Preparation method and application of wide temperature range battery electrolyte
By designing a wide-temperature battery electrolyte composed of lithium salt, solvent and composite additives, the problem of electrochemical performance deterioration of lithium-ion batteries under low and high temperature conditions is solved, and the range of -60 to 60℃ is achieved Stable operation and high rate performance significantly improve the wide temperature performance of the battery.
Patent Information
- Application Number
- CN202410314710.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-03-19
AI Technical Summary
The electrochemical performance of lithium-ion batteries deteriorates under low or high temperature conditions, resulting in thermal runaway, limiting their wide temperature range applications. The wide temperature performance, low oxidation voltage, and poor rate performance of existing electrolytes are difficult to be in the ultra-wide temperature range. Work stably.
Using a wide temperature-domain battery electrolyte composed of lithium salts, solvents, diluents and composite additives, by reducing the use of carbonate, introducing fluorinated solvents and carboxylate solvents, reducing the viscosity of the electrolyte, improving the conductivity, and introducing effects. Excellent film-forming additives form an anion-dominated solid interface film to enhance the wide temperature performance of the battery.
The electrolyte is stable and reversible charging and discharging in the ultra-wide temperature range of -60~60℃. The battery can be cycled stably for 800 cycles at room temperature, and can still cyclize stably at 10C ultra-high magnification, which significantly improves the wide temperature of lithium batteries. Performance and electrochemical properties.
Smart Images

Figure CN118198491B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wide-temperature-range secondary batteries, and relates to a preparation method and application of a wide-temperature-range battery electrolyte. Background Art
[0002] With the continuous growth of energy demand, the consumption rate of fossil fuels is also rapidly accelerating, and the resulting environmental problems are becoming increasingly prominent. In the face of energy and environmental crises, efficient, clean and safe renewable energy has always been the direction of people's exploration, and the development, storage and utilization of these new energy sources have also become a global hotspot. Since its invention in 1990, lithium-ion batteries have quickly occupied the power supply market for electronic devices as a new energy source. With the further improvement of energy density and the gradual decline of production costs, lithium-ion batteries have almost monopolized the electric vehicle power battery market and extended their tentacles to the field of grid-level energy storage. As the most advanced battery technology at present, lithium-ion batteries have the advantages of high energy density, high output voltage, long cycle life, low self-discharge, no memory effect, and green environmental protection, which make them always maintain strong competitiveness, but their operating range is usually around room temperature (RT, close to 25°C). For the power battery of electric vehicles, in order to adapt to regional and seasonal differences, its operating temperature range is required to be wider (-20°C to 60°C). In addition, in the extreme application fields of aerospace, defense and military industries, the lower limit of the operating temperature of lithium-ion batteries even needs to be extended to -50°C or lower. Therefore, developing lithium batteries with a wide range of temperature resistance is crucial to improving battery stability, safety and applicability.
[0003] However, when lithium-ion batteries are operated at low temperatures (LT, below -20°C) or high temperatures (HT, above 60°C), the electrochemical performance will usually deteriorate, and even lead to thermal runaway, which severely limits the wide temperature range application of rechargeable lithium batteries. Due to reasons such as the structure of the electrode material itself, fundamentally improving the wide temperature performance of the battery is limited. The electrolyte is called the "blood" of the battery and plays an important role in transferring ions and conducting internal circuits. Therefore, it is expected that the wide temperature performance of lithium-ion batteries can be improved by modifying the electrolyte. In view of this, requiring the electrolyte to have a high boiling point, a low freezing point, a high ionic conductivity, and good compatibility with the cathode and anode are key factors in determining whether rechargeable lithium batteries can operate under wide temperature conditions.
[0004] In recent years, there have been many studies on the high-temperature or low-temperature performance of lithium-ion batteries, but few studies have taken both into account at the same time. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing and using a wide-temperature range battery electrolyte; the oxidation potential of the electrolyte is as high as 5.40V, and a battery prepared using the electrolyte can be stably and reversibly charged and discharged in an ultra-wide temperature range of -60 to 60°C; at the same time, the prepared battery can be stably cycled for 800 cycles at room temperature; it can still be stably cycled even at an ultra-high rate of 10C, solving the problems existing in the prior art.
[0006] The electrolyte designed by the present invention exhibits excellent electrical properties at ultra-low temperature, low temperature, room temperature, and 30-60°C.
[0007] The present invention starts with lithium salts and solvents, and then supplements with composite additives and diluents to prepare a local high-concentration electrolyte system. By reducing the use of carbonates, introducing fluorinated solvents, carboxylic acid ester solvents, and diluents, the wide temperature viscosity of the electrolyte is reduced while maintaining a high dielectric constant, thereby improving the conductivity of the electrolyte; lithium salts with high conductivity and low low-temperature charge transfer resistance are used to ensure the reaction kinetics of the electrolyte; excellent film-forming additives, weak solvating solvents, etc. are introduced as wide temperature additives to reduce the charge transfer impedance of the electrode interface, promote the formation of a solid interface film dominated by anions, and improve the wide temperature performance of the battery. The present invention breaks through the defects of existing electrolytes with poor wide temperature performance, low oxidation voltage, and poor rate performance, reduces the viscosity and economic cost of the electrolyte, improves ionic conductivity, and promotes further commercial applications of the propeller.
[0008] The technical solution adopted by the present invention is:
[0009] A wide temperature range battery carboxylate-based electrolyte, which consists of a lithium salt, a solvent, a diluent, and a composite additive.
[0010] The lithium salt includes at least one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium hexafluorophosphate, lithium difluorophosphate, lithium perchlorate, and lithium nitrate.
[0011] The organic solvent comprises at least one of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl propionate, ethyl acetate, ethyl butyrate, butyl formate, butyl propionate, isobutyl formate, methyl difluoroacetate, ethyl difluoroacetate, methyl trifluoroacetate, and ethyl trifluoroacetate.
[0012] The diluent comprises at least one of fluorobenzene, o-difluorobenzene, m-difluorobenzene, p-difluorobenzene, o-fluorotoluene, m-fluorotoluene and p-fluorotoluene.
[0013] The composite additive comprises at least two of fluorosulfonyl fluorocarboxylates such as fluoroethylene carbonate, ethylene carbonate, tris(trimethylsilyl)phosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, lithium difluorobisoxalate phosphate, lithium difluorophosphate, and methyl fluorosulfonyl difluoroacetate. The present invention must use the composite additive, and each component in the additive must be strictly limited, otherwise even if the types of the composite additives are exactly the same, the performance of the products will be very different.
[0014] Preferably, the composite additive is composed of at least one of fluorosulfonyl fluorocarboxylates such as fluoroethylene carbonate, ethylene carbonate, tris(trimethylsilyl)phosphate, methyl fluorosulfonyldifluoroacetate, and at least one of lithium difluorooxalatoborate, lithium tetrafluoroborate, lithium difluorobisoxalatophosphate, and lithium difluorophosphate.
[0015] Preferably, the lithium salt is selected from at least one of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium hexafluorophosphate, and lithium difluorophosphate.
[0016] As a further preferred embodiment, the lithium salt used is different from the lithium-containing substance used in the subsequent additives. That is, as a further preferred embodiment, before the use of the electrolyte of the present invention, Li is provided by the lithium salt and the lithium-containing substance in the composite additive, so as to ensure that all lithium salts can be effectively dissolved, maintain high lithium ion transmission and high conductivity at low temperatures, ensure stable film formation and high-voltage performance at room temperature, and have good thermal stability at high temperatures.
[0017] Preferably, the lithium salt accounts for 0.1% to 20% of the electrolyte and its concentration can be 0.1 to 2.5 mol / L.
[0018] Preferably, the solvent accounts for 10% to 60% of the total amount of the electrolyte.
[0019] Preferably, the diluent accounts for 20% to 80% of the total amount of the electrolyte.
[0020] It is further defined that the amount of the composite additive added is 1%-15% of the total amount of the electrolyte.
[0021] The operating temperature of the wide temperature range battery electrolyte is -60 to 60°C.
[0022] As a further preferred embodiment, the lithium salt includes lithium bis(trifluoromethanesulfonyl)imide and / or lithium bis(fluorosulfonyl)imide.
[0023] As a preferred embodiment, the organic solvent includes methyl propionate. The solvent has a high dielectric constant and a low melting point, which ensures that it will not solidify at low temperatures and dissolve as much lithium salt as possible.
[0024] As a preferred embodiment, the diluent includes o-difluorobenzene.
[0025] As a preferred embodiment, the composite additive includes methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate.
[0026] As a further preference, the composite additive is composed of methyl fluorosulfonyl difluoroacetate and lithium difluorooxalatoborate in a molar ratio of 5-15:1-2.5.
[0027] As a preferred embodiment, the molar ratio of the lithium salt, the solvent and the diluent is 3-12:20-50:30-60.
[0028] As a further preference, the molar ratio of the lithium salt, the solvent and the diluent is 1:4:5.
[0029] As a preferred embodiment, methyl fluorosulfonyl difluoroacetate accounts for 5% to 15% of the total amount of the electrolyte.
[0030] As a further preference, lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate are in a molar ratio of 1:4:5:1; or lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate are in a molar ratio of 1:4:5:2.
[0031] As a preferred solution, lithium difluorooxalate borate accounts for 1%-2.5% of the total amount of electrolyte. As a further preferred solution, lithium difluorooxalate borate accounts for 1.5%-2% of the total amount of electrolyte. In the process of developing the technology of the present invention, it was found that when lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, methyl fluorosulfonyl difluoroacetate were used and the molar ratio was controlled to be 1:4:5:1 and lithium difluorooxalate borate was used, the amount of lithium difluorooxalate borate must be strictly controlled to account for 1%-2.5% (preferably 1.5-2%) of the total amount of electrolyte. Otherwise, the product is very easy to precipitate lithium salts during low-temperature use, resulting in a sharp decline in battery performance. It was also found that the above-mentioned solution that is very easy to precipitate lithium salts can still exhibit excellent electrical properties at room temperature and in an environment of room temperature to 60 degrees Celsius. This also illustrates from the side that it is not easy to obtain an electrolyte for a wide temperature range product.
[0032] The wide temperature range battery carboxylate-based electrolyte designed by the present invention can be used as a lithium battery electrolyte.
[0033] The wide-temperature range battery carboxylate-based electrolyte designed by the present invention can still achieve a conductivity of 1.034 mS / cm even at an extremely low temperature of -60°C.
[0034] The upper limit of the electrochemical window of the carboxylate-based electrolyte of the wide-temperature range battery designed by the present invention can be as high as 5.4V.
[0035] When the wide temperature range battery carboxylate-based electrolyte designed by the present invention is used for NCM811 lithium batteries, at 25°C, when the charging voltage reaches 4.7V, the first cycle capacity is 202mAh / g, and after 267 cycles, the capacity retention rate (CR) is 80%; after 800 cycles, the capacity retention rate is 63%, showing excellent room temperature stability.
[0036] When the wide temperature range battery carboxylate-based electrolyte designed by the present invention is used for NCM811 lithium batteries, at room temperature, at 0.1C, the average capacity is greater than or equal to 220mAh / g, and at 10C, the average capacity is greater than or equal to 160mAh / g.
[0037] When the wide temperature range battery carboxylate-based electrolyte designed by the present invention is used for NCM811 lithium battery, under the conditions of 25°C 2.8-4.7V and 4C high rate; after 250 cycles, the capacity retention rate is greater than 85% (such as 85.5-86%), and the average charge and discharge efficiency is greater than 99.9%.
[0038] When the wide temperature range battery carboxylate-based electrolyte designed by the present invention is used for NCM811 lithium battery, the capacity retention rate after 100 cycles is greater than 76% (such as 76.5-77%) under the conditions of 25°C 2.8-4.7V and 10C high rate.
[0039] When the wide temperature range battery carboxylate-based electrolyte designed by the present invention is used for NCM811 lithium battery, under -40°C 2.8-4.7V, 0.2C high rate conditions, the first cycle capacity is 150mAh / g, and the capacity retention rate after 55 cycles is greater than 96% (such as 96.5-97%).
[0040] When the wide temperature range battery carboxylate-based electrolyte designed by the present invention is used for NCM811 lithium battery, under the conditions of 60°C 2.8-4.7V and 4C high rate, the first cycle capacity is 185mAh / g, and after 80 cycles, the capacity retention rate is greater than 81% (such as 81.5-82%).
[0041] Beneficial Effects
[0042] The present invention adopts a composite additive of special components in combination with other electrolyte components, which can not only broaden the operating temperature range, but also improve the performance of the lithium battery. The most obvious thing is that after the battery is assembled, the voltage of the battery can be increased to be greater than or equal to 4.7V.
[0043] The present invention improves the comprehensive performance of the battery under a wide temperature range through the synergistic effect of each component in the electrolyte. First, a lithium salt with high solubility, high conductivity and excellent comprehensive performance is used. Subsequently, an organic reagent with high dielectric constant, small number of donors, low freezing point, low viscosity and high boiling point is introduced as the solvent of the electrolyte. On the one hand, the electrolyte can still maintain liquid phase stability in an ultra-wide temperature range, not solidify at low temperatures, and not boil at high temperatures; on the other hand, the electrolyte can dissolve more lithium salts and maintain a certain desolvation ability, promote the rapid desolvation of lithium ions, enhance dynamics, and improve fast charging and discharging and wide temperature range performance. At the same time, an appropriate amount of diluent that does not dissolve lithium salts is introduced into the electrolyte to promote the interaction between lithium salts and anions while ensuring the stability of the lithium ion-solvent-anion structure, thereby forming a solid interface film with low interface impedance and rich in inorganic substances. Finally, an appropriate amount of composite additives is introduced into the electrolyte to reduce the viscosity of the electrolyte, reduce the degree of solvation, stabilize the film formation, and protect the electrode. Through the synergistic effect of the special lithium salt, solvent, diluent and composite additive of the present invention, the wide temperature range electrolyte has better redox stability and conductive properties, and can adapt to wide temperature range, high voltage and high rate conditions.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] (1) The wide temperature range electrolyte has the advantages of wide application temperature range, high voltage resistance, and support for fast charge and discharge. At the same time, it overcomes the problems of electrolyte solidification and large polarization at low temperatures, serious side reactions at high temperatures, and rapid deterioration of electrochemical performance. It greatly improves the wide temperature, high voltage, and high rate performance of lithium batteries, and effectively improves the defects of lithium batteries such as low low temperature capacity, rapid high temperature capacity loss, and small voltage range. It is particularly suitable for wide temperature range, high voltage, and high rate lithium batteries.
[0046] (2) In the optimized scheme, through the synergistic effect of the electrolyte components, the high conductivity and high solubility of an appropriate amount of lithium bis(trifluoromethanesulfonyl)imide ensure the conductivity of the electrolyte at low temperatures; an appropriate amount of methyl propionate with low viscosity, low freezing point and high dielectric constant ensures the liquid phase range of the electrolyte and promotes the dissolution of more lithium salts; an appropriate amount of o-difluorobenzene is used as a diluent to reduce the overall viscosity of the electrolyte, improve conductivity and reduce costs; an appropriate amount of methyl fluorosulfonyl difluoroacetate reduces viscosity and promotes the dissolution of more lithium salts, and at the same time has the characteristic of low binding energy with lithium ions, which promotes dissolution and promotes the high rate performance of the battery; an appropriate amount of lithium difluorooxalate borate can not only stabilize the film formation, but also provide part of Li, which not only increases the battery cut-off voltage and helps provide more capacity, but also has excellent electrical properties in a wider temperature range. The synergy of the electrolyte components ensures that the electrolyte does not solidify at low temperatures and does not boil at high temperatures, maintains a stable liquid phase, has high conductivity, enhances the dynamics of the electrolyte, and improves fast charging and discharging and wide temperature range performance. At the same time, by introducing diluents and additives, the electrolyte's anti-oxidation performance is improved, the voltage range is expanded, and the cycle stability and charge and discharge efficiency of the battery prepared with the electrolyte are stabilized.
[0047] (3) The preparation process is simple, the cost is low, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is the conductivity diagram of the electrolyte of Example 1 and Comparative Examples 1 and 2 at different temperatures.
[0049] Figure 2 It is the electrochemical window diagram of Comparative Examples 1, 2 and Example 1.
[0050] Figure 3 This is the cycle performance diagram of the NCM811||Li battery prepared in Example 1 at room temperature.
[0051] Figure 4 This is a rate performance diagram of the NCM811||Li battery prepared with the electrolyte of Example 1 at 25°C and 2.8-4.7V.
[0052] Figure 5 This is a cycle performance diagram of the NCM811||Li battery prepared with the electrolyte of Example 1 at 25°C, 2.8-4.7V, and 4C high rate conditions.
[0053] Figure 6 This is a cycle performance diagram of the NCM811||Li battery prepared with the electrolyte of Example 1 at 25°C, 2.8-4.7V, and 10C high rate conditions.
[0054] Figure 7 This is a cycle performance diagram of the NCM811||Li battery prepared with the electrolyte of Example 1 at -40℃0.2C conditions.
[0055] Figure 8 This is the cycle performance diagram of the NCM811||Li battery prepared with the electrolyte of Example 1 at 60℃4C. DETAILED DESCRIPTION
[0056] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to these specific embodiments. Those skilled in the art should recognize that the present invention covers all possible alternatives, improvements and equivalents within the scope of the claims.
[0057] Embodiment 1:
[0058] A wide temperature range battery electrolyte, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, o-difluorobenzene as diluent, and methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate as additives. The preparation method is: first dissolve lithium bis(trifluoromethanesulfonyl imide) into methyl propionate, add methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate respectively after fully dissolved, then stir the electrolyte fully until it is colorless and transparent, and finally add the diluent o-difluorobenzene. The proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate in a molar ratio of 1:4:5:1, and lithium difluorooxalate borate accounts for 2% of the total mass of the electrolyte.
[0059] Embodiment 2:
[0060] A wide temperature range battery electrolyte, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, o-difluorobenzene as diluent, and methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate as additives. The preparation method is: first dissolve lithium bis(trifluoromethanesulfonyl imide) into methyl propionate, add methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate respectively after fully dissolved, then stir the electrolyte fully until it is colorless and transparent, and finally add the diluent o-difluorobenzene. The proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate in a molar ratio of 1:4:5:1, and lithium difluorooxalate borate accounts for 1% of the total mass of the electrolyte.
[0061] Embodiment 3:
[0062] A wide temperature range battery electrolyte, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, o-difluorobenzene as diluent, and methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate as additives. The preparation method is: first dissolve lithium bis(trifluoromethanesulfonyl imide) into methyl propionate, add methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate respectively after fully dissolved, then stir the electrolyte fully until it is colorless and transparent, and finally add the diluent o-difluorobenzene. The proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate in a molar ratio of 1:4:5:1, and lithium difluorooxalate borate accounts for 3% of the total mass of the electrolyte.
[0063] Embodiment 4:
[0064] A wide temperature range battery electrolyte, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, o-difluorobenzene as diluent, and methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate as additives. The preparation method is: first dissolve lithium bis(trifluoromethanesulfonyl imide) into methyl propionate, add methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate respectively after fully dissolved, then stir the electrolyte fully until it is colorless and transparent, and finally add the diluent o-difluorobenzene. The proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate in a molar ratio of 2:8:10:1, and lithium difluorooxalate borate accounts for 2% of the total mass of the electrolyte.
[0065] Embodiment 5:
[0066] A wide temperature range battery electrolyte, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, o-difluorobenzene as diluent, and methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate as additives. The preparation method is: first dissolve lithium bis(trifluoromethanesulfonyl imide) into methyl propionate, add methyl fluorosulfonyl difluoroacetate and lithium difluorooxalate borate respectively after fully dissolved, then stir the electrolyte fully until it is colorless and transparent, and finally add the diluent o-difluorobenzene. The proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and methyl fluorosulfonyl difluoroacetate in a molar ratio of 1:4:5:2, and lithium difluorooxalate borate accounts for 2% of the total mass of the electrolyte.
[0067] Comparative Example 1:
[0068] An electrolyte without diluent and additives, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt and methyl propionate as solvent. The preparation method is as follows: lithium bis(trifluoromethanesulfonyl imide) is dissolved in methyl propionate, and then the electrolyte is fully stirred until it is colorless and transparent. The proportion of each component of the electrolyte is lithium bis(trifluoromethanesulfonyl imide) and methyl propionate in a molar ratio of 1:4.
[0069] Comparative Example 2:
[0070] An electrolyte without additives, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, and o-difluorobenzene as diluent. The preparation method is as follows: firstly, lithium bis(trifluoromethanesulfonyl imide) is dissolved in methyl propionate, and after fully dissolved, o-difluorobenzene is added as diluent, and then the electrolyte is fully stirred until it becomes colorless and transparent. The proportion of each component of the electrolyte is lithium bis(trifluoromethanesulfonyl imide), methyl propionate, and o-difluorophenyl ester in a molar ratio of 1:4:5.
[0071] Comparative Example 3:
[0072] A wide temperature range battery electrolyte, with lithium bis(trifluoromethanesulfonyl imide) as lithium salt, methyl propionate as solvent, o-difluorobenzene as diluent, and fluoroethylene carbonate as additive. The preparation method is as follows: firstly, lithium bis(trifluoromethanesulfonyl imide) is dissolved in methyl propionate, fluoroethylene carbonate is added after it is fully dissolved, then the electrolyte is fully stirred until it is colorless and transparent, and finally o-difluorobenzene as diluent is added. The proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl imide), methyl propionate, o-difluorobenzene, and fluoroethylene carbonate in a molar ratio of 1:4:5:1.
[0073] Comparative Example 4
[0074] Other conditions are consistent with those in Example 1, except that: the electrolyte does not contain methyl fluorosulfonyldifluoroacetate, and the components are lithium bis(trifluoromethanesulfonyl)imide, methyl propionate, o-difluorobenzene, and lithium difluorooxalatoborate in a molar ratio of 1:4:5:0.2.
[0075] Comparative Example 5
[0076] Other conditions are consistent with those in Example 1, except that: the electrolyte does not contain lithium difluorooxalatoborate, and the proportions of the components of the electrolyte are lithium bis(trifluoromethanesulfonyl)imide, methyl propionate, o-difluorobenzene, and methyl fluorosulfonyldifluoroacetate in a molar ratio of 1:4:5:1.
[0077] Electrolyte performance test:
[0078] The conductivity of the electrolyte was tested in a low-temperature oven using a conductivity meter, and the electrochemical window upper limit of the electrolyte was obtained using linear voltammetry.
[0079] Battery low temperature charge and discharge test:
[0080] The electrochemical performance of the NMC811||Li battery prepared using the electrolytes of the above examples and comparative examples was tested using the Xinwei battery testing system. The obtained battery was activated at room temperature and tested for room temperature capacity, then placed in a low-temperature oven, and allowed to stand for 2 hours at the tested temperature before conducting a 0.2C constant current discharge test (when the temperature is less than -20°C, the cut-off voltage is modified to 2.5V, and the rest is 2.8V), and the capacity at different temperatures was recorded and compared with the room temperature capacity.
[0081] from Figure 1 It can be seen that the conductivity of Example 1 is improved to a certain extent at -70 to 60°C, especially at an extremely low temperature of -60°C, the conductivity can still reach 1.034mS / cm. The considerable conductivity ensures the excellent performance of the electrolyte in a wide temperature range. At the same time, within this temperature range, the electrolyte does not solidify or evaporate, and the liquid phase remains stable.
[0082] The upper limits of the electrochemical windows of the above three electrolytes were also tested. Figure 2 As shown, the upper limits of the electrochemical windows of Comparative Examples 1, 2, and Example 1 are 4.65 V, 4.94 V, and 5.40 V, respectively. Compared with the electrochemical window of 4.3 V of the reported traditional commercial carbonate, the upper limit of the electrochemical window is increased, and the oxidation resistance of the electrolyte is increased.
[0083] As shown in Table 1, it is a comparison table of low temperature specific capacities of NCM811||Li (0.2C) batteries prepared using the electrolytes of Examples 1, 2, 3, 4, 5 of the present invention and Comparative Examples 1, 2, 3.
[0084] Table 1 Comparison of battery low temperature discharge capacity and voltage
[0085]
[0086]
[0087] As can be seen from Table 1, by introducing diluents and additives to obtain Examples 1, 2, 3, 4, and 5, the cut-off voltage can be increased to 4.7V, bringing more capacity to the battery in a wide temperature range. By comparing Example 3, it can be seen that fluorosulfonyl fluorocarboxylate as an additive can better reduce the degree of solvation. By comparing Examples 1, 2, 4, and 5, it can be seen that the selected electrolyte components can bring more capacity to the battery by increasing the voltage to 4.7V under the synergistic effect, while promoting the dissolution of lithium salts and promoting the overall low-temperature performance of the battery. At the same time, by comparing Example 1 with Examples 2, 3, 4, and 5, the capacity of the battery at low temperatures is optimized by adjusting the proportion of additives.
[0088] from Figure 3It can be seen from the figure that the cycle performance of the electrolyte designed in Example 1 at 25°C is that when the charging voltage reaches 4.7V, the first cycle capacity is 202mAh / g. After 267 cycles, the capacity retention rate (CR) is 80%; after 800 cycles, the capacity retention rate is 63%, showing excellent room temperature stability.
[0089] from Figure 4 It can be seen that at 0.1C, the average capacity is 221 mAh / g, at 10C it is 161 mAh / g, and the retention rate is 73%, indicating that the rate performance of the electrolyte is effectively improved through the coordinated effect of the various components in the electrolyte.
[0090] from Figure 5 It can be seen that after 250 cycles, the capacity retention rate is 85.8%, and the average charge and discharge efficiency is greater than 99.9%, showing excellent high-rate fast charging and long-cycle performance.
[0091] from Figure 6 It can be seen that the NCM811||Li battery prepared by the electrolyte of Example 1 has a capacity retention rate of 76.6% after 100 cycles under the conditions of 25°C 2.8-4.7V and 10C high rate, showing ultra-high rate fast charge and discharge performance.
[0092] In order to test the wide temperature performance of the electrolyte, the NCM811||Li battery prepared using the electrolyte of Example 1 was tested for its cycle performance at -40℃0.2C and 60℃4C. The test results are as follows: Figure 7 and Figure 8 As shown. Figure 7 , Figure 8 It can be seen that at -40°C, the first cycle capacity is 150mAh / g, and the capacity retention rate after 55 cycles is 96.7%, showing excellent low-temperature cycle performance. At 60°C and 4C, after 80 cycles, the capacity retention rate is 81.6%, reflecting excellent high-temperature and high-rate performance, which is far higher than the existing technology.
[0093] It can be seen that the present invention vividly demonstrates the excellent wide temperature range, high voltage and high rate performance of the wide temperature range battery electrolyte.
[0094] The above description is only a preferred embodiment of the present invention. In view of the fact that technicians in the field of the present invention can make appropriate changes and modifications to the above implementation, the present invention is not limited to the specific implementation described above. Some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention.
Claims
1. A wide temperature range battery carboxylate-based electrolyte, Features: The electrolyte is composed of lithium salt, organic solvent, diluent and composite additive; the molar ratio of lithium salt, organic solvent and diluent is 5-10:30-40:40-50; The lithium salt includes at least one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium hexafluorophosphate, lithium difluorophosphate, lithium perchlorate, and lithium nitrate; The organic solvent comprises at least one of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl propionate, ethyl acetate, ethyl butyrate, butyl formate, butyl propionate, isobutyl formate, methyl difluoroacetate, ethyl difluoroacetate, methyl trifluoroacetate, and ethyl trifluoroacetate; The diluent comprises at least one of fluorobenzene, o-difluorobenzene, m-difluorobenzene, p-difluorobenzene, o-fluorotoluene, m-fluorotoluene and p-fluorotoluene; The composite additive is composed of methyl fluorosulfonyl difluoroacetate and lithium difluorooxalatoborate in a molar ratio of 5-15:1-2.5; Methyl fluorosulfonyl difluoroacetate accounts for 5% - 15% of the total amount of the electrolyte; lithium difluorooxalatoborate accounts for 1% - 2.5% of the total amount of the electrolyte.
2. A wide temperature range battery carboxylate-based electrolyte according to claim 1, Features: The lithium salt is selected from at least one of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium hexafluorophosphate, and lithium difluorophosphate.
3. A wide temperature range battery carboxylate-based electrolyte according to claim 1, Features: The percentage of lithium salt in the electrolyte is 0.1%~20%; The percentage of solvent in the total amount of electrolyte is 10%~60%; The percentage of diluent in the total amount of electrolyte is 20%~80%; The amount of the composite additive added is 1%-15% of the total amount of the electrolyte.
4. The wide temperature range battery carboxylate-based electrolyte according to claim 1, Features: The operating temperature of the wide temperature range battery electrolyte is -60 ~ 60 ° C.
5. The wide temperature range battery carboxylate-based electrolyte according to claim 1, Features: The lithium salt includes lithium bis(trifluoromethanesulfonyl imide) and / or lithium bis(fluorosulfonyl imide); Organic solvents include methyl propionate; The diluent includes o-difluorobenzene.
6. An application of the wide temperature range battery carboxylate-based electrolyte according to any one of claims 1 to 5, Features: The wide temperature range battery carboxylate-based electrolyte is used as a lithium battery electrolyte.