Memory foam containing plant raw materials, application and pillow

By mixing the alkali solution and corona treated rice bran with nano-silver powder as memory foam pillow core material, the problem of insufficient breathability and antibacteriality of the existing pillow core is solved, and pillows adapted to different sleeping positions and cleaning and drying are achieved. The core design improves sleep quality and environmental protection.

CN117069906BActive Publication Date: 2024-11-12TENGFEI TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311066702.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-23
Publication Date
2024-11-12
Estimated Expiration
2043-08-23

AI Technical Summary

Technical Problem

The existing memory foam pillow core has poor breathability and moisture dissipation, which is prone to breeding mites and bacteria, and cannot be adjusted according to different sleeping positions and physical states, affecting the quality of sleep.

Method used

The rice bran treated with alkali solution and corona are mixed with nano-silver powder as the pillow core filling material, and designed as a partition structure to meet different sleeping positions and cleaning and drying needs.

Benefits of technology

It improves the breathability and antibacteriality of the pillow core, adapts to the needs of different sleeping positions, ensures the quality of sleep and is easy to clean and dry, and meets the needs of low-carbon and environmentally friendly development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117069906B_ABST
    Figure CN117069906B_ABST
Patent Text Reader

Abstract

The invention discloses a memory foam containing plant raw materials, application and pillow, wherein the memory foam comprises the following raw materials in parts by weight: 1-30 parts of rice bran-nano silver powder, 40-70 parts of polyether polyol composition, 10-50 parts of diphenylmethane diisocyanate, 1-10 parts of water, and 1-10 parts of auxiliary agent, wherein the rice bran-nano silver powder is mixed with nano silver powder after rice bran is treated with alkaline solution and corona. In the present invention, rice bran is used as waste of agricultural products and applied to memory foam pillows, which can broaden the application field of rice bran; rice bran contains rich bioactive ingredients such as palmitic acid, ethyl oleate, squalene, etc., and has antioxidant, antibacterial, anti-mite and sleep-aiding effects, which helps to improve sleep quality; at the same time, after the rice bran is treated, the physical structure of its surface changes, which can improve the dispersion stability of nano silver powder and help to combine with other foaming raw materials; its structure is also looser and softer, and as the raw material of the memory foam pillow, it helps to improve air permeability and moisture dissipation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the technical field of pillows, and in particular relates to memory foam containing plant raw materials, applications and pillows. Background technology:

[0002] Ensuring adequate sleep every day plays a significant role in the physical and mental health of the human body. Pillows, as sleep support, directly affect the quality of a person's sleep.

[0003] The pillow cores of common pillows on the market are mainly memory foam and latex. Memory foam is widely loved by people because of its good softness and reasonable price. However, the existing memory foam pillow cores still have the defects of poor air permeability and moisture dissipation. Especially when used in summer, sweat cannot be discharged in time. On the one hand, mites and other bacteria are easy to breed on the pillow core, which has a certain impact on human health. On the other hand, it is easy to produce stickiness and stuffiness, thus affecting the quality of sleep.

[0004] In addition, most of the existing pillows are integrated and can only adapt to a specific lying position, such as lying on the back or lying on the side, and cannot adapt to multiple sleeping positions. People have different requirements for the height of the pillow when lying on the back and lying on the side, such as requiring the pillow to be low when lying on the back and high when lying on the side, etc.; and in different physical conditions, the requirements for the pillow are also different, such as when the shoulder and neck are tired, the pillow is expected to have support for the shoulder and neck, when taking a short rest, the pillow is expected to be high when lying on the side, and when sleeping deeply, the pillow is expected to be only slightly higher than when lying on the back, etc. Although there are some partitioned pillows in the existing pillows, most of them only use quilting or splicing to distinguish the shapes of the two supports of the neck and the head, and cannot adjust the height of the side-lying area and the shoulder and neck support parts according to people's needs. Furthermore, in order to keep the pillow clean during use, it needs to be cleaned and dried regularly, and even the existing pillows with partition functions are mostly integral structures. When cleaning and drying, the inside is easy to be not cleaned cleanly and not dried thoroughly, thus affecting people's sleep health.

[0005] Rice bran is a waste product of agricultural products and is rich in resources. Studies have shown that rice bran is rich in bioactive ingredients such as palmitic acid, ethyl oleate, and squalene, which makes rice bran have antioxidant, breathable, antibacterial, anti-mite and sleep-inducing effects. After being treated with alkaline solution and corona, the physical structure of the rice bran surface can be changed, making it have better dispersion stability.

[0006] Nanosilver has extremely strong nanoactivity and shows extraordinary antibacterial ability. It can kill common bacteria, fungi, mycoplasma, chlamydia and other pathogenic microorganisms. However, nanosilver is expensive on the one hand, and it is easy to agglomerate and has poor compatibility on the other hand. Studies have shown that mixing rice bran with nanosilver after alkaline solution and corona treatment can improve its easy agglomeration and poor compatibility by wrapping the nanosilver with rice bran. Using the mixed powder of rice bran and nanosilver as the filling material of pillows can not only make waste items more widely used, but also because rice bran has a certain antibacterial effect, by adding a small amount of nanosilver, a better antibacterial effect can be achieved, which can effectively control costs; at the same time, due to the unique active ingredients of rice bran, it can give memory foam filling materials better performance, thereby providing people with a better sleeping environment.

[0007] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention:

[0008] The object of the present invention is to provide a memory foam, application and pillow based on plant raw materials, so as to overcome the defects in the above-mentioned prior art.

[0009] In order to achieve the above-mentioned object, the present invention provides a memory foam containing plant raw materials, comprising the following raw materials in parts by weight: 1-30 parts of rice bran-nano silver powder, 40-70 parts of a polyether polyol composition, 10-50 parts of diphenylmethane diisocyanate, 1-10 parts of water, and 1-10 parts of an auxiliary agent. The rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0010] Further, preferably, the method for preparing the rice bran-nano silver powder comprises the following steps:

[0011] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0012] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 5-12 hours;

[0013] Step 3: Take out the rice bran and soak it in ethanol for 5-12 hours;

[0014] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0015] Step 5: Grind the rice bran into 60-80 mesh powder;

[0016] Step 6: using a corona treatment device to perform corona treatment on the rice bran powder;

[0017] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder.

[0018] Furthermore, preferably, the size of the nanosilver is 10-60 nanometers.

[0019] Further, preferably, the polyether polyol composition comprises two or more polyether polyols, and the specific polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are (30%-60%), (15%-30%), (15%-30%), and (5%-15%).

[0020] Furthermore, preferably, the auxiliary agent includes an antioxidant, a foam stabilizer, a foaming agent, a catalyst, and a surfactant.

[0021] The present invention also provides an application of the memory foam containing plant materials, and the memory foam containing plant materials is used as a pillow core material of a pillow.

[0022] The present invention further provides a memory foam pillow containing plant materials, comprising a pillowcase and a pillow core, wherein the pillow core is made of memory foam containing plant materials, the pillowcase is divided into three areas, namely a middle headrest area, a first side sleeping area on both sides, and a second side sleeping area, and the pillow core is correspondingly divided into three parts, namely a middle head pillow core, a first side sleeping pillow core, and a second side sleeping pillow core, wherein the middle head pillow core comprises a headrest and a shoulder and neck pillow, and the shoulder and neck pillow can be folded into the headrest.

[0023] Further, as a preference, the first side sleeping pillow core and the second side sleeping pillow core are both composed of a side sleeping pillow core body and a replaceable module.

[0024] Further, as a preference, the side sleeping pillow core body is a sheet-like structure, and the side sleeping pillow core body wraps around the replaceable module when rolled up.

[0025] Furthermore, as a preference, the side sleeping pillow core body is provided with a plurality of ventilation holes.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) In the present invention, rice bran is a waste product of agricultural products and is abundant in resources. Applying it to memory foam pillows can broaden the application field of rice bran and meet the development needs of low-carbon and environmental protection;

[0028] (2) After the rice bran is treated in the present invention, the physical structure of its surface changes, so that it has better dispersion stability. When it is mixed with nano silver powder, it has superior antibacterial properties and can improve the dispersion stability of the nano silver powder, which is helpful for combining with other foaming raw materials;

[0029] (3) After the rice bran is processed in the present invention, its structure becomes looser and softer, and as the raw material of the memory foam pillow, it helps to improve the air permeability and moisture dissipation;

[0030] (4) The rice bran of the present invention is rich in bioactive ingredients such as palmitic acid, ethyl oleate, squalene, etc., and has antioxidant, antibacterial, anti-mite and sleep-aiding effects, which helps to improve sleep quality;

[0031] (5) The pillow structure of the present invention adopts three independent areas for easy cleaning and drying; at the same time, the middle head pillow core adopts a foldable head pillow and shoulder and neck pillow combination design, so that the user can choose whether to use the shoulder and neck pillow function according to needs;

[0032] (6) The structural design of the pillow in the present invention is a side sleeping pillow that is a combination of a main body and a replaceable module. The user can choose whether to use the replaceable module according to the needs, and can easily adjust the height of the side sleeping pillow according to the needs;

[0033] (7) The structural design of the pillow in the present invention is that the main body of the side sleeping pillow core is a sheet structure, which is more convenient for thorough cleaning and drying on the one hand, and also more convenient for installing replaceable modules on the other hand. Description of the drawings:

[0034] Figure 1 This is a schematic diagram of a pillowcase of a memory foam pillow containing plant materials according to Example 7 of the present invention;

[0035] Figure 2 This is a schematic diagram of a pillow core of a memory foam pillow containing plant materials according to Example 7 of the present invention;

[0036] Figure 3 This is a schematic diagram of a memory foam pillow containing plant materials according to Example 7 of the present invention when the shoulder and neck pillow is pulled out during use.

[0037] Figure 4 This is a schematic diagram of a head pillow core of a memory foam pillow containing plant materials according to Example 7 of the present invention.

[0038] Figure 5 This is a schematic diagram of a first side sleeping pillow core and a second side sleeping pillow core of a memory foam pillow containing plant materials according to Example 7 of the present invention;

[0039] Figure 6 This is a schematic diagram of a side sleeping pillow core body of a memory foam pillow containing plant materials according to Example 7 of the present invention;

[0040] Description of the drawings: 1-pillowcase, 10-invisible zipper, 11-middle headrest area, 12-first side sleeping area, 13-second side sleeping area, 2-pillow core, 21-head pillow core, 211-headrest, 212-shoulder and neck pillow, 213-hole position, 214-side sleeping pillow core body, 215-replaceable module, 216-ventilation hole, 22-first side sleeping pillow core, 23-second side sleeping pillow core, 24-second side sleeping pillow. Specific implementation method:

[0041] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0042] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or critical elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.

[0043] Embodiment 1:

[0044] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 5 parts of rice bran-nano silver powder, 58 parts of polyether polyol composition, 31 parts of diphenylmethane diisocyanate, 3 parts of water, and 3 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0045] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0046] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0047] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 10 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 90°C.

[0048] Step 3: Take out the rice bran and soak it in ethanol for 8 hours;

[0049] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0050] Step 5: Grind the rice bran into powder of about 80 mesh;

[0051] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2, the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0052] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0053] In this embodiment, the nanosilver is selected in the form of powder with a size of 50 nanometers.

[0054] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 22%, and 7%.

[0055] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0056] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0057] Embodiment 2:

[0058] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 10 parts of rice bran-nano silver powder, 54 parts of polyether polyol composition, 30 parts of diphenylmethane diisocyanate, 3 parts of water, and 3 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0059] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0060] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0061] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 8 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 95°C.

[0062] Step 3: Take out the rice bran and soak it in ethanol for 7.5 hours;

[0063] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0064] Step 5: Grind the rice bran into powder of about 75 mesh;

[0065] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 12000-13000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0066] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0067] In this embodiment, the nanosilver is selected in the form of powder with a size of 50 nanometers.

[0068] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 21%, and 8%.

[0069] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0070] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0071] Embodiment 3:

[0072] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 15 parts of rice bran-nano silver powder, 52 parts of polyether polyol composition, 28 parts of diphenylmethane diisocyanate, 3 parts of water, and 2 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0073] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0074] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0075] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 9 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 93°C.

[0076] Step 3: Take out the rice bran and soak it in ethanol for 8 hours;

[0077] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0078] Step 5: Grind the rice bran into powder of about 80 mesh;

[0079] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0080] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0081] In this embodiment, the nanosilver is selected in the form of powder with a size of 55 nanometers.

[0082] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 21%, and 8%.

[0083] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0084] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0085] Embodiment 4:

[0086] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 20 parts of rice bran-nano silver powder, 49 parts of polyether polyol composition, 27 parts of diphenylmethane diisocyanate, 2 parts of water, and 2 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0087] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0088] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0089] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 10 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 90°C.

[0090] Step 3: Take out the rice bran and soak it in ethanol for 6 hours;

[0091] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0092] Step 5: Grind the rice bran into powder of about 75 mesh;

[0093] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0094] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0095] In this embodiment, the nanosilver is selected in the form of powder with a size of 50 nanometers.

[0096] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 20%, 20%, and 10%.

[0097] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0098] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0099] Embodiment 5:

[0100] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 25 parts of rice bran-nanosilver powder, 46 parts of polyether polyol composition, 25 parts of diphenylmethane diisocyanate, 2 parts of water, and 2 parts of additives, wherein the rice bran-nanosilver powder is prepared by mixing rice bran with nanosilver powder after being treated with an alkaline solution and corona.

[0101] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0102] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0103] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 10 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 90°C.

[0104] Step 3: Take out the rice bran and soak it in ethanol for 6 hours;

[0105] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0106] Step 5: Grind the rice bran into powder of about 75 mesh;

[0107] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0108] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0109] In this embodiment, the nanosilver is selected in the form of powder with a size of 50 nanometers.

[0110] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 20%, 20%, and 10%.

[0111] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0112] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0113] Embodiment 6:

[0114] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 30 parts of rice bran-nano silver powder, 43 parts of polyether polyol composition, 23 parts of diphenylmethane diisocyanate, 2 parts of water, and 2 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0115] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0116] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0117] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 10 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 90°C.

[0118] Step 3: Take out the rice bran and soak it in ethanol for 8 hours;

[0119] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0120] Step 5: Grind the rice bran into powder of about 80 mesh;

[0121] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0122] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0123] In this embodiment, the nanosilver is selected in the form of powder with a size of 50 nanometers.

[0124] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 22%, and 7%.

[0125] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0126] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0127] Comparative Example 1:

[0128] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 60 parts of polyether polyol composition, 34 parts of diphenylmethane diisocyanate, 3 parts of water, and 3 parts of auxiliary agent;

[0129] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 22%, and 7%.

[0130] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0131] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0132] Comparative Example 2:

[0133] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 15 parts of rice bran-nano silver powder, 52 parts of polyether polyol composition, 28 parts of diphenylmethane diisocyanate, 3 parts of water, and 2 parts of additives, wherein the rice bran-nano silver powder is obtained by mixing rice bran with nano silver powder after corona treatment.

[0134] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0135] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0136] Step 2: Grind the rice bran into powder of about 80 mesh;

[0137] Step 3: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0138] Step 4: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0139] In this embodiment, the nanosilver is selected in the form of powder with a size of 55 nanometers.

[0140] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 21%, and 8%.

[0141] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0142] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0143] Comparative Example 3:

[0144] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 15 parts of rice bran-nano silver powder, 52 parts of polyether polyol composition, 28 parts of diphenylmethane diisocyanate, 3 parts of water, and 2 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution.

[0145] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0146] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0147] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 9 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 93°C.

[0148] Step 3: Take out the rice bran and soak it in ethanol for 8 hours;

[0149] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0150] Step 5: Grind the rice bran into powder of about 80 mesh;

[0151] Step 6: Evenly mix the rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0152] In this embodiment, the nanosilver is selected in the form of powder with a size of 55 nanometers.

[0153] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are 50%, 21%, 21%, and 8%.

[0154] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0155] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0156] Comparative Example 4:

[0157] The memory foam containing plant raw materials of this embodiment includes the following raw materials in parts by weight: 15 parts of rice bran-nano silver powder, 52 parts of polyether polyol composition, 28 parts of diphenylmethane diisocyanate, 3 parts of water, and 2 parts of additives, wherein the rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona.

[0158] In this embodiment, the preparation method of rice bran-nano silver powder comprises the following steps:

[0159] Step 1: Wash the rice bran with pure water, remove impurities and dry;

[0160] Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 9 hours. During cooking, the rice bran is placed in a sealed container and the temperature is controlled at about 93°C.

[0161] Step 3: Take out the rice bran and soak it in ethanol for 8 hours;

[0162] Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry;

[0163] Step 5: Grind the rice bran into powder of about 80 mesh;

[0164] Step 6: Use a corona treatment device to perform corona treatment on the rice bran powder. During the corona treatment, the corona discharge voltage is 10000-12000V / m 2 , the discharge power is controlled at 3-4KW, and the corona treatment is 3-5s;

[0165] Step 7: Evenly mix the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder, wherein the mass ratio of the rice bran powder to the nano-silver powder is 10:1.

[0166] In this embodiment, the nanosilver is selected in the form of powder with a size of 55 nanometers.

[0167] In this embodiment, the polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, and polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and the weight percentages of the four are 50%, 25%, and 25%.

[0168] In this embodiment, the auxiliary agents include an antioxidant, a foam stabilizer, a blowing agent, a catalyst, and a surfactant, wherein the antioxidant is antioxidant 1010, the foam stabilizer is silicone, the blowing agent is T-9 organic blowing agent, the catalyst is cobalt formate, and the surfactant is fatty alcohol polyoxyethylene ether sodium sulfate.

[0169] After the above raw materials are evenly mixed, the existing memory foam foaming process is used to make a foam material sample.

[0170] Compared with Examples 1-6, in Comparative Example 1, rice bran-nanosilver powder was not added to the raw materials; compared with Example 3, the rice bran treatment in Comparative Example 2 was not subjected to alkaline solution cooking; compared with Example 3, the rice bran treatment in Comparative Example 3 was not subjected to corona treatment; compared with Example 4, plant-based polyether polyol was not added to the polyether polyol composition in Comparative Example 4.

[0171] The performance of the foam material samples prepared in the above examples 1-6 was tested, and the test results are shown in the following table:

[0172] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Antibacterial rate (%) 45.3 50.1 53.2 58.7 60.5 65.3 Air permeability (L / min) 7.9 8.5 10.8 15.1 18.5 20.3 Moisture removal (2h%) 61.3 61.9 63.8 64.5 66.3 68.5 Tensile strength(Kpa) 60.1 59.8 59.6 59.4 57.3 56.2 Tear strength (N / cm) 1.13 1.12 1.15 1.13 0.98 0.96 Rebound rate (%) 15.1 15.3 14.7 14.5 14.8 15.7

[0173] The performance of the foam material samples prepared in the above comparative examples 1-4 was tested, and the test results are shown in the following table:

[0174] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Antibacterial rate (%) 30.2 53.8 45.8 53.1 Air permeability (L / min) 5.3 5.3 8.7 8.9 Moisture discharge (2h%) 57.2 60.5 61.8 61.3 Tensile strength(Kpa) 60.3 59.7 59.8 59.6 Tear strength (N / cm) 1.15 1.13 1.12 1.12 Rebound rate (%) 15.2 14.6 14.8 15.3

[0175] The above-mentioned antibacterial rate test is tested using the GB / T 31402-2015 standard; the air permeability is tested using the TQD-01 tester; the moisture drainage test is tested using the immersion method, and specifically, a 50cm*50cm sample is cut and immersed in water for 12 hours and then weighed, recorded as m1. The water-soaked sample is placed on a drain rack and naturally drained for 24 hours and then weighed again, recorded as m2, moisture drainage = (m1-m2) / m1*100%; the tensile strength test is tested using the GBT6344-2008 standard; the tear strength test is tested using the GB / T10808-2006 standard; the resilience test is tested using the ASTM D3574 standard.

[0176] From the test results of the above-mentioned Examples 1-6 and Comparative Examples 1-4, it can be seen that:

[0177] (1) Rice bran-nanosilver powder is added to the foaming raw material, and the prepared memory foam material has excellent antibacterial properties, air permeability, and moisture discharge properties, and the mechanical properties are not changed too much. When used as a raw material for a pillow, it can help improve sleep quality;

[0178] (2) The performance is most superior when the amount of rice bran-nanosilver powder added is 10-20 parts. When the amount of rice bran-nanosilver powder added is too low, the antibacterial rate, air permeability, and moisture removal are slightly lacking, but still have a significant improvement compared with no addition of rice bran-nanosilver powder; when the amount of rice bran-nanosilver powder added is too high, the mechanical properties are slightly reduced, but still within the applicable range;

[0179] (3) After the surface of rice bran is treated with alkali solution, its structure becomes looser and softer, and the memory foam material made from it has better air permeability and moisture dissipation;

[0180] (4) After the surface of rice bran is treated with corona, the physical structure of its surface changes, making it have better dispersion stability. Mixing it with nano-silver powder can improve the dispersion stability of the nano-silver powder, thereby making the nano-silver powder better exert its antibacterial properties;

[0181] (5) Plant-based polyether polyols are added to the polyether polyol composition, which improves the air permeability, moisture discharge and resilience of the material;

[0182] In the present invention, the rice bran also contains abundant bioactive ingredients such as palmitic acid, ethyl oleate, squalene, etc., and has antioxidant, antibacterial, anti-mite and sleep-aiding effects, which helps to improve sleep quality; at the same time, as a waste of agricultural products, rice bran is rich in resources, and applying it to memory foam pillows can broaden the application field of rice bran, which meets the development needs of low-carbon and environmental protection;

[0183] Embodiment 7:

[0184] like Figure 1-6 As shown, a memory foam pillow containing plant materials in this embodiment comprises a pillowcase 1 and a pillow core 2, wherein the pillow core 2 is made of the memory foam containing plant materials, the pillowcase 1 is divided into three areas, namely a middle headrest area 11, first side sleeping areas 12 on both sides, and a second side sleeping area 13, the first side sleeping area 12 and the middle headrest area 11 are separated by sewing, and the second side sleeping area 13 and the middle headrest area 11 are also separated by sewing, the three areas of the pillowcase 1 are respectively preset with hard zippers 10, and the pillow core 2 is also divided into three parts, namely a middle head pillow core 21, a first side sleeping pillow core 22 and a second side sleeping pillow core 23, wherein the middle head The pillow core 21 includes a headrest 211 and a shoulder and neck pillow 212. The shoulder and neck pillow 212 can be folded into the headrest 211 or pulled out from the headrest 211. Specifically, a hole 213 is provided on the headrest 211 at a position corresponding to the shoulder and neck. The hole 213 is used to insert the shoulder and neck pillow 212. The shoulder and neck pillow 212 and the headrest 211 are integrated. When the shoulder and neck pillow 212 is inserted into the hole 213, it serves as a part of the headrest 211. Therefore, people can pull out the shoulder and neck pillow 212 when they need to use it, and put it back in when they don't need it. The pillow core adopts three independent designs, which is more convenient to wash and dry, and can keep the pillow clean.

[0185] In this embodiment, the first side sleeping pillow core 22 and the second side sleeping pillow core 23 are both composed of a side sleeping pillow core body 214 and a replaceable module 215; the pillow core body 214 can be a circular ring structure with an installation hole, and the replaceable module 215 is inserted into the installation hole; it can also be a sheet structure that can be fully unfolded. When in use, the pillow core body 214 wraps the replaceable module 215 and then inserts it into the corresponding side sleeping area. This structural design can be more thoroughly cleaned and dried during cleaning and drying, and the inclination of the pillow core can be maintained; the replaceable module 215 can be a flat sheet structure, and the shape can be rectangular, elliptical, arc-shaped, irregular sheet structure, etc.; the replaceable module 215 can be designed into a variety of specifications with different thicknesses; people can choose whether to use the replaceable module 215 according to their physical needs, as well as the specific specifications to use, to achieve adjustment of the height of the side sleeping pillow.

[0186] In this embodiment, the side sleeping pillow core body 214 is provided with a plurality of ventilation holes 216 for improving ventilation performance.

[0187] The pillow usage method of this embodiment is as follows:

[0188] When in use, the middle head pillow core 21 is placed in the middle head pillow area 11 of the pillowcase 1, the first side sleeping pillow core 22 is placed in the first side sleeping area 12, and the second side sleeping pillow core 23 is placed in the second side sleeping area;

[0189] When the shoulder and neck pillow 212 is needed, the shoulder and neck pillow 212 is pulled out from the headrest 211, and when it is not needed, the shoulder and neck pillow is put back into the headrest 211;

[0190] When it is time to wash and dry, just take out the three pillow cores and wash and dry them separately;

[0191] In this embodiment: the pillow core 2 adopts three independent structural designs, which is more convenient for thorough drying and cleaning to keep the pillow clean; you can also choose whether to use the shoulder and neck pillow function according to your needs, and adjust the height of the side sleeping pillow as needed to improve people's comfort.

[0192] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A memory foam containing plant raw materials, characterized in that: The invention comprises the following raw materials in parts by weight: 1-30 parts of rice bran-nano silver powder, 40-70 parts of a polyether polyol composition, 10-50 parts of diphenylmethane diisocyanate, 1-10 parts of water, and 1-10 parts of an auxiliary agent. The rice bran-nano silver powder is prepared by mixing rice bran with nano silver powder after being treated with an alkaline solution and corona. The preparation method of the rice bran-nano silver powder comprises the following steps: Step 1: Wash the rice bran with pure water, remove impurities and dry; Step 2: Place the dried rice bran in a sodium hydroxide solution and cook for 5-12 hours; Step 3: Take out the rice bran and soak it in ethanol for 5-12 hours; Step 4: Take out the rice bran, wash it with pure water, and place it in an oven to dry; Step 5: Grind the rice bran into 60-80 mesh powder; Step 6: using a corona treatment device to perform corona treatment on the rice bran powder; Step 7: Evenly mixing the corona-treated rice bran powder and the nano-silver powder to form rice bran-nano-silver powder; The polyether polyol composition is selected from terminal hydroxyl polyether polyol with a hydroxyl value of 30-50 mg KOH / g, slow resilience polyether polyol with a hydroxyl value of 150-600 mg KOH / g, polymer polyol with a hydroxyl value of 30-60 mg KOH / g, and soybean oil-based polyether polyol with a molecular weight of 2000-2500, and the weight percentages of the four are (30%-60%), (15%-30%), (15%-30%), and (5%-15%).

2. The memory foam containing plant materials according to claim 1, characterized in that: The size of the nano silver powder is 10-60 nanometers.

3. The memory foam containing plant materials according to claim 1, characterized in that: The polyether polyol composition comprises two or more polyether polyols.

4. The memory foam containing plant materials according to claim 1, characterized in that: The auxiliary agents include antioxidants, foam stabilizers, foaming agents, catalysts and surfactants.

5. An application of the memory foam containing plant raw materials according to any one of claims 1 to 4, characterized in that: The memory foam containing plant raw materials is used as a pillow core material of a pillow.

6. A memory foam pillow containing plant materials, comprising a pillowcase and a pillow core, characterized in that: The pillow core is made of the memory foam containing plant materials as described in any one of claims 1 to 4, the pillowcase is divided into three areas, namely the middle headrest area, the first side sleeping areas on both sides, and the second side sleeping areas, the pillow core is correspondingly divided into three parts, namely the middle head pillow core, the first side sleeping pillow core and the second side sleeping pillow core, the middle head pillow core includes a headrest and a shoulder and neck pillow, and the shoulder and neck pillow can be folded into the headrest.

7. A memory foam pillow containing plant materials according to claim 6, characterized in that: The first side sleeping pillow core and the second side sleeping pillow core are both composed of a side sleeping pillow core body and a replaceable module.

8. The memory foam pillow containing plant materials according to claim 7, characterized in that: The side sleeping pillow core body is a sheet-like structure, and when the side sleeping pillow core body is rolled up, it wraps the replaceable module.

9. The memory foam pillow containing plant materials according to claim 7, characterized in that: The side sleeping pillow core body is provided with a plurality of ventilation holes.

Citation Information

Patent Citations

  • Preparation method of nano bamboo charcoal antibacterial fiber

    CN109402754A

  • Anion-producing pillow

    JP2003000413A

  • Setting strength enhancing damage care agent, hair care composition containing the same and hair styling composition

    JP2018131408A

  • Nano silver and contain perfume a pillow

    KR1020060071898A

  • Cosmetic composition of silver coated silica powder and their dispersion having conduct antibacterial activities