A method for preparing a detachable precision casting frame

Through the assembly of multiple assemblies and the design of high-alloy steel materials, the problems of deformation and high heat loss of the existing material frame at high temperatures are solved, achieving higher thermomechanical strength and lower operating costs.

CN118326142BActive Publication Date: 2024-10-29XINGHUA JIANDA CASTING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410749039.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-29
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The existing integrated material frame has problems such as easy deformation during high-temperature heat treatment, insufficient bearing capacity, high heat loss, high replacement costs, and high production and operation costs.

Method used

Multiple assembly parts are used to assemble a detachable precision-cast material frame. High-alloy steel materials are used, and the material density and tightness are increased through the wax mold casting process. The interspersed fixed structure and reasonable gaps between the fence and the chassis are designed to reduce thermal expansion and deformation. , and improve the thermo-mechanical strength and wear resistance of the material through rare metal elements such as W, Co, and Nb.

Benefits of technology

It effectively reduces the deformation and heat loss of the material frame at high temperatures, improves the thermo-mechanical strength and service life of the material frame, reduces replacement costs and production and operation costs, and increases the number of cycles and load-bearing capacity of the material frame.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326142B_ABST
    Figure CN118326142B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method of a detachable precision casting material frame, which belongs to the field of precision casting technology and solves the problems that the material, structure and casting strength of the existing push rod furnace bearing material frame are not high and are easy to crack and deform. A preparation method of a detachable precision casting material frame, the preparation method comprises: separately manufacturing assembly parts of the precision casting material frame, the assembly parts include a chassis, a sub-fence, a chassis and a sub-fence connector, and a sub-fence connector; assembling the assembly parts of the precision casting material frame to form a detachable precision casting material frame. The assembly parts are made of high-alloy steel, and the element composition of the high-alloy steel is: C: 0.1-0.2%, Cr: 24-27%, Ni: 19-22%, W: 2.5-3.5%; Co: 1.0-2.0%; Nb: 0.5-1.0%, S: ≤0.035%, P: ≤0.035%, and the rest are Fe and unavoidable impurities. The thermomechanical strength of the push rod furnace material frame is improved, and the use cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of precision casting, and in particular to a method for preparing a detachable precision casting frame. Background Art

[0002] As a continuous heat treatment tool, the push rod furnace periodically heats, quenches, tempers and other heat treatment processes on the trays or frames containing the parts to be processed. The heating temperature is as high as 1050°C. This requires that the frame that carries the parts must be able to adapt to high temperatures and chemical corrosion in terms of material and structural design, and have high thermomechanical fatigue strength; and it is necessary to consider the impact of high-temperature thermal expansion and frequent temperature changes on the dimensional stability and matching accuracy of the frame.

[0003] The prior art uses an integral lost foam casting process to cast an integrated material frame. The density of the material frame steel body is not enough, resulting in cracks in the material frame during the quenching process. The cracks gradually deepen during use, resulting in a break in the chassis, which requires the replacement of the material tray, resulting in high cost losses; the material frame is easily deformed during the heating process, and the deformed material tray is easily stuck in the continuous push rod furnace, resulting in production line interruption and high equipment shutdown and maintenance costs; the material tray itself is heavy, which limits its carrying capacity and reduces the overall work efficiency; because the heat treatment tooling must be heated together with the parts, sometimes the heat taken away by the tooling is equal to or greater than the heat of the workpiece, accounting for about 18% to 29% of the total heat, increasing the heat treatment production cost. Summary of the invention

[0004] In view of the above analysis, an embodiment of the present invention aims to provide a method for preparing a detachable precision casting material frame, so as to solve at least one of the problems existing in the existing one-piece material frame, such as easy deformation and insufficient bearing capacity, high heat loss, insufficient thermal cycle performance, easy to get stuck, high replacement cost and production and operation cost.

[0005] An embodiment of the present invention provides a method for preparing a detachable precision casting frame, the method comprising:

[0006] Preparing an assembly part of a precision casting frame, the assembly part comprising a chassis, a sub-rail, a chassis and sub-rail connecting piece, and a sub-rail connecting piece;

[0007] Assemble the assembly parts of the precision casting frame to form a detachable precision casting frame.

[0008] Furthermore, the assembly part is made of high alloy steel, and the element composition of the high alloy steel is, by mass percentage, C: 0.1-0.2%, Cr: 24-27%, Ni: 19-22%, W: 2.5-3.5%; Co: 1.0-2.0%; Nb: 0.5-1.0%, S: ≤0.035%, P: ≤0.035%, and the rest is Fe and unavoidable impurities.

[0009] Specifically, the thermal expansion coefficient of the high alloy steel in the range of room temperature to 1100°C is 10×10 -6 / ℃~13×10 -6 / ℃.

[0010] Furthermore, wax casting is used to manufacture the assembly parts of the precision casting frame respectively.

[0011] Specifically, the wax casting includes: a smelting process of high alloy steel, and the smelting process of high alloy steel includes:

[0012] Step 1. Put the alloy raw materials into a vacuum melting chamber, evacuate and maintain the vacuum degree below 0.67Pa;

[0013] Step 2: heating to above 1700°C to melt the alloy raw materials in the vacuum melting chamber;

[0014] Step 3: After the raw materials in the vacuum melting chamber are completely melted, they are refined to obtain a refined alloy liquid.

[0015] Exemplarily, in step 3, the refining process is to introduce inert gas argon into the vacuum melting chamber, maintain the vacuum degree between 15-150 Pa, continue heating to 1750° C. to 1850° C., and keep warm for 15 to 25 minutes to obtain a molten alloy.

[0016] Furthermore, the preparation method also includes: assembling and welding a wax mold according to the shape of the supporting frame assembly, and coating a shell material on the surface of the wax mold.

[0017] Furthermore, the preparation method also includes shell casting, pouring molten alloy into the shell to obtain an assembly part of the precision casting frame.

[0018] Preferably, the pouring temperature is 1550-1650°C, and the mold shell temperature is controlled to be 1000-1100°C during pouring.

[0019] Furthermore, the assembly parts of the precision casting frame to form a detachable precision casting frame include:

[0020] Step 1. Assemble the long side fences: After the connecting rings at one end of the adjacent long side fences are alternately arranged in the height direction to reach a coaxial state, the connecting rods are passed through the connecting rings at the ends of the adjacent long side fences from top to bottom in sequence to achieve the articulation between the adjacent long side fences, with a connection angle of 180°, to form a set of long side fences;

[0021] Step 2. Assemble the frame: Place a set of long side fences and short side sub-fences at a 90° angle, ensure that the connecting rings at the ends of the long side fences and the short side sub-fences are alternately arranged in the height direction and reach a coaxial state, and pass the connecting rods through the connecting rings at the ends of the long side fences and the short side sub-fences from top to bottom to form a fence assembly;

[0022] The two fence assemblies are assembled into a rectangular frame structure in a manner that the long side fences are parallel and the short side sub-fences are parallel; after the connecting rings at the connection of the long side fence of one fence assembly and the short side sub-fence of the other fence are alternately arranged in the height direction to reach a coaxial state, the connecting rods are sequentially passed through the connecting rings at the connection of the ends of the adjacent fences from top to bottom to achieve connection;

[0023] Step 3. Position adjustment: Place the chassis with the bottom plate and frame integrally formed horizontally, put the assembled frame into the inner side of the chassis frame, make the bottom edge of the fence abut against the bottom plate of the chassis, and ensure that the movable clearance between the four fences constituting the frame and the frame of the chassis is 5-13mm;

[0024] Step 4. Connect the chassis: Insert the pins from the outside of the chassis frame to the inside through the frame pin holes and the fence round holes in sequence, insert and fix the fence on the inner side of the frame to complete the assembly of the material frame with one side open.

[0025] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0026] 1. The preparation method of the material frame of the present invention uses multiple assembly parts to assemble into an integral material frame, and decomposes the precision casting material frame into a chassis, a sub-fence, a chassis and a sub-fence connection piece, and a sub-fence connection piece assembly part to form an assembleable and detachable precision casting material frame. Compared with the one-piece material frame in the prior art, on the one hand, the single casting part of the present invention has a smaller volume, and the thermal expansion and contraction values ​​during the heating and cooling process are smaller, which reduces the possibility of the material frame being stuck in the continuous push rod furnace due to thermal expansion; on the other hand, the material frame of the present invention is a detachable structure, and damaged parts can be replaced separately, which greatly reduces the cost of replacing the material frame.

[0027] 2. The present invention is based on a preparation method of assembling a whole material frame using a plurality of assembly parts, and designs the material of the material frame. By adjusting the alloy elements of the material frame material, heat-resistant alloy steel with Cr and Ni as the main elements is selected, and the design adds rare metal elements W, Co and Nb. The W element promotes the transformation of austenite into martensite to enhance hardness, improve wear resistance and abrasion resistance, the Co element promotes martensite transformation, increases toughness and strength, and the Nb element refines the grains to increase the thermal strength of the material tray, and the ability to resist rapid cooling, that is, thermal stress, and effectively prevents excessive penetration of the C element during the heat treatment process, avoiding product cracking. The above-mentioned element ratio ensures that the material frame material of the present invention has a lower thermal expansion coefficient, the ability to resist rapid cooling and thermal stress, avoids product cracking, improves the thermal mechanical strength of the material frame, and increases the number of recycling times of the material frame, thereby saving production and operation costs.

[0028] 3. The present invention can adopt the traditional wax mold casting process to produce assembly parts, increase the density and compactness of alloy steel, increase the smoothness of product surface, effectively block the infiltration of external elements during use of the material frame, especially the infiltration of some harmful elements during quenching, and increase the service life of the material frame.

[0029] 4. The present invention is based on a preparation method of assembling a plurality of assembly parts into an integral material frame, and designs the assembly part structure, thereby reducing the weight and heat permeability of the material frame itself while ensuring the load-bearing capacity, further reducing the heat energy loss of ineffective heating, effectively saving energy and reducing costs;

[0030] For example, the interlaced fixed design of the fence and the chassis of the present invention maintains a reasonable gap between the outer periphery of the fence and the inner periphery of the frame, effectively avoiding deformation caused by repeated thermal expansion and contraction; improving the thermal mechanical fatigue life of the material frame; the present invention respectively sets through and non-through thermal expansion joints on the fence chassis frame, while ensuring that the structural strength of the frame meets the use requirements, further avoiding deformation caused by repeated hot and cold changes, and improving the number of cycles of the frame; the interlaced movable connection between the fence and the chassis of the present invention and the non-fixed contact between the bottom end of the fence and the chassis, while ensuring that the chassis provides effective support for the fence, can buffer the kinetic energy impact through a certain elastic deformation when the parts fall into the material frame, thereby increasing the effective bearing capacity of the material frame, thereby reducing the weight of the material frame itself under a certain bearing capacity requirement, compared with the material frame with an integrated structure. The amount can be reduced by 25-30%, further reducing the heat energy loss of ineffective heating, effectively saving energy and reducing costs; the chassis frame of the material frame of the present invention adopts a corrugated rectangular structure design, which reduces the weight of the material frame while ensuring a certain bearing capacity and anti-deformation ability; the material frame chassis of the present invention is evenly distributed with regular hexagonal through holes and fence openings, which ensures good heat permeability of the material frame when in use; the honeycomb design of the chassis ensures the bearing capacity without affecting the heat transfer of parts during the heat treatment process, and the reasonable arrangement of long and short circular holes on the fence ensures the overall structural strength, while reducing the weight of the structure, and further reducing the heat loss caused by heat absorption of the material frame; the present invention arranges a number of reinforcing structures in the long side direction of the bottom plate according to the bearing capacity requirements of the material frame, without affecting the heat permeability of the material frame, and can still meet the use requirements when the bearing capacity requirements are high.

[0031] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The accompanying drawings are only used for the purpose of illustrating specific embodiments and are not to be considered as limiting the present invention. In the entire drawings, the same reference symbols represent the same components;

[0033] Figure 1 It is a three-dimensional picture of the material frame combination;

[0034] Figure 2 The material frame structure is three-dimensional Figure 1 ;

[0035] Figure 3 The material frame structure is three-dimensional Figure 2 ;

[0036] Figure 4 It is a top view of the material frame structure;

[0037] Figure 5 It is the main view of the material frame structure;

[0038] Figure 6 It is the left view of the material frame structure;

[0039] Figure 7 This is a bottom view of the material frame structure;

[0040] Figure 8 For the short side connecting ring of the material frame ( Figure 1 Part A in the middle) Partial enlarged view;

[0041] Fig. 9 When assembling the connecting ring of the long side a of the material frame and the connecting ring of the short side ( Figure 1 Part B in the middle) Partial enlargement;

[0042] Fig.10 Expansion joint for the short frame of the material frame fence ( Figure 1 Partial enlargement of the center (C);

[0043] Fig.11 Expansion joint for the long frame of the material frame fence ( Figure 1 Partial enlarged view of the D part in the middle;

[0044] Fig.12 The clearance between one side of the material frame fence and the chassis frame ( Figure 7 Part E in the middle) Partial enlargement;

[0045] Reference numerals:

[0046] 1- chassis; 11- bottom plate; 12- frame; 111- hexagonal through hole; 112- first bottom plate reinforcement structure; 113- second bottom plate reinforcement structure; 114- third bottom plate reinforcement structure; 115- fourth bottom plate reinforcement structure; 121- expansion joint of short frame of fence; 122- expansion joint of long frame of fence; 123- frame pin hole; 2- short side of fence; 21- short side connecting ring; 211- short side connecting ring limiting ring; 212- short side connecting ring Support rib; 213-short side connecting ring body connecting part; 22-short side elliptical hole; 23-short side small circular hole; 3-long side of fence; 31-long side a of fence; 311-long side a connecting ring; 3111-long side connecting ring limiting ring; 3112-long side connecting ring supporting rib; 3113-long side connecting ring body connecting part; 312-long side elliptical hole; 313-long side small circular hole; 32-long side b of fence; 321-long side b connecting ring; 4-connecting rod. DETAILED DESCRIPTION

[0047] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0048] A specific embodiment of the present invention discloses a method for preparing a detachable precision casting frame, the method comprising:

[0049] Preparing an assembly part of a precision casting frame, the assembly part comprising a chassis, a sub-rail, a chassis and sub-rail connecting piece, and a sub-rail connecting piece;

[0050] Assemble the assembly parts of the precision casting frame to form a detachable precision casting frame.

[0051] The preparation method of the material frame of the present invention uses a plurality of assembly parts to assemble an integral material frame, and decomposes the precision casting material frame into a chassis, a sub-fence, a chassis and a sub-fence connection piece, and a sub-fence connection piece assembly part to form an assembleable and detachable precision casting material frame. Compared with the one-piece material frame in the prior art, on the one hand, the single casting part of the present invention is smaller in volume, and the thermal expansion and contraction values ​​during the heating and cooling process are smaller, which reduces the possibility of the material frame being stuck in the continuous push rod furnace due to thermal expansion; on the other hand, the material frame of the present invention is a detachable structure, and damaged parts can be replaced separately, which greatly reduces the cost of replacing the material frame.

[0052] Furthermore, the assembly part is made of high alloy steel, and the element composition of the high alloy steel is, by mass percentage, C: 0.1-0.2%, Cr: 24-27%, Ni: 19-22%, W: 2.5-3.5%; Co: 1.0-2.0%; Nb: 0.5-1.0%, S: ≤0.035%, P: ≤0.035%, and the rest is Fe and unavoidable impurities.

[0053] Specifically, the thermal expansion coefficient of the high alloy steel in the range of room temperature to 1100°C is 10×10 -6 / ℃~13×10 -6 / ℃.

[0054] Reasonable main element ratio: The main elements of the material frame are chromium Cr and nickel Ni metal. Cr can increase the hardenability of steel and has a secondary hardening effect. It can improve the hardness and wear resistance of carbon steel without making the steel brittle, so that the steel has better comprehensive mechanical properties after quenching and tempering. Adjusting the Cr content makes it have the effects of high-temperature oxidation resistance and oxidation corrosion resistance, while increasing the thermal strength of steel. It can also form chromium-containing carbides, such as (Fe, Cr)7C3, thereby improving the wear resistance of the material surface; nickel elements mainly strengthen ferrite and refine pearlescent, which can improve the strength of steel without significantly reducing its toughness. At the same time, the yield degree of steel increases faster than the tensile strength, and the damage to the toughness, plasticity and other process properties of steel is less than that of other alloying elements. Ni can improve the fatigue resistance of steel and reduce the sensitivity of steel to notches;

[0055] Increase of trace elements: Rare metal elements tungsten W, cobalt Co and niobium Nb are added to the casting tray design. A small part of the W element is soluble in liquid iron and will form special carbides with carbon, which promotes the transformation of austenite to martensite to enhance hardness, improve wear resistance and abrasion resistance; the Co element promotes martensite transformation, increases toughness and strength; the Nb element can refine the grains and increase the thermal strength of the tray, resist rapid cooling and thermal stress, and effectively prevent excessive penetration of the C element during heat treatment to avoid product cracking.

[0056] The alloy steel used in the present invention has a low thermal expansion coefficient of 10×10 -6 / ℃~13×10 -6 / ℃, combined with the structural design of the material frame, the deformation of the material frame during the use of the continuous pusher furnace can be effectively reduced.

[0057] Preferably, the thermal expansion coefficient of the alloy steel used in the present invention is 11.5×10 -6 / ℃.

[0058] Specifically, each assembly part of the material-carrying frame can be cast.

[0059] Furthermore, wax casting is used to manufacture the assembly parts of the precision casting frame. Wax casting increases the density and compactness of the alloy steel, increases the smoothness of the product surface, and effectively blocks the infiltration of external elements during the use of the tray, especially the infiltration of some harmful elements during the quenching process.

[0060] Specifically, the wax casting includes: a smelting process of high alloy steel, and the smelting process of high alloy steel includes:

[0061] Step 1. Put the alloy raw materials into a vacuum melting chamber, evacuate and maintain the vacuum degree below 0.67Pa;

[0062] Step 2: heating to above 1700°C to melt the alloy raw materials in the vacuum melting chamber;

[0063] Step 3: After the raw materials in the vacuum melting chamber are completely melted, they are refined to obtain a refined alloy liquid.

[0064] Exemplarily, in step 3, the refining process is to introduce inert gas argon into the vacuum melting chamber, maintain the vacuum degree between 15-150 Pa, continue heating to 1750° C. to 1850° C., and keep warm for 15 to 25 minutes to obtain a molten alloy.

[0065] Furthermore, the preparation method also includes: assembling and welding a wax mold according to the shape of the supporting frame assembly, and coating a shell material on the surface of the wax mold.

[0066] Specifically, the shell material is coated with three layers, including a surface layer, a transition layer and a back layer; the surface layer material is composed of: 33.2-37.4% silica sol, 62.3-66.4% zircon sand powder, 0.24-0.32% defoaming agent, the zircon sand powder is 80-120 mesh, and the defoaming agent is polydimethylsiloxane; the transition layer material is composed of: 40-46.2% silica sol, 53.9-60% mullite sand powder, and the transition layer sand is 40-55 mesh; the back layer material is composed of: 36.4-42.9% silica sol, 57.2-63.7% mullite sand powder, and the back layer sand is 20-30 mesh.

[0067] Furthermore, the preparation method also includes shell casting, pouring molten alloy into the shell to obtain an assembly part of the precision casting frame.

[0068] Preferably, the pouring temperature is 1550-1650°C, and the mold shell temperature is controlled to be 1000-1100°C during pouring.

[0069] In a possible design, the pouring temperature is 1600°C, and the mold shell temperature is controlled at 1100°C during pouring; the heat treatment temperature is 950°C, and the insulation time is 15 hours.

[0070] In a possible design, the assembly includes a chassis, a sub-fence, a chassis and sub-fence connecting piece, and a sub-fence connecting piece; wherein the chassis and sub-fence connecting piece may be a connecting pin, and the sub-fence connecting piece may be a connecting rod;

[0071] The chassis comprises a bottom plate and a frame body perpendicular to the bottom plate, wherein the bottom plate and the frame body are integrally formed;

[0072] The sub-fence is fixed on the inner side of the frame body by means of latches, and the sub-fence and the chassis enclose a material-carrying frame with an opening on one side;

[0073] The sub-fences include a plurality of sub-fences, and the ends of adjacent sub-fences are detachably connected; there is a movable gap between one side of the fence and the frame of the chassis, and the bottom edge of the fence is in contact with the bottom plate of the chassis.

[0074] Furthermore, the assembly parts of the precision casting frame to form a detachable precision casting frame include:

[0075] Step 1. Assemble the long side fences: After the connecting rings at one end of the adjacent long side fences are alternately arranged in the height direction to reach a coaxial state, the connecting rods are passed through the connecting rings at the ends of the adjacent long side fences from top to bottom in sequence to achieve the articulation between the adjacent long side fences, with a connection angle of 180°, to form a set of long side fences;

[0076] Step 2. Assemble the frame: Place a set of long side fences and short side sub-fences at a 90° angle, ensure that the connecting rings at the ends of the long side fences and the short side sub-fences are alternately arranged in the height direction and reach a coaxial state, and pass the connecting rods through the connecting rings at the ends of the long side fences and the short side sub-fences from top to bottom to form a fence assembly;

[0077] The two fence assemblies are assembled into a rectangular frame structure in a manner that the long side fences are parallel and the short side sub-fences are parallel; after the connecting rings at the connection of the long side fence of one fence assembly and the short side sub-fence of the other fence are alternately arranged in the height direction to reach a coaxial state, the connecting rods are sequentially passed through the connecting rings at the connection of the ends of the adjacent fences from top to bottom to achieve connection;

[0078] Step 3. Position adjustment: Place the chassis with the bottom plate and frame integrally formed horizontally, put the assembled frame into the inner side of the chassis frame, make the bottom edge of the fence abut against the bottom plate of the chassis, and ensure that the movable clearance between the four fences constituting the frame and the frame of the chassis is 5-13mm;

[0079] Step 4. Connect the chassis: Insert the pins from the outside of the chassis frame to the inside through the frame pin holes and the fence round holes in sequence, insert and fix the fence on the inner side of the frame to complete the assembly of the material frame with one side open.

[0080] The material frame of the present invention is assembled from a plurality of parts, and is a non-integrated material frame, including a chassis in which a bottom plate and a frame are integrally formed, as well as a plurality of sub-fences and connectors between adjacent sub-fences, and connectors between sub-fences and the frame. By setting the connection method between the components and the gap, deformation caused by repeated thermal expansion and contraction, and the impact of a falling ball can be effectively avoided while ensuring the load-bearing capacity. In addition, the material frame of the present invention is assembled from a plurality of parts, and the volume of a single casting part is relatively small, and the thermal expansion and contraction values ​​during the heating and cooling processes are relatively small, which reduces the possibility of the material frame being stuck in the continuous push rod furnace due to thermal expansion.

[0081] The fence of the present invention is movably connected to the chassis through an interlaced connection, and the bottom end of the fence is in non-fixed contact with the chassis. While ensuring that the chassis provides effective support for the fence, when the parts fall into the material frame, the kinetic energy impact can be buffered through a certain elastic deformation, thereby increasing the effective bearing capacity of the material frame, thereby reducing the weight of the material frame itself under a certain bearing capacity requirement. Compared with a material frame with an integrated structure, the weight can be reduced by 25-30%, further reducing the heat energy loss of ineffective heating, effectively saving energy and reducing costs.

[0082] Furthermore, the movable gap between one side of the fence and the frame of the chassis has an movable size of 5 to 13 mm. On the one hand, a reasonable gap provides expansion space when the material frame has a large temperature change, thereby avoiding the accumulation of internal stress inside the material frame; on the other hand, when the iron ball falls from a high place, the collision between the iron ball and the fence obtains a certain release interval, so that the fence's anti-collision ability is increased.

[0083] In one possible design, the gap between one side of the fence and the inner periphery of the frame is 10 mm, and the thermal expansion coefficient of the frame material is 11.5×10 -6 / ℃, when the working temperature is 1100℃ and the dynamic load is 50MPa, the material frame is only slightly deformed after 300 cycles and can continue to be used. The material frame has strong thermal bearing capacity.

[0084] Furthermore, the frame is composed of two long sides and two short sides, and each side is a corrugated rectangular structure.

[0085] The frame is provided with a frame pin hole at the protruding portion of the corrugated rectangular structure; correspondingly, the fence is provided with a fence circular hole corresponding to the frame pin hole, and the fence is inserted and fixed to the inner side of the frame by a pin that passes through the fence circular hole and the frame pin hole in sequence. It should be noted that the length of the pin is greater than the sum of the fence thickness and the frame thickness.

[0086] It should be noted that, in addition to the corrugations formed by the convex and concave parts on the long sides and the short sides, the right-angled intersection of the long sides and the short sides is also a concave part of the corrugated rectangular structure.

[0087] Furthermore, the concave portion of the short side of the frame is provided with a short frame body expansion joint, and the short frame body expansion joint of the fence is a through joint;

[0088] The concave portion of the long side of the frame is provided with an expansion joint of the long frame body of the fence, and the expansion joint of the long frame body of the fence is a non-through joint.

[0089] In order to ensure that the expansion gap has an impact on the strength of the frame structure of less than 2% and does not affect the overall strength level, the size of the expansion joint needs to be controlled. For through-holes, the width of the expansion joint needs to be no greater than 8mm. For non-through-holes, the length of the expansion joint needs to be at least 10mm smaller than the distance from the concave part to the bottom plate, and the width of the expansion joint needs to be no greater than 8mm.

[0090] Specifically, the bottom plate is provided with evenly distributed regular hexagonal through holes and a bottom plate reinforcement structure.

[0091] In one possible design, the bottom plate is a mesh plate with a reinforcement structure, the unit mesh is a regular hexagon, and adjacent unit meshes share a side; the thickness of the mesh plate is 40~60mm, that is, the hole depth is 40~60mm. The thickness of the frame can be consistent with the mesh plate. The honeycomb-shaped bottom plate can ensure the heat permeability of the material frame during use, does not affect the heat transfer during the heat treatment process, and takes into account the bearing capacity of the material frame. The thickness of the regular hexagon side is consistent with the thickness of the frame, which is conducive to uniform stress distribution and uniform heat transfer;

[0092] In a possible design, the outer perimeter of the material frame is 1460 mm, the width is 840 mm, the side length of the regular hexagonal through hole in the bottom plate is 30 mm, the wall thickness is 10 mm, and the number is 23×18.

[0093] The bottom plate reinforcement structure is parallel to the long side of the bottom plate and has the same length as the long side of the bottom plate, a width equal to the distance between two opposite vertices of the regular hexagon, a thickness consistent with the thickness of the frame, and a thickness direction flush with the frame; the number of the bottom plate reinforcement structures is at least 2, one side of which coincides with the long side of the bottom plate, and is arranged symmetrically.

[0094] When the required bearing capacity of the material frame is large, the bottom plate reinforcement structure can be used to assist in enhancing the structural strength; the thickness of the reinforcement structure is consistent with the thickness of the frame, which is conducive to uniform stress distribution and uniform heat transfer.

[0095] In a possible design, the outer perimeter of the material frame body 12 is 1460 mm, the width is 840 mm, the side length of the regular hexagonal through hole 111 of the bottom plate is 30 mm, the wall thickness is 10 mm, and when the number is 23×18, 4 reinforcement structures are added to the bottom plate, and the material frame bearing capacity is increased by more than 35%.

[0096] Furthermore, the fence includes multiple sub-fences. Specifically, the fence includes 2 groups of long sides and 2 groups of short sides; each group of short sides is 1 sub-fence, each group of long sides is more than 1 sub-fence, more than 1 sub-fences constitute 1 long side, and the long sides and short sides are connected in sequence to form a complete fence.

[0097] The left and right ends of the sub-fences are both provided with a plurality of connecting rings, wherein the connecting rings of the connecting ends of adjacent sub-fences are alternately arranged in the height direction.

[0098] The connecting pins pass through the corresponding fence circular holes and frame pin holes in sequence to fix the fence inside the frame. The length of the connecting pin is greater than the sum of the fence thickness and the frame thickness. The difference between the pin length and the sum of the two must at least meet the size requirements of the movable gap between one side of the fence and the frame of the chassis, and the movable size range is 5~13mm.

[0099] The connecting rod passes through the connecting rings at the ends of adjacent sub-fences in sequence to achieve the articulation of adjacent sub-fences, and the connecting angle between adjacent sub-fences is 90°.

[0100] In order to ensure that there is a freely adjustable movable gap between one side of the fence and the frame of the chassis, the sub-fence includes a sub-fence body and connecting rings at both ends, the connecting ring includes a connecting rod sleeve and a body connecting part, and the connecting rod sleeve is connected to the fence body through the body connecting part; the connecting rod sleeve includes two limiting rings and two supporting ribs arranged along the circumference of the ring, the two supporting ribs are located between the two limiting rings, and the upper and lower ends are respectively vertically connected to the two limiting rings; the vertical distance between the two limiting rings is 30~40mm; the two supporting ribs are symmetrically distributed along the radial direction of the ring, and the central angle corresponding to each supporting rib is 30°~60°. By setting the length of the connecting pin and the setting of the sub-fence connecting ring, a freely adjustable movable gap is achieved between one side of the fence and the frame of the chassis.

[0101] The number of connecting rings at both ends of the same sub-fence is not equal. When connected with the adjacent sub-fence, it is convenient to form a connection ring of the sub-fence at one end when connected, and the connection ring of the sub-fence at the other end when connected, the connection ring of the sub-fence adjacent to the sub-fence is the top. In this way, for the same sub-fence, relative to the adjacent sub-fence, the connecting ring at one end is located above, and the connecting ring at the other end is located below. Through the asymmetric setting of the connecting rings at both ends of the sub-fence, when the connecting rings of the adjacent sub-fences are alternately connected to form an overall material frame structure, the stability principle of the triangle is fully utilized, thereby providing additional stability and anti-deformation ability, thereby improving the anti-deformation ability of the structure.

[0102] Exemplarily, each set of fence long sides is divided into at least two parts, and the connection is provided with connecting rings alternately arranged in the height direction. When in use, they are hinged together by connecting rods, and the connection angle is 180°.

[0103] Preferably, the long side and the short side of the fence are provided with several layers of circular holes along the height direction, wherein the bottom layer is provided with pin holes of the same size at positions corresponding to the pin holes provided in the frame;

[0104] The circular holes are all long circular holes in the middle layer along the height direction, and the long and short circular holes are alternately arranged in the uppermost layer and the lowermost layer.

[0105] Exemplarily, the sub-fence is rectangular, and along the height direction, the middle layer of the short side sub-fence is an oblong hole, and the top and bottom layers are both elliptical holes and small round holes alternately distributed, of which 2 elliptical holes are arranged adjacent to each other, 2 elliptical holes and one small round hole are arranged alternately, a total of 3 groups, and there is 1 small round hole at both ends. The middle layer of the long side sub-fence is an oblong hole, and the top and bottom layers are both elliptical holes and round holes alternately distributed, of which 2 elliptical holes are arranged adjacent to each other, 2 small round holes are arranged adjacent to each other, 2 elliptical holes and 2 small round holes are arranged alternately, and both ends are small round holes. The overall opening rate of elliptical holes and small round holes in each fence is 50%~70%.

[0106] Among them, the specifications of the oblong holes of the short side fence and the long side fence are the same, the specifications of the elliptical holes are the same, and the specifications of the small round holes are the same. The present invention can reduce the weight of the structure while ensuring the strength through the structural design of the short side fence and the long side fence. Under the condition of the same size, compared with the existing material frame with a weight of 275kg / piece, the material frame of the present invention has a light weight itself, and will not waste more heat energy to heat itself when the iron ball is heated, thereby reducing the energy loss that is worthless for product production. Through the reasonable arrangement of long and short round holes, the strength can be improved, the stress deformation can be reduced, and the service life of the material frame can be increased.

[0107] It should be noted that the small round holes on the bottom layer are used as fence pin holes, and the number is set according to the fixed positions of the pins.

[0108] The technical solution of the present invention is explained below in conjunction with specific embodiments.

[0109] Example 1

[0110] The element composition of the materials for the assembly parts of the material frame is: C: 0.1-0.2%, Cr: 24-27%, Ni: 19-22%, W: 2.5-3.5%; Co: 1.0-2.0%; Nb: 0.5-1.0%, S: ≤0.035%, P: ≤0.035%, and the rest are Fe and unavoidable impurities.

[0111] The main size parameters of each assembly part of the material frame are as follows: the outer perimeter of the material frame body 12 is 1460mm and the width is 840mm; the distance between the protruding part of the corrugated rectangular structure and the bottom plate is 110mm, and the distance between the concave part and the bottom plate is 50mm. The length of the protruding or concave part adjacent to the hinge is 100mm, and the length of the remaining part is 200mm; the expansion joint 2 of the long side non-penetrating fence short side fence long frame body is 5mm wide and 40mm long; the expansion joint 1 of the short side penetrating fence short side fence long frame body is 5mm wide and 50mm long;

[0112] The heights of the short side 2, the long side a31 and the long side b32 of the fence are all 250mm. The number of holes in the fence along the height direction is 3, of which the middle layer is all oblong holes, and there is a short circular hole between every two oblong holes in the upper and lower layers. The dimensions of the oblong holes 22 on the short side and the oblong holes 312 on the long side are 130mm long axis × 50mm short axis, and the dimensions of the short side circular holes 23 and the short side circular holes 313 on the long side are 45mm long axis × 35mm short axis. There are 3 sets of connecting rings at the ends of the long and short sides of the fence, and the interconnected parts are arranged alternately. The gap between the outer periphery of the fence and the inner periphery of the chassis frame 12 is 10mm.

[0113] The bottom plate regular hexagonal through hole 111 has a side length of 30 mm, a wall thickness of 10 mm, and a number of 23×18;

[0114] Two reinforcement structures are provided in each of the two long sides of the bottom plate, wherein one side of the first bottom plate reinforcement structure 112 coincides with the long side, the second bottom plate reinforcement structure 113 is separated from the first bottom plate reinforcement structure 112 by a row of hexagonal through holes, and the third bottom plate reinforcement structure 114 is separated from the fourth bottom plate reinforcement structure 115 by a row of hexagonal through holes.

[0115] The wax casting process of each assembly part of the material frame includes the following steps:

[0116] Step 1: Membrane shell preparation: assemble and weld the wax mold according to the shape of the required casting;

[0117] Step 2, shell production: coating the shell material on the surface of the wax mold, the surface layer is made of zircon sand powder, the transition layer and the back layer are made of mullite sand powder, the transition layer sand is 40-55 mesh, and the reinforcement layer sand is 20-30 mesh;

[0118] Step 3, steam dewaxing: dewaxing the wax mold coated with the shell material, the dewaxing temperature is 140°C, and the dewaxing time is 25 minutes;

[0119] Step 4, heating and heat preservation of the film shell: put the dewaxed shell into the baking furnace, heating temperature is 1250℃, and heat preservation for 1h;

[0120] Step 5, pouring: the pouring temperature is 1600°C, and the shell temperature is controlled at 1100°C during pouring;

[0121] Step 6, clear the shell and obtain the frame casting;

[0122] Step 7: Heat treatment: heat treatment temperature 950°C, keep warm for 15 hours.

[0123] The assembly steps of each assembly part of the material frame are as follows:

[0124] Step 1. Assemble the long side fence: After arranging the connecting rings at the ends of the two sub-fences alternately in the height direction to achieve a coaxial state, pass the connecting rod through the connecting rings at the ends of adjacent sub-fences from top to bottom in sequence to achieve the articulation between adjacent sub-fences with a connection angle of 180°.

[0125] Step 2. Assemble the frame: Place a set of long side fences and a sub-fence at a 90° angle, ensure that the connecting rings at the ends of the long side fences and the sub-fences are alternately arranged in the height direction and are coaxial, and pass the connecting rods through the connecting rings at the ends of adjacent sub-fences from top to bottom to form a fence assembly.

[0126] Repeat this step to secure another set of long side fences to one of the branch fences.

[0127] Place the two connected fence assemblies together, ensuring that the corners and edges are aligned, and use the connecting rods again to fix the two fence assemblies together to form a rectangular frame structure.

[0128] Step 3. Position adjustment: Place the chassis with the bottom plate and frame integrally formed horizontally, put the assembled frame into the inner side of the chassis frame, make the bottom edge of the fence abut against the bottom plate of the chassis, and ensure that the movable gap between the four fences constituting the frame and the frame of the chassis is 10mm.

[0129] Step 4. Connect the chassis: Insert the pins from the outside of the chassis frame to the inside through the frame pin holes and the fence round holes in sequence, and fix the fence on the inner side of the frame to complete the assembly of the material frame with one side open.

[0130] The assembled material frame was subjected to a thermal mechanical fatigue test: the material frame was subjected to a thermal cycle treatment, where one thermal cycle was defined as heating at 1100°C for 2 hours and then water cooling for 2 to 4 seconds. During the thermal cycle, a dynamic load of 50 MPa was applied. The number of thermal cycles increased from 0 to 300, and the deformation of the material frame was observed, as shown in Table 1.

[0131]

[0132] Comparative Example 1

[0133] The dimensions of the various assembly parts of the material frame are the same as those in Example 1.

[0134] The material of each assembly part of the material frame is nickel-based alloy, and the element composition is: Ni: about 36%, Cr: about 3%, and the balance is Fe and other inevitable impurities.

[0135] The wax casting process parameters of each assembly part of the material frame and the assembly steps of each assembly part of the material frame are the same as those in Example 1.

[0136] The assembled material frame was subjected to a thermal mechanical fatigue test: the material frame was subjected to a thermal cycle treatment, where one thermal cycle was defined as heating at 1100°C for 2 hours and then water cooling for 2 to 4 seconds. During the thermal cycle, a dynamic load of 50 MPa was applied. The number of thermal cycles increased from 0 to 300, and the deformation of the material frame was observed, as shown in Table 1.

[0137] Comparative Example 2

[0138] The material element composition of each assembly part of the material frame is the same as that of Example 1.

[0139] The difference is that the chassis is only composed of a base plate, without a corrugated rectangular structure frame, the outer circumference of the fence is equal to that of the base plate, and the four corners of the base plate and the middle of the long side and the middle of the long side a and b of the fence are hinged with connecting holes matching the connecting rods. The fence is directly connected to the base plate by hinged means.

[0140] The wax casting process parameters of each assembly part of the material frame and the assembly steps of each assembly part of the material frame are the same as those in Example 1.

[0141] The assembled material frame was subjected to a thermal mechanical fatigue test: the material frame was subjected to a thermal cycle treatment, where one thermal cycle was defined as heating at 1100°C for 2 hours and then water cooling for 2 to 4 seconds. During the thermal cycle, a dynamic load of 50 MPa was applied. The number of thermal cycles increased from 0 to 300, and the deformation of the material frame was observed, as shown in Table 1.

[0142] Comparative Example 3

[0143] The material element composition of each assembly part of the material frame is the same as that of Example 1.

[0144] The difference is that the chassis frame does not have a frame expansion joint.

[0145] The wax casting process parameters of each assembly part of the material frame and the assembly steps of each assembly part of the material frame are the same as those in Example 1.

[0146] The assembled material frame was subjected to a thermal mechanical fatigue test: the material frame was subjected to a thermal cycle treatment, where one thermal cycle was defined as heating at 1100°C for 2 hours and then water cooling for 2 to 4 seconds. During the thermal cycle, a dynamic load of 50 MPa was applied. The number of thermal cycles increased from 0 to 300, and the deformation of the material frame was observed, as shown in Table 1.

[0147] It can be seen from Table 1 that, compared with Example 1, Comparative Example 1 uses a nickel-chromium alloy without adding trace W, Co and Nb elements as the material for making the material frame, and the number of thermal cycle uses of the material frame is much lower than that of the present invention; Compared with Example 1, although Comparative Example 2 is a detachable design of the fence and the bottom plate, it is fixedly connected, resulting in repeated thermal expansion and contraction during use, and is unable to buffer dynamic loads and is extremely easy to deform; Compared with Example 1, Comparative Example 3 does not set an expansion joint at the chassis frame, and the thermal mechanical life of the material frame is significantly lower than that of Example 1.

[0148] In summary, the present invention increases the rare metal elements W, Co and Nb by regulating the alloy elements of the material frame material, thereby ensuring that the material frame material of the present invention has a lower thermal expansion coefficient, improving the thermal mechanical strength of the material frame, increasing the number of recycling times of the material frame, and thus saving production and operation costs.

[0149] On this basis, the wax casting process is adopted to regulate the alloy elements of the frame material, increase the density and compactness of the alloy steel, increase the smoothness of the product surface, effectively block the infiltration of external elements during the use of the frame, and improve the service life of the frame.

[0150] At the same time, a detachable material frame with multiple structural components that can be replaced individually is designed. By improving the chassis structure and the connection method and position relationship between the chassis and the fence, a reasonable gap between the chassis and the fence and a frame expansion joint are designed, which greatly improves the thermal mechanical life of the material frame. The interlaced movable connection between the fence and the chassis and the non-fixed contact between the bottom end of the fence and the chassis can effectively buffer dynamic loads while ensuring that the chassis provides effective support for the fence, meet flexible use requirements, and save replacement costs.

[0151] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a detachable precision casting frame, characterized in that: The preparation method comprises: Prepare an assembly part of a precision casting frame, the assembly part comprising a chassis, a sub-fence, a chassis and sub-fence connecting piece, and a sub-fence connecting piece; wherein the chassis and sub-fence connecting piece is a latch, and the sub-fence connecting piece is a connecting rod; The chassis comprises a bottom plate and a frame perpendicular to the bottom plate, wherein the bottom plate and the frame are integrally formed; the frame consists of two long sides and two short sides, each side is a corrugated rectangular structure, and the frame is provided with a frame pin hole at the protruding part of the corrugated rectangular structure; the concave part of the short side of the frame is provided with a short frame body expansion joint; the concave part of the long side of the frame is provided with a fence long frame body expansion joint; The sub-fences are fixed on the inner sides of the frame body by means of latches; the sub-fences include a plurality of sub-fences, and the ends of adjacent sub-fences are detachably connected; The sub-fence comprises a sub-fence body and connecting rings at both ends, the connecting ring comprises a connecting rod sleeve portion and a body connecting portion, the connecting rod sleeve portion is connected to the fence body through the body connecting portion; the connecting rod sleeve portion comprises two limiting rings and two supporting ribs arranged along the circumference of the ring; There is a movable gap between one side of the fence and the frame of the chassis, and the bottom edge of the fence abuts against the bottom plate of the chassis; Assembling the assembly parts of the precision casting frame to form a detachable precision casting frame; The assembly part is made of high alloy steel. The element composition of the high alloy steel is, by mass percentage, C: 0.1-0.2%, Cr: 24-27%, Ni: 19-22%, W: 2.5-3.5%; Co: 1.0-2.0%; Nb: 0.5-1.0%, S: ≤0.035%, P: ≤0.035%, and the rest is Fe and unavoidable impurities.

2. The preparation method according to claim 1, characterized in that: The thermal expansion coefficient of the high alloy steel in the range of room temperature to 1100°C is 10×10 -6 / ℃~13×10 -6 / ℃.

3. The preparation method according to claim 1, characterized in that: The assembly parts of the precision casting frame are manufactured separately by wax casting.

4. The preparation method according to claim 3, characterized in that: The wax casting includes: a smelting process of high alloy steel, and the smelting process of high alloy steel includes: Step 1. Put the alloy raw materials into a vacuum melting chamber, evacuate and maintain the vacuum degree below 0.67Pa; Step 2: heating to above 1700°C to melt the alloy raw materials in the vacuum melting chamber; Step 3: After the raw materials in the vacuum melting chamber are completely melted, they are refined to obtain a refined alloy liquid.

5. The preparation method according to claim 4, characterized in that: In step 3, the refining process is to introduce inert gas argon into the vacuum melting chamber, maintain the vacuum degree between 15-150Pa, continue to heat to 1750°C~1850°C, and keep warm for 15~25min to obtain alloy liquid.

6. The preparation method according to claim 3, characterized in that: The preparation method further comprises: assembling and welding a wax mold according to the shape of the supporting frame assembly, and coating a shell material on the surface of the wax mold.

7. The preparation method according to claim 6, characterized in that: The preparation method also includes shell casting, pouring alloy liquid into the shell to obtain the assembly parts of the precision casting frame.

8. The preparation method according to claim 7, characterized in that: The mold shell pouring temperature is 1550-1650°C, and the mold shell temperature is controlled to be 1000-1100°C during pouring.

9. The preparation method according to claim 1, characterized in that: The assembly parts for assembling the precision casting frame to form a detachable precision casting frame include: Step 1. Assemble the long side fences: After the connecting rings at one end of the adjacent long side fences are alternately arranged in the height direction to reach a coaxial state, the connecting rods are passed through the connecting rings at the ends of the adjacent long side fences from top to bottom in sequence to achieve the articulation between the adjacent long side fences, with a connection angle of 180°, to form a set of long side fences; Step 2. Assemble the frame: Place a set of long side fences and short side sub-fences at a 90° angle, ensure that the connecting rings at the ends of the long side fences and the short side sub-fences are alternately arranged in the height direction and reach a coaxial state, and pass the connecting rods through the connecting rings at the ends of the long side fences and the short side sub-fences from top to bottom to form a fence assembly; The two fence assemblies are assembled into a rectangular frame structure in a manner that the long side fences are parallel and the short side sub-fences are parallel; after the connecting rings at the connection of the long side fence of one fence assembly and the short side sub-fence of the other fence are alternately arranged in the height direction to reach a coaxial state, the connecting rods are sequentially passed through the connecting rings at the connection of the ends of the adjacent fences from top to bottom to achieve connection; Step 3. Position adjustment: Place the chassis with the bottom plate and frame integrally formed horizontally, put the assembled frame into the inner side of the chassis frame, make the bottom edge of the fence abut against the bottom plate of the chassis, and ensure that the movable clearance between the four fences constituting the frame and the frame of the chassis is 5-13mm; Step 4. Connect the chassis: Insert the pins from the outside of the chassis frame to the inside through the frame pin holes and the fence round holes in sequence, and fix the fence on the inner side of the frame to complete the assembly of the material frame with one side open.

Citation Information

Patent Citations

  • Material Containing Device on Isothermal Normalizing Line for Gear

    AU2020102200A4

  • Material frame for heat treatment furnace

    CN104928442A

  • Casting tray for chamber furnace

    CN115537527A

  • Bearing material frame for heat treatment process of spherical parts

    CN118326146A

  • Simple combined material frame convenient to assemble and disassemble for heat treatment

    CN214735947U