Environmentally friendly highly flame-retardant sponge and preparation method thereof
By using a combination technology of environmentally friendly base liquid and high-efficiency flame retardant in the sponge, the problem of smoke and bacterial growth generated by the combustion of flame retardant sponge is solved, the hydrophobicity and flame retardant properties of the sponge are improved, and the environmentally friendly high-fire retardant sponge is realized. preparation.
Patent Information
- Application Number
- CN202410496006.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-24
AI Technical Summary
Existing flame retardant sponges produce a large amount of smoke and toxic and corrosive gases when burned, and are prone to breeding bacteria during use, affecting environmental protection and human health.
Compounds such as 6-ethylindole, 7-ethylindole-3-formaldehyde are reacted with catalyst to form an environmentally friendly base liquid, and the melamine sponge is soaked in the base liquid and added high-efficiency flame retardant, and pass through magnetic groups. Fixed iron tetroxide, modified sponge surface, and prepared an environmentally friendly high flame retardant sponge.
This method transforms the sponge from hydrophilic lipophilicity to hydrophilic lipophilicity, and enhances the antibacterial properties through π-π action, improves the hydrophobic properties and flame retardant effects of the sponge. It is suitable for harsh environments, and the flame retardant is stable in the sponge. Existing, avoiding the toxicity problem of traditional flame retardants.
Smart Images

Figure GDA0005057550870000031 
Figure GDA0005057550870000032 
Figure GDA0005057550870000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmentally friendly high flame retardant sponges, and in particular to an environmentally friendly high flame retardant sponge and a preparation method thereof. Background Art
[0002] Sponge is a porous material with good water absorption and can be used to clean objects. The commonly used sponges are made of wood cellulose fibers or foamed plastic polymers. There are also natural sponges made from sponge animals. Most natural sponges are used for body cleaning or painting. There are also three types of synthetic sponges made of other materials, namely low-density polyether (non-absorbent sponge), polyvinyl alcohol (highly absorbent material, no obvious pores) and polyester;
[0003] The sponge foamed from chemical raw materials is easy to burn. Flame-retardant sponge is generally a fire-retardant material synthesized by adding flame retardants to various polyurethanes. It is mainly used in furniture manufacturing, massage equipment manufacturing, baby carriage manufacturing, decoration, automotive accessories, wall sound absorption, insulation pipes, fire doors and fire shutters. The main raw materials are flame retardants, isocyanates, polyethers, polyols, etc., and auxiliary raw materials include a small amount of freon, water, etc. Flame retardants currently mainly include organic flame retardants and inorganic flame retardants, halogen and non-halogen. Organic flame retardants are some flame retardants represented by bromine, phosphorus nitrogen, nitrogen and red phosphorus and compounds. Inorganic flame retardants are mainly antimony trioxide, magnesium hydroxide, aluminum hydroxide, silicon and other flame retardant systems. These flame retardants have been widely used in the field of polymer materials, but the sponge products made by adding these flame retardants will produce a lot of smoke and toxic corrosive gases when burning, so they are very environmentally unfriendly, and during use, they are easy to breed bacteria when recycled, which is harmful to health. Summary of the invention
[0004] In order to overcome the above technical problems, the object of the present invention is to provide an environmentally friendly highly flame retardant sponge and a preparation method thereof:
[0005] (1) Weighing 6-ethylindole, 7-ethylindole-3-carboxaldehyde, and a catalyst into a single-mouth bottle in sequence, then using a measuring cylinder to measure anhydrous ethanol and adding it to the single-mouth bottle to obtain an intermediate A, weighing the intermediate A and ferric chloride, then measuring 1,2-dichloroethane and adding it to a flask to obtain an intermediate B, weighing FeCl3·6H20 and intermediate B and adding them to a beaker, measuring distilled water and pouring it into the beaker, then adding FeSO4·7H20 and NH3·H20 into the beaker respectively and stirring to obtain an environmentally friendly base liquid, adding a melamine sponge into the environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring, taking out and rinsing with deionized water, and drying to obtain the environmentally friendly high flame retardant sponge, which solves the problem that sponge products generate a large amount of smoke and toxic corrosive gases when burned, which is very environmentally unfriendly, and are easily breeding bacteria during recycling during use, which is harmful to human health;
[0006] (2) Weigh polystyrene, trans-2-phenylvinyl borate pinacol ester, 1,5-cyclooctadiene iridium chloride dimer, and 4,4'-di-tert-butyl-2,2'-bipyridine, and add them to a round-bottom flask in sequence; add tetrahydrofuran, stir to react, and pour into cold methanol to obtain intermediate D; weigh 2-[(4-bromobenzyl)oxy]benzoyl chloride, trineopentyl phosphite, and 1,4-dioxane into a round-bottom flask to obtain intermediate E; weigh intermediate D, intermediate E, [1,1'-bis(diphenylphosphino)ferrocene]dichloropalladium dichloromethane complex, and potassium phosphate, and add them to a round-bottom flask in sequence; add tetrahydrofuran, heat, add deionized water, pour into cold water, dry, and grind to obtain a high-efficiency flame retardant. The invention solves the problem that sponge products prepared by traditional methods generate a large amount of smoke and toxic and corrosive gases when burned, which is very environmentally unfriendly.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] An environmentally friendly highly flame-retardant sponge is prepared by the following steps:
[0009] S1: Weigh 6-ethylindole, 7-ethylindole-3-carboxaldehyde, and the catalyst into a single-necked bottle in sequence, then use a measuring cylinder to measure anhydrous ethanol and add it into the single-necked bottle, stir at room temperature for 1-3 hours, and then spin dry to obtain intermediate A;
[0010] The chemical reaction formula is as follows:
[0011]
[0012] S2: weigh intermediate A and ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 1,2-dichloroethane and add it into the flask, stir the mixture at room temperature for 24-36 hours to obtain intermediate B;
[0013] The chemical reaction formula is as follows:
[0014]
[0015] S3: Weigh FeCl3·6H20 and intermediate B into a beaker, measure distilled water and pour it into the beaker, heat it to 60-80°C, then add FeSO4·7H20 and NH3·H20 into the beaker respectively and stir to obtain an environmentally friendly base liquid;
[0016] S4: adding melamine sponge to an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring for 24-36 hours, introducing magnetic groups to the sponge surface, taking it out and rinsing it with deionized water, drying it, and fixing ferroferric oxide on the sponge surface by the adhesion between the polymer and the sponge, thereby obtaining the environmentally friendly high flame retardant sponge;
[0017] The high-efficiency flame retardant in step S4 is prepared by the following steps:
[0018] S61: Weigh polystyrene, trans-2-phenylvinyl borate pinacol ester, 1,5-cyclooctadiene iridium chloride dimer, and 4,4'-di-tert-butyl-2,2'-bipyridine, add them into a round-bottom flask in sequence, add tetrahydrofuran, replace the reaction system with nitrogen atmosphere, continue to stir the reaction at 80-100°C for 24-36h, cool to room temperature, pour into cold methanol, stir for 2-3h, collect the precipitated polymer by filtration, and dry under vacuum at 50-80°C for 24-36h to obtain intermediate D;
[0019] The chemical reaction formula is as follows:
[0020]
[0021] S62: Under nitrogen environment, weigh 2-[(4-bromobenzyl)oxy]benzoyl chloride, trineopentyl phosphite and 1,4-dioxane into a round-bottom flask, and reflux at 100-120° C. for 48-60 h to obtain intermediate E;
[0022] The chemical reaction formula is as follows:
[0023]
[0024] S63: Weigh intermediate D, intermediate E, [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, and potassium phosphate, add them into a round-bottom flask in sequence, add tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. After heating to 80-100°C, add deionized water, and then continue to stir the reaction for 24-36 hours. After the reaction solution is cooled to room temperature, pour it into cold water, stir for 1-3 hours, and then dry it under vacuum at 50-70°C for 48-60 hours, grind it, and obtain a high-efficiency flame retardant.
[0025] The chemical reaction formula is as follows:
[0026]
[0027] As a further scheme of the present invention: the usage ratio of 6-ethylindole, 7-ethylindole-3-carboxaldehyde, catalyst and anhydrous ethanol in step S1 is 1.5 g: 0.9 g: 0.2 g: 40 mL, and the catalyst is p-toluenesulfonic acid.
[0028] As a further solution of the present invention: the usage ratio of the intermediate A, ferric chloride and 1,2-dichloroethane in step S2 is 0.5 g:0.6 g:25 mL.
[0029] As a further solution of the present invention: the usage ratio of FeCl3·6H20, intermediate B, distilled water, FeSO4·7H20, and NH3·H20 in step S3 is 6.5g:2g:100mL:3.6g:24mL.
[0030] As a further solution of the present invention: the usage ratio of the environmentally friendly base liquid to the high-efficiency flame retardant in step S4 is 50 mL:25 g.
[0031] As a further solution of the present invention: the usage ratio of polystyrene, trans-2-phenylvinyl boronate pinacol ester, 1,5-cyclooctadiene iridium chloride dimer, 4,4'-di-tert-butyl-2,2'-bipyridine, tetrahydrofuran and cold methanol in step S61 is 6g:23.0g:0.5g:0.4g:100mL:500mL.
[0032] As a further solution of the present invention: the usage ratio of 2-[(4-bromobenzyl)oxy]benzoyl chloride, trineopentyl phosphite and 1,4-dioxane in step S62 is 20 g:20 mL:100 mL.
[0033] As a further scheme of the present invention: the usage ratio of intermediate D, intermediate E, [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, potassium phosphate, tetrahydrofuran, deionized water and cold water in step S63 is 10.5g:19.4g:0.9g:15g:150mL:15mL:600mL.
[0034] A method for preparing an environmentally friendly highly flame-retardant sponge comprises the following steps:
[0035] S1: Weigh 6-ethylindole, 7-ethylindole-3-carboxaldehyde, and the catalyst into a single-necked bottle in sequence, then use a measuring cylinder to measure anhydrous ethanol and add it into the single-necked bottle, stir at room temperature for 1-3 hours, and then spin dry to obtain intermediate A;
[0036] S2: weigh intermediate A and ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 1,2-dichloroethane and add it into the flask, stir the mixture at room temperature for 24-36 hours to obtain intermediate B;
[0037] S3: Weigh FeCl3·6H20 and intermediate B into a beaker, measure distilled water and pour it into the beaker, heat it to 60-80°C, then add FeSO4·7H20 and NH3·H20 into the beaker respectively and stir to obtain an environmentally friendly base liquid;
[0038] S4: Add melamine sponge to environmentally friendly base liquid, then add high-efficiency flame retardant, soak and stir for 24-36 hours, introduce magnetic groups into the sponge surface, take it out and rinse with deionized water, dry it, and fix ferroferric oxide on the sponge surface by relying on the adhesion between the polymer and the sponge to obtain the environmentally friendly high flame retardant sponge.
[0039] Beneficial effects of the present invention:
[0040] (1) The present invention comprises the following steps: weighing 6-ethylindole, 7-ethylindole-3-carboxaldehyde, and a catalyst, and then using a measuring cylinder to measure anhydrous ethanol and add it to the single-mouth bottle to obtain an intermediate A; weighing intermediate A and ferric chloride; and then measuring 1,2-dichloroethane and adding it to a flask to obtain an intermediate B; weighing FeCl3·6H20 and intermediate B and adding them to a beaker; measuring distilled water and pouring it into the beaker; and then respectively adding FeSO4·7H20 and NH3·H20 to the beaker and stirring to obtain an environmentally friendly base liquid; adding a melamine sponge to the environmentally friendly base liquid; and then adding a high-efficiency flame retardant, soaking and stirring, and then taking out and rinsing with deionized water and drying to obtain the environmentally friendly high flame retardant sponge. The environmentally friendly high flame retardant sponge is formed by interlacing stick-like fiber structures, has a rich pore structure, a smooth surface without a microscopic rough structure, and a melamine sponge. After the sponge is loaded with polymer, the surface becomes uneven and has a microscopic rough structure. This change in surface roughness causes the melamine sponge to change from hydrophilic to hydrophobic, and the sponge surface has a more complex rough structure. The introduction of ferroferric oxide increases the surface roughness, which further improves the hydrophobicity of the composite sponge, changing from hydrophobic to super-hydrophobic. The indole group is cheap and easy to obtain, and indole derivatives are also used for antibacterial activity. The environmentally friendly base liquid has a larger conjugated system, and the structural unit is evenly and firmly distributed on the sponge skeleton through the face-to-face π-π interaction with the triazine ring in the sponge. Compared with the point-to-point hydrogen bonding, the face-to-face π-π interaction has a larger action surface and a stronger force, and also gives the sponge excellent antibacterial properties, so that the sponge material can be used in harsher environments.
[0041] (2) Weigh polystyrene, trans-2-phenylvinyl borate pinacol ester, 1,5-cyclooctadiene iridium chloride dimer, and 4,4'-di-tert-butyl-2,2'-bipyridine, and add them to a round-bottom flask in sequence. Add tetrahydrofuran, stir to react, and pour into cold methanol to obtain intermediate D. Weigh 2-[(4-bromobenzyl)oxy]benzoyl chloride, trineopentyl phosphite, and 1,4-dioxane to a round-bottom flask to obtain intermediate E. Weigh intermediate D, intermediate E, [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride, and dichloromethane. The complex and potassium phosphate are sequentially added into a round-bottom flask, tetrahydrofuran is added, heated, deionized water is added, poured into cold water, dried, and ground to obtain a high-efficiency flame retardant. The present invention utilizes three simple steps with high yield to functionalize polystyrene to prepare a phosphate functionalized flame retardant, wherein the phosphorus-containing macromolecular flame retardant has good compatibility with the polymer sponge substrate, can stably exist in the polymer matrix, and is not easy to migrate out. Compared with other types of flame retardants, it has the advantages of environmental protection, safety, and good flame retardant effect, thereby achieving the purpose of improving flame retardancy. DETAILED DESCRIPTION
[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Embodiment 1:
[0044] This embodiment is an environmentally friendly highly flame-retardant sponge, which is prepared by the following steps:
[0045] S1: Weigh 1.5 g of 6-ethylindole, 0.9 g of 7-ethylindole-3-carboxaldehyde, and 0.2 g of a catalyst and add them into a single-necked bottle in sequence. Then use a measuring cylinder to measure 40 mL of anhydrous ethanol and add it into the single-necked bottle. Stir at room temperature for 1 h and then spin dry to obtain intermediate A.
[0046] S2: Weigh 0.5 g of intermediate A and 0.6 g of ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 25 mL of 1,2-dichloroethane and add it into the flask, and stir the mixture at room temperature for 24 hours to obtain intermediate B;
[0047] S3: Weigh 6.5 g of FeCl3·6H20 and 2 g of intermediate B into a beaker, measure 100 mL of distilled water and pour it into the beaker, heat it to 60°C, then add 3.6 g of FeSO4·7H20 and 24 mL of NH3·H20 into the beaker and stir to obtain an environmentally friendly base liquid;
[0048] S4: adding melamine sponge to an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring for 24 hours, introducing magnetic groups to the sponge surface, taking it out and rinsing it with deionized water, drying it, and fixing ferroferric oxide on the sponge surface by the adhesion between the polymer and the sponge, thereby obtaining the environmentally friendly high flame retardant sponge;
[0049] The high-efficiency flame retardant is prepared by the following steps:
[0050] S61: 6 g of polystyrene, 23.0 g of trans-2-phenylvinyl boronate pinacol ester, 0.5 g of 1,5-cyclooctadiene iridium chloride dimer, and 0.4 g of 4,4'-di-tert-butyl-2,2'-bipyridine were weighed and added into a round-bottom flask in sequence, and 100 mL of tetrahydrofuran was added, and the reaction system was replaced with a nitrogen atmosphere. The reaction was continued under stirring at 80° C. for 24 h, cooled to room temperature, poured into 500 mL of cold methanol, stirred for 2 h, filtered to collect the precipitated polymer, and dried under vacuum at 50° C. for 24 h to obtain intermediate D;
[0051] S62: Under nitrogen environment, 20 g of 2-[(4-bromobenzyl)oxy]benzoyl chloride, 20 mL of trineopentyl phosphite and 100 mL of 1,4-dioxane were weighed into a round-bottom flask, and the mixture was refluxed at 100° C. for 48 h to obtain intermediate E;
[0052] S63: Weigh 10.5 g of intermediate D, 19.4 g of intermediate E, 0.9 g of [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, and 15 g of potassium phosphate, add them into a round-bottom flask in sequence, add 150 mL of tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. After heating to 80°C, add 15 mL of deionized water, and then continue to stir the reaction for 24 hours. After the reaction solution is cooled to room temperature, pour it into 600 mL of cold water, stir for 1 hour, and then dry it under vacuum at 50°C for 48 hours, grind it, and obtain a high-efficiency flame retardant.
[0053] Embodiment 2:
[0054] This embodiment is an environmentally friendly highly flame-retardant sponge, which is prepared by the following steps:
[0055] S1: Weigh 1.5 g of 6-ethylindole, 0.9 g of 7-ethylindole-3-carboxaldehyde, and 0.2 g of a catalyst and add them into a single-necked bottle in sequence. Then use a measuring cylinder to measure 40 mL of anhydrous ethanol and add it into the single-necked bottle. Stir at room temperature for 1 h and then spin dry to obtain intermediate A.
[0056] S2: Weigh 0.5 g of intermediate A and 0.6 g of ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 25 mL of 1,2-dichloroethane and add it into the flask, and stir the mixture at room temperature for 24 hours to obtain intermediate B;
[0057] S3: Weigh 6.5 g of FeCl3·6H20 and 2 g of intermediate B into a beaker, measure 100 mL of distilled water and pour it into the beaker, heat it to 60°C, then add 3.6 g of FeSO4·7H20 and 24 mL of NH3·H20 into the beaker and stir to obtain an environmentally friendly base liquid;
[0058] S4: adding melamine sponge to an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring for 24 hours, introducing magnetic groups to the sponge surface, taking it out and rinsing it with deionized water, drying it, and fixing ferroferric oxide on the sponge surface by the adhesion between the polymer and the sponge, thereby obtaining the environmentally friendly high flame retardant sponge;
[0059] The high-efficiency flame retardant is prepared by the following steps:
[0060] S61: 6 g of polystyrene, 23.0 g of trans-2-phenylvinyl boronate pinacol ester, 0.5 g of 1,5-cyclooctadiene iridium chloride dimer, and 0.4 g of 4,4'-di-tert-butyl-2,2'-bipyridine were weighed and added into a round-bottom flask in sequence, and 100 mL of tetrahydrofuran was added, and the reaction system was replaced with a nitrogen atmosphere. The reaction was continued under stirring at 100° C. for 36 h, cooled to room temperature, poured into 500 mL of cold methanol, stirred for 3 h, filtered to collect the precipitated polymer, and dried under vacuum at 80° C. for 36 h to obtain intermediate D;
[0061] S62: Under nitrogen environment, 20 g of 2-[(4-bromobenzyl)oxy]benzoyl chloride, 20 mL of trineopentyl phosphite and 100 mL of 1,4-dioxane were weighed into a round-bottom flask, and the mixture was refluxed at 120° C. for 60 h to obtain intermediate E;
[0062] S63: Weigh 10.5 g of intermediate D, 19.4 g of intermediate E, 0.9 g of [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, and 15 g of potassium phosphate, add them into a round-bottom flask in sequence, add 150 mL of tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. After heating to 100°C, add 15 mL of deionized water, and then continue to stir the reaction for 36 hours. After the reaction solution is cooled to room temperature, pour it into 600 mL of cold water, stir for 3 hours, and then dry it under vacuum at 70°C for 60 hours. Grind it to obtain a high-efficiency flame retardant.
[0063] Embodiment 3:
[0064] This embodiment is an environmentally friendly highly flame-retardant sponge, which is prepared by the following steps:
[0065] S1: Weigh 1.5 g of 6-ethylindole, 0.9 g of 7-ethylindole-3-carboxaldehyde, and 0.2 g of a catalyst and add them into a single-necked bottle in sequence. Then use a measuring cylinder to measure 40 mL of anhydrous ethanol and add it into the single-necked bottle. Stir at room temperature for 3 h and then spin dry to obtain intermediate A.
[0066] S2: Weigh 0.5 g of intermediate A and 0.6 g of ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 25 mL of 1,2-dichloroethane and add it into the flask, and stir the mixture at room temperature for 36 hours to obtain intermediate B;
[0067] S3: Weigh 6.5 g of FeCl3·6H20 and 2 g of intermediate B into a beaker, measure 100 mL of distilled water and pour it into the beaker, heat it to 80°C, then add 3.6 g of FeSO4·7H20 and 24 mL of NH3·H20 into the beaker and stir to obtain an environmentally friendly base liquid;
[0068] S4: adding melamine sponge to an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring for 36 hours, introducing magnetic groups to the sponge surface, taking it out and rinsing it with deionized water, drying it, and fixing ferroferric oxide on the sponge surface by the adhesion between the polymer and the sponge, thereby obtaining the environmentally friendly high flame retardant sponge;
[0069] The high-efficiency flame retardant is prepared by the following steps:
[0070] S61: 6 g of polystyrene, 23.0 g of trans-2-phenylvinyl boronate pinacol ester, 0.5 g of 1,5-cyclooctadiene iridium chloride dimer, and 0.4 g of 4,4'-di-tert-butyl-2,2'-bipyridine were weighed and added into a round-bottom flask in sequence, and 100 mL of tetrahydrofuran was added, and the reaction system was replaced with a nitrogen atmosphere. The reaction was continued under stirring at 80° C. for 24 h, cooled to room temperature, poured into 500 mL of cold methanol, stirred for 2 h, filtered to collect the precipitated polymer, and dried under vacuum at 50° C. for 24 h to obtain intermediate D;
[0071] S62: Under nitrogen environment, 20 g of 2-[(4-bromobenzyl)oxy]benzoyl chloride, 20 mL of trineopentyl phosphite and 100 mL of 1,4-dioxane were weighed into a round-bottom flask, and the mixture was refluxed at 100° C. for 48 h to obtain intermediate E;
[0072] S63: Weigh 10.5 g of intermediate D, 19.4 g of intermediate E, 0.9 g of [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, and 15 g of potassium phosphate, add them into a round-bottom flask in sequence, add 150 mL of tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. After heating to 80°C, add 15 mL of deionized water, and then continue to stir the reaction for 36 hours. After the reaction solution is cooled to room temperature, pour it into 600 mL of cold water, stir for 1 hour, and then dry it under vacuum at 50°C for 48 hours, grind it, and obtain a high-efficiency flame retardant.
[0073] Embodiment 4:
[0074] This embodiment is an environmentally friendly highly flame-retardant sponge, which is prepared by the following steps:
[0075] S1: Weigh 1.5 g of 6-ethylindole, 0.9 g of 7-ethylindole-3-carboxaldehyde, and 0.2 g of a catalyst and add them into a single-necked bottle in sequence. Then use a measuring cylinder to measure 40 mL of anhydrous ethanol and add it into the single-necked bottle. Stir at room temperature for 3 h and then spin dry to obtain intermediate A.
[0076] S2: Weigh 0.5 g of intermediate A and 0.6 g of ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 25 mL of 1,2-dichloroethane and add it into the flask, and stir the mixture at room temperature for 36 hours to obtain intermediate B;
[0077] S3: Weigh 6.5 g of FeCl3·6H20 and 2 g of intermediate B into a beaker, measure 100 mL of distilled water and pour it into the beaker, heat it to 80°C, then add 3.6 g of FeSO4·7H20 and 24 mL of NH3·H20 into the beaker and stir to obtain an environmentally friendly base liquid;
[0078] S4: adding melamine sponge to an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring for 36 hours, introducing magnetic groups to the sponge surface, taking it out and rinsing it with deionized water, drying it, and fixing ferroferric oxide on the sponge surface by the adhesion between the polymer and the sponge, thereby obtaining the environmentally friendly high flame retardant sponge;
[0079] The high-efficiency flame retardant is prepared by the following steps:
[0080] S61: 6 g of polystyrene, 23.0 g of trans-2-phenylvinyl boronate pinacol ester, 0.5 g of 1,5-cyclooctadiene iridium chloride dimer, and 0.4 g of 4,4'-di-tert-butyl-2,2'-bipyridine were weighed and added into a round-bottom flask in sequence, and 100 mL of tetrahydrofuran was added, and the reaction system was replaced with a nitrogen atmosphere. The reaction was continued under stirring at 100° C. for 36 h, cooled to room temperature, poured into 500 mL of cold methanol, stirred for 3 h, filtered to collect the precipitated polymer, and dried under vacuum at 80° C. for 36 h to obtain intermediate D;
[0081] S62: Under nitrogen environment, 20 g of 2-[(4-bromobenzyl)oxy]benzoyl chloride, 20 mL of trineopentyl phosphite and 100 mL of 1,4-dioxane were weighed into a round-bottom flask, and the mixture was refluxed at 120° C. for 60 h to obtain intermediate E;
[0082] S63: Weigh 10.5 g of intermediate D, 19.4 g of intermediate E, 0.9 g of [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, and 15 g of potassium phosphate, add them into a round-bottom flask in sequence, add 150 mL of tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. After heating to 100°C, add 15 mL of deionized water, and then continue to stir the reaction for 36 hours. After the reaction solution is cooled to room temperature, pour it into 600 mL of cold water, stir for 3 hours, and then dry it under vacuum at 70°C for 60 hours. Grind it to obtain a high-efficiency flame retardant.
[0083] Comparative Example 1:
[0084] The difference between Comparative Example 1 and Example 1 is that no flame retardant is added.
[0085] Comparative Example 2:
[0086] Comparative Example 2 used a commercially available flame retardant sponge.
[0087] Performance Testing
[0088] The flame retardant sponges of Examples 1-4 and Comparative Examples 1-2 were subjected to vertical combustion tests according to GBT5455-1997 standard, with standard classification as follows: B1: damage length <150 mm, afterflame time <5 s, smoldering time <5 s; B2: damage length <200 mm, afterflame time <15 s, smoldering time <10 s, sample size: 30 × 80 cm, 15 samples were taken in each of the warp and weft directions, the flame height was controlled at 40 ± 2 mm, and the ignition time was 12 s; instrument model: vertical flame retardant tester HK-HVR;
[0089] The test results are shown in the following table:
[0090] Test items Smoldering time / s Afterburning time / s Droplets Flame retardant grade Rebound rate / % Example 1 0 0 none B1 55 Example 2 0 0 none B1 54 Example 3 0 0 none B1 55 Example 4 0 0 none B1 56 Comparative Example 1 3 6 none B2 53 Comparative Example 2 5 8 none B2 43
[0091] It can be seen from the above table that the smoldering time of the embodiment is 0s, the afterflaming time is also 0s, there is no droplet phenomenon, the flame retardant grade is B1, and the rebound rate of the embodiment is 44%-56%, while the smoldering time of comparative example 1 is 3s, the afterflaming time is 6s, there is no droplet phenomenon, the flame retardant grade is B2, and the rebound rate of comparative example 1 is 53%, while the smoldering time of comparative example 2 is 5s, the afterflaming time is 8s, there is no droplet phenomenon, the flame retardant grade is B2, and the rebound rate of comparative example 2 is 43%. The experimental effects of the embodiments are better than those of the comparative examples, so the performance of the flame retardant sponge prepared by the present invention is greatly improved compared with the prior art.
[0092] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0093] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An environmentally friendly highly flame-retardant sponge, characterized in that: The environmentally friendly highly flame-retardant sponge is prepared by the following steps: S1: Weigh 6-ethylindole, 7-ethylindole-3-carboxaldehyde, and the catalyst into a single-necked bottle in sequence, then use a measuring cylinder to measure anhydrous ethanol and add it into the single-necked bottle, stir at room temperature, and then spin dry to obtain intermediate A; S2: weighing intermediate A and ferric chloride, adding them into a flask in sequence under a nitrogen atmosphere, then weighing 1,2-dichloroethane and adding it into the flask, stirring the mixture at room temperature to obtain intermediate B; S3: Weigh FeCl3·6H20 and intermediate B into a beaker, measure distilled water and pour it into the beaker, heat it, then add FeSO4·7H20 and NH3·H20 into the beaker and stir to obtain an environmentally friendly base liquid; S4: adding melamine sponge into an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring, taking out, rinsing with deionized water, and drying to obtain the environmentally friendly high flame retardant sponge; The high-efficiency flame retardant in step S4 is prepared by the following steps: S61: Weigh polystyrene, trans-2-phenylvinyl borate pinacol ester, 1,5-cyclooctadiene iridium chloride dimer, and 4,4'-di-tert-butyl-2,2'-bipyridine, and add them into a round-bottom flask in sequence, add tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. Continue to stir the reaction under heating conditions, cool to room temperature, pour into cold methanol, stir, collect the precipitated polymer by filtration, and dry under vacuum to obtain intermediate D; S62: Under nitrogen environment, 2-[(4-bromobenzyl)oxy]benzoyl chloride, trineopentyl phosphite and 1,4-dioxane were weighed into a round-bottom flask, and refluxed under heating conditions to obtain intermediate E; S63: Weigh intermediate D, intermediate E, [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride dichloromethane complex, and potassium phosphate, add them into a round-bottom flask in sequence, add tetrahydrofuran, and replace the reaction system with a nitrogen atmosphere. Heat, add deionized water, and then continue to stir the reaction. After the reaction solution is cooled to room temperature, pour it into cold water, stir, dry under vacuum, and grind to obtain a high-efficiency flame retardant.
2. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: In step S1, the usage ratio of 6-ethylindole, 7-ethylindole-3-carboxaldehyde, catalyst and anhydrous ethanol is 1.5 g: 0.9 g: 0.2 g: 40 mL, and the catalyst is p-toluenesulfonic acid.
3. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: The usage ratio of the intermediate A, ferric chloride and 1,2-dichloroethane in step S2 is 0.5 g:0.6 g:25 mL.
4. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: The usage ratio of FeCl3·6H20, intermediate B, distilled water, FeSO4·7H20, and NH3·H20 in step S3 is 6.5g:2g:100mL:3.6g:24mL.
5. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: The usage ratio of the environmentally friendly base liquid to the high-efficiency flame retardant in step S4 is 50 mL: 25 g.
6. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: The usage ratio of polystyrene, trans-2-phenylvinyl boronate pinacol ester, 1,5-cyclooctadiene iridium chloride dimer, 4,4'-di-tert-butyl-2,2'-bipyridine, tetrahydrofuran and cold methanol in step S61 is 6g:23.0g:0.5g:0.4g:100mL:500mL.
7. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: The usage ratio of 2-[(4-bromobenzyl)oxy]benzoyl chloride, trineopentyl phosphite and 1,4-dioxane in step S62 is 20 g:20 mL:100 mL.
8. The environmentally friendly highly flame-retardant sponge according to claim 1, characterized in that: The usage ratio of intermediate D, intermediate E, [1,1'-bis(diphenylphosphino)ferrocene] dichloropalladium dichloromethane complex, potassium phosphate, tetrahydrofuran, deionized water and cold water in step S63 is 10.5g:19.4g:0.9g:15g:150mL:15mL:600mL.
9. A method for preparing an environmentally friendly highly flame-retardant sponge according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: Weigh 6-ethylindole, 7-ethylindole-3-carboxaldehyde, and the catalyst into a single-necked bottle in sequence, then use a measuring cylinder to measure anhydrous ethanol and add it into the single-necked bottle, stir at room temperature for 1-3 hours, and then spin dry to obtain intermediate A; S2: weigh intermediate A and ferric chloride, add them into a flask in sequence under a nitrogen atmosphere, then weigh 1,2-dichloroethane and add it into the flask, stir the mixture at room temperature for 24-36 hours to obtain intermediate B; S3: Weigh FeCl3·6H20 and intermediate B into a beaker, measure distilled water and pour it into the beaker, heat it to 60-80°C, then add FeSO4·7H20 and NH3·H20 into the beaker respectively and stir to obtain an environmentally friendly base liquid; S4: adding melamine sponge into an environmentally friendly base liquid, then adding a high-efficiency flame retardant, soaking and stirring, taking out, rinsing with deionized water, and drying to obtain the environmentally friendly high flame retardant sponge.