A composite lithium supplement, preparation method and application thereof

By using nanocomposite catalysts on the positive electrode of lithium-ion batteries to prepare composite lithium replenishing agents, the problem of irreversible loss of lithium during the charging process of lithium-ion batteries is solved, the discharge capacity and electrochemical performance of the battery are improved, and lower delithiation batteries are achieved. bits and higher cycling stability.

CN118507701BActive Publication Date: 2024-10-01JIANGSU LIONG0 NEW ENERGY TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410964880.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

During the charging process of existing lithium-ion batteries, the formation of the solid electrolyte membrane (SEI membrane) causes irreversible loss of lithium, which affects battery performance. Moreover, the existing lithium replenishing reagents have a low lithium replenishing amount, low efficiency, and are detrimental to the stability of the cathode structure. .

Method used

A nanocomposite catalyst is used as a nucleating agent, and a nanocomposite catalyst is prepared through solvothermal reaction and sintering, and a lithium oxalate coating layer is formed on its surface to form a composite lithium replenishing agent, which is used to improve the specific discharge capacity and electrochemistry of lithium-ion batteries. performance.

Benefits of technology

It achieves low delithiation potential and high first charge-discharge specific capacity of lithium-ion batteries, improves the cycle performance and stability of the battery, and avoids the negative impact of side reactions on battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium-ion batteries, and in particular to a composite lithium supplement, a preparation method and application thereof. The composite lithium supplement comprises: a nano-composite catalyst; a lithium oxalate coating layer formed on the surface of the nano-composite catalyst; the nano-composite catalyst is prepared from raw materials including a catalyst precursor, a carbon source and a conductive agent dispersion. The present invention synthesizes a nano-catalyst in situ on conductive carbon to form a nano-composite catalyst. Further, the nano-composite catalyst is used as a nucleating agent, and a high-concentration lithium salt is used to quickly synthesize a nano-lithium oxalate-coated composite catalyst to form a composite lithium oxalate lithium supplement. Compared with conventional lithium oxalate sacrificial lithium supplements such as the commonly used lithium supplement Li5FeO4 in the market, the composite lithium supplement is the first to form a nano-lithium oxalate lithium supplement with a conductive agent and a catalyst as the internal core. The internal core can effectively reduce the internal lithium delithiation energy barrier of lithium oxalate, so that it has a lower delithiation potential and better electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite lithium supplement, a preparation method and application thereof. Background Art

[0002] During the charging process of traditional lithium-ion batteries, a solid electrolyte film (SEI film) is generated on the negative electrode surface, which consumes the active lithium released by the positive electrode, resulting in irreversible loss of some lithium, thus affecting battery performance and causing the first coulomb efficiency of the whole battery to decrease and the discharge specific capacity to decrease. Therefore, improving the discharge specific capacity and lithium ion transmission performance of the battery positive electrode has become a key topic of current research.

[0003] To solve this problem, research focus is currently on adding lithium replenishing agents to the positive electrode. These agents can provide additional lithium ions without affecting the positive electrode structure, thereby increasing the discharge capacity of the battery positive electrode. However, the existing lithium replenishing agents have a series of problems, including low lithium replenishment amount, low lithium replenishment efficiency, and adverse effects on the stability of the positive electrode structure. These problems limit the promotion and application of lithium replenishing agents in practical applications.

[0004] Patent application CN117559013A uses a lithium replenishing agent and a conductor to form a lithium replenishing agent composite material. By adding the lithium replenishing agent composite material to the positive electrode of the battery, the lithium replenishing effect on the positive electrode is achieved during the battery charging and discharging process, effectively improving the discharge specific capacity of the positive electrode of the battery. However, the byproducts of the lithium replenishing agent used in the patent decompose during the cycle process will aggravate the interface side reaction between the electrode liquid and the positive electrode, resulting in reduced cycle performance. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a composite lithium supplement, a preparation method and application thereof. The lithium-ion battery prepared by the composite lithium supplement of the present invention has a low delithiation potential and a high initial charge and discharge specific capacity.

[0006] The present invention provides a composite lithium supplement, comprising:

[0007] Nanocomposite catalysts;

[0008] A lithium oxalate coating layer formed on the surface of the nanocomposite catalyst;

[0009] The nano composite catalyst is prepared from raw materials including a catalyst precursor, a carbon source and a conductive agent dispersion liquid.

[0010] Preferably, the catalyst precursor includes at least one of a metal salt, a metal salt hydrate, a metal complex, a metal oxide and a metal organic; the metal element in the catalyst precursor includes at least one of ammonium, nickel, cobalt, iron, cerium, neodymium and titanium.

[0011] Preferably, the carbon source includes at least one of an organic carbon source and an inorganic carbon source;

[0012] The organic carbon source includes at least one of glucose, cellulose, lignin, amino acids, biopolymers, organic acids and macromolecular carbon chains;

[0013] The inorganic carbon source comprises at least one of graphite, graphene, fullerene, carbon microspheres, carbon quantum dots, carbon aerogel, carbon fiber, glassy carbon, carbon nanohorns, carbon nanofibers, carbon nanofoams, carbon nanoonions and carbon-coated substances;

[0014] The mass ratio of the catalyst precursor to the carbon source is (4-6):1.

[0015] Preferably, the conductive agent includes at least one of acetylene black, carbon black, graphene, carbon nanotubes, carbon fibers, carbon quantum dots, graphite oxide materials, oxidized carbon nanotubes, reduced graphite materials, carbon microspheres and carbon aerogels.

[0016] Preferably, the method for preparing the nanocomposite catalyst comprises the following steps:

[0017] S1) mixing a catalyst precursor, a carbon source, a solvent and a conductive agent dispersion, and performing a solvothermal reaction to obtain a solid product;

[0018] S2) sintering the solid product under a protective gas atmosphere to obtain the nanocomposite catalyst.

[0019] Preferably, the solvent of the conductive agent dispersion is selected from at least one of water, alcohol solvents and polar solvents; the concentration of the conductive agent dispersion is 3-6 mg / mL;

[0020] The reaction temperature of the solvent thermal reaction is 140-220° C.; the protective gas is selected from nitrogen or argon.

[0021] Preferably, the sintering temperature is 700-800° C. and the sintering time is 3-6 h.

[0022] Preferably, in the composite lithium supplement, the mass proportion of the nanocomposite catalyst is 5% to 20%.

[0023] The present invention also provides a method for preparing the composite lithium supplement agent described above, characterized in that it comprises the following steps:

[0024] The nano composite catalyst solution, oxalic acid solution and lithium hydroxide solution are mixed and reacted to obtain a composite lithium supplement agent.

[0025] Preferably, mixing the nanocomposite catalyst solution, the oxalic acid solution and the lithium hydroxide solution comprises:

[0026] Pumping oxalic acid solution and lithium hydroxide solution into the nanocomposite catalyst solution for reaction, thereby obtaining a composite lithium supplement;

[0027] The pumping rate is 10-25 r / min;

[0028] The mass concentration of the nanocomposite catalyst solution is 5% to 30%; the molar concentration of the oxalic acid solution is 0.5 to 1 mol / L; the molar concentration of the lithium hydroxide solution is 8 to 10 mol / L;

[0029] The temperature of the pumped oxalic acid solution is 50-80°C; the temperature of the lithium hydroxide solution is room temperature; and the temperature of the reaction is 10-25°C.

[0030] The present invention also provides a lithium ion battery, wherein the positive electrode of the lithium ion battery comprises a composite lithium supplement;

[0031] The composite lithium supplement is the composite lithium supplement described above, or is the composite lithium supplement prepared by the preparation method described above.

[0032] The present invention provides a composite lithium supplement, comprising: a nano-composite catalyst; a lithium oxalate coating layer formed on the surface of the nano-composite catalyst; the nano-composite catalyst is prepared from raw materials including a catalyst precursor, a carbon source and a conductive agent dispersion. The present invention proposes a new composite lithium supplement, which is prepared by preparing a nano-composite catalyst, and then using the nano-composite catalyst as a nucleating agent to deposit and coat lithium oxalate on the surface by heterogeneous nucleation to prepare a nano-scale composite lithium oxalate as a composite lithium supplement, which is applied to positive electrode materials. Compared with conventional lithium oxalate sacrificial lithium supplements such as Li5FeO4 commonly used in the market, the composite lithium supplement of the present invention is the first to form a nano-lithium oxalate lithium supplement with a conductive agent and a catalyst as the internal core, and the internal core can effectively reduce the internal lithium delithiation energy barrier of lithium oxalate, so that it has a lower delithiation potential and better electrochemical performance, and has a wider range of usage scenarios. DETAILED DESCRIPTION

[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention provides a composite lithium supplement, comprising:

[0035] Nanocomposite catalysts;

[0036] A lithium oxalate coating layer formed on the surface of the nanocomposite catalyst;

[0037] The nano composite catalyst is prepared from raw materials including a catalyst precursor, a carbon source and a conductive agent dispersion liquid.

[0038] In certain embodiments of the present invention, the catalyst precursor is at least one of a metal salt, a metal salt hydrate, a metal complex, a metal oxide and a metal organic. The metal element in the catalyst precursor includes at least one of ammonium, nickel, cobalt, iron, cerium, neodymium and titanium. Specifically, the metal salt is ammonium molybdate, ammonium vanadate, ammonium tungstate, nickel chloride, cobalt chloride, cobalt iron sulfate, cerium nitrate, neodymium sulfate, ferric acetate hydrate, titanyl sulfate sulfate hydrate, ferric acetylacetonate, metal-organic complex or metal-organic framework.

[0039] In certain embodiments of the present invention, the carbon source comprises at least one of an organic carbon source and an inorganic carbon source. The organic carbon source is at least one of glucose, cellulose, lignin, amino acids, biopolymers, organic acids and macromolecular carbon chains. The inorganic carbon source is at least one of graphite, graphene, fullerene, carbon microspheres, carbon quantum dots, carbon aerogels, carbon fibers, glassy carbon, carbon nanohorns, carbon nanofibers, carbon nanofoams, carbon nanoonions and carbon-coated substances.

[0040] The mass ratio of the catalyst precursor to the carbon source is (4-6):1; for example, 5:1, 4:1, 6:1.

[0041] In some embodiments of the present invention, the solvent is at least one of water, an alcohol solvent and a polar solvent. The alcohol solvent may be at least one of methanol and ethanol. The polar solvent may be dimethylformamide (DMF).

[0042] The mass ratio of the catalyst precursor to the solvent is 1:(4-6), such as 1:4, 1:6, 1:5.

[0043] In certain embodiments of the present invention, the conductive agent is at least one of acetylene black, carbon black, graphene, carbon nanotubes, carbon fibers, carbon quantum dots, graphite oxide materials (such as graphene oxide), oxidized carbon nanotubes, reduced graphite materials, carbon microspheres, and carbon aerogels. The solvent of the conductive agent dispersion is at least one of water, an alcohol solvent, and a polar solvent. The alcohol solvent may be at least one of methanol and ethanol. The polar solvent may be dimethylformamide (DMF). The concentration of the conductive agent dispersion is 3 to 6 mg / mL, such as 5 mg / mL and 4 mg / mL.

[0044] The mass ratio of the catalyst precursor to the conductive agent dispersion is (3-5):1, such as 5:1, 3:1.

[0045] In certain embodiments of the present invention, the method for preparing the nanocomposite catalyst comprises the following steps:

[0046] S1) mixing a catalyst precursor, a carbon source, a solvent and a conductive agent dispersion, and performing a solvothermal reaction to obtain a solid product;

[0047] S2) sintering the solid product under a protective gas atmosphere to obtain the nanocomposite catalyst.

[0048] In step S1):

[0049] After the mixing, the method further comprises: ultrasonic treatment.

[0050] The power of the ultrasonic treatment is 100-2000 W, such as 2000 W, 100 W, 1000 W, 1500 W, and the time is 20-50 min, such as 30 min, 50 min. The purpose of ultrasonic treatment is to evenly disperse the catalyst, carbon source and conductive agent in the solvent.

[0051] The reaction temperature of the solvent thermal reaction is 140-220°C, such as 180°C, and the time is 8-36 hours, such as 12 hours. The solvent thermal reaction is carried out in a polytetrafluoroethylene-lined pressure vessel, such as a stainless steel autoclave with a polytetrafluoroethylene lining.

[0052] After obtaining the solid product, the method further comprises: collecting the obtained solid product.

[0053] The collection method is centrifugation. The centrifugation speed is 8000-12000 rpm, such as 10000 rpm, and the time is 10-20 min, such as 10 min.

[0054] After collecting the obtained solid product, the method further comprises: washing with a detergent and drying. The detergent is specifically at least one of water, an alcohol solvent and a polar solvent. The alcohol solvent may be methanol. The polar solvent may be dimethylformamide (DMF). The drying may be freeze vacuum drying, vacuum drying, forced air drying or spray drying.

[0055] In step S2):

[0056] The protective gas is selected from nitrogen or argon.

[0057] The sintering temperature is 700-800° C., such as 750° C., and the sintering time is 3-6 h, such as 4 h.

[0058] Before sintering, the process further includes: heating the sample to a sintering temperature. The heating rate is 3-7 °C min -1 , for example 5℃min -1 .

[0059] In certain embodiments of the present invention, the size of the nanocomposite catalyst is 30-200 nm, such as 50-100 nm, 30-70 nm, 100-150 nm, 50-80 nm, 85-125 nm, 75-100 nm.

[0060] In certain embodiments of the present invention, the size of the composite lithium supplement is 75-500 nm, such as 200-300 nm, 75-150 nm, 100-200 nm, 200-400 nm, 200-300 nm, 125-150 nm.

[0061] In certain embodiments of the present invention, in the composite lithium supplement, the mass proportion of the nanocomposite catalyst is 5% to 20%, such as 16%.

[0062] The present invention forms a lithium oxalate coating layer on the surface of the nano composite catalyst by means of heterogeneous nucleation.

[0063] The present invention also provides a method for preparing the composite lithium supplement agent described above, comprising the following steps:

[0064] The nano composite catalyst solution, oxalic acid solution and lithium hydroxide solution are mixed and reacted to obtain a composite lithium supplement agent.

[0065] Specifically, they include:

[0066] Pumping oxalic acid solution and lithium hydroxide solution into the nanocomposite catalyst solution for reaction, thereby obtaining a composite lithium supplement;

[0067] The pumping rate is 10-25 r / min, such as 15 r / min, 25 r / min, 10 r / min.

[0068] The mass concentration of the nanocomposite catalyst solution is 5% to 30%, such as 10%, 12%, 20%, 7%, and 5%. The solvent of the nanocomposite catalyst solution is selected from at least one of water, an alcohol solvent, and a polar solvent. The alcohol solvent may be methanol. The polar solvent may be dimethylformamide (DMF).

[0069] The molar ratio of the oxalic acid to the lithium hydroxide is 1:1.

[0070] The molar concentration of the oxalic acid solution is 0.5-1 mol / L, such as 1 mol / L. The solvent of the oxalic acid solution is water.

[0071] The molar concentration of the lithium hydroxide solution is 8-10 mol / L. The solvent of the lithium hydroxide solution is water.

[0072] The temperature of the pumped oxalic acid solution is 50-80°C, such as 70°C, 80°C, 60°C, 65°C; the temperature of the lithium hydroxide solution is room temperature. The reaction temperature is 10-25°C, such as 25°C, 10°C; the reaction time is 10-30 min, such as 30 min, 10 min.

[0073] After the reaction, a lithium oxalate coating is formed on the surface of the nanocomposite catalyst to obtain a composite lithium supplement.

[0074] The present invention also provides a lithium ion battery, wherein the positive electrode of the lithium ion battery comprises a composite lithium supplement; the composite lithium supplement is the composite lithium supplement described above, or a composite lithium supplement prepared by the preparation method described above.

[0075] The lithium ion battery can be a button cell or a soft pack cell.

[0076] When the lithium-ion battery is a button battery:

[0077] The positive electrode of the lithium-ion battery is prepared by coating a positive electrode slurry including a positive electrode active material, a conductive agent, a binder and a solvent on a positive electrode current collector; the positive electrode active material is the composite lithium supplement agent described above, or the composite lithium supplement agent prepared by the preparation method described above.

[0078] The conductive agent is conductive carbon black (SP). The binder is polyvinylidene fluoride (PVDF). The solvent is N-methylpyrrolidone (NMP). The positive electrode current collector is aluminum foil.

[0079] In the positive electrode slurry, the mass ratio of the positive electrode active material, the conductive agent and the binder is 84-87:8-12:3-7, such as 85:10:5. The solid content of the positive electrode slurry is 20%-35%, such as 25%.

[0080] In certain embodiments of the present invention, the method for preparing the positive electrode of the lithium ion battery comprises the following steps:

[0081] After the positive electrode active material conductive agent, binder and solvent are mixed evenly, the obtained mixed slurry is coated on the positive electrode collector, and after drying, the mixed slurry is rolled and punched to obtain a positive electrode sheet.

[0082] The coating thickness is 100-250 μm, such as 250 μm.

[0083] The drying temperature is 100-140° C. and the drying time is 10-14 h.

[0084] When the lithium-ion battery is a button battery, the negative electrode is a lithium sheet; the separator is a polypropylene porous membrane, specifically a celgard2400 polypropylene porous membrane; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC), with a volume ratio of 1:1. The button battery is assembled in a glove box filled with argon gas, the water oxygen value in the glove box is controlled to be less than 0.01 ppm, and the battery is pressurized and sealed with a sealing machine to obtain a button battery.

[0085] When the lithium-ion battery is a soft-pack battery:

[0086] The positive electrode of the lithium-ion battery is prepared by coating a positive electrode slurry including a positive electrode active material, a binder, a conductive agent, a lithium supplement agent and a solvent on the surface of a positive electrode current collector; the lithium supplement agent is the composite lithium supplement agent described above, or the composite lithium supplement agent prepared by the preparation method described above.

[0087] The positive electrode active material is a single crystal high nickel ternary material or lithium iron phosphate. The single crystal high nickel ternary material is LiNi 0.92 Co 0.055 Mn 0.25 O2. The binder is a PVDF NMP solution with a mass concentration of 1% to 2%; or the binder is PVDF. The conductive agent is conductive carbon black (SP). The positive electrode current collector is aluminum foil with a thickness of 20 μm.

[0088] The mass ratios of the single crystal high nickel ternary material, the binder, the conductive agent and the lithium supplement agent are 94:3:2.5:0.5, 94:3:1.5:1.5, and 97:1.5:1:0.5. The solid content of the positive electrode slurry is 40% to 60%, such as 50% and 60%.

[0089] In certain embodiments of the present invention, the negative electrode of the lithium-ion battery is a graphite negative electrode. Or the negative electrode of the lithium-ion battery is prepared by coating a negative electrode slurry including silicon-carbon negative electrode 1800 (Cruder), conductive agent Super P, thickener (deionized aqueous solution of sodium carboxymethyl cellulose CMC), binder (deionized aqueous solution of styrene-butadiene rubber SBR), deionized aqueous solution of polyacrylic acid PAA and deionized aqueous solution of single-walled carbon nanotube CNT on the surface of the negative electrode current collector.

[0090] In certain embodiments of the present invention, the method for preparing the positive electrode of the lithium ion battery comprises the following steps:

[0091] After uniformly mixing the single crystal high nickel ternary material, the binder, the conductive agent, the lithium supplement agent and the solvent, the obtained mixed slurry is coated on the surface of the positive electrode collector, and after drying, the positive electrode sheet is obtained.

[0092] The single-sided thickness of the coating is 100-250 μm, such as 244 μm, 246 μm, 300 μm. The coating speed is 0.5-1.5 m / min, such as 1 m / min. The coating on the surface of the positive electrode current collector can be coated on both sides of the positive electrode current collector. The drying temperature is 140-150°C.

[0093] The positive electrode sheet is rolled, the tabs are welded, and the positive electrode sheet is paired with the graphite negative electrode to prepare a soft pack battery. The design voltage of the soft pack battery is 3-4.25 V and the design capacity is 2.5 Ah.

[0094] Or the positive electrode sheet and the negative electrode sheet are rolled separately, and the tabs are welded to prepare a soft-pack battery; the negative electrode sheet is prepared by uniformly coating a negative electrode slurry including a silicon-carbon composite material, a conductive agent, a thickener, a binder, a polyacrylic acid solution and a single-walled carbon nanotube solution on a negative electrode collector.

[0095] The present invention proposes a new composite lithium supplement, in which a nano catalyst is synthesized in situ on conductive carbon to form a nano composite catalyst. The nano composite catalyst is further used as a nucleating agent, and a high concentration of lithium salt is used to quickly synthesize a nano lithium oxalate coated composite catalyst to form a composite lithium oxalate lithium supplement.

[0096] The present invention directly prepares a Mo2C-MoO2 heterogeneous structure quantum dot nanocatalyst, and the quantum dot has abundant surface active sites and quantum edge effects, can provide effective catalytic activity, promote the decomposition reaction of lithium oxalate, reduce the boundary point of lithium oxalate, so that it can be decomposed in the conventional formation stage, release a large amount of active lithium, and increase the battery capacity. At the same time, the quantum dot has a high specific surface area and quantum size effect, can provide a large number of reactive sites, and accelerate the catalytic reaction. This helps to improve the reaction rate and efficiency, reduce energy consumption, and thus achieve efficient catalytic decomposition of lithium oxalate.

[0097] The present invention synthesizes nano quantum dot catalysts in situ on a conductive agent, and then quickly synthesizes nano lithium oxalate on the surface with the composite catalyst as the core to form a composite lithium oxalate lithium supplement. Compared with the existing lithium oxalate lithium supplement material with too high decomposition potential, the nano composite catalyst prepared in the present application can be quickly decomposed at a voltage of 4.12V to supplement a large amount of active lithium for the battery system.

[0098] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.

[0099] In order to further illustrate the present invention, a composite lithium supplement provided by the present invention, its preparation method and application are described in detail below in combination with examples, but it should not be understood as limiting the scope of protection of the present invention.

[0100] Example 1

[0101] 1) Preparation of nanocomposite catalysts:

[0102] The catalyst precursor (ammonium molybdate) and the carbon source (glucose) were added to water at a mass ratio of 5:1 (the mass ratio of the catalyst precursor to water was 1:4), and then mixed with the oxidized carbon nanotube dispersion (5 mg / mL, the solvent was water, and the mass ratio of the catalyst precursor to the oxidized carbon nanotube dispersion was 5:1), and ultrasonically treated (power was 2000 W) for 30 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 200 °C for 24 h. The product was collected by centrifugation at 10,000 rpm for 15 min, then washed repeatedly with water, and after freeze-drying, the sample was placed in an argon atmosphere at 5 °C min -1 The nanocomposite catalyst is heated to 750°C at a heating rate of 10000 nm and sintered at 750°C for 5 h to obtain a nanocomposite catalyst having a size of 50-100 nm.

[0103] 2) Preparation of composite lithium oxalate lithium supplement:

[0104] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in water to obtain a nanocomposite catalyst solution with a mass concentration of 10%, and a peristaltic pump is pumped (the pumping rate is 15 r / min) into a 70°C 1 mol / L oxalic acid aqueous solution and a 10 mol / L lithium hydroxide aqueous solution (room temperature), wherein the molar ratio of the oxalic acid to the lithium hydroxide is 1:1; the reaction is carried out at 25°C for 30 min, and lithium oxalate is coated on the surface of the nanocomposite catalyst to obtain a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 10%. The size of the composite lithium supplement is 200-300 nm.

[0105] 3) Button cell preparation:

[0106] The composite lithium supplement is used as a positive electrode active material, a conductive agent Sp, and a binder PVDF are mixed in a mass ratio of 85:10:5, and then mixed with a solvent N-methylpyrrolidone (NMP). The obtained mixed slurry (solid content is 25%) is coated (coating thickness is 250 μm) on an aluminum foil, and then placed in a 120°C forced air oven for drying for 12 h, and then rolled and punched to make a positive electrode sheet; a metal lithium sheet is used as a negative electrode, a celgard2400 polypropylene porous membrane is used as a diaphragm, and a 1 mol / L LiPF6 solution (the solvent is ethylene carbonate (EC) and dimethyl carbonate (DMC), and the volume ratio is 1:1) is used as an electrolyte; the process is carried out in a glove box filled with argon gas, the water oxygen value in the glove box is controlled to be less than 0.01 ppm, and the battery is pressurized and sealed with a sealing machine to obtain a button battery.

[0107] 4) Preparation of soft pack batteries:

[0108] Using single crystal morphology LiNi 0.92 Co 0.055 Mn 0.25 O2, a binder PVDF solution with a mass concentration of 1.5% (the solvent is NMP), a conductive agent Super P and the composite lithium supplement are mixed in a mass ratio of 94:3:2.5:0.5, and then NMP is added to obtain a positive electrode slurry with a solid content of 50%; the obtained positive electrode slurry is coated (the coating speed is 1 m / min, and the single-sided coating thickness is 244 μm) on both sides of a 20μm aluminum foil, and dried at 145°C to obtain a positive electrode sheet; the positive electrode sheet is rolled, the tabs are welded, and paired with a graphite negative electrode to prepare a soft-pack battery. The design voltage of the soft-pack battery is 3~4.25 V, and the design capacity is 2.5Ah.

[0109] Example 2

[0110] 1) Preparation of nanocomposite catalysts:

[0111] The catalyst precursor (nickel oxide) and the carbon source (lignin) were added to ethanol at a mass ratio of 4:1 (the mass ratio of the catalyst precursor to ethanol was 1:6), and then blended with acetylene black dispersion (3 mg / mL, the solvent was ethanol, and the mass ratio of the catalyst precursor to the acetylene black dispersion was 3:1), and ultrasonically treated (power was 100 W) for 50 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 150 °C for 20 h. The product was collected by centrifugation at 8000 rpm for 15 min, then washed repeatedly with water, and after freeze-drying, the sample was placed in an argon atmosphere at 5 °C min -1 The nanocomposite catalyst is heated to 750°C at a heating rate of 10000 nm and sintered at 750°C for 5 h to obtain a nanocomposite catalyst having a size of 50-100 nm.

[0112] 2) Preparation of composite lithium oxalate lithium supplement:

[0113] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in methanol to obtain a nanocomposite catalyst solution with a mass concentration of 12%, and a peristaltic pump is pumped (the pumping rate is 25 r / min) into an 80°C 1 mol / L oxalic acid aqueous solution and an 8 mol / L lithium hydroxide aqueous solution (room temperature), wherein the molar ratio of the oxalic acid to the lithium hydroxide is 1:1; the nanocomposite catalyst is rapidly reacted in 10°C cold water for 10 min to form a lithium oxalate coating on the surface of the nanocomposite catalyst, thereby obtaining a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 5%. The size of the composite lithium supplement is 75-150 nm.

[0114] The obtained composite lithium supplement was used to prepare button cells and soft pack cells according to steps 3) and 4) of Example 1.

[0115] Example 3

[0116] 1) Preparation of nanocomposite catalysts:

[0117] The catalyst precursor (molybdenum oxide) and the carbon source (carbon microspheres) were added to methanol at a mass ratio of 6:1 (the mass ratio of the catalyst precursor to methanol was 1:5), and then blended with a graphene oxide dispersion (6 mg / mL, the solvent was methanol, and the mass ratio of the catalyst precursor to the graphene oxide dispersion was 5:1), and ultrasonically treated (power was 1000 W) for 40 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 220 °C for 8 h. The product was collected by centrifugation at 12000 rpm for 10 min, then washed repeatedly with water, freeze-dried, and the sample was placed in an argon atmosphere at 5 °C min -1The catalyst was heated to 800°C at a heating rate of 10000 °C and sintered at 800°C for 3 h to obtain a nanocomposite catalyst having a size of 30-70 nm.

[0118] 2) Preparation of composite lithium oxalate lithium supplement:

[0119] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in methanol to obtain a nanocomposite catalyst solution with a mass concentration of 20%, and a peristaltic pump is used to pump (the pumping rate is 10 r / min) a 50°C 0.5 mol / L oxalic acid aqueous solution and an 8 mol / L lithium hydroxide aqueous solution (room temperature), wherein the molar ratio of the oxalic acid to the lithium hydroxide is 1:1, and a rapid reaction is carried out in 10°C cold water for 10 min to form a lithium oxalate coating on the surface of the nanocomposite catalyst to obtain a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 20%. The size of the composite lithium supplement is 100-200nm.

[0120] The obtained composite lithium supplement was used to prepare button cells and soft pack cells according to steps 3) and 4) of Example 1.

[0121] Example 4

[0122] 1) Preparation of nanocomposite catalysts:

[0123] Same as Example 1.

[0124] 2) Preparation of composite lithium oxalate lithium supplement:

[0125] Same as Example 1.

[0126] 3) The obtained composite lithium supplement was used to prepare a button cell according to step 3) of Example 1.

[0127] 4) Preparation of soft pack batteries:

[0128] Using single crystal morphology LiNi 0.92 Co 0.055 Mn 0.25 O2, a PVDF solution with a mass concentration of 1.5% (the solvent is NMP), a conductive agent Super P and the composite lithium supplement are mixed in a mass ratio of 94:3:1.5:1.5, and then NMP is added to obtain a positive electrode slurry with a solid content of 50%; the obtained positive electrode slurry is coated (the coating speed is 1 m / min, and the single-sided coating thickness is 246 μm) on both sides of a 20 μm aluminum foil, and dried at 145°C to obtain a positive electrode sheet.

[0129] The negative electrode material silicon carbon negative electrode 1800 (Cruder), conductive agent Super P, thickener (deionized water solution of sodium carboxymethyl cellulose CMC, mass concentration of 1.5%), binder (deionized water solution of styrene-butadiene rubber SBR, mass concentration of 48%), deionized water solution of polyacrylic acid PAA (mass concentration of 6%), and deionized water solution of single-walled carbon nanotube CNT (mass concentration of 0.4%) were mixed at a mass ratio of 95:0.9:1:1:2:0.1. After mixing, deionized water was added to control the theoretical solid content to 35%. The negative electrode slurry was obtained by homogenization using a vacuum defoamer, and the negative electrode slurry was evenly coated on a copper foil with a thickness of 17 μm. After drying, rolling and cutting, a 52 mm×72 mm negative electrode sheet was obtained. The N / P ratio of the positive and negative electrodes is 1.1.

[0130] The positive electrode sheet and the negative electrode sheet are respectively rolled and the tabs are welded to prepare a soft pack battery. The design voltage of the soft pack battery is 3-4.25 V and the design capacity is 2.5 Ah.

[0131] Example 5

[0132] 1) Preparation of nanocomposite catalysts:

[0133] The catalyst precursor (cobalt iron sulfate) and the carbon source (isonicotinic acid) were added to water at a mass ratio of 4:1 (the mass ratio of the catalyst precursor to water was 1:5), and then blended with a carbon black dispersion (6 mg / mL, the solvent was water, and the mass ratio of the catalyst precursor to the carbon black dispersion was 5:1), and ultrasonically treated (power was 1000 W) for 40 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 220 °C for 8 h. The product was collected by centrifugation at 12000 rpm for 10 min, then repeatedly washed with water, freeze-dried, and the sample was placed in an argon atmosphere at 5 °C min -1 The catalyst was heated to 800°C at a heating rate of 100°C and sintered at 800°C for 3 h to obtain a nanocomposite catalyst having a size of 100-150 nm.

[0134] 2) Preparation of composite lithium oxalate lithium supplement:

[0135] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in water to obtain a nanocomposite catalyst solution with a mass concentration of 7%, and a peristaltic pump is pumped (the pumping rate is 15 r / min) into a 60°C 0.5 mol / L oxalic acid aqueous solution and an 8 mol / L lithium hydroxide aqueous solution (room temperature) to react at 25°C for 30 min to form a lithium oxalate coating on the surface of the nanocomposite catalyst to obtain a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 8%. The size of the composite lithium supplement is 200-400 nm.

[0136] 3) The composite lithium supplement obtained in step 2) is used to prepare a button cell according to step 3) of Example 1.

[0137] 4) Preparation of soft pack batteries:

[0138] The composite lithium supplement agent obtained in step 2) is used to prepare a soft pack battery according to step 3) of Example 4. The design voltage of the soft pack battery is 3-4.25 V, and the design capacity is 2.5 Ah.

[0139] Example 6

[0140] 1) Preparation of nanocomposite catalysts:

[0141] The catalyst precursor (nickel acetylacetonate) and carbon source (graphite) were added to water at a mass ratio of 5:1 (the mass ratio of the catalyst precursor to water was 1:5), and then blended with acetylene black dispersion (5 mg / mL, the solvent was water, and the mass ratio of the catalyst precursor to acetylene black dispersion was 5:1), and ultrasonically treated (power was 2000 W) for 30 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 160 °C for 24 h. The product was collected by centrifugation at 10000 rpm for 15 min, then repeatedly washed with water, freeze-dried, and the sample was placed in an argon atmosphere at 5 °C min -1 The catalyst was heated to 700°C at a heating rate of 1.50°C and sintered at 700°C for 6 h to obtain a nanocomposite catalyst having a size of 50-80 nm.

[0142] 2) Preparation of composite lithium oxalate lithium supplement:

[0143] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in water to obtain a nanocomposite catalyst solution with a mass concentration of 20%, and a 1 mol / L oxalic acid aqueous solution at 70°C and a 9 mol / L lithium hydroxide aqueous solution (room temperature) are pumped into the solution by a peristaltic pump (the pumping rate is 10 r / min), and reacted at 20°C for 30 min to form a lithium oxalate coating on the surface of the nanocomposite catalyst to obtain a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 10%. The size of the composite lithium supplement is 200-300 nm.

[0144] 3) The composite lithium supplement obtained in step 2) is used to prepare a button cell according to step 3) of Example 1.

[0145] 4) Preparation of soft pack batteries:

[0146] The composite lithium supplement agent obtained in step 2) is used to prepare a soft pack battery according to step 3) of Example 4. The design voltage of the soft pack battery is 3-4.25 V, and the design capacity is 2.5 Ah.

[0147] Example 7

[0148] 1) Preparation of nanocomposite catalysts:

[0149] Same as Example 1.

[0150] 2) Preparation of composite lithium oxalate lithium supplement:

[0151] Same as Example 1.

[0152] 3) The composite lithium supplement obtained in step 2) is used to prepare a button cell according to step 3) of Example 1.

[0153] 4) Preparation of soft pack batteries:

[0154] Lithium iron phosphate, PVDF, conductive agent Super P and the composite lithium supplement are mixed in a mass ratio of 97:1.5:1:0.5, and then NMP is added to obtain a positive electrode slurry with a solid content of 60%; the obtained positive electrode slurry is coated (coating speed is 1m / min, and the single-sided thickness of the coating is 300 μm) on both sides of a 20μm aluminum foil, and dried at 145°C to obtain a positive electrode sheet; the positive electrode sheet is rolled, the tabs are welded, and paired with the graphite negative electrode to prepare a soft-pack battery. The design voltage of the soft-pack battery is 2.5~3.75 V, and the design capacity is 2.5 Ah.

[0155] Example 8

[0156] 1) Preparation of nanocomposite catalysts:

[0157] The catalyst precursor (ferric acetate hydrate) and the carbon source (polyether P123) were added to water at a mass ratio of 5:1 (the mass ratio of the catalyst precursor to water was 1:4), and then blended with the oxidized carbon nanotube dispersion (5 mg / mL, the solvent was water, and the mass ratio of the catalyst precursor to the oxidized carbon nanotube dispersion was 5:1), and ultrasonically treated (power was 2000 W) for 40 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 190 °C for 20 h. The product was collected by centrifugation at 11000 rpm for 18 min, then washed repeatedly with water, and after freeze-drying, the sample was placed in an argon atmosphere at 5 °C min -1 The catalyst was heated to 720°C at a heating rate of 1000 nm and sintered at 720°C for 4 h to obtain a nanocomposite catalyst having a size of 85-125 nm.

[0158] 2) Preparation of composite lithium oxalate lithium supplement:

[0159] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in water to obtain a nanocomposite catalyst solution with a mass concentration of 5%, and a peristaltic pump is pumped (the pumping rate is 15 r / min) into a 65°C 0.8 mol / L oxalic acid aqueous solution and an 8.5 mol / L lithium hydroxide aqueous solution (room temperature) to react at 20°C for 30 min to form a lithium oxalate coating on the surface of the nanocomposite catalyst to obtain a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 12%. The size of the composite lithium supplement is 200-300 nm.

[0160] 3) The composite lithium supplement obtained in step 2) is used to prepare a button cell according to step 3) of Example 1.

[0161] 4) Preparation of soft pack batteries:

[0162] The composite lithium supplement agent obtained in step 2) is used to prepare a soft pack battery according to step 3) of Example 7. The design voltage of the soft pack battery is 2.5-3.75 V, and the design capacity is 2.5 Ah.

[0163] Example 9

[0164] 1) Preparation of nanocomposite catalysts:

[0165] The catalyst precursor (titanic acid sulfate hydrate) and the carbon source (glycine) were added to DMF at a mass ratio of 6:1 (the mass ratio of the catalyst precursor to DMF was 1:4), and then mixed with a graphene oxide dispersion (4 mg / mL, the solvent was DMF, and the mass ratio of the catalyst precursor to the graphene oxide dispersion was 5:1), and ultrasonically treated (power was 1500W) for 30 min. The solution was then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and reacted in an oven at 200°C for 12 h. The product was collected by centrifugation at 10,000 rpm for 20 min, then washed repeatedly with water, and after freeze-drying, the sample was placed in an argon atmosphere at 5°C min -1 The nanocomposite catalyst is heated to 780°C at a heating rate of 1000 nm and sintered at 780°C for 5 h to obtain a nanocomposite catalyst having a size of 75-100 nm.

[0166] 2) Preparation of composite lithium oxalate lithium supplement:

[0167] The nanocomposite catalyst is used as a nucleating agent, stirred and dispersed uniformly in water to obtain a nanocomposite catalyst solution with a mass concentration of 10%, and a 1 mol / L oxalic acid aqueous solution at 70°C and a 9.5 mol / L lithium hydroxide aqueous solution (room temperature) are pumped into the solution by a peristaltic pump (at a pumping rate of 10 r / min), and reacted rapidly at 10°C for 10 min to form a lithium oxalate coating on the surface of the nanocomposite catalyst to obtain a nanoscale composite lithium supplement. In the composite lithium supplement, the mass content of the nanocomposite catalyst is 16%. The size of the composite lithium supplement is 125-150 nm.

[0168] 3) The composite lithium supplement obtained in step 2) is used to prepare a button cell according to step 3) of Example 1.

[0169] 4) Preparation of soft pack batteries:

[0170] The composite lithium supplement agent obtained in step 2) is used to prepare a soft pack battery according to step 3) of Example 7. The design voltage of the soft pack battery is 2.5-3.75 V, and the design capacity is 2.5 Ah.

[0171] Comparative Example 1

[0172] The difference from Example 1 is:

[0173] The composite lithium supplement is replaced with lithium oxalate.

[0174] Comparative Example 2

[0175] The difference from Example 2 is:

[0176] The composite lithium supplement is replaced by: lithium oxalate, carbon nanotubes and MoC 1-x / NC ball milled mixture; the lithium oxalate, carbon nanotubes and MoC 1-x The mass ratio of / NC is 6:1:3.

[0177] MoC 1-x / NC preparation: Graphitized carbon trinitrogen tetrakis (g-C3N4) and ammonium molybdate hexahydrate ((NH4)6Mo7O 24 ·4H2O) were mixed by ball milling at a mass ratio of 2:1 for 3 h to obtain a Mo-C3N4 precursor. Subsequently, the Mo-C3N4 precursor was kept at 800°C for 2 h in a high-temperature furnace protected by argon to obtain MoC 1-x / NC catalyst.

[0178] Comparative Example 3

[0179] The difference from Example 3 is:

[0180] The nanocomposite catalyst in step 2) was replaced by carbon black and Mo2C in a mass ratio of 5:1.

[0181] Comparative Example 4

[0182] The difference from Example 4 is:

[0183] The 1 mol / L oxalic acid aqueous solution at 70°C in step 2) was replaced with a 0.05 mol / L oxalic acid aqueous solution at 25°C.

[0184] Comparative Example 5

[0185] The difference from Example 5 is:

[0186] The 8 mol / L lithium hydroxide aqueous solution was replaced with a 1 mol / L lithium hydroxide aqueous solution.

[0187] Comparative Example 6

[0188] The difference from Example 6 is:

[0189] In step 2), the nanocomposite catalyst is directly mixed with lithium oxalate to obtain a composite lithium supplement agent. The mass content of the nanocomposite catalyst in the composite lithium supplement agent is 10%.

[0190] Comparative Example 7

[0191] The difference from Example 7 is that:

[0192] In step 2), the mass content of the nanocomposite catalyst in the composite lithium supplement is 5%.

[0193] Comparative Example 8

[0194] The difference from Example 8 is that:

[0195] In step 3), the composite lithium supplement is replaced with Li5FeO4.

[0196] Comparative Example 9

[0197] The difference from Example 9 is:

[0198] In step 3), the composite lithium supplement is replaced with Li2NiO2.

[0199] The button cells of Examples 1 to 3, 5, 6, 8, 9 and Comparative Examples 1 to 9 were subjected to electrochemical performance tests to test the lithium de-lithiation potential and the initial charge and discharge specific capacity of the lithium supplement material. The lithium de-lithiation potential of the lithium supplement material is reduced, which effectively alleviates the interfacial side reactions between the positive electrode material and the electrolyte under high de-lithiation potential. The initial charge and discharge specific capacity also reflects the amount of active lithium provided by the lithium supplement material in the battery system. The battery test was carried out at a constant temperature of 25°C, and the charge and discharge mode was: 0.1C constant current charging to 4.6V.

[0200] Table 1 Electrochemical properties of button cells of Examples 1 to 3, 5, 6, 8, 9 and Comparative Examples 1 to 9

[0201]

[0202] As can be seen from Table 1, under the same battery system, compared with Comparative Examples 1 to 7, the lithium de-lithiation potential of Examples 1 to 3, 5, 6, 8, and 9 is significantly lower than that of the comparative example battery, and the lithium oxalate in Comparative Example 1 without a catalyst cannot be de-lithiated at a voltage of 4.6V, and no active lithium is released. This shows that the composite nanocatalyst can reduce the reaction energy barrier and improve the solid-solid catalytic effect. This is because the quantum dots have abundant surface active sites and quantum edge effects, which help promote the decomposition reaction of lithium oxalate. At the same time, the quantum dots have a high specific surface area and quantum size effect, provide a large number of reactive sites, accelerate the catalytic reaction, thereby improving the reaction rate and efficiency, reducing energy consumption, and achieving efficient catalytic decomposition of lithium oxalate. At the same time, the first charge and discharge specific capacity and the first charge and discharge efficiency are improved, indicating that the lithium supplement can provide more active lithium to compensate for the negative effects such as capacity reduction caused by the loss of active lithium due to the formation of SEI film. Although Comparative Example 8 has a lower de-lithiation potential and a higher specific capacity for releasing active lithium, it will produce electrochemically inert LiFeO2 after de-lithiation, reducing the capacity of the overall battery system. The Li2NiO2 used in Comparative Example 9 was delithiated to generate unstable LiNiO2, Ni 3+ It has high reactivity and can aggravate the side reaction of the electrolyte inside the battery, thus reducing the long cycle stability of the battery. It can be seen that after lithium supplementation in Comparative Examples 8-9, substances that are not conducive to the electrochemical performance of the battery are produced, while the composite lithium supplement in the embodiment is a sacrificial lithium supplement, and there is no residue after lithium supplementation, and it does not affect the stability of the battery system.

[0203] The design voltage of the soft-pack batteries of Examples 1-6 and Comparative Examples 1-6 is 3-4.25V, and the design capacity is 2.5Ah.

[0204] The design voltage of the soft-pack batteries of Examples 7 to 9 and Comparative Examples 7 to 9 is 2.5 to 3.75 V, and the design capacity is 2.5 Ah.

[0205] The soft-pack batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 9 were respectively subjected to room temperature cycle performance tests, and the results obtained are shown in Table 2.

[0206] Formation:

[0207] The sealed soft-pack batteries of Examples 1 to 9 and Comparative Examples 1 to 9 were clamped with a glass clamp, and the formation program was set as 0.1C constant current charging to 3.4 V, leaving for 5 min, 0.2C constant current charging to 3.9 V, leaving for 5 min, 0.5C constant current charging to 4.35 V, and stopping; the charged batteries were placed in an oven at 45°C and left to stand for 24 h to complete the formation of the soft-pack batteries.

[0208] Battery room temperature cycle performance test:

[0209] The soft-pack batteries prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were placed in a constant temperature room at an ambient temperature of 25°C, charged at a constant current of 1C to a voltage of 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C, and then discharged at a constant current of 1C to a voltage of 3.0V. The cycle was repeated for 2000 cycles, and the capacity retention rate was recorded. The capacity retention rate of the nth cycle (%) = (discharge capacity of the nth cycle / discharge capacity of the first cycle) × 100%.

[0210] The soft-pack batteries prepared in Examples 7 to 9 and Comparative Examples 7 to 9 were placed in a constant temperature room at an ambient temperature of 25°C, charged at a constant current of 1C to a voltage of 3.75V, then charged at a constant voltage of 3.75V to a current of 0.05C, and then discharged at a constant current of 1C to a voltage of 2.5V. The cycle was repeated for 2000 cycles, and the capacity retention rate was recorded. The capacity retention rate of the nth cycle (%) = (discharge capacity of the nth cycle / discharge capacity of the first cycle) × 100%.

[0211] Table 2 Room temperature cycle performance of soft pack batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 9

[0212]

[0213] As can be seen from Table 2, under the same battery system, after 2000 cycles, the batteries prepared in Examples 1 to 9 show good cycle stability. This is because as the cycle progresses, the SEI on the surface of the positive and negative electrode materials will be destroyed and reconstructed due to factors such as material volume expansion and interface side reactions between the electrolyte and the surface of the positive and negative electrode materials. This process will re-form a new SEI, and a portion of active lithium will be lost. The use of a composite lithium oxalate lithium supplement can provide a large amount of active lithium, so the cycle retention rate of 2000 weeks is relatively high. The lithium oxalate lithium supplement with a common catalyst composite used in Comparative Examples 1 to 7 has no effect because the lithium de-lithiation potential is too high and cannot provide active lithium in the conventional formation stage. Although the lithium supplement agent used in Comparative Examples 8 to 9 has a certain lithium supplement effect, it will generate electrochemically inert or highly active substances after lithium supplementation, so there are application problems to be solved. The composite lithium oxalate lithium supplement agent prepared in Examples 1 to 9 avoids this problem due to its specific sacrificial lithium supplement agent characteristics. The remaining composite nanocatalyst can improve electronic conductivity, reduce internal impedance, reduce internal energy loss, and improve electrochemical stability.

[0214] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A composite lithium supplement, characterized in that: include: Nanocomposite catalysts; A lithium oxalate coating layer formed on the surface of the nanocomposite catalyst; The nanocomposite catalyst is prepared from raw materials including a catalyst precursor, a carbon source and a conductive agent dispersion; the nanocomposite catalyst is synthesized in situ on the conductive agent; The preparation method of the nanocomposite catalyst comprises the following steps: S1) mixing a catalyst precursor, a carbon source, a solvent and a conductive agent dispersion, and performing a solvothermal reaction to obtain a solid product; S2) sintering the solid product under a protective gas atmosphere to obtain the nanocomposite catalyst.

2. The composite lithium supplement according to claim 1, characterized in that: The catalyst precursor includes at least one of metal salts, metal salt hydrates, metal complexes, metal oxides and metal organics; the metal element in the catalyst precursor includes at least one of ammonium, nickel, cobalt, iron, cerium, neodymium and titanium.

3. The composite lithium supplement according to claim 1, characterized in that: The carbon source includes at least one of an organic carbon source and an inorganic carbon source; The organic carbon source includes at least one of glucose, cellulose, lignin, amino acids, biopolymers, organic acids and macromolecular carbon chains; The inorganic carbon source comprises at least one of graphite, graphene, fullerene, carbon microspheres, carbon quantum dots, carbon aerogel, carbon fiber, glassy carbon, carbon nanohorns, carbon nanofibers, carbon nanofoams, carbon nanoonions and carbon-coated substances; The mass ratio of the catalyst precursor to the carbon source is (4-6):

1.

4. The composite lithium supplement according to claim 1, characterized in that: The conductive agent includes at least one of acetylene black, carbon black, graphene, carbon nanotubes, carbon fibers, carbon quantum dots, oxidized graphite materials, oxidized carbon nanotubes, reduced graphite materials, carbon microspheres and carbon aerogels.

5. The composite lithium supplement according to claim 1, characterized in that: The solvent of the conductive agent dispersion is selected from at least one of water, alcohol solvents and polar solvents; the concentration of the conductive agent dispersion is 3-6 mg / mL; The reaction temperature of the solvent thermal reaction is 140-220° C.; the protective gas is selected from nitrogen or argon.

6. The composite lithium supplement according to claim 1, characterized in that: The sintering temperature is 700-800°C and the sintering time is 3-6 h.

7. The composite lithium supplement according to claim 1, characterized in that: In the composite lithium supplement, the mass proportion of the nanocomposite catalyst is 5% to 20%.

8. A method for preparing the composite lithium supplement according to any one of claims 1 to 7, characterized in that: The following steps are involved: The nano composite catalyst solution, oxalic acid solution and lithium hydroxide solution are mixed and reacted to obtain a composite lithium supplement agent.

9. The preparation method according to claim 8, characterized in that: Mixing the nanocomposite catalyst solution, the oxalic acid solution and the lithium hydroxide solution comprises: Pumping oxalic acid solution and lithium hydroxide solution into the nanocomposite catalyst solution for reaction, thereby obtaining a composite lithium supplement; The pumping rate is 10-25 r / min; The mass concentration of the nanocomposite catalyst solution is 5% to 30%; the molar concentration of the oxalic acid solution is 0.5 to 1 mol / L; the molar concentration of the lithium hydroxide solution is 8 to 10 mol / L; The temperature of the pumped oxalic acid solution is 50-80°C; the temperature of the lithium hydroxide solution is room temperature; and the temperature of the reaction is 10-25°C.

10. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery includes a composite lithium supplement; The composite lithium supplement is the composite lithium supplement according to any one of claims 1 to 7, or is the composite lithium supplement obtained by the preparation method according to any one of claims 8 to 9.

Citation Information

Cited By

  • A lithium supplement additive, Li5FeO4, and its preparation method

    CN120398125B