), the moisture content of the comprehensive slurry is generally controlled below 37%. This is mainly because: 1. The moisture content of the comprehensive slurry is too high, the energy consumption of spray drying is too high, and the cost is high. 2. When the moisture content of the comprehensive slurry is high, the obtained powder particles are fine, and the exhaust performance and fluidity are poor. For example, in the relevant document "Discussion on the Influencing Factors of Spray Drying Powder Particle Size Distribution", it is clearly pointed out that when the moisture content changes from 36% to 38%, the particle grading will deteriorate. Therefore, although those skilled in the art know that increasing the moisture content will improve the ball milling efficiency, they still control the moisture content of the comprehensive slurry below 37wt% based on comprehensive consideration of ball milling energy consumption, spraying energy consumption, and powder performance. The present invention subsequently utilizes the process of spray primary drying-fluidized secondary drying (waste heat from the kiln) to reduce the energy consumption in the powder making stage, so it can be considered to increase the moisture content of the comprehensive slurry to improve the ball milling efficiency.
[0032] S2: drying the comprehensive slurry by a spray drying device to obtain a first powder;
[0033] The spray drying device is a common spray drying tower in the art, which includes a drying tower, an atomizing device and a first heat supply device. The atomizing device is arranged inside the drying tower, and includes a spray gun and an atomizing nozzle. The atomizing device is used to atomize the comprehensive slurry into droplets. The first heat supply device is used to provide the first hot air to the drying tower, and then the droplets are dried under the action of the first hot air to obtain the first powder.
[0034] Wherein, the moisture content of the first powder is 12-18wt%. When the moisture content is greater than 18wt%, it is easy to adhere to the wall of the drying tower or accumulate at the discharge port of the drying tower, making it difficult for spray drying to proceed smoothly. When the moisture content is less than 12wt%, the energy saving effect is poor, and the subsequent vibrating fluidizing device is also difficult to play a shaping role. Exemplarily, the moisture content of the first powder is 13wt%, 14wt%, 15wt%, 16wt% or 17wt%, but is not limited thereto.
[0035] The temperature of the first hot air is 400-600° C., exemplarily 415° C., 430° C., 445° C., 460° C., 475° C., 490° C., 505° C., 520° C., 535° C., 550° C., 565° C., 580° C. or 595° C., but not limited thereto. The pressure in the drying tower is 100-500 Pa, exemplarily 120 Pa, 160 Pa, 200 Pa, 240 Pa, 280 Pa, 320 Pa, 360 Pa, 400 Pa, 440 Pa or 480 Pa, but not limited thereto.
[0036] The inclination angle of the spray gun is 100° to 150°, and is exemplarily 105°, 110°, 115°, 120°, 125°, 130° or 140°, but is not limited thereto. The aperture of the atomizing nozzle is 1 to 5 mm, and is exemplarily 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm or 4.5 mm, but is not limited thereto.
[0037] Preferably, in one embodiment of the present invention, the temperature of the first hot air is controlled to be 400-450°C, the pressure in the drying tower is controlled to be 300-500Pa, and the comprehensive slurry moisture content is controlled to be 33-37wt%. Based on the above control, the drying tower can be kept running stably without changing other conditions (comprehensive slurry moisture content (33-37wt%), spray gun setting angle (100°-120°), spray plate aperture (1-1.5mm), atomization pressure (1.2-1.5MPa)), and the first powder with a moisture content of 12-18wt% is obtained. It should be noted that the design of the drying tower in the spray drying device is based on a certain thermal balance. When the feed amount (atomization pressure), heat source temperature (first hot air temperature), and atomization parameters (spray gun angle, spray plate aperture, etc.) are not changed, the moisture content of the first powder discharged is relatively low, about 5-8wt%, that is, it is difficult to obtain the first powder with a moisture content of 12-18wt% in the present invention. To this end, in this embodiment, the temperature of the first hot air is lowered, that is, the time for the droplets to dry into shells is prolonged; and the negative pressure in the drying tower is increased, that is, the contact time between the first hot air and the droplets and the droplets being converted into powder is shortened. Through the coordinated control of the above two, the first powder with a specific moisture content can be obtained without changing the structure of the drying tower. However, it should be noted that increasing the negative pressure in the drying tower will also lead to an increase in the outlet temperature of the drying tower and increased energy consumption; it will also lead to an increase in the amount of fine powder in the first powder, affecting the performance of the powder. Too much fine powder will also increase the amount of material that needs to be circulated in the drying tower, reducing the output of the drying tower. Although the composite late fluidized drying still has a certain energy-saving effect, the energy-saving effect is poor.
[0038] Preferably, in another embodiment of the present invention, the aperture of the spray piece of the atomizing nozzle is controlled to be 1.5-5 mm, and the atomizing pressure of the comprehensive slurry is 1.5-2.2 MPa. Based on the above control, the drying tower can be kept running stably without changing other conditions (comprehensive slurry moisture content (33-37 wt%), spray gun setting angle (100°-120°), first hot air temperature (400-600°C), negative pressure in the drying tower (100-250 Pa)), and the first powder with a moisture content of 12-18 wt% is obtained. It should be noted that the design of the drying tower in the spray drying device is based on a certain thermal balance. When the feed amount (atomizing pressure), heat source temperature (first hot air temperature), and atomization parameters (spray gun angle, spray piece aperture, etc.) are not changed, the moisture content of the first powder discharged is relatively low, about 5-8 wt%, that is, it is difficult to obtain the first powder with a moisture content of 12-18 wt% in the present invention. To this end, in this embodiment, the atomization pressure is increased, that is, the comprehensive slurry feed amount is increased; and the nozzle aperture is increased, that is, the droplet diameter is increased. Through the coordinated control of the above two, the first powder with a specific moisture content can be obtained without changing the structure of the drying tower. However, it should be noted that increasing the atomization pressure will also increase the amount of fine powder in the first powder.
[0039] In order to solve the above problems, in another embodiment of the present invention, the moisture content of the comprehensive slurry is increased to 37.5-39wt%, and the temperature of the first hot air is reduced to 400-500°C. In addition, the aperture of the spray piece is controlled to be 1-3mm, and the atomization pressure of the comprehensive slurry is 2-2.5MPa, so that the atomization angle of the atomizing nozzle is 120°-160°. In addition, the inclination angles of multiple spray guns arranged along the circumference of the drying tower are controlled to be 120°-140°, and the atomization angle of the atomizing nozzle is 120°-160°, so that the droplets sprayed by multiple spray guns overlap in a preset area. Based on this arrangement, the particle size of the first powder can be greatly improved and fine powder can be reduced; and then, it can be shaped through fluidized drying in the later stage to obtain a powder with good performance.
[0040] It should be noted that those skilled in the art generally believe that if the droplets overlap, it will lead to uneven drying and too many irregular large particles. The present invention has found that the problem can be effectively solved through the process of spray drying-fluidized shaping. On the contrary, when there are some twin particles with high humidity in the first powder, they can be quickly broken by absolute dry waste heat hot air in the early stage of fluidized drying, thereby obtaining a second powder with good performance. Moreover, the inventor unexpectedly found that after the above control, the amount of fine powder in the drying tower was greatly reduced, and it did not even need to be recycled to the ball mill.
[0041] S3: drying the first powder using a vibrating fluidizing device to obtain a second powder;
[0042] The vibrating fluidizing device includes a fluidized bed, a second heat supply device and an exhaust gas treatment device. The heat source of the second heat supply device is the waste heat hot air of the ceramic brick kiln, and its temperature is 150-300°C. The waste heat hot air can be the waste heat hot air obtained by mixing all the gases in the kiln, or the waste heat hot air of the kiln flue gas from the preheating section of the kiln and the tail cooling waste heat hot air from the rapid cooling section of the kiln, but it is not limited to this.
[0043] Preferably, in one embodiment of the present invention, the kiln waste heat hot air includes kiln flue gas waste heat hot air and tail cooling waste heat hot air, and the temperature of the kiln flue gas waste heat hot air is 200-220°C, which contains a certain amount of moisture in the preheating section and has a certain humidity. The temperature of the tail cooling waste heat hot air is 150-180°C, and it is an absolute dry gas. The tail cooling waste heat hot air is introduced into the first hot air port of the vibrating fluidizing device, and the kiln flue gas waste heat hot air is introduced into the second hot air port of the vibrating fluidizing device. The first hot air port is arranged near the inlet of the vibrating fluidizing device, and the second hot air port is arranged near the outlet of the vibrating fluidizing device. Based on this arrangement, one is to dry by the absolute dry tail cooling waste heat hot air, so that the surface of the twin particles quickly hardens, and then separation is achieved under the joint action of vibration and air fluidization. Second, the kiln flue gas waste heat hot air with a certain humidity is used for drying near the outlet to reduce the amount of fine powder generated by the vibrating fluidizing device.
[0044] The preparation method of the present invention is compared with the traditional wet powder making process and the novel dry powder making process (CN205269568U), as shown in the following table.
[0045]
[0046] As can be seen from the table, the preparation method of the present invention effectively reduces the powder consumed in the unit powder preparation process. The particle size distribution and fluidity of the obtained powder are very similar to those of the traditional wet powder preparation, which can meet the production requirements of various types of ceramic tiles.
[0047] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A method for preparing ceramic tile powder, characterized in that: The following steps are involved: (1) Ball milling the raw materials according to the proportions to obtain a comprehensive slurry; (2) Drying the comprehensive slurry with a spray drying device to obtain a first powder with a moisture content of 12-18 wt%; wherein the spray drying device comprises a drying tower, an atomizing device and a first heat supply device, the atomizing device is arranged in the drying tower, and is used to atomize the comprehensive slurry into droplets; the atomizing device comprises an atomizing nozzle and a spray gun arranged along the circumference of the drying tower, the outlet of the spray gun is connected to the atomizing nozzle, and the first heat supply device is used to provide a first hot air to the drying tower so that the droplets are dried to form a first powder; the temperature of the first hot air is 400-600°C; the pressure in the drying tower is 300-500 Pa, and the atomization pressure of the comprehensive slurry is 1.5-2.2 MPa; the inclination angle of the spray gun is 120°-140°, the aperture of the spray piece of the atomizing nozzle is 1.5-5 mm, and the atomization angle of the atomizing nozzle is 120°-160°, so that the droplets sprayed by multiple spray guns overlap in a preset area; (3) Drying the first powder by a vibrating fluidizing device to obtain a second powder with a moisture content of 5.5-7.5wt%, that is; wherein the second hot air used for drying by the vibrating fluidizing device is waste heat hot air from a ceramic brick kiln, and its temperature is 150-300°C, and the kiln waste heat hot air includes kiln flue gas waste heat hot air and tail cooling waste heat hot air, and the temperature of the kiln flue gas waste heat hot air is 200-220°C, and the temperature of the tail cooling waste heat hot air is 150-180°C; the tail cooling waste heat hot air is introduced into the first hot air port of the vibrating fluidizing device, and the kiln flue gas waste heat hot air is introduced into the second hot air port of the vibrating fluidizing device, the first hot air port is arranged close to the inlet of the vibrating fluidizing device, and the second hot air port is arranged close to the outlet of the vibrating fluidizing device.
2. The method for preparing ceramic tile powder according to claim 1, characterized in that: The temperature of the first hot air is 400-450°C.
3. The method for preparing ceramic tile powder according to claim 1 or 2, characterized in that: The water content of the comprehensive slurry is 33-37wt%.
4. A ceramic tile powder, characterized in that: Prepared by the preparation method according to any one of claims 1 to 3.
5. A ceramic tile, characterized in that: Made from the ceramic tile powder as claimed in claim 4.