Preparation and application of a water-based graphene / carbon nanotube composite hybrid

By using mixed solvents to unwind carbon nanotubes and emulsify the preparation of aqueous graphene oxide/carbon nanotube composite hybrids, the problems of long-term ultrasonic treatment and surfactant use in the prior art have been solved, and the problems of long-term ultrasonic treatment and surfactant use have been improved. The stability and performance of the material are suitable for a variety of high-performance applications.

CN117819535BActive Publication Date: 2024-12-03JIANGNAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202311654231.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2024-12-03
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

The prior art requires long-term, high-intensity ultrasonic treatment or addition of surfactants when preparing aqueous graphene oxide/carbon nanotube composite hybrids, resulting in low order, low yield and conductive paste of hybrids. Unstable.

Method used

Use a suitable mixed solvent to dissolve the carbon nanotubes, prepare the carbon nanotube dispersion as the oil phase, and add it dropwise to the graphene oxide aqueous solution and stir and emulsify it. The aqueous graphene oxide/carbon with water dispersion is obtained by evaporation of solvent or water washing and centrifugation. Nanotube composite hybrids are subsequently reduced to improve stability.

Benefits of technology

Improve the stability and interaction efficiency of graphene oxide/carbon nanotube composite hybrids, reduce environmental pollution, enhance the conductive, thermal and electromagnetic shielding properties of the material, and is suitable for ink printing, transparent electrodes, supercapacitors and heat dissipation. Film and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117819535B_ABST
    Figure CN117819535B_ABST
Patent Text Reader

Abstract

The present invention discloses the preparation and application of an aqueous graphene / carbon nanotube composite hybrid, and belongs to the application field of carbon materials and energy materials. The present invention adopts a suitable mixed solvent to disentangle and disperse carbon nanotubes, prepares a carbon nanotube dispersion as an oil phase, and then adds dropwise to the aqueous dispersion phase graphene oxide aqueous dispersion for stirring and emulsification, and obtains a water-dispersible and stable aqueous graphene oxide / carbon nanotube composite hybrid through solvent evaporation or water washing and centrifugation. Subsequently, the aqueous graphene oxide / carbon nanotube composite hybrid is gradually reduced to obtain an aqueous graphene oxide / carbon nanotube composite dispersion. The composite hybrid and composite dispersion prepared by the present invention have good stability, and do not require long-term and high-intensity ultrasound, nor do they require the addition of surfactants or dispersants; they have good application prospects in the fields of ink printing, transparent electrodes, supercapacitors or heat dissipation films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation and application of a water-based graphene / carbon nanotube composite hybrid, and belongs to the application field of carbon materials and energy materials. Background Art

[0002] Graphene and carbon nanotubes have a wide range of applications in electromagnetic shielding, sensors, optoelectronic devices, and energy storage devices due to their excellent electrical, mechanical, and thermal properties. In particular, carbon nanotubes are considered an important application material due to their high surface area, high conductivity, and stability under electrochemical conditions. The structural similarity between graphene and carbon nanotube π regions makes the hybrid combination of the two have a synergistic effect in functional applications. In addition, the composite hybridization of graphene and carbon nanotubes can form an excellent three-dimensional network structure, so that the prepared nanohybrid has better carrier mobility, mechanical flexibility, and higher electrical and thermal conductivity than a single component. Therefore, graphene / carbon nanotube hybrids can be widely used in energy storage and thermal management devices, supercapacitors, and fuel cells.

[0003] However, due to the stacking of graphene sheets and the entanglement of carbon nanotube bundles in aqueous solution, the preparation of aqueous graphene oxide / carbon nanotube composite hybrids and even aqueous graphene oxide / carbon nanotube slurries has become a great challenge; it requires aqueous graphene oxide / carbon nanotube composite hybrids and conductive slurry to be dispersed and stable in water, and the dispersion state of the two will further affect the subsequent functional application. At present, there is a method of treating graphene and carbon nanotubes with surfactants or dispersants to obtain aqueous dispersions, but direct ultrasound using dispersions lacks effective interaction between graphene and carbon nanotubes, and the disentanglement efficiency of carbon nanotubes is very limited. In addition, some people use graphene oxide as a dispersant for carbon nanotubes by virtue of the water dispersion stability of graphene oxide and the conjugated interaction with carbon nanotubes, but the mixed solution treatment process requires long-term high-intensity ultrasound treatment, which will lead to severe damage to graphene oxide sheets and shortening of the length of carbon nanotubes by shearing, which is not conducive to the performance and subsequent application of the material. Summary of the invention

[0004] [Technical issues]

[0005] When graphene oxide and carbon nanotubes are mixed, long-term, high-intensity ultrasound is required, or a surfactant or dispersant needs to be added;

[0006] The conventionally prepared hybrid has low order and low yield, which results in poor order and instability of the prepared conductive paste.

[0007] [Technical solution]

[0008] In order to solve at least one of the above problems, the present invention provides a preparation and application of an aqueous graphene / carbon nanotube composite hybrid. The present invention uses a suitable mixed solvent to disentangle and disperse carbon nanotubes to prepare a carbon nanotube dispersion as an oil phase, and then add dropwise to an aqueous dispersion phase of graphene oxide aqueous solution for stirring and emulsification, and obtain a water-dispersible and stable aqueous graphene oxide / carbon nanotube composite hybrid through solvent evaporation or water washing and centrifugation. Subsequently, the aqueous graphene oxide / carbon nanotube composite hybrid is reduced to obtain an aqueous graphene oxide / carbon nanotube composite dispersion. The graphene oxide / carbon nanotube composite hybrid and the aqueous graphene oxide / carbon nanotube composite dispersion prepared by the present invention have good application prospects in the fields of ink printing, transparent electrodes, supercapacitors or heat dissipation films.

[0009] The first object of the present invention is to provide a method for preparing an aqueous graphene oxide / carbon nanotube composite hybrid, comprising the following steps:

[0010] (1) Oil phase:

[0011] Ultrasonic dispersion of carbon nanotube powder in a solvent to obtain a carbon nanotube dispersion; wherein the solvent is a single phenol solvent or a mixed solvent of a phenol solvent and a low dielectric constant solvent;

[0012] (2) Aqueous Dispersed Phase:

[0013] dispersing graphene oxide having a pH of 5-6 in water to obtain a graphene oxide aqueous dispersion;

[0014] (3) Preparation of hybrids:

[0015] The carbon nanotube dispersion is added drop by drop into the graphene oxide aqueous dispersion, stirred, ultrasonically emulsified, centrifuged and washed with water or the solvent evaporated to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

[0016] In one embodiment of the present invention, the concentration of the carbon nanotube dispersion in step (1) is 5-10 mg / mL.

[0017] In one embodiment of the present invention, the ultrasonic dispersion in step (1) is water bath ultrasonic dispersion, specifically ultrasonic treatment at 15-25W and 20-30°C for 15-20min.

[0018] In one embodiment of the present invention, the phenol solvent in step (1) is any one or more of m-cresol, o-cresol, p-cresol, and resorcinol; the low dielectric constant solvent is one or more of n-hexane, 1,4-dioxane, toluene, anisole, and chloroform.

[0019] In one embodiment of the present invention, the mass ratio of the phenol solvent to the low dielectric constant solvent in the mixed solvent of the phenol solvent and the low dielectric constant solvent in step (1) is 3-5:1.

[0020] In one embodiment of the present invention, the preparation method of graphene oxide with a pH of 5-6 in step (2) is:

[0021] Add the graphene oxide filter cake to water at a concentration of 5-10 mg / mL, perform ultrasonic treatment at 15-25 W and 20-30 ° C for 15-20 min, wash and centrifuge at 10000 rpm-11000 rpm for 10-20 min, and obtain graphene oxide with a pH of 5-6;

[0022] Among them, water washing and centrifugation are performed 1 to 4 times.

[0023] In one embodiment of the present invention, the concentration of the graphene oxide aqueous dispersion in step (2) is 0.1-1 mg / mL.

[0024] In one embodiment of the present invention, the volume ratio of the carbon nanotube dispersion to the graphene oxide aqueous dispersion in step (3) is 4-200:800.

[0025] In one embodiment of the present invention, the dropping speed in step (3) is 0.8-1.2 mL / min.

[0026] In one embodiment of the present invention, the stirring in step (3) is performed while adding dropwise, specifically, stirring at 3000-4000 rpm and 20-30° C. (room temperature) for 20-30 min.

[0027] In one embodiment of the present invention, the ultrasound in step (3) is 100-300W, 20-30°C (room temperature) for 5-10 min.

[0028] In one embodiment of the present invention, the centrifugation in step (3) is 10000rpm-11000rpm water washing centrifugation for 10-20min, and the number of centrifugation is 1-3 times.

[0029] The second object of the present invention is the aqueous graphene oxide / carbon nanotube composite hybrid prepared by the method described in the present invention.

[0030] The third object of the present invention is to provide a method for preparing an aqueous graphene oxide / carbon nanotube composite dispersion using an aqueous graphene oxide / carbon nanotube composite hybrid, comprising the following steps:

[0031] S1: dispersing an aqueous graphene oxide / carbon nanotube composite hybrid in water to obtain an aqueous graphene oxide / carbon nanotube composite hybrid solution; adding an L-ascorbic acid aqueous solution dropwise to the aqueous graphene oxide / carbon nanotube composite hybrid solution to perform a preliminary reduction reaction, centrifugally washing with water to obtain a preliminary reduction product;

[0032] S2: dispersing the preliminary reduction product obtained in S1 in water, adding hydrazine hydrate solution dropwise, further reducing, centrifuging and washing with water, to obtain an aqueous graphene oxide / carbon nanotube composite hybrid;

[0033] S3: dispersing the aqueous graphene oxide / carbon nanotube composite hybrid obtained in S2 in water to obtain an aqueous graphene oxide / carbon nanotube composite dispersion.

[0034] In one embodiment of the present invention, the concentration of the aqueous graphene oxide / carbon nanotube composite hybrid solution in S1 is 1-50 mg / mL.

[0035] In one embodiment of the present invention, the concentration of the L-ascorbic acid aqueous solution in S1 is 10 mg / mL.

[0036] In one embodiment of the present invention, the volume ratio of the aqueous graphene oxide / carbon nanotube composite hybrid solution and the L-ascorbic acid aqueous solution in S1 is 4-6:1.

[0037] In one embodiment of the present invention, the dropping speed in S1 is 0.8-1.2 mL / min.

[0038] In one embodiment of the present invention, the reduction reaction in S1 is stirred at 3000-4000 rpm and 20-30° C. (room temperature) for 10-12 h.

[0039] In one embodiment of the present invention, the water washing centrifugation in S1 is 10000 rpm-11000 rpm for 10-20 min.

[0040] In one embodiment of the present invention, the concentration of the primary reduction precipitate in water in S2 is 1-50 mg / mL.

[0041] In one embodiment of the present invention, the volume ratio of the aqueous solution of the primary reduction precipitate to the hydrazine hydrate solution in S2 is 300:1-2.

[0042] In one embodiment of the present invention, the hydrazine hydrate solution in S2 is an aqueous solution of hydrazine hydrate, and the solid content is 80-90%.

[0043] In one embodiment of the present invention, the reduction reaction in S2 is stirred at 3000-4000 rpm and 20-30° C. (room temperature) for 20-40 min.

[0044] In one embodiment of the present invention, the water washing centrifugation in S2 is 10000 rpm-11000 rpm for 10-20 min.

[0045] In one embodiment of the present invention, the dispersion in S3 is ultrasonic dispersion, specifically ultrasonic treatment at 15-25W and 20-30°C (room temperature) for 1-5 min.

[0046] The fourth object of the present invention is an aqueous graphene oxide / carbon nanotube composite dispersion prepared by the method described in the present invention.

[0047] The fifth object of the present invention is to use the aqueous graphene oxide / carbon nanotube composite hybrid and aqueous graphene oxide / carbon nanotube composite dispersion described in the present invention in the fields of ink printing, transparent electrodes, supercapacitors or heat dissipation films.

[0048] A sixth object of the present invention is to provide a flexible electrode film suitable for high-power supercapacitors, which uses the aqueous graphene oxide / carbon nanotube composite dispersion of the present invention.

[0049] A seventh object of the present invention is to provide a supercapacitor, which uses the flexible electrode film described in the present invention.

[0050] The eighth object of the present invention is to provide a method for preparing a water-based graphene oxide / carbon nanotube composite hybrid conductive coating, comprising the following steps:

[0051] A water-based graphene oxide / carbon nanotube composite hybrid dispersion with a concentration of 10-50 mg / mL is prepared, and then a scraper is used to scrape the dispersion on the surface of the substrate, and the dispersion is dried to obtain a water-based graphene oxide / carbon nanotube composite hybrid conductive coating;

[0052] Wherein, the substrate includes PET film, PI film or glass;

[0053] Drying is done at 50-80℃;

[0054] The thickness of the conductive coating is 5-30 μm;

[0055] The surface resistance of the conductive coating is 40-600Ω / sq.

[0056] A ninth object of the present invention is to provide a method for improving the dispersion performance of carbon nanotubes in graphite oxide dispersion, comprising the following steps:

[0057] (1) Oil phase:

[0058] Ultrasonic dispersion of carbon nanotube powder in a solvent to obtain a carbon nanotube dispersion; wherein the solvent is a single phenol solvent or a mixed solvent of a phenol solvent and a low dielectric constant solvent;

[0059] (2) Aqueous Dispersed Phase:

[0060] dispersing graphene oxide having a pH of 5-6 in water to obtain a graphene oxide aqueous dispersion;

[0061] (3) Preparation of hybrids:

[0062] The carbon nanotube dispersion is added drop by drop into the graphene oxide aqueous dispersion, stirred, ultrasonically emulsified, centrifuged and washed with water or the solvent evaporated to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

[0063] [Beneficial Effects]

[0064] (1) In the process of preparing the aqueous graphene oxide / carbon nanotube composite hybrid of the present invention, the solvent is removed by evaporation or water washing and centrifugation, and the dispersion medium is water, which greatly reduces the pollution to the environment.

[0065] (2) The present invention uses a graphene oxide aqueous dispersion as the aqueous dispersion phase and a carbon nanotube dispersion as the oil phase for uniform mixing and stirring to prepare a uniform and stable water-in-oil emulsion; in this way, there is graphene oxide as an emulsifier near thousands of small oil droplets for stabilization, which is convenient for inducing subsequent interface assembly between graphene oxide and carbon nanotubes, greatly increasing the interaction efficiency between graphene oxide and carbon nanotubes, and improving the stability of the prepared aqueous graphene oxide / carbon nanotube composite hybrid.

[0066] (3) The present invention adopts the interaction between graphene oxide and carbon nanotubes. After efficient dispersion and structural assembly between the two, the graphene oxide avoids the self-entanglement of carbon nanotubes in the aqueous medium due to van der Waals forces to a certain extent. The interlayer insertion of carbon nanotubes also effectively prevents the stacking of graphene oxide sheets, thereby improving the stability of the prepared aqueous graphene oxide / carbon nanotube composite hybrid.

[0067] (4) The present invention uses a combination of L-ascorbic acid and hydrazine hydrate to synergistically reduce the graphene oxide / carbon nanotube composite hybrid dispersion. The presence of carbon nanotubes effectively avoids the stacking of reduced graphene oxide. During the reduction process, the reduction product of L-ascorbic acid also enables the graphene / carbon nanotubes to maintain a certain water dispersion stability.

[0068] (5) The aqueous graphene oxide / carbon nanotube composite dispersion prepared by the present invention has excellent electrical conductivity, thermal conductivity and electromagnetic shielding properties, and has good application prospects in the fields of ink printing, transparent electrodes, supercapacitors or heat dissipation films. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 (a) and (b) are the SEM cross-sectional images and TEM images of the aqueous graphene oxide / carbon nanotube composite hybrid prepared in Example 1.

[0070] Figure 2 These are pictures of the aqueous graphene oxide / carbon nanotube composite hybrid solution prepared in Example 1 placed at room temperature 25° C. for 6 months, a is a picture placed upright after being inverted, and b is a picture after being inverted.

[0071] Figure 3 These are pictures of the aqueous graphene oxide / carbon nanotube composite hybrid solutions prepared with graphene oxides of different pH values ​​in Comparative Example 1 after being placed for 10 days, wherein the pH value of graphene oxide in a is 3, the pH value of graphene oxide in b is 5, and the pH value of graphene oxide in c is 10.

[0072] Figure 4 These are super-depth-of-field three-dimensional microscopy test images of the graphene oxide / carbon nanotube hybrid emulsion prepared with graphene oxide of different pH values ​​in Comparative Example 1 before and after placement, wherein a, b, and c are super-depth-of-field three-dimensional microscopy images of the hybrid emulsions prepared with pH values ​​of 3, 5, and 10 after being placed for 0 days, respectively, and d, e, and f are super-depth-of-field three-dimensional microscopy images of the hybrid emulsions prepared with pH values ​​of 3, 5, and 10 after being placed for 10 days, respectively.

[0073] Figure 5 (a) and (b) are the SEM cross-sectional images and TEM images of the aqueous graphene oxide / carbon nanotube composite hybrid prepared by direct dispersion in Comparative Example 2.

[0074] Figure 6 (a) and (b) are the SEM cross-sectional images and TEM images of the aqueous graphene oxide / carbon nanotube composite hybrid prepared in Comparative Example 3.

[0075] Figure 7 This is the SEM cross-sectional image of the aqueous graphene oxide / carbon nanotube composite hybrid prepared in Comparative Example 4.

[0076] Figure 8 This is a graph showing the surface resistance of the coating of the aqueous graphene oxide / carbon nanotube composite dispersion rGO / CNT(8 / 2)-Lh in Example 3, rGO / CNT(8 / 2)-L in Comparative Example 5, and rGO / CNT(8 / 2)-h in Comparative Example 6.

[0077] Fig. 9 These are pictures of the aqueous graphene oxide / carbon nanotube composite hybrid solution prepared in Comparative Example 7 after being placed for 20 minutes, wherein a is a picture placed upright after being inverted, and b is a picture after being inverted. DETAILED DESCRIPTION

[0078] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.

[0079] Test method:

[0080] 1. Test of electrical conductivity:

[0081] The test was conducted using a four-probe resistance tester. Specifically, the conductive coating prepared by the conductive slurry on the substrate maintained a uniform thickness (20 μm) and a probe contact area (8×10 mm). After the probes were in stable contact, the surface resistance value was stably read.

[0082] 2. Test of dispersion stability:

[0083] The solution was left to stand for several months to observe whether there was precipitation, stratification or flocculation; the size, state and distribution of the oil droplets in the solution were observed using an ultra-depth-of-field microscope.

[0084] 3. Dispersion uniformity test:

[0085] Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) were used for testing. Specifically, the microstructure and arrangement assembly of the aqueous graphene oxide / carbon nanotube composite hybrid were observed to evaluate the uniformity of the dispersion of the two.

[0086] The raw materials used in the embodiment:

[0087] Graphene oxide filter cake: pH = 2-5, size <10 μm, purchased from Changzhou Sixth Element Material Technology Co., Ltd.;

[0088] Carbon nanotube powder: Multi-walled carbon nanotube powder with a length of 5-20 μm and an average diameter of 7-11 nm and a purity of 99.0% was purchased from Jiangsu Tiannai Technology Co., Ltd.

[0089] Phenol solvent: mass content>98%, purchased from Sigma-Aldrich.

[0090] Example 1

[0091] A method for preparing an aqueous graphene oxide / carbon nanotube composite hybrid comprises the following steps;

[0092] (1) Oil phase:

[0093] 0.5 g of carbon nanotube powder was added to 100 g of a mixed solvent of m-cresol and 1,4-dioxane (mass ratio was 4:1), and ultrasonically dispersed at 20 W and 25 ° C for 15 min using an ultrasonic cleaner to obtain a carbon nanotube dispersion;

[0094] (2) Aqueous Dispersed Phase:

[0095] The graphene oxide filter cake was dispersed in water to form a 10 mg / mL aqueous dispersion, and then ultrasonicated in a water bath at 20W and 25°C for 20 minutes using an ultrasonic cleaner, and then washed and centrifuged at 10,000 rpm for 15 minutes, and the washing and centrifugation were repeated 3 times to obtain graphene oxide with a pH of 5;

[0096] Dispersing graphene oxide at a pH of 5 in water to obtain a 0.5 mg / mL graphene oxide aqueous solution;

[0097] (3) Preparation of hybrids:

[0098] 800 mL of graphene oxide aqueous dispersion was taken into a 1000 mL three-necked flask, stirred at room temperature, 3500 rpm, and 25°C, and then 20 mL of carbon nanotube dispersion was added dropwise at a dropping speed of 1 mL / min. Stirring was continued for 30 min, and then a cell disruptor was used for ultrasonication at 200 W power and 25°C for 10 min. Then, the mixture was washed and centrifuged at 10000 rpm for 15 min. The washing and centrifugation were repeated twice to obtain an aqueous graphene oxide / carbon nanotube composite hybrid, recorded as GO / CNT (8 / 2).

[0099] The SEM cross-sectional images and TEM images of the aqueous graphene oxide / carbon nanotube composite hybrid are shown in Figure 1 ,from Figure 1 It can be seen that the carbon nanotubes have a high degree of disentanglement, are evenly dispersed, and interact stably with the graphene oxide sheets. The two have a relatively regular and orderly structural arrangement.

[0100] The aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) was dispersed in water to obtain a 1 mg / mL aqueous graphene oxide / carbon nanotube composite hybrid solution, which was then placed at room temperature 25°C for 6 months and then inverted for stability testing. The test results are as follows: Figure 2 :

[0101] from Figure 2 It can be seen that the aqueous graphene oxide / carbon nanotube composite hybrid solution is stable and does not precipitate or sink to the bottom for a long time, indicating that the graphene oxide / carbon nanotube composite hybrid is well dispersed.

[0102] Example 2

[0103] The amount of carbon nanotube dispersion in step (3) of Example 1 was adjusted to 4.21, 8.89, 34.29, 120, and 186.67 mL, and the rest was consistent with Example 1 to obtain aqueous graphene oxide / carbon nanotube composite hybrids, recorded as GO / CNT (9.5 / 0.5), GO / CNT (9 / 1), GO / CNT (7 / 3), GO / CNT (4 / 6), and GO / CNT (3 / 7).

[0104] The obtained aqueous graphene oxide / carbon nanotube composite hybrid was subjected to elemental analysis test, and the actual interaction ratio of the graphene oxide / carbon nanotube composite hybrid was calculated according to the elemental test results. The calculation results are as follows:

[0105] Table 1

[0106] Dosage(mL) Graphene oxide (%) Carbon nanotubes (%) 20 (Example 1, GO / CNT (8 / 2)) 79.7398 20.2602 4.21(GO / CNT(9.5 / 0.5)) 97.6580 2.3420 8.89(GO / CNT(9 / 1)) 94.9071 5.0929 34.29(GO / CNT(7 / 3)) 77.1933 22.8067 120GO / CNT(4 / 6) 72.6394 27.3606 186.67GO / CNT(3 / 7) 60.4089 35.5911

[0107] It can be seen from Table 1 that in the elemental analysis process of the aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) obtained in Example 1, the actual interaction ratio of graphene oxide and carbon nanotubes is closest to the feed ratio. The loss of graphene oxide and carbon nanotubes is reduced to a minimum during the preparation process, and the interaction between the two can be intuitively reflected through the feed ratio.

[0108] Comparative Example 1

[0109] The pH of the graphene oxide in Example 1 is adjusted to 3 or 10;

[0110] Omit the water washing and centrifugation in step (3);

[0111] The rest was consistent with Example 1 to obtain an aqueous graphene oxide / carbon nanotube composite dispersion emulsion.

[0112] The obtained aqueous graphene oxide / carbon nanotube composite dispersion emulsion was tested for stability before and after standing. The test results are as follows:

[0113] Figure 3 The pictures of aqueous graphene oxide / carbon nanotube composite hybrid solutions prepared by graphene oxide with different pH values ​​after being placed for 10 days, where the pH value of graphene oxide in a is 3, the pH value of graphene oxide in b is 5, and the pH value of graphene oxide in c is 10. Figure 3 It can be seen that after 10 days of standing, the hybrid emulsion with graphene oxide pH of 5 still maintains dispersion stability, while the hybrid emulsions with graphene oxide pH of 3 and 10 gradually coagulate and precipitate, and the emulsion dispersion is unstable.

[0114] Figure 4The ultra-depth 3D microscope test images of graphene oxide / carbon nanotube hybrid emulsions prepared with graphene oxide of different pH values ​​before and after being placed, where a, b, and c are ultra-depth 3D microscope images of hybrid emulsions prepared with pH values ​​of 3, 5, and 10 placed for 0 days, and d, e, and f are ultra-depth 3D microscope images of hybrid emulsions prepared with pH values ​​of 3, 5, and 10 placed for 10 days. Figure 4 It can be seen that the small oil droplets in the graphene oxide / carbon nanotube hybrid emulsion prepared with a graphene oxide pH of 5 can remain relatively stable under long-term standing; while in the hybrid emulsions prepared with graphene oxide pH of 3 and 10, due to the influence of the amphiphilicity of graphene oxide, the oil droplets gradually converge during the standing process, and the uniformity and stability of the hybrid emulsion dispersion are insufficient.

[0115] Comparative Example 2 Direct Dispersion

[0116] A method for preparing an aqueous graphene oxide / carbon nanotube composite hybrid comprises the following steps:

[0117] (1) The graphene oxide filter cake is dispersed in water to form a 10 mg / mL aqueous dispersion, and then ultrasonicated in a water bath at 20W and 25°C for 20 minutes using an ultrasonic cleaner, and then washed and centrifuged at 10,000 rpm for 15 minutes, and the washing and centrifugation are repeated 3 times to obtain graphene oxide with a pH of 5; the graphene oxide with a pH of 5 is dispersed in water to obtain a 0.5 mg / mL aqueous solution of graphene oxide;

[0118] (2) Take 800 mL of graphene oxide aqueous dispersion into a 1000 mL beaker, then add 0.10 g of carbon nanotube powder, stir evenly with a glass rod, use an ultrasonic cleaner 20 W, 25 ° C water bath ultrasonic for 2 h, continue to use an ultrasonic cell crusher 200 W power ultrasonic for 2 h, then wash and centrifuge at 10000 rpm for 15 min, repeat the water washing and centrifugation twice to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

[0119] The SEM cross-sectional images and TEM images of the aqueous graphene oxide / carbon nanotube composite hybrid are shown in Figure 5 ,from Figure 5 It can be seen that the carbon nanotubes are seriously entangled in the aqueous medium, and even in the presence of graphene oxide, the carbon nanotubes are not well dispersed. When the same proportion of carbon nanotubes is added as in Example 1, the interaction efficiency between the two is low, an ideal structural arrangement is not formed, and material loss is serious.

[0120] Comparative Example 3

[0121] A method for preparing an aqueous graphene oxide / carbon nanotube composite hybrid comprises the following steps;

[0122] (1) The graphene oxide filter cake is dispersed in water to form a 10 mg / mL aqueous dispersion, and then ultrasonicated in a water bath at 20W and 25°C for 20 minutes using an ultrasonic cleaner, and then washed and centrifuged at 10,000 rpm for 15 minutes, and the washing and centrifugation are repeated 3 times to obtain graphene oxide with a pH of 5; the graphene oxide with a pH of 5 is dispersed in water to obtain a 0.5 mg / mL aqueous solution of graphene oxide;

[0123] (2) adding 0.5 g of carbon nanotube powder to 100 g of NMP (N-methylpyrrolidone), and using an ultrasonic cleaner to ultrasonically disperse the powder at 20 W and room temperature for 30 min to obtain a carbon nanotube dispersion;

[0124] (3) 800 mL of graphene oxide aqueous dispersion was taken into a 1000 mL three-necked flask, stirred at room temperature at 3500 rpm, and then 20 mL of carbon nanotube dispersion was added dropwise at a dropping speed of 1 mL / min. Stirring was continued for 30 min, and then a cell disruptor was used for ultrasonication at room temperature (25°C) at 200 W power for 20 min, and then washed and centrifuged at 10000 rpm for 15 min. The washing and centrifugation were repeated twice to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

[0125] The SEM cross-sectional images and TEM images of the aqueous graphene oxide / carbon nanotube composite hybrid are shown in Figure 6 ,from Figure 6 It can be seen that the carbon nanotubes are seriously entangled in the aqueous medium. Even if NMP is used to initially disperse the carbon nanotubes, the dispersion method is inefficient and the effect is not ideal. When the same proportion of carbon nanotubes is added as in Example 1, the interaction efficiency between the two is low, an ideal structural arrangement is not formed, and material loss is serious.

[0126] Comparative Example 4: One-time addition of carbon nanotube dispersion

[0127] A method for preparing an aqueous graphene oxide / carbon nanotube composite hybrid comprises the following steps;

[0128] (1) Oil phase:

[0129] 0.5 g of carbon nanotube powder was added to 100 g of a mixed solvent of m-cresol and 1,4-dioxane (mass ratio was 4:1), and ultrasonically dispersed for 15 min at 20 W and room temperature using an ultrasonic cleaning machine to obtain a carbon nanotube dispersion;

[0130] (2) Aqueous Dispersed Phase:

[0131] The graphene oxide filter cake was dispersed in water to form a 10 mg / mL aqueous dispersion, and then ultrasonicated in a water bath at 20W and 25°C for 20 minutes using an ultrasonic cleaner, and then washed and centrifuged at 10,000 rpm for 15 minutes, and the washing and centrifugation were repeated 3 times to obtain graphene oxide with a pH of 5;

[0132] Dispersing graphene oxide at a pH of 5 in water to obtain a 0.5 mg / mL graphene oxide aqueous solution;

[0133] (3) Preparation of hybrids:

[0134] Take 800 mL of graphene oxide aqueous dispersion into a 1000 mL three-necked flask, stir at room temperature at 3500 rpm, then directly add 20 mL of carbon nanotube dispersion, continue stirring for 30 min, then use a cell disruptor to ultrasonicate at room temperature (25°C) for 10 min at 200 W power, then wash and centrifuge at 10000 rpm for 15 min, repeat the water washing and centrifugation twice to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

[0135] The SEM cross-sectional image of the aqueous graphene oxide / carbon nanotube composite hybrid is shown in Figure 7 .from Figure 7 It can be seen that the one-time addition of the carbon nanotube dispersion liquid easily causes carbon nanotube aggregation in the graphene oxide aqueous solution, and the obtained graphene oxide / carbon nanotube composite hybrid has a poor dispersion effect.

[0136] Example 3

[0137] A method for preparing an aqueous graphene oxide / carbon nanotube composite dispersion using an aqueous graphene oxide / carbon nanotube composite hybrid comprises the following steps:

[0138] S1: Dispersing aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) (Example 1) in water to obtain a 1 mg / mL aqueous graphene oxide / carbon nanotube composite hybrid solution; adding 60 mL of a 10 mg / mL L-ascorbic acid aqueous solution dropwise (1 mL / min) to 300 mL of the aqueous graphene oxide / carbon nanotube composite hybrid solution, performing a reduction reaction at room temperature (25° C.) and 3500 rpm for 12 h, and after completion, washing and centrifuging at 10000 rpm for 15 min to obtain a preliminary reduction product;

[0139] S2: The preliminary reduction product in S1 was dispersed in water with a volume of 300 mL and a concentration of 1 mg / mL, and then 0.7 mL of a hydrazine hydrate solution with a solid content of 85% was added dropwise (1 mL / min), and further reduced at room temperature (25°C) and 3500 rpm for 30 min. After the reduction, the mixture was washed and centrifuged at 10000 rpm for 15 min to obtain an aqueous graphene oxide / carbon nanotube composite hybrid;

[0140] S3: Dispersing the aqueous graphene oxide / carbon nanotube composite hybrid in water to obtain an aqueous graphene oxide / carbon nanotube composite dispersion with a concentration of 20 mg / mL, recorded as rGO / CNT(8 / 2)-Lh.

[0141] The aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) was replaced with the aqueous graphene oxide / carbon nanotube composite hybrid prepared in Comparative Example 2-4, and a composite dispersion was prepared according to the above method; a scraper was used to scrape the PET surface, and dried to obtain an aqueous graphene oxide / carbon nanotube composite hybrid conductive coating with a thickness of 20 μm, and then a performance test was performed. The test results are as follows:

[0142] Table 2

[0143] example Coating surface resistance (Ω / sq) Example 3 57 Comparative Example 2 50000 Comparative Example 3 7900 Comparative Example 4 945

[0144] Comparative Example 5

[0145] S2 in Example 3 is omitted, and the details are as follows:

[0146] S1: Dispersing aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) (Example 1) in water to obtain a 1 mg / mL aqueous graphene oxide / carbon nanotube composite hybrid solution; adding 60 mL of a 10 mg / mL L-ascorbic acid aqueous solution dropwise (1 mL / min) to 300 mL of the aqueous graphene oxide / carbon nanotube composite hybrid solution, performing a reduction reaction at room temperature (25° C.) and 3500 rpm for 12 h, and after completion, washing and centrifuging at 10000 rpm for 15 min to obtain a reduced product;

[0147] S2: The reduced product was dispersed in water to obtain an aqueous graphene oxide / carbon nanotube composite dispersion with a concentration of 20 mg / mL, which was recorded as rGO / CNT(8 / 2)-L.

[0148] Comparative Example 6

[0149] S1 in Example 3 is omitted, and the details are as follows:

[0150] S1: Dispersing aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) (Example 1) in water to obtain a 1 mg / mL aqueous graphene oxide / carbon nanotube composite hybrid solution; adding 0.7 mL of a hydrazine hydrate solution having a solid content of 85% dropwise (1 mL / min) to 300 mL of the aqueous graphene oxide / carbon nanotube composite hybrid solution, performing secondary reduction at room temperature (25° C.) and 3500 rpm for 30 min, and after completion, washing and centrifuging at 10000 rpm for 15 min to obtain a reduced product;

[0151] S2: The reduced product is dispersed in water to obtain an aqueous graphene oxide / carbon nanotube composite dispersion with a concentration of 20 mg / mL, which is recorded as rGO / CNT(8 / 2)-h.

[0152] The surface resistance curves of the coatings of Example 3 and Comparative Examples 5 and 6 are as follows: Figure 8 ,from Figure 8 It can be seen that Example 3 uses a combination of L-ascorbic acid and hydrazine hydrate to synergistically reduce the graphene oxide / carbon nanotube composite hybrid dispersion, so that the reduction degree of the aqueous graphene oxide / carbon nanotube composite dispersion and the recovery of the graphene oxide conductive network are significantly improved, and the surface resistance of the coating can be further reduced compared with Comparative Examples 5 and 6.

[0153] Comparative Example 7

[0154] A method for preparing an aqueous graphene oxide / carbon nanotube composite dispersion using an aqueous graphene oxide / carbon nanotube composite hybrid comprises the following steps:

[0155] S1: Dispersing aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) (Example 1) in water to obtain a 1 mg / mL aqueous graphene oxide / carbon nanotube composite hybrid solution; adding 60 mL of a 10 mg / mL L-ascorbic acid aqueous solution and 0.7 mL of a hydrazine hydrate solution with a solid content of 85% dropwise (1 mL / min) to 300 mL of the aqueous graphene oxide / carbon nanotube composite hybrid solution, performing a reduction reaction at room temperature (25° C.) and 3500 rpm for 12 h, and after completion, washing and centrifuging at 10000 rpm for 15 min to obtain a reduced product;

[0156] S2: Dispersing the reduced product in water to obtain an aqueous graphene oxide / carbon nanotube composite dispersion with a concentration of 20 mg / mL.

[0157] Comparative Example 7: L-ascorbic acid aqueous solution and hydrazine hydrate solution were added simultaneously to reduce the aqueous graphene oxide / carbon nanotube composite hybrid solution. The prepared composite dispersion was inverted after being placed for about 20 minutes. Fig. 9As shown, from Fig. 9 It can be seen that the composite dispersion prepared in Comparative Example 7 begins to flocculate and precipitate, indicating that the reduction dispersion is unstable.

[0158] Example 4

[0159] The aqueous graphene oxide / carbon nanotube composite hybrid GO / CNT (8 / 2) of Example 1 was used to prepare a supercapacitor, as follows:

[0160] The aqueous graphene oxide / carbon nanotube composite dispersion prepared in Example 3 was mixed with carbon black and polytetrafluoroethylene in a mass ratio of 85:10:5 to prepare a slurry, which was evenly coated on the surface of the stainless steel current collector and dried to obtain a flexible electrode film with an active area of ​​1 cm 2 , with a thickness of 20μm, and then used to prepare the positive electrode material in high-power supercapacitors.

[0161] The prepared supercapacitor has good conductivity, as well as high specific capacitance and rate performance.

[0162] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing an aqueous graphene oxide / carbon nanotube composite hybrid, characterized in that: The steps include: (1) Oil phase: Ultrasonic dispersion of carbon nanotube powder in a solvent to obtain a carbon nanotube dispersion; wherein the solvent is a single phenol solvent or a mixed solvent of a phenol solvent and a low dielectric constant solvent; The phenol solvent is any one or more of m-cresol, o-cresol, p-cresol and resorcinol; the low dielectric constant solvent is one or more of n-hexane, 1,4-dioxane, toluene, anisole and chloroform; the mass ratio of the phenol solvent to the low dielectric constant solvent in the mixed solvent of the phenol solvent and the low dielectric constant solvent is 3-5:1; (2) Aqueous dispersed phase: dispersing graphene oxide having a pH of 5-6 in water to obtain a graphene oxide aqueous dispersion; (3) Preparation of hybrids: The carbon nanotube dispersion is added drop by drop into the graphene oxide aqueous dispersion, stirred, ultrasonically emulsified, centrifuged and washed with water or the solvent evaporated to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

2. The aqueous graphene oxide / carbon nanotube composite hybrid prepared by the method according to claim 1.

3. A method for preparing an aqueous graphene oxide / carbon nanotube composite dispersion using an aqueous graphene oxide / carbon nanotube composite hybrid, characterized in that: The steps include: S1: dispersing the aqueous graphene oxide / carbon nanotube composite hybrid according to claim 2 in water to obtain an aqueous graphene oxide / carbon nanotube composite hybrid solution; adding L-ascorbic acid aqueous solution dropwise to the aqueous graphene oxide / carbon nanotube composite hybrid solution, stirring, performing preliminary reduction, centrifuging and washing with water to obtain a preliminary reduction product; S2: The preliminary reduction product obtained in the above S1 is dispersed in water, and then a hydrazine hydrate solution is added dropwise, stirred, further reduced, centrifuged and washed with water, and then dispersed in water to obtain a 1-50 mg / mL aqueous graphene oxide / carbon nanotube composite dispersion.

4. The aqueous graphene oxide / carbon nanotube composite dispersion prepared by the method according to claim 3.

5. Application of the aqueous graphene oxide / carbon nanotube composite hybrid according to claim 2 in the fields of ink printing, transparent electrodes, supercapacitors or heat dissipation films.

6. Use of the aqueous graphene oxide / carbon nanotube composite dispersion according to claim 4 in the fields of ink printing, transparent electrodes, supercapacitors or heat dissipation films.

7. A flexible electrode film suitable for high-power supercapacitors, characterized in that: The aqueous graphene oxide / carbon nanotube composite dispersion is prepared according to claim 4.

8. A supercapacitor, characterized in that: The flexible electrode film according to claim 7 is used.

9. A method for preparing a water-based graphene oxide / carbon nanotube composite hybrid conductive coating, characterized in that: The steps include: The aqueous graphene oxide / carbon nanotube composite dispersion of claim 4 is prepared at a concentration of 10-50 mg / mL, and then coated on the surface of the substrate using a scraper, and dried to obtain an aqueous graphene oxide / carbon nanotube composite hybrid conductive coating; Wherein, the substrate is PET film, PI film or glass; Drying is done at 50-80℃; The thickness of the conductive coating is 5-30 μm; The surface resistance of the conductive coating is 40-600Ω / sq.

10. A method for improving the dispersibility of carbon nanotubes in graphite oxide dispersion, characterized in that: The steps include: (1) Oil phase: Ultrasonic dispersion of carbon nanotube powder in a solvent to obtain a carbon nanotube dispersion; wherein the solvent is a single phenol solvent or a mixed solvent of a phenol solvent and a low dielectric constant solvent; The phenol solvent is any one or more of m-cresol, o-cresol, p-cresol and resorcinol; the low dielectric constant solvent is one or more of n-hexane, 1,4-dioxane, toluene, anisole and chloroform; the mass ratio of the phenol solvent to the low dielectric constant solvent in the mixed solvent of the phenol solvent and the low dielectric constant solvent is 3-5:1; (2) Aqueous dispersed phase: dispersing graphene oxide having a pH of 5-6 in water to obtain a graphene oxide aqueous dispersion; (3) Preparation of hybrids: The carbon nanotube dispersion is added drop by drop into the graphene oxide aqueous dispersion, stirred, ultrasonically emulsified, centrifuged and washed with water or the solvent evaporated to obtain an aqueous graphene oxide / carbon nanotube composite hybrid.

Citation Information

Cited By

  • Polymer as well as preparation method and application thereof

    CN121226618A

  • A polymer, its preparation and use