A catalyst for continuous synthesis of HMT, preparation method and application thereof

By using styrene, vinylbenzene and styrenepropylene to synthesize polymer acidic catalysts, the problems of wastewater pollution and low purity caused by aluminum trichloride in the synthesis of HMT are solved, and the continuous synthesis of high-purity HMT and the efficient production of tona musk are achieved. , suitable for industrial applications.

CN117964829BActive Publication Date: 2024-09-27JINAN ENLIGHTEN BIOTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410121632.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2024-09-27
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

The use of aluminum trichloride in the existing HMT synthesis process leads to wastewater pollution, high cost and low purity, making it difficult to meet the environmental protection and safety requirements of industrial production.

Method used

Styrene, vinylbenzene and styrenepropylene are used as raw materials to synthesize a polymeric acidic catalyst. The spherical granular catalyst is prepared through polymerization and sulfonation reactions for continuous synthesis of HMT, avoiding the use of aluminum trichloride and improving synthesis efficiency. and purity.

Benefits of technology

The high-purity continuous synthesis of HMT is achieved, which reduces the risk of waste water generation and quenching. The catalyst can be used repeatedly, which is suitable for industrial production and improves the production efficiency of musk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117964829B
    Figure CN117964829B
Patent Text Reader

Abstract

The invention discloses a catalyst for continuous synthesis of HMT, a preparation method and application thereof, and belongs to the technical field of organic catalytic synthesis. The invention uses styrene, divinylbenzene and styrene propylene as raw materials to synthesize a new polymer acid catalyst, which has a sulfonic acid group on the polymer of the cross-linked structure, similar to a resin catalyst, and has the advantages of acid and alkali resistance, organic corrosion resistance, etc., and has a strong catalytic effect. When it continuously catalytically synthesizes HMT, it has high selectivity, is easy to realize continuous production, has low corrosiveness, and has low requirements on equipment materials. Less "three wastes" are generated during the reaction, and it has a cross-linked structure, high mechanical strength, heat resistance and chemical stability, and long service life. After testing, when the catalyst continuously synthesizes HMT, the reaction conversion rate of isopropyl toluene reaches more than 95%. The catalyst can be used repeatedly, and after 30 days of recycling, the catalytic reaction conversion rate of isopropyl toluene still reaches more than 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic catalytic synthesis, and particularly relates to a catalyst for continuous synthesis of HMT, and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Tonalide is a synthetic musk with a tetralin structure. It has a strong powdery aroma, excellent fragrance quality, elegant aroma, long-lasting fragrance, acid and alkali resistance, and no photosensitivity. It is internationally recognized as a safe and harmless fragrance, ranking first among synthetic musks. Tonalide is usually prepared by the Friedel-Crafts acylation reaction of the intermediate 1,1,3,4,4,6-hexamethyltetralin (HMT) and acetylating agents such as acetyl chloride or acetic anhydride under the catalysis of Lewis acid.

[0004] Musk Synthesis:

[0005]

[0006] In the synthesis of musk decanter, HMT is a very important reactant. With the development of the economy, the consumption of musk decanter continues to rise, so the demand for HMT is also gradually increasing. At present, when synthesizing HMT, p-isopropyl toluene, 2,3-dimethyl-1-butene and tert-butyl chloride are often used to generate HMT under the catalysis of a catalyst, and aluminum chloride is used as a catalyst (such as CN101200419A, CN102050715A, etc.). When synthesizing HMT by this route, aluminum chloride is used, and the reaction solution or product needs to be washed to produce a large amount of wastewater, which pollutes the environment. It increases the cost of synthesis and does not meet the current requirements of the chemical industry for environmental protection and safety. Furthermore, the purity of HMT obtained by the existing synthesis method is about 85%, which is not high and cannot be directly used to synthesize musk decanter. It must be distilled or refined to obtain HMT with higher purity, which is not conducive to industrial scale-up production. In addition, in the prior art, the purification of HMT mostly adopts the recrystallization method, which consumes corresponding solvents and the production of materials is easy to cause environmental pollution.

[0007] In summary, it is necessary to develop a process for synthesizing high-purity HMT with high production efficiency, environmental protection, safety and stability. Summary of the invention

[0008] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a catalyst for continuous synthesis of HMT, a preparation method and application thereof. The present invention provides a new catalyst for catalytic synthesis of HMT, avoiding the use of aluminum chloride, making the operation in HMT synthesis simpler, with less three wastes, and more guaranteed yield and product quality of HMT, which is more suitable for industrial scale-up production.

[0009] In order to achieve the above object, the technical solution of the present invention is:

[0010] The first aspect of the present invention provides a method for preparing a catalyst for continuous synthesis of HMT, comprising the following steps:

[0011] Styrene, divinylbenzene and propylene are mixed, toluene and water are added, and then an azo catalyst is added, and the polymerization reaction is carried out by pressurizing and heating;

[0012] After the polymerization is completed, the obtained spherical particles are sequentially sulfonated to obtain spherical particle catalysts.

[0013] The present invention uses styrene, divinylbenzene and styrene propene as raw materials to synthesize a new polymer acid catalyst, which is similar to a resin catalyst, has the advantages of acid and alkali resistance, organic corrosion resistance, etc., and has a strong catalytic effect. The present invention uses styrene, divinylbenzene and styrene propene as raw materials for cross-linking to obtain a polymer material with a cross-linked structure, and then combines sulfonic acid groups on the cross-linked polymer material through a sulfonation reaction to obtain a spherical granular catalyst. As a catalyst, it has the advantages of high selectivity, easy to realize continuous production, low corrosiveness, low requirements on equipment materials, less "three wastes" generated during the reaction, and has a cross-linked structure, high mechanical strength, heat resistance and chemical stability, and long service life.

[0014] In some embodiments of the present invention, the molar ratio of styrene, divinylbenzene and styrene propene is 1-2:1:1-2, preferably 2:1:1.

[0015] In some embodiments of the present invention, the amount of toluene used is 10-15% of the mass of styrene, and the amount of water used is 1-3 times the mass of styrene.

[0016] In some embodiments of the present invention, the azo catalyst is selected from azobisisobutyronitrile or azobisisoheptanenitrile. The amount of the catalyst is 0.1-0.5% of the mass of styrene.

[0017] In some embodiments of the present invention, the polymerization reaction has a reaction pressure of 0.8-1.2 Mpa, a reaction temperature of 58-62° C., and a reaction time of 5-7 h.

[0018] In some embodiments of the present invention, after the polymerization is completed, petroleum ether is added to the obtained spherical particles, the temperature is raised and refluxed for 5-7 hours, then the temperature is lowered, filtered, and dried to obtain solid particles;

[0019] Concentrated sulfuric acid is added to the solid particles to carry out sulfonation reaction. After the reaction is completed, the solid particles are filtered, washed to neutrality, and dried to obtain a spherical particle catalyst, which is then filled into a column for later use.

[0020] Wherein, the temperature is lowered to 20-25°C.

[0021] Wherein, the reaction temperature of the sulfonation reaction is 95-105°C, and the reaction time is 12-18 h.

[0022] The second aspect of the present invention provides a catalyst for continuous synthesis of HMT, which is prepared by the above-mentioned preparation method.

[0023] The present invention uses styrene, divinylbenzene and styrene propene as raw materials to synthesize a new polymer acid catalyst, which is similar to a resin catalyst, has the advantages of acid and alkali resistance, organic corrosion resistance, etc., and has a strong catalytic effect. After testing, when the catalyst is used to continuously synthesize HMT, the reaction conversion rate of isopropyl toluene reaches more than 95%. And the catalyst can be used repeatedly. After experimental testing, after 30 days of recycling, the catalytic reaction conversion rate of isopropyl toluene still reaches more than 90%. The present invention greatly improves the synthesis efficiency of HMT and reduces the generation of a large amount of wastewater and the danger of quenching by improving the catalyst to replace aluminum chloride.

[0024] In some embodiments of the present invention, the continuous service life of the catalyst is at least 30 days.

[0025] The third aspect of the present invention provides the use of the above-mentioned catalyst for continuous synthesis of HMT in the synthesis of HMT;

[0026] The synthesis of HMT comprises the following steps: using p-isopropyltoluene, 2,3-dimethyl-1-butene and tert-butyl chloride as raw materials, mixing them evenly, and flowing them through a packing column filled with the above-mentioned catalyst for continuous synthesis of HMT, wherein the effluent at the end of the packing column is a reaction liquid after the reaction is completed, and after removing the solvent from the reaction liquid, HMT with a purity of more than 97% is obtained.

[0027] A fourth aspect of the present invention provides a method for continuously synthesizing high-purity HMT, comprising the following steps:

[0028] P-isopropyltoluene, 2,3-dimethyl-1-butene, tert-butyl chloride and a diluent solvent are mixed to obtain a mixed solution, and the mixed solution flows through a packing column filled with the above-mentioned catalyst for continuous synthesis of HMT. The effluent at the end of the packing column is a reaction liquid after the reaction is completed. After removing the solvent from the reaction liquid, HMT with a purity of more than 97% is obtained.

[0029] It has been tested that the reaction conversion rate of isopropylbenzene using the above catalyst for continuous synthesis of HMT is above 95%. The above catalyst column can be used repeatedly. It has been tested that the catalytic reaction conversion rate of isopropylbenzene on the 30th day is still above 90%. The reaction solution does not need to be washed with water, and the solvent is directly distilled off, and the fractions are collected to obtain high-purity HMT.

[0030] In some embodiments of the present invention, the molar ratio of p-isopropyltoluene, 2,3-dimethyl-1-butene, and tert-butyl chloride is 1:1-2:1-2, preferably 1:1.1:1.1.

[0031] In some embodiments of the present invention, the dilution solvent includes but is not limited to one of n-hexane, cyclohexane or dichloromethane, preferably cyclohexane. The molar ratio of the dilution solvent to p-isopropyl toluene is 1.4-1.6:1, preferably 1.5:1.

[0032] In some embodiments of the present invention, the length of the filler column filled with the catalyst for continuous synthesis of HMT according to claim 7 is ≥2 m.

[0033] In some embodiments of the present invention, the flow rate of the mixed solution in the packing column is 1-5 mL / min.

[0034] In some embodiments of the present invention, the column temperature of the packing column is 5-35°C, preferably 15-25°C.

[0035] In some embodiments of the present invention, the HMT obtained by the above-mentioned continuous synthesis of high-purity HMT does not need to be refined, and can be directly subjected to Friedel-Crafts acylation reaction. The musk dehydrogenase obtained by acetylation of HMT does not need to be refined with alcohol, and a qualified product with a purity of more than 98% can be directly obtained. Specifically, Lewis acid is added to the reaction medium, and the acetylation agent and HMT are added in sequence. After the addition, the reaction is carried out at room temperature for 1-3 hours to finally obtain the product musk dehydrogenase.

[0036] Wherein, the mass ratio of Lewis acid, acetylating agent and HMT is 10-15:1-5:14-16, preferably 11:4:15.

[0037] Wherein, the reaction medium includes but is not limited to dichloromethane, tetrahydrofuran, diethyl ether, methyl tert-butyl ether, N-methylpyrrolidone, etc., preferably dichloromethane.

[0038] The Lewis acid includes but is not limited to aluminum trichloride, ferric trichloride or zinc chloride, preferably aluminum trichloride.

[0039] Wherein, the acetylating agent includes but is not limited to acetyl chloride or acetic anhydride, preferably acetyl chloride.

[0040] The reaction temperature of the Friedel-Crafts acylation reaction is 5-35°C, preferably 15-25°C; the reaction time is 0.5-6 h, preferably 1-3 h, and more preferably 1-1.5 h.

[0041] The beneficial effects of the present invention are:

[0042] The present invention provides a method for preparing a catalyst for continuous synthesis of HMT, comprising the following steps: mixing styrene, divinylbenzene and styrene propylene, adding toluene and water, then adding azobisisobutyronitrile as a catalyst, pressurizing, heating to carry out polymerization reaction; after the polymerization is completed, the obtained spherical particles are sequentially sulfonated to obtain a spherical granular catalyst. The present invention uses styrene, divinylbenzene and styrene propylene as raw materials to synthesize a new polymer acid catalyst, which has a sulfonic acid group on the polymer of the cross-linked structure, similar to a resin catalyst, and has the advantages of acid and alkali resistance, organic corrosion resistance, etc., and has a strong catalytic effect. When it is used as a catalyst for continuous catalytic synthesis of HMT, it has the advantages of high selectivity, easy to realize continuous production, low corrosiveness, low requirements on equipment materials, less "three wastes" generated during the reaction, and has a cross-linked structure, high mechanical strength, heat resistance and chemical stability, and long service life. After testing, when the catalyst is used to continuously synthesize HMT, the reaction conversion rate of isopropyl toluene reaches more than 95%. The column filled with the catalyst can be used repeatedly. According to experimental detection, after 30 days of recycling, the catalytic conversion rate of isopropyl toluene still reaches more than 90%. The present invention improves the catalyst and replaces aluminum chloride to greatly improve the synthesis efficiency of HMT, reduce the generation of a large amount of wastewater, reduce the risk of quenching, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0044] Figure 1 The process flow chart of the synthesis of the polymer acid catalyst and the synthesis of HMT and musk denatonium of the present invention is as follows;

[0045] Figure 2 The gas phase spectrum of the musk toniferum synthesized in Example 2 of the present invention;

[0046] Figure 3This is the hydrogen spectrum of the musk denatonium synthesized in Example 2 of the present invention. DETAILED DESCRIPTION

[0047] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0048] Example 1

[0049] Preparation of catalyst: Add 500 g styrene, 312 g divinylbenzene, 283 g styrene propylene, 60 g toluene and 1 kg water into a stainless steel kettle, add 1 g azobisisobutyronitrile, pressurize with nitrogen to 1 MPa, stir and heat to 60°C to initiate polymerization for 6 h, filter, wash and dry to obtain 1.05 kg of spherical material. Add 1 L petroleum ether to the spherical particles, heat and reflux for 6 h, cool to 20-25°C, filter and dry to obtain 1.0 kg of solid. Add 2 kg of concentrated sulfuric acid to the solid, heat to 100°C and react for 15 h, filter, wash to neutral, dry to obtain spherical brown-yellow particles, fill into a column and set aside.

[0050] Embodiment 2:

[0051] Preparation of HMT: 100 g of p-isopropyltoluene, 69 g of 2,3-dimethyl-1-butene, 75 g of tert-butyl chloride and 50 mL of cyclohexane were mixed evenly and poured onto the top of the column (prepared in Example 1). The flow rate was controlled to be about 1 mL / min. Circulating water was passed through the column jacket to keep the temperature at 15-25°C. The reaction liquid was received at the lower end of the column. The reaction liquid was directly evaporated under reduced pressure to remove the solvent and a small amount of low-boiling substances, and then the fraction of 103-107°C / 3.5 mmHg was collected under reduced pressure, which was 150 g of HMT, with a yield of 94% and a purity of 97.5%.

[0052] Preparation of musk denamate: add 150 g of dichloromethane, 110 g of aluminum chloride, and 40 g of acetyl chloride to a flask, add 150 g of HMT while stirring and keeping warm at 15-25°C, stir and react for 1 h, add 200 g of ice water to quench, then wash with alkali, wash the organic layer with water, dry with sodium sulfate, evaporate the solvent under reduced pressure, and collect the fraction of 145-152°C / 2 mmHg under reduced pressure, which is musk denamate. MS (ES + ):M / Z=259(M + )

[0053] Embodiment 3:

[0054] Preparation of HMT: 50 kg of p-isopropyltoluene, 34.5 kg of 2,3-dimethyl-1-butene, 37.5 kg of tert-butyl chloride and 25 L of cyclohexane were mixed evenly and poured into the top of the column (prepared in Example 1). The flow rate was controlled to be about 2 mL / min. The temperature was kept at 15-25°C by circulating water in the column jacket. The reaction liquid was received at the lower end of the column. The solvent and a small amount of low-boiling substances were directly evaporated under reduced pressure in the reaction liquid, and the fraction of 103-107°C / 3.5 mmHg was collected under reduced pressure, which was 76 kg of HMT, with a yield of 94.5% and a purity of 97.2%.

[0055] Preparation of musk denamate: add 75 kg of dichloromethane, 55 kg of aluminum chloride, and 20 kg of acetyl chloride to the reactor, add 75 kg of HMT while stirring and keeping the temperature at 15-25℃, stir and react for 1 hour, add 100 kg of ice water to quench, then wash with alkali, wash the organic layer with water, dry with sodium sulfate, evaporate the solvent under reduced pressure, and collect the fraction of 145-152℃ / 2 mmHg under reduced pressure, which is musk denamate. MS (ES + ):M / Z=259(M + )

[0056] Embodiment 4:

[0057] P-isopropyltoluene, 2,3-dimethyl-1-butene, and tert-butyl chloride were mixed evenly in a molar ratio of 1:1.1:1.1, and then mixed evenly with cyclohexane (the molar ratio of cyclohexane to p-isopropyltoluene was 1.5:1), and passed through a catalyst packing column (prepared in Example 1) at room temperature (flow rate 1 mL / min), and the reaction liquid was collected at the bottom of the column. After testing, the catalyst obtained in Example 1 had a reaction conversion rate of p-isopropyltoluene of more than 95%. And the catalyst column can be used repeatedly. After experimental testing, the catalytic reaction conversion rate of p-isopropyltoluene on the 30th day was still more than 90%. The reaction liquid does not need to be washed with water, and the solvent is directly distilled off, and the posterior fraction is collected to obtain HMT, as shown in Table 1.

[0058] Table 1

[0059]

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a catalyst for continuous synthesis of HMT, It is characterized in that The steps include: Styrene, divinylbenzene and styrene propene are mixed, toluene and water are added, and then an azo catalyst is added, and the pressure is increased and the temperature is increased to carry out a polymerization reaction; the molar ratio of styrene, divinylbenzene and styrene propene is 1-2:1:1-2; the polymerization reaction has a reaction pressure of 0.8-1.2 Mpa, a reaction temperature of 58-62°C, and a reaction time of 5-7 h; After the polymerization is completed, petroleum ether is added to the obtained spherical particles, the temperature is raised and refluxed for 5-7 hours, the temperature is lowered, filtered, and dried to obtain solid particles; Concentrated sulfuric acid is added to the solid particles to carry out sulfonation reaction. After the reaction is completed, the solid particles are filtered, washed to neutrality, and dried to obtain a spherical particle catalyst.

2. The method for preparing a catalyst for continuous synthesis of HMT according to claim 1, It is characterized in that The amount of toluene used is 10-15% of the mass of styrene, and the amount of water used is 1-3 times the mass of styrene.

3. The method for preparing a catalyst for continuous synthesis of HMT according to claim 1, It is characterized in that The azo catalyst includes one of azobisisobutyronitrile or azobisisoheptanenitrile; The dosage of the azo catalyst is 0.1-0.5% of the mass of styrene.

4. A catalyst for continuous synthesis of HMT, It is characterized in that It is prepared by the preparation method of the catalyst for continuous synthesis of HMT according to any one of claims 1 to 3; The continuous service life of the catalyst is at least 30 days.

5. Use of the catalyst for continuous synthesis of HMT according to claim 4 in the synthesis of HMT; The synthesis of HMT comprises the following steps: using p-isopropyltoluene, 2,3-dimethyl-1-butene and tert-butyl chloride as raw materials, mixing them evenly, and flowing them through a packing column filled with the catalyst for continuous synthesis of HMT according to claim 4, wherein the effluent at the end of the packing column is a reaction liquid with a complete reaction, and after removing the solvent from the reaction liquid, HMT with a purity of more than 97% is obtained.

6. A method for continuously synthesizing high-purity HMT, It is characterized in that The steps include: P-isopropyltoluene, 2,3-dimethyl-1-butene, tert-butyl chloride and a diluent solvent are mixed to obtain a mixed solution, and the mixed solution flows through a packing column filled with the catalyst for continuous synthesis of HMT according to claim 4, and the effluent at the end of the packing column is the reaction liquid after the reaction is completed. After removing the solvent from the reaction liquid, HMT with a purity of more than 97% is obtained.

7. The method for continuously synthesizing high-purity HMT as claimed in claim 6, It is characterized in that The dilution solvent includes one of n-hexane, cyclohexane or dichloromethane; the molar ratio of the dilution solvent to p-isopropyl toluene is 1.4-1.6:1; The length of the catalyst for continuous synthesis of HMT according to claim 4 filled in the packing column is ≥2 m; The flow rate of the mixed solution in the packing column is 1-5 mL / min; The column temperature of the packing column is 5-35°C.