A kind of degradable starch hydrogel microsphere and preparation method thereof

By using a starch hydrogel material with a core-shell structure in the embolization microspheres and utilizing the difference in degradation speed between the core and the shell layer, the degradation time of the microspheres can be controlled and the risk of inflammation can be reduced, solving the problem of incompatible degradation time in the existing technology. It can control the problem of inflammatory response and is suitable for the treatment of various blood vessel diameters.

CN117717646BActive Publication Date: 2024-10-29CARDIOLINK SCI (SHENZHEN) MEDICAL TECH DEV CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311733208.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-10-29
Estimated Expiration
2043-12-15

AI Technical Summary

Technical Problem

Existing embolization microspheres have problems with uncontrollable degradation time and inflammatory reaction in tumor treatment, resulting in poor embolization effect or premature degradation, and cannot meet the treatment needs of different blood vessel diameters.

Method used

Degradable starch hydrogel microspheres with a core-shell structure are used. By selecting different degradation rates of the core material and shell material, the degradation time of the microspheres can be controlled. The shell layer degrades before the core to prolong the embolization effect, and in the core Decomposes rapidly after complete degradation to reduce the risk of inflammation.

Benefits of technology

It achieves better degradation time control of microspheres during the embolization process, prolongs the embolization effect and reduces the risk of inflammation, and is suitable for the treatment needs of different blood vessel diameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117717646B_ABST
    Figure CN117717646B_ABST
Patent Text Reader

Abstract

A degradable starch hydrogel microsphere and a preparation method thereof, belonging to the technical field of embolic microspheres; the microspheres have a core-shell structure, and the degradation rate of the core material of the microspheres is greater than the degradation rate of the shell material of the microspheres; by using microspheres with a core-shell structure, and the degradation of the shell layer of the core-shell structure precedes the degradation of the core layer, the microspheres can have a good embolic effect during the period when the shell layer is completely degraded, and then the core is rapidly degraded, thereby reducing the possibility of inflammation during the embolic treatment process, and the degradation time of the embolic microspheres can be controlled through the difference in degradation rates between the shell layer and the core.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of embolic microspheres, and in particular to a degradable starch hydrogel microsphere and a preparation method thereof. Background Art

[0002] Embolization was originally developed by Sadek Hilal in 1968 as a minimally invasive surgical technique. Its purpose is to block blood flow to a certain area of ​​the body, which can effectively shrink tumors or block aneurysms. It is currently used in the treatment of various malignant and benign tumors. Different indications have different requirements for the size and material of embolic agents, so the choice of embolic agents plays a vital role in the treatment of interventional embolization.

[0003] At present, the main embolic agents used in clinical practice are non-degradable. They have embolic and drug-carrying functions, and their effectiveness and performance have been confirmed in clinical literature. However, there are still the following problems in clinical application: (1) Collateral circulation problem: Since the non-degradable microsphere embolization time is long, after the target artery supplying the tumor is blocked, the blood vessels of the original anastomotic branches in this area expand to form bypasses, causing blood to bypass these bypasses, restoring circulation so that the cancer cell area can get enough blood supply again without necrosis and loss of embolic function. (2) Carrier residence time problem: For non-biodegradable embolic agents, the microspheres remain in the body after the drug is completely released, and patients usually express concerns about foreign matter remaining in the body.

[0004] As for degradable embolic microspheres, there are only a few reports, and in practical applications, these degradable microsphere products have many limitations. For example, the starch microsphere products launched by PharmaCept The vascular embolization time is short (degradation half-life is 30-40 minutes), and it may not cause tumor necrosis. At the same time, the particle size is single (the product currently has only one particle size specification of 50μm±7μm), which cannot meet the requirements of embolization treatment of blood vessels of different diameters in various parts. Teleflex has developed and marketed gelatin degradable microsphere products (Gel-Bead TM ) includes several particle sizes of 100-300μm, 300-500μm, 500-700μm and 700-1000μm, which can meet most clinical use needs. However, its degradation performance in the body is affected by many factors (such as type, uniformity, enzymes, local inflammatory response, etc.), making it difficult to standardize measurement. IMBiotechnologies' biodegradable microspheres - (Also known as ), whose main component is a copolymer of D, L-lactic acid and glycolic acid (PLGA), which is coated with a layer of type I bovine fibrillar collagen. It still takes more than several months for it to degrade in the body, and there is an inflammatory response during the treatment process. It can be seen that the current biodegradable microsphere products all have the problem of uncontrollable degradation time. Summary of the invention

[0005] The present application provides a degradable starch hydrogel microsphere and a preparation method thereof, which can realize controllable degradation time of the embolic microsphere.

[0006] In a first aspect, an embodiment of the present application provides a degradable starch hydrogel microsphere, wherein the microsphere has a core-shell structure, and the degradation rate of the inner core material of the microsphere is greater than the degradation rate of the shell material of the microsphere.

[0007] In the above implementation process, by using microspheres with a core-shell structure, and the degradation of the shell layer of the core-shell structure precedes the degradation of the core, the microspheres can have a good embolic effect during the period of complete degradation of the shell layer, and then the core is rapidly degraded, thereby reducing the possibility of inflammation during the embolic treatment process. The degradation time of the embolic microspheres can be controlled through the difference in degradation speed between the shell layer and the core.

[0008] As an optional embodiment, the core material of the microspheres includes a soluble starch polymer; and / or

[0009] The shell material of the microspheres includes pullulan polymer.

[0010] In the above implementation process, different starch materials have different degradation rates, and the degradation rate of the material is usually negatively correlated with the degradation time. Selecting soluble starch as the core material can make the core degrade quickly after the shell of the microsphere is completely degraded, which is beneficial to reduce the occurrence of inflammation during embolization treatment. Selecting amylopectin as the shell material can help the microsphere maintain a good embolization effect.

[0011] As an optional embodiment, in the microspheres, the mass ratio of the core material to the shell material is (1-5): (1-5).

[0012] In the above implementation process, the mass proportion of the shell material is positively correlated with the degradation time of the entire microsphere, and the degradation time of the entire microsphere can be controlled by adjusting the mass ratio of the core material and the shell material.

[0013] In a second aspect, the present application provides a method for preparing degradable starch hydrogel microspheres, the method comprising:

[0014] The microsphere skeleton material is prepared into an aqueous phase, wherein the microsphere skeleton material comprises a core material and a shell material, the degradation rate of the core material is greater than the degradation rate of the shell material, and the hydrophilicity of the core material is greater than that of the shell material;

[0015] The water phase and the oil phase are mixed to form an inverse suspension polymerization system, and then a polymerization reaction is carried out to obtain microspheres.

[0016] In the above implementation process, two materials with different hydrophilicity are used as microsphere skeleton materials, and microspheres are prepared by reverse suspension polymerization, which will naturally form a core-shell structure, and the preparation of microspheres with a core-shell structure can be realized relatively simply. In addition, the degradation of the shell layer of the core-shell structure precedes the degradation of the core, so that the microspheres can have a good embolization effect during the period when the shell layer is completely degraded, and then the core is rapidly degraded, reducing the possibility of inflammation during the embolization treatment process. Through the difference in degradation speed between the shell layer and the core, the degradation time of the embolization microspheres can be controlled.

[0017] As an optional embodiment, the core material of the microspheres includes a soluble starch polymer; and / or

[0018] The shell material of the microspheres includes pullulan polymer.

[0019] In the above implementation process, different starch materials have different degradation rates, and the degradation rate of the material is usually negatively correlated with the degradation time. Selecting a soluble starch polymer as the core material can make the core degrade quickly after the shell of the microsphere is completely degraded, which is beneficial to reduce the occurrence of inflammation during embolization therapy. Selecting a branched-chain starch polymer as the shell material can help the microsphere maintain a good embolization effect.

[0020] As an optional implementation, during the preparation process, the mass ratio of the core material to the shell material is (1-5): (1-5).

[0021] In the above implementation process, the mass proportion of the shell material is positively correlated with the degradation time of the entire microsphere, and the degradation time of the entire microsphere can be controlled by adjusting the mass ratio of the core material and the shell material.

[0022] As an optional embodiment, the aqueous phase includes microsphere skeleton material, sodium trimetaphosphate and sodium tripolyphosphate.

[0023] As an optional embodiment, the polymerization reaction includes a first-stage reaction and a second-stage reaction; the temperature of the first-stage reaction is 60-80°C; the time of the first-stage reaction is 2-4 hours; the temperature of the second-stage reaction is 60-80°C; the time of the second-stage reaction is 18-24 hours.

[0024] As an optional implementation, sodium trimetaphosphate and sodium tripolyphosphate are added during the second-stage reaction.

[0025] In the above implementation process, the addition of sodium trimetaphosphate and sodium tripolyphosphate in the second-stage reaction process is more conducive to the formation of the microsphere core-shell structure.

[0026] As an optional embodiment, the oil phase includes cyclohexane, Span-60 and Tween-60.

[0027] As an optional embodiment, during the reverse polymerization process, the mass ratio of sodium trimetaphosphate to sodium tripolyphosphate is (5-10):1.

[0028] As an optional implementation, during the reverse polymerization process, the mass ratio of Span-60 to Tween-60 is (1-3): (0.5-1.5). BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] Figure 1 A flowchart of a method provided in an embodiment of the present application;

[0032] Figure 2 A schematic diagram of the degradation rate of microspheres provided in Comparative Example 1 of the present application;

[0033] Figure 3 A schematic diagram of the degradation rate of the microspheres provided in Examples 1 to 5 of the present application;

[0034] Figure 4 This is an image of the microspheres provided in Example 1 of the present application under an optical microscope;

[0035] Figure 5 This is an image of the microspheres provided in Example 2 of the present application under an optical microscope. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0038] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0039] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0040] At present, the skeleton material of degradable microspheres is basically a single component, and its degradation rate during embolization therapy remains basically unchanged. Some microspheres still need a long time to be completely degraded after the embolization therapy takes effect, resulting in inflammatory response during the treatment process, while some microspheres degrade quickly, resulting in complete degradation after the embolization therapy takes effect, or even degradation occurs before the embolization therapy effect is achieved, resulting in a poor embolization therapy effect.

[0041] The inventor intends to provide an embolic microsphere with controllable degradation time, so as to achieve slower degradation in the early stage and better embolic effect, and faster degradation in the later stage and reduce the probability of inflammation.

[0042] The embodiment of the present application provides a degradable starch hydrogel microsphere, the microsphere having a core-shell structure, and the degradation rate of the core material of the microsphere is greater than the degradation rate of the shell material of the microsphere.

[0043] The degradation rate test method can be: take 1 mL of microspheres, add them to 9 mL of PBS (PH = 7.4), incubate them on a shaker at 37°C, take 0.5 mL after different time intervals T, mix and dilute to 1 mL, use DLS method to analyze the average particle size, and calculate the average particle size according to D T The degradation rate was calculated by the ratio of D0:D1.

[0044] The microspheres have a core-shell structure, and the degradation of the shell layer of the core-shell structure precedes the degradation of the core layer, so that the microspheres can have a good embolization effect during the period of complete degradation of the shell layer, and then the core layer degrades rapidly, reducing the possibility of inflammation during the embolization treatment process. The degradation time of the embolic microspheres can be controlled by the difference in degradation speed between the shell layer and the core layer.

[0045] Furthermore, the core material of the microsphere includes a soluble starch polymer; the shell material of the microsphere includes a branched starch polymer. Different starch materials have different degradation rates, and the degradation rate of the material is usually negatively correlated with the degradation time. Selecting a soluble starch polymer as the core material can make the core degrade quickly after the shell of the microsphere is completely degraded, which is beneficial to reduce the occurrence of inflammation during embolization therapy. Selecting a branched starch polymer as the shell material can help the microsphere maintain a good embolic effect. Exemplarily, the branched starch polymer can be specifically selected from corn branched starch, potato branched starch, sweet potato branched starch, etc. The extraction of corn branched starch can be carried out by the following method: accurately weigh 100g of purchased corn starch, add 3000mL of dimethyl sulfoxide (DMSO) and stir it at 200RPM for 24 hours at room temperature. After stirring, centrifuge at 2000RPM, take the supernatant and add it to 2 times the amount of n-butanol, stand for 24 hours, centrifuge at 4000RPM, wash the precipitate with n-butanol 3 times, remove dimethyl sulfoxide (DMSO) and filter, boil and dissolve the filter cake with sufficient distilled water, cool to 60°C, add 10g thymol and stir well, stand at room temperature for 3 days, and filter to obtain a filtrate. Precool the filtrate in a 4°C refrigerator, then add an appropriate amount of ether to extract 3 times to remove thymol, take the aqueous phase, add a large amount of ethanol until the flocculent precipitate no longer increases, stand at room temperature for 3 days, filter to obtain a filter cake, and dry it to obtain a white powder, which is the extracted corn amylopectin.

[0046] The shell thickness of the microsphere can be adjusted according to actual needs (usually the more shell material is used, the thicker the shell is). The thickness of the shell is positively correlated with the degradation time of the entire microsphere. The thicker the shell, the longer the degradation time of the entire microsphere. The degradation time of the microsphere can be regulated by controlling the shell thickness of the microsphere. At the same time, the diameter of the microsphere can also be adjusted according to actual needs, and different embolization treatments can be applied by controlling the diameter of the microsphere.

[0047] In some embodiments, in the microsphere, the mass ratio of the core material to the shell material is (1-5): (1-5). The mass ratio of the shell material is positively correlated with the degradation time of the entire microsphere, and the degradation time of the entire microsphere can be controlled by regulating the mass ratio of the core material to the shell material. Exemplarily, the mass ratio of the core material to the shell material can be 1:1, 1:2, 1:3, 1:4, 1:5, 2:1, 2:3, 2:5, 3:1, 3:2, 3:4, 3:5, 4:1, 4:3, 4:5, 5:1, 5:2, 5:3 or 5:4, etc., and it can also be any value within the range of (1-5): (1-5).

[0048] Figure 1 A flowchart of the method provided in the embodiment of the present application, such as Figure 1 As shown, the present application embodiment also provides a method for preparing degradable starch hydrogel microspheres, the method comprising:

[0049] S1. The microsphere skeleton material is formulated into an aqueous phase, wherein the microsphere skeleton material includes a core material and a shell material, the degradation rate of the core material is greater than the degradation rate of the shell material, and the hydrophilicity of the core material is greater than that of the shell material;

[0050] In some embodiments, the core material of the microsphere includes soluble starch, and the shell material of the microsphere includes amylopectin. The core material and the shell material can be first prepared into solutions respectively. During the preparation process, the mass ratio of the core material and the shell material is (1-5): (1-5). Exemplarily, 1. Preparation of corn amylopectin solution: add 10g corn amylopectin and 1g NaOH to 100ml distilled water, stir and heat until gelatinization is transparent, and let it stand and cool for use. 2. Preparation of soluble starch solution: add 10g soluble starch and 1g NaOH to 100ml distilled water, stir and heat until gelatinization is transparent, and let it stand and cool for use.

[0051] In some embodiments, the aqueous phase includes a microsphere skeleton material, sodium trimetaphosphate and sodium tripolyphosphate. Further, the mass ratio of sodium trimetaphosphate to sodium tripolyphosphate is (5-10):1. Exemplarily, the mass ratio of sodium trimetaphosphate to sodium tripolyphosphate can be 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, etc., and it can also be any value within the range of (5-10):1.

[0052] Specifically, in this embodiment, an aqueous solution containing sodium trimetaphosphate (STMP) and sodium tripolyphosphate (STPP) is added to a starch solution (including a soluble starch solution and a corn amylopectin solution) under stirring, and the mixture is stirred until fully mixed to obtain an aqueous phase.

[0053] S2. The water phase and the oil phase are mixed to form an inverse suspension polymerization system, and then a polymerization reaction is carried out to obtain microspheres.

[0054] In some embodiments, the polymerization reaction includes a first stage reaction and a second stage reaction; the temperature of the first stage reaction is 60 to 80°C; the time of the first stage reaction is 2 to 4 hours; sodium trimetaphosphate and sodium tripolyphosphate are added during the second stage reaction; the temperature of the second stage reaction is 60 to 80°C; the time of the second stage reaction is 18 to 24 hours. By adding sodium trimetaphosphate and sodium tripolyphosphate during the second stage reaction, it is more conducive to the formation of the microsphere core-shell structure. Further, the mass ratio of sodium trimetaphosphate and sodium tripolyphosphate is (5 to 10): 1. Exemplarily, the mass ratio of sodium trimetaphosphate and sodium tripolyphosphate can be 5: 1, 6: 1, 7: 1, 8: 1, 9: 1 or 10: 1, etc., which can also be any value within the range of (5 to 10): 1.

[0055] In some embodiments, the oil phase includes cyclohexane, Span-60 and Tween-60. Further, the mass ratio of Span-60 to Tween-60 is (1-3): (0.5-1.5). Exemplarily, the mass ratio of Span-60 to Tween-60 can be 1:0.5, 1:1:1:1.5, 2:0.5, 2:1, 2:1.5, 3:0.5, 3:1 or 3:1.5, etc., which can be any value within the range of (1-3): (0.5-1.5).

[0056] Specifically, in the present embodiment, under stirring conditions, Span-60 and Tween-60 are added to cyclohexane to form a continuous phase oil phase. After stirring for a period of time, an aqueous phase is added to the oil phase. After being fully mixed, stirring, the reaction temperature is 70°C, and after reacting for a period of time, sodium trimetaphosphate (STMP) and sodium tripolyphosphate (STPP) are added and the reaction is continued for a period of time, followed by stirring at room temperature overnight, stirring throughout the process without standing, adding a certain amount of ethyl acetate, filtering, and removing oil-soluble impurities after washing with ethyl acetate, and washing and sieving with purified water to obtain core-shell starch hydrogel microspheres of different particle sizes. It should be noted that the room temperature referred to in this application is about 25°C, i.e., 20°C to 30°C.

[0057] This method uses two materials with different hydrophilicity as microsphere skeleton materials, and adopts inverse suspension polymerization to prepare microspheres, which will naturally form a core-shell structure, and can relatively simply realize the preparation of microspheres with a core-shell structure. In addition, the degradation of the shell layer of the core-shell structure precedes the degradation of the core, so that the microspheres can have a good embolization effect during the period when the shell layer is completely degraded, and then the core is rapidly degraded, reducing the possibility of inflammation during the embolization treatment process. Through the difference in degradation speed between the shell layer and the core, the degradation time of the embolization microspheres can be controlled.

[0058] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0059] Example 1

[0060] A method for preparing degradable starch hydrogel microspheres, the method comprising:

[0061] Preparation of corn amylopectin solution: Add 10g corn amylopectin and 1g NaOH into 100ml distilled water, stir and heat until gelatinized and transparent, let stand and cool for use.

[0062] Preparation of soluble starch solution: Add 10g soluble starch and 1g NaOH into 100ml distilled water, stir and heat until gelatinization and transparency, let stand and cool for later use.

[0063] Aqueous phase preparation: under stirring conditions, add 12.5 ml of an aqueous solution containing 0.3 g of STMP and 0.03 g of STPP to 12.5 ml of a starch solution (mass ratio: soluble starch solution: corn amylopectin solution = 1:5), and stir for 5 minutes to mix thoroughly.

[0064] Preparation of microspheres: Under stirring conditions, add 1g Span-60 and 0.5g Teween-60 to 100ml cyclohexane to form a continuous oil phase; after stirring for a period of time, add 25ml water phase to the oil phase. After fully mixing, stir, the reaction temperature is 70°C, after reacting for 3 hours, add 0.3g STMP and 0.03g STPP and continue to react for 21 hours, then stir at room temperature overnight, stirring without standing during the whole process, add a certain amount of ethyl acetate, filter, and wash with ethyl acetate 3 times to remove oil-soluble impurities, rinse and sieve with purified water to obtain core-shell starch hydrogel microspheres of different particle sizes.

[0065] Example 2

[0066] A method for preparing degradable starch hydrogel microspheres, the method comprising:

[0067] Preparation of corn amylopectin solution: Add 10g corn amylopectin and 1g NaOH into 100ml distilled water, stir and heat until gelatinized and transparent, let stand and cool for use.

[0068] Preparation of soluble starch solution: Add 10g soluble starch and 1g NaOH into 100ml distilled water, stir and heat until gelatinization and transparency, let stand and cool for later use.

[0069] Aqueous phase preparation: Under stirring conditions, add 12.5 ml of an aqueous solution containing 0.24 g of STMP and 0.03 g of STPP to 12.5 ml of a starch solution (mass ratio: soluble starch solution: corn amylopectin solution = 1:2), and stir for 5 minutes to mix thoroughly.

[0070] Under stirring conditions, 1g Span-60 and 0.5g Teween-60 were added to 100ml cyclohexane to form a continuous oil phase; after stirring for a period of time, 25ml of water phase was added to the oil phase. After thorough mixing, stirring was performed at a reaction temperature of 70°C. After 3 hours of reaction, 0.24g STMP and 0.03g STPP were added and the reaction continued for 21 hours, followed by stirring at room temperature overnight without standing during the whole process, adding a certain amount of ethyl acetate, filtering, and washing with ethyl acetate 3 times to remove oil-soluble impurities, and washing and sieving with purified water to obtain corn amylopectin hydrogel microspheres of different particle sizes.

[0071] Example 3

[0072] A method for preparing degradable starch hydrogel microspheres, the method comprising:

[0073] Preparation of corn amylopectin solution: Add 10g corn amylopectin and 1g NaOH into 100ml distilled water, stir and heat until gelatinized and transparent, let stand and cool for use.

[0074] Preparation of soluble starch solution: Add 10g soluble starch and 1g NaOH into 100ml distilled water, stir and heat until gelatinization and transparency, let stand and cool for later use.

[0075] Aqueous phase preparation: Under stirring conditions, add 12.5 ml of an aqueous solution containing 0.16 g of STMP and 0.03 g of STPP to 12.5 ml of a starch solution (mass ratio: soluble starch solution: corn amylopectin solution = 1:1), and stir for 5 minutes to mix thoroughly.

[0076] Under stirring conditions, 1g Span-60 and 0.5g Teween-60 were added to 100ml cyclohexane to form a continuous oil phase; after stirring for a period of time, 25ml of water phase was added to the oil phase. After thorough mixing, stirring was performed at a reaction temperature of 70°C. After reacting for 3 hours, 0.16g STMP and 0.03g STPP were added and the reaction continued for 21 hours, followed by stirring at room temperature overnight without standing during the whole process, adding a certain amount of ethyl acetate, filtering, and washing with ethyl acetate 3 times to remove oil-soluble impurities, and washing and sieving with purified water to obtain core-shell starch hydrogel microspheres of different particle sizes.

[0077] Example 4

[0078] A method for preparing degradable starch hydrogel microspheres, the method comprising:

[0079] Preparation of corn amylopectin solution: Add 10g corn amylopectin and 1g NaOH into 100ml distilled water, stir and heat until gelatinized and transparent, let stand and cool for use.

[0080] Preparation of soluble starch solution: Add 10g soluble starch and 1g NaOH into 100ml distilled water, stir and heat until gelatinization and transparency, let stand and cool for later use.

[0081] Aqueous phase preparation: Under stirring conditions, add 12.5 ml of an aqueous solution containing 0.21 g of STMP and 0.03 g of STPP to 12.5 ml of a starch solution (mass ratio: soluble starch solution: corn amylopectin solution = 2:1), and stir for 5 minutes to mix thoroughly.

[0082] Under stirring conditions, 1g Span-60 and 0.5g Teween-60 were added to 100ml cyclohexane to form a continuous oil phase; after stirring for a period of time, 25ml of water phase was added to the oil phase. After thorough mixing, stirring was performed at a reaction temperature of 70°C. After reacting for 3 hours, 0.21g STMP and 0.03g STPP were added and the reaction continued for 21 hours, followed by stirring overnight at room temperature without standing during the whole process, adding a certain amount of ethyl acetate, filtering, and washing with ethyl acetate 3 times to remove oil-soluble impurities, and washing and sieving with purified water to obtain core-shell starch hydrogel microspheres of different particle sizes.

[0083] Example 5

[0084] A method for preparing degradable starch hydrogel microspheres, the method comprising:

[0085] Preparation of corn amylopectin solution: Add 10g corn amylopectin and 1g NaOH into 100ml distilled water, stir and heat until gelatinized and transparent, let stand and cool for use.

[0086] Preparation of soluble starch solution: Add 10g soluble starch and 1g NaOH into 100ml distilled water, stir and heat until gelatinization and transparency, let stand and cool for later use.

[0087] Aqueous phase preparation: Under stirring conditions, add 12.5 ml of an aqueous solution containing 0.15 g of STMP and 0.03 g of STPP to 12.5 ml of a starch solution (mass ratio: soluble starch solution: corn amylopectin solution = 5:1), and stir for 5 minutes to mix thoroughly.

[0088] Under stirring conditions, 1g Span-60 and 0.5g Teween-60 were added to 100ml cyclohexane to form a continuous oil phase; after stirring for a period of time, 25ml of water phase was added to the oil phase. After thorough mixing, stirring was performed at a reaction temperature of 70°C. After reacting for 3 hours, 0.15g STMP and 0.03g STPP were added and the reaction continued for 21 hours, followed by stirring at room temperature overnight without standing during the whole process, adding a certain amount of ethyl acetate, filtering, and washing with ethyl acetate 3 times to remove oil-soluble impurities, and washing and sieving with purified water to obtain core-shell starch hydrogel microspheres of different particle sizes.

[0089] Comparative Example 1

[0090] A method for preparing degradable starch hydrogel microspheres, the method comprising:

[0091] Preparation of soluble starch solution: Add 10g soluble starch and 1g NaOH into 100ml distilled water, stir and heat until gelatinization and transparency, let stand and cool for later use.

[0092] Aqueous phase preparation: Under stirring conditions, add 12.5 ml of an aqueous solution containing 0.6 g of STMP and 0.06 g of STPP to 12.5 ml of the soluble starch solution, and stir for 5 minutes to mix thoroughly.

[0093] Under stirring conditions, 1g Span-60 and 0.5g Teween-60 were added to 100ml cyclohexane to form a continuous oil phase; after stirring for a period of time, 25ml of water phase was added to the oil phase. After sufficient mixing, stirring was performed at a reaction temperature of 70°C for 24 hours, followed by stirring at room temperature overnight, stirring without standing during the whole process, adding a certain amount of ethyl acetate, filtering, and washing with ethyl acetate 3 times to remove oil-soluble impurities, and rinsing and sieving with purified water to obtain soluble starch hydrogel microspheres of different particle sizes.

[0094] The microspheres provided in Examples 1 to 5 and Comparative Example 1 were subjected to a degradation test. The specific test process was as follows: 1 mL of 300-600 μm microspheres were added to 9 mL of PBS (pH = 7.4), incubated on a shaker at 37 ° C, 0.5 mL was taken after different time intervals T and mixed and diluted to 1 mL, and the Z average particle size was analyzed by DLS method. T The ratio of :D0 is used as the degradation standard, where D0 is the diameter of the undegraded microspheres and D T is the diameter of the microsphere after degradation time T.

[0095] The test results of Example 1 are shown in the following table:

[0096] Time 0 120 144 168 192 288 292 296 <![CDATA[D T :D0]]> 100.00% 66.46% 55.70% 47.30% 41.01% 8.53% 6.63% 2.22%

[0097] The test results of Example 2 are shown in the following table:

[0098]

[0099] The test results of Example 3 are shown in the following table:

[0100]

[0101] The test results of Example 4 are shown in the following table:

[0102]

[0103] The test results of Example 5 are shown in the following table:

[0104] Time 0 120 144 168 172 180 184 188 192 194 <![CDATA[D T :D0]]> 100.00% 67.44% 57.16% 47.66% 44.85% 30.36% 23.32% 15.47% 7.04% 2.93%

[0105] The test results of Comparative Example 1 are shown in the following table:

[0106] Time 0 4 8 24 28 48 <![CDATA[D T :D0]]> 100.00% 85.46% 78.26% 60.35% 42.12% 2.02%

[0107] According to the test results of Examples 1 to 5 and Comparative Example 1, a scatter plot was prepared. The results are as follows: Figure 2 and Figure 3 As shown, Figure 2 This is a schematic diagram of the degradation rate of the microspheres provided in Comparative Example 1, Figure 3 This is a schematic diagram of the degradation rate of the microspheres provided in Examples 1 to 5. It can be seen from the figure that the degradable starch microspheres with a core-shell structure synthesized after adjusting the ratio of soluble starch to corn amylopectin clearly have two different degradation stages and degradation rates, showing a gradient degradation characteristic.

[0108] The microspheres provided in Examples 1 and 2 were observed by optical microscope imaging. Figure 4 and 5 As shown, Figure 4 and Figure 5 These are images of the microspheres provided in Examples 1 and 2 under an optical microscope. It can be seen from the images that the microspheres prepared by the method provided in the examples of the present application have a core-shell structure.

[0109] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A degradable starch hydrogel microsphere, characterized in that: The microspheres are embolic microspheres having a core-shell structure. The degradation rate of the core material of the microspheres is greater than the degradation rate of the shell material of the microspheres. The core material of the microspheres is a soluble starch polymer. The shell material of the microspheres is a branched starch polymer. In the microspheres, the mass ratio of the core material to the shell material is (1 to 5): (1 to 5).

2. A method for preparing the degradable starch hydrogel microspheres according to claim 1, characterized in that: The method comprises: Aqueous phase preparation: adding sodium trimetaphosphate and sodium tripolyphosphate to a mixed solution of a soluble starch polymer and amylopectin polymer under stirring to obtain an aqueous phase; Oil phase preparation: Add Spam-60 and Tween-60 to cyclohexane under stirring to obtain an oil phase; Reverse polymerization: maintaining stirring, adding the water phase to the oil phase, controlling the reaction temperature to 60-80° C., adding sodium trimetaphosphate and sodium tripolyphosphate after reacting for 2-4 hours and continuing the reaction for 18-24 hours, then stirring at room temperature for at least 16 hours to obtain degradable starch hydrogel microspheres.

3. The method for preparing degradable starch hydrogel microspheres according to claim 2, characterized in that: During the aqueous phase preparation process, the mass ratio of the soluble starch polymer to the branched-chain starch polymer is (1-5): (1-5).

4. The method for preparing degradable starch hydrogel microspheres according to claim 2, characterized in that: During the aqueous phase preparation process, the mass ratio of the sodium trimetaphosphate to sodium tripolyphosphate is (5-10):

1.

5. The method for preparing degradable starch hydrogel microspheres according to claim 2, characterized in that: During the reverse polymerization process, the mass ratio of the sodium trimetaphosphate to sodium tripolyphosphate is (5-10):

1.

6. The method for preparing degradable starch hydrogel microspheres according to claim 2, characterized in that: During the reverse polymerization process, the mass ratio of Span-60 to Tween-60 is (1-3): (0.5-1.5).

Citation Information

Patent Citations

  • Core-shell microspheres

    CN103703079A

  • Starch hydrogel embolization microsphere and preparation method thereof

    CN116942888A