Heat treatment method for preparing bimetallic band saw blade and bimetallic band saw blade
By adopting a process of specific temperature and multiple tempering in the heat treatment of bimetallic band saw blades, the problem of overheating of the back material is solved, its fatigue resistance and service life are improved, and the overall performance is improved.
Patent Information
- Application Number
- CN202311450459.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-11-02
AI Technical Summary
The traditional bimetallic band saw blade heat treatment process causes the back material to overheat or overburn, reducing its fatigue performance and service life.
Using insulation platform heating at 760-820℃ and quenching treatment at 1140-1180℃, combined with multiple tempering treatments, the cooling speed and tempering temperature are controlled, the metallographic structure and grain size of the back material are improved, and the fatigue resistance of the back material is improved. performance.
It improves the service life and overall performance of the bimetallic band saw blade, including hardness, plastic toughness and fatigue properties, avoids the problem of coarse grains of the back material in traditional processes, and improves the sawing performance.
Smart Images

Figure CN117568584B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of steel smelting, and specifically relates to a heat treatment method for preparing a bimetallic band saw blade and a bimetallic band saw blade. Background Art
[0002] Bimetallic band saw blades are made by welding two different types of steel with different performances, and then heat treating them. The tip of the teeth of bimetallic band saw blades generally uses high-hardness and high-wear-resistant tooth materials, such as high-speed steel or cemented carbide. The backing material that connects the bimetallic band saw blade to the tooth material generally uses high-strength fatigue-resistant backing material, such as low-alloy spring steel or ultra-high-strength steel. The backing material and tooth material of the bimetallic band saw blade are made by laser or electron beam welding the steel plate raw materials, milling the teeth, and finally heat treating them. Band saw blades for metal cutting have become the main preparation method in the sawing industry because they combine the unique advantages of tooth materials and backing materials and have excellent performance.
[0003] The last final heat treatment of the bimetallic band saw blade in the preparation process is to perform the tooth material and back material at the same time. In order to highlight the high hardness and sharpness of the tooth part, the heat treatment process currently adopted is formulated according to the requirements of high-speed steel, which is the traditional "three-time high quenching", that is, high quenching temperature. Sometimes, in order to pursue higher hardness and dissolve more carbides, the quenching temperature is even close to 1280-1300℃; tempering also adopts the traditional 560℃ and above temperature. This process reduces the service life of the bimetallic band saw blade.
[0004] The above process causes the backing material to overheat or even burn, affecting the performance of the backing. Summary of the invention
[0005] In view of this, the present application provides a heat treatment method for preparing a bimetallic band saw blade and a bimetallic band saw blade, aiming to improve the service life and mechanical properties of the bimetallic band saw blade.
[0006] In a first aspect, an embodiment of the present application provides a heat treatment method for preparing a bimetallic band saw blade, the method comprising:
[0007] The raw saw blade is heated to 760-820° C., kept at 760-820° C. for 80-130 seconds, and then continued to be heated to 1140-1180° C. and kept at 1140-1180° C. for 120-150 seconds, wherein the raw saw blade includes a tooth material and a backing material;
[0008] Then, quenching treatment is performed at a cooling rate of 80 to 100°C / s to obtain a cooled saw blade;
[0009] The cooled saw blade is tempered at least three times to produce a bimetallic band saw blade.
[0010] In some embodiments, the backing material includes the following chemical composition in mass percentage: C: 0.30% to 0.35%, Cr: 3.00% to 3.25%, Ni: 0.25% to 1.00%, Mo: 1.80% to 2.25%, Si: 0.30% to 0.50%, Mn: 0.60% to 1.00%, V: 0.30% to 0.50%, and the remainder is iron and unavoidable impurity elements.
[0011] In some embodiments, the thickness of the backing material is 0.8-1.3 mm.
[0012] In some embodiments, the metallographic structure of the backing material includes 100% spheroidized pearlite structure by volume percentage.
[0013] In some embodiments, the quenching temperature during the quenching treatment is 1140-1180°C.
[0014] In some embodiments, the temperature of any one tempering is 620-640°C.
[0015] In some embodiments, the holding time of any tempering is 180s to 300s.
[0016] In some embodiments, the number of tempering is 3 to 4 times.
[0017] In a second aspect, an embodiment of the present application provides a bimetallic band saw blade produced by the method of the first aspect.
[0018] In some embodiments, the torsional fatigue life of the bimetallic band saw blade is more than 6250 times, and the mechanical properties of the bimetallic band saw blade include: the hardness of the saw blade backing material is 450HV~500HV; the elongation of the saw blade backing material is more than 12%, the yield strength is ≥1100MPa, and the tensile strength is ≥1500MPa.
[0019] This application has at least the following beneficial effects:
[0020] The preparation method provided in the present application can ensure the hardness and sawing performance of the tooth tip and tooth material by setting an insulation platform within the temperature range of 760 to 820°C and controlling the processes and parameters of related heat treatments such as heating, quenching and tempering. It can also improve the performance of the back material of the bimetallic band saw blade, avoid the coarse grains caused by traditional processes, reduce the impact of the fatigue performance of the back material, increase the service life of the bimetallic band saw blade, and also improve the overall performance of the bimetallic band saw blade such as hardness, plasticity, toughness, fatigue performance and sawing performance to the optimal level. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solution of the implementation regulations of this application, the following is a brief introduction to the drawings required for use in the embodiments of this application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0022] Figure 1 A schematic diagram showing the relationship between temperature and time in a heat treatment method for preparing a bimetallic band saw blade according to an embodiment of the present application is shown. DETAILED DESCRIPTION
[0023] In order to make the application purpose, technical solution and beneficial technical effect of this application clearer, the application is further described in detail below in conjunction with the embodiments. It should be understood that the implementation regulations described in this specification are only for explaining this application, not for limiting this application.
[0024] For simplicity, the present application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.
[0025] In the description of the present application, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number, and the “multiple” in “one or more” means two or more than two.
[0026] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided through a series of embodiments, and these implementation regulations can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0027] The last step in the process of making bimetallic band saw blades is heat treatment. That is, heat treatment of the saw blade containing the tooth material and the back material, and the heat treatment treats the tooth material and the back material at the same time. In order to highlight the high hardness and sharpness of the teeth, the heat treatment process currently used is formulated according to the requirements of high-speed steel, which is the traditional "three-time high quenching", that is, high quenching temperature. Sometimes, in order to pursue higher hardness and dissolve more carbides, the quenching temperature is even close to 1280-1300℃; tempering also adopts the traditional 560℃.
[0028] The traditional "three-time high quenching" process often causes overheating or even overburning of backing materials such as low-alloy spring steel or ultra-high strength steel in actual production. The coarse grains in the backing material seriously affect the fatigue performance and reduce the service life of the bimetallic band saw blade.
[0029] In view of this, the present application provides a suitable heat treatment process for bimetallic band saw blades that ensures that the performance of the tooth material meets the requirements of the back material, so as to improve the overall performance of the band saw blades.
[0030] Heat treatment method for preparing bimetallic band saw blades
[0031] In a first aspect, an embodiment of the present application provides a heat treatment method for preparing a bimetallic band saw blade, the method comprising:
[0032] The raw saw blade is heated to 760-820° C., kept at 760-820° C. for 80-130 seconds, and then continued to be heated to 1140-1180° C. and kept at 1140-1180° C. for 120-150 seconds, wherein the raw saw blade includes a tooth material and a backing material;
[0033] Then, quenching treatment is performed at a cooling rate of 80 to 100°C / s to obtain a cooled saw blade;
[0034] The cooled saw blade is tempered at least three times to produce a bimetallic band saw blade.
[0035] According to the embodiments of the present application, the method of the present application can ensure the hardness and sawing performance of the tooth material, and can also improve the performance of the back material of the bimetallic band saw blade, avoid the coarseness of the grains caused by traditional processes, reduce the impact on the fatigue performance of the back material, and increase the service life of the bimetallic band saw blade. It also improves the overall performance of the bimetallic band saw blade, such as hardness, plasticity, and fatigue performance and sawing performance to reach the optimal level.
[0036] The raw material saw blade including the tooth material and the back material can be understood as the raw material purchased from the steel mill, which has not been processed yet and cannot be used as a saw blade.
[0037] According to the embodiment of the present application, during the heating process, a heat preservation platform is set, that is, the temperature is kept at 760-820°C for a specific time, which can be understood as a preliminary heat treatment. The preliminary heat treatment plays a role of recrystallization annealing, and is designed for the segregated banded structure of the cold-rolled strip used in the saw blade. Through recovery and recrystallization, the rolling stress of the strip is eliminated, and the structure is transformed into recrystallized equiaxed grains. At the same time, the carbonitrides of the microalloy V and Ti can be dispersed and precipitated to prepare for subsequent quenching, and it is also beneficial to stabilize the carbides (such as iron carbide and chromium carbide, etc.) in the tooth material to achieve solid solution.
[0038] According to the embodiments of the present application, controlling the relevant parameters of the heat treatment process can affect the hardness and strength of the backing material of the bimetallic band saw blade, and affect the metallographic structure and grain size of the backing material, such as the distribution of carbides and the formation of precipitation phases, thereby improving the hardness and fatigue resistance of the backing material while ensuring the hardness of the tooth tip and sawing performance.
[0039] According to the embodiment of the present application, the cooling rate of quenching is controlled within the above range. When the back material is in a hardened state, it is beneficial to the fatigue resistance of the back, and it is beneficial to improve the sawing performance of the tooth material to obtain highly saturated solid solution martensite and improve the hardness of the tooth tip part.
[0040] See also Figure 1 , a schematic diagram of the heat treatment in the heat treatment method for preparing a bimetallic band saw blade of the present application, wherein the temperature of t1 is 620-640°C, the temperature of t2 is 760-820°C, and the temperature of t3 is 1140-1180°C.
[0041] According to the embodiment of the present application, the heat treatment process of the back material of the bimetallic band saw blade can significantly improve the strength and plasticity of the back material steel, and is particularly suitable for steel bands for the back of saw blades such as spring steel and high-strength steel.
[0042] In some embodiments, the backing material includes the following chemical composition in mass percentage: C: 0.30% to 0.35%, Cr: 3.00% to 3.25%, Ni: 0.25% to 1.00%, Mo: 1.80% to 2.25%, Si: 0.30% to 0.50%, Mn: 0.60% to 1.00%, V: 0.30% to 0.50%, and the remainder is iron and unavoidable impurity elements.
[0043] The components in the backing material of the present application are closely related to the heat treatment process of the present application. On the one hand, the plastic toughness of the steel is ensured, and on the other hand, there is enough carbon to form Cr, Mo, and V carbides, which is beneficial to the improvement of fatigue performance.
[0044] C: Carbon is a basic element in steel. It is an austenite-forming element and also a strengthening element for martensite and ferrite. The increase in carbon content significantly increases the hardness of steel while reducing its plasticity and toughness. In alloy steel, carbon can react with alloying elements such as Cr, Mo, and V in steel to form various types of carbides such as M23C6, M6C, and M2C. If these carbides can be distributed in a fine and dispersed manner, the grains can be refined while precipitation strengthening occurs, thereby improving the strength and toughness of the material.
[0045] The present invention controls the C content within a medium-low carbon range, which ensures the plasticity and toughness of the steel on the one hand, and on the other hand has a sufficient amount of carbon to form Cr, Mo, and V carbides, which is beneficial to the improvement of fatigue performance.
[0046] Chromium can significantly improve the hardenability and tempering stability of steel, ensuring the high-temperature tempering heat treatment process performance of the bimetallic band saw blade backing material; Cr can greatly increase the tough-brittle transition temperature of steel and improve the wear resistance of steel. During the tempering process, Cr combines with carbon to precipitate carbides such as (Fe, Cr)23C6 and Cr23C6, which play a pinning role on the grain boundaries.
[0047] The present invention controls the Cr content within a relatively high range to ensure the tempering stability of the steel, a high ductile-brittle transition temperature, and improve the brittle fracture resistance of the bimetallic band saw blade.
[0048] Ni: It has a lattice constant similar to that of γ-iron and can form a continuous solid solution, which is beneficial to improving the hardenability and hardenability of steel. Nickel can improve the strength of steel while maintaining good plasticity and toughness, and has rust prevention and heat resistance at high temperatures. However, since nickel is a scarce resource and chromium-nickel steel is susceptible to temper brittleness and white spots, its content is selected within the above-mentioned appropriate range.
[0049] Mo: The most obvious effect of molybdenum is to improve the tempering stability of steel. When it coexists with chromium, manganese, etc., molybdenum inhibits the tempering brittleness caused by other elements. In addition, Mo has a solid solution strengthening effect on ferrite, and also improves the stability of carbides, thereby increasing the strength of steel. Molybdenum plays a beneficial role in improving the ductility, toughness and wear resistance of steel.
[0050] The steel of the present invention increases the content of Mo to a certain range, mainly for the high quenching and high tempering heat treatment of the bimetallic band saw blade, which easily causes the steel to form an overheated structure, especially when the tempering temperature is below the high temperature temper brittleness. Therefore, the role of Mo in inhibiting temper brittleness is extremely important in the steel used as the back material of the bimetallic band saw blade. The price of Mo is relatively expensive, and Mo promotes decarburization, so it is not good for high temperature quenching, so the optimized quality range is selected.
[0051] Si: Silicon is added as a reducing agent and deoxidizer during the steelmaking process. Silicon can significantly increase the elastic limit, yield point and tensile strength of steel. Silicon combined with molybdenum, tungsten, chromium, etc. can improve corrosion resistance and oxidation resistance. However, too much silicon will reduce the welding performance of steel, so the appropriate range is selected.
[0052] Mn: In the steelmaking process, manganese is a good deoxidizer and desulfurizer. Generally, steel contains 0.30-0.50% manganese. This steel slightly increases the content of Mn. Compared with ordinary steel, it not only has sufficient toughness, but also has higher strength and hardness, improves the hardenability of steel, and improves the hot working performance of steel. However, too high Mn content will weaken the corrosion resistance of steel and reduce welding performance.
[0053] V: Since vanadium and carbon can form stable and refractory carbides, the steel can maintain a fine-grained structure at higher temperatures, greatly reducing the overheating sensitivity of the steel. The dispersed VC carbides can improve the hardness and wear resistance of tool steel.
[0054] A small amount of V is added to the steel of the present invention for microalloying, and its fine grain structure and reduced overheating sensitivity of the steel play a positive role in improving the fatigue performance of the bimetallic band saw blade.
[0055] In some embodiments, the thickness of the backing material is 0.8-1.3 mm. The thickness of the backing material is also closely related to the heat treatment process and can affect the hardness, fatigue resistance, etc. of the backing material after heat treatment.
[0056] In some embodiments, the metallographic structure of the backing material includes 100% spheroidized pearlite structure by volume percentage.
[0057] According to the embodiment of the present application, the volume fraction of the metallographic structure of the back material is within the above range, which is beneficial to controlling the hardness of the back and improving the anti-fatigue performance.
[0058] In some embodiments, the quenching temperature during the quenching treatment is 1140-1180°C.
[0059] According to the embodiment of the present application, the quenching temperature is within the above range, which promotes the full solid solution of carbides in the tip part and back steel of the saw blade, and prepares the composition for subsequent tempering and secondary hardening.
[0060] In some embodiments, the temperature of any one tempering is 620-640°C.
[0061] In some embodiments, the holding time of any tempering is 180s to 300s.
[0062] In some embodiments, the number of tempering is 3 to 4 times.
[0063] According to the embodiment of the present application, controlling the tempering temperature and tempering time within the above range is conducive to eliminating the residual austenite at the tip of the tooth, fully precipitating carbides, and fully realizing secondary hardening and secondary quenching. At the same time, the metallographic structure of the back material is a quenched and tempered troostite structure, which can achieve good comprehensive mechanical properties. Air cooling can be used between each tempering, and it is ensured to be fully cooled to room temperature.
[0064] In a second aspect, an embodiment of the present application provides a bimetallic band saw blade produced by the method of the first aspect.
[0065] In some embodiments, the torsional fatigue life of the bimetallic band saw blade is more than 6250 times, and the mechanical properties of the bimetallic band saw blade include: the hardness of the saw blade backing material is 450HV~500HV; the elongation of the saw blade backing material is more than 12%, the yield strength is ≥1100MPa, and the tensile strength is ≥1500MPa.
[0066] In the embodiment of the present application, the saw blade backing material is a material that has been processed as described above, and the saw blade can be used normally at this time, wherein the metallographic structure of the saw blade backing material includes tempered troostite and original austenite; and the grain size thereof is level 8-9.
[0067] Example
[0068] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations may be made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0069] Example 1
[0070] A heat treatment method (heat treatment process) for preparing a bimetallic band saw blade, comprising:
[0071] A raw saw blade is provided, including a tooth material and a back material. The chemical composition of the tooth material, calculated by mass percentage, includes: C, 1.07%, Si, 0.58%, Mn, 0.31%, Cr, 3.72%, Mo, 9.27%, V, 1.15%, W, 1.31%, Co, 7.88%, and the balance is iron and inevitable impurities; the chemical composition of the back material, calculated by mass percentage, includes: C, 0.31%, Cr, 3.05%, Ni, 0.29%, Mo, 1.83%, Mn, 0.66%, V, 0.34%, and the balance is iron and inevitable impurities.
[0072] Heating and insulation treatment: After placing the sample in the heating furnace, the first insulation temperature is 780℃, and the insulation time is 100s. After the first insulation stage, the temperature continues to rise to 1150℃, and the total time is less than 20min. Then the back steel sample is placed in the heating furnace for 120s.
[0073] Quenching treatment: Set the quenching temperature to 1150℃, put the steel strip with a length of 90mm, a width of 40mm and a thickness of 1.3mm into the resistance furnace, then take it out and put it into the quenching tank for oil cooling quenching, and cool it to room temperature. During oil cooling, the oil temperature is controlled below 30℃, the oil cooling time is 100s, and the cooling rate is 91℃ / s.
[0074] Tempering treatment: within half an hour after quenching, after the quenched sample has cooled to room temperature, place the sample in a resistance furnace for tempering treatment, and air cool to room temperature, repeat the tempering treatment three times; the uniformity of the resistance furnace temperature for tempering treatment is less than or equal to ±2°C; during tempering treatment, the temperature is raised to 620°C within 20 minutes, and then the sample is placed in a heating furnace, and the holding time for tempering treatment is 200 seconds; after the tempering treatment is completed, the time for air cooling the sample to room temperature is 25 minutes.
[0075] After the tempering treatment, the properties of the samples were tested: the hardness of the backing material was 492HV, the yield strength and tensile strength were 1244MPa and 1590MPa respectively, and the elongation was 12.0%.
[0076] Example 2
[0077] A heat treatment method (heat treatment process) for preparing a bimetallic band saw blade, comprising:
[0078] A raw saw blade is provided, including a tooth material and a back material. The chemical composition of the tooth material, calculated by mass percentage, includes: C, 1.07%, Si, 0.58%, Mn, 0.31%, Cr, 3.72%, Mo, 9.27%, V, 1.15%, W, 1.31%, Co, 7.88%; the chemical composition of the back material, calculated by mass percentage, includes: C, 0.31%, Cr, 3.05%, Ni, 0.29%, Mo, 1.83%, Mn, 0.66%, V, 0.34%, and the balance is iron and inevitable impurities.
[0079] Heating and insulation treatment: Put a steel strip with a specification of 90mm in length, 40mm in width and 1.1mm in thickness into a resistance furnace. After placing the sample in a heating furnace, heat it to 800℃ and keep it for 100s. After that, the temperature continues to rise to 1160℃. The total time is within 20min. Then, place the back steel sample in a heating furnace for 120s.
[0080] Quenching treatment: Place the backing steel sample in a heating furnace for heating; then put the sample into a quenching tank at a temperature of 1160°C for oil-cooling quenching and cool to room temperature; the cooling rate is 85°C / s. The temperature uniformity of the sample box heating furnace is less than or equal to ±5°C. During quenching treatment, the oil temperature is controlled at 28°C during oil cooling, and the oil cooling time is 120s;
[0081] Tempering treatment: After the quenched sample is cooled to room temperature, the sample is placed in a resistance furnace for tempering treatment, and air-cooled to room temperature. The tempering experiment is repeated three times in the same way. The temperature is raised to 640°C within 20 minutes; the holding time of the tempering treatment is 240 seconds; the time for air cooling the sample to room temperature after the tempering treatment is completed is 30 minutes.
[0082] After the tempering treatment, the properties of the samples were tested: the hardness of the backing material was 495HV, the yield strength and tensile strength were 1157MPa and 1500MPa respectively, and the elongation was 12.6%.
[0083] Example 3
[0084] A heat treatment method (heat treatment process) for preparing a bimetallic band saw blade, comprising:
[0085] A raw saw blade is provided, including a tooth material and a back material. The chemical composition of the tooth material, calculated by mass percentage, includes: C, 1.05%, Si, 0.59%, Mn, 0.30%, Cr, 3.75%, Mo, 9.23%, V, 1.19%, W, 1.26%, Co, 7.92%; the chemical composition of the back material, calculated by mass percentage, includes: C, 0.31%, Cr, 3.13%, Ni, 0.28%, Mo, 1.85%, Mn, 0.65%, V, 0.34%, and the balance is iron and inevitable impurities.
[0086] Heating and insulation treatment: After placing the sample in a heating furnace, the temperature is raised to 820°C and the insulation time is 130s. After the end, the temperature continues to rise to 1180°C. A steel strip with a length of 100mm, a width of 100mm and a thickness of 1.5mm is placed in a resistance furnace, and the temperature is kept for 150s, and then taken out for oil cooling.
[0087] Quenching treatment: The backing steel sample is placed in a heating furnace for heating; then the sample is put into a quenching tank from a temperature of 1180°C for oil quenching at a cooling rate of 96°C / s until it is cooled to room temperature.
[0088] Tempering treatment: After the quenched sample is cooled to room temperature, it is placed in a resistance furnace set at 640 °C for 300 s, then air-cooled to room temperature. The tempering experiment is repeated three times in the same way.
[0089] After the tempering treatment, the properties of the samples were tested: the hardness of the backing material was 497HV, the yield strength and tensile strength were 1186MPa and 1584MPa respectively, and the elongation was 13.4%.
[0090] Comparative Example 1
[0091] The present application is different from Example 1 in that the heating and heat preservation treatment and the quenching treatment are different. The temperature is directly heated to 1280°C, and there is no heat preservation stage during the heating process. The quenching treatment is then carried out at a temperature of 1280°C, and the cooling rate is 85°C / s.
[0092] The tempering treatment is the same as in Example 1.
[0093] Comparative Example 2
[0094] The difference between this application and Example 2 is that the heating and heat preservation treatment and the quenching treatment are different. The temperature is directly heated to 1300°C, and then quenched. There is no heat preservation stage during the heating process, and the cooling rate is 88°C / s. The tempering treatment is the same as that of Example 1.
[0095] Test Section
[0096] The bimetallic band saw blades prepared in the examples and comparative examples were sampled according to GB / T 2975 “Sampling location and specimen preparation for mechanical properties test of steel and steel products”.
[0097] (1) Metallographic structure observation:
[0098] Use nitric acid alcohol corrosion reagent, drop 1-2 drops of reagent on the surface of the steel plate, and stay on the sample surface for a short time until the sample surface turns dark from the mirror image. After rinsing with alcohol, quickly process it on absorbent paper, and finally blow dry it with a hair dryer to determine the organization type under a metallographic microscope. The metallographic structure of the back material of the heat-treated bimetallic band saw blade of Example 1-3 is tempered troostite and original austenite; the grain size is 9 levels, and the metallographic structure of the back material of the heat-treated bimetallic band saw blade of Comparative Example 1-3 is tempered troostite and original austenite; the grain size is 7.5 levels.
[0099] (2) Mechanical properties testing:
[0100] According to GB / T228.1-2010 "Metallic material tensile test part 1 room temperature test method", the bimetallic band saw blades prepared in the embodiment and the comparative example were sampled, and the test results of the samples are shown in Table 2;
[0101] The tensile test was carried out using a German Zwick tensile testing machine with a load range of 50 to 1500 kN and a displacement speed of 2 mm / min. The tensile strength, yield limit, elongation and other test data of the material were obtained by computer output. The test results are shown in Table 3.
[0102] (3) Hardness test: According to the hardness standard: GB / T 4340.1-2009 Metallic material Vickers hardness test Part 1: Test method, the backing materials of the bimetallic band saw blades prepared in the examples and comparative examples were tested.
[0103] (4) Torsional fatigue life testing method: According to the internally developed tension-torsion fatigue testing machine testing method, the fatigue stress was set to 380 MPa and the frequency was 1 Hz. The backing materials of the bimetallic band saw blades prepared in the examples and comparative examples were tested.
[0104] Table 3 Mechanical properties of bimetallic band saw blade backing materials of embodiments and comparative examples
[0105]
[0106] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto, and any modification or replacement of the present technology should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A heat treatment method for preparing a bimetallic band saw blade, characterized in that: The method comprises: The raw saw blade is heated to 760-820° C., kept at 760-820° C. for 80-130 seconds, and then continued to be heated to 1140-1160° C. and kept at 1140-1160° C. for 120-150 seconds, wherein the raw saw blade comprises a tooth material and a backing material; the backing material comprises the following chemical composition in mass percentage: C: 0.30%-0.35%, Cr: 3.00%-3.25%, Ni: 0.25%-1.00%, Mo: 1.80%-2.25%, Si: 0.30%-0.50%, Mn: 0.60%-1.00%, V: 0.30%-0.50%, and the remainder is iron and unavoidable impurity elements; Then, quenching treatment is performed at a cooling rate of 80 to 100°C / s to obtain a cooled saw blade; The cooled saw blade is tempered at least three times to obtain the bimetallic band saw blade; the holding time of any tempering is 180s to 300s; and the temperature of any tempering is 620 to 640°C.
2. The heat treatment method according to claim 1, characterized in that The thickness of the backing material is 0.8-1.3 mm.
3. The heat treatment method according to claim 1, characterized in that: The metallographic structure of the backing material includes 100% spheroidized pearlite structure in terms of volume percentage.
4. The method according to claim 1, characterized in that: The quenching temperature during the quenching treatment is 1140-1160°C.
5. The method according to claim 1, characterized in that The number of tempering is 3 to 4 times.
6. A bimetallic band saw blade, characterized in that: Prepared by the method according to any one of claims 1 to 5.
7. The bimetallic band saw blade according to claim 6, characterized in that: The torsional fatigue life of the bimetallic band saw blade is more than 6250 times, and the mechanical properties of the bimetallic band saw blade include: the hardness of the saw blade backing material is 450HV~500HV; the elongation of the saw blade backing material is more than 12%, the yield strength is ≥1100MPa, and the tensile strength is ≥1500MPa.