A method for preparing a modified liquid-permeable surface layer
By setting a hydrophobic layer and a skin care layer in the surface layer of sanitary products, a spaced connection structure is formed, which solves the problem that the existing surface layer is difficult to achieve fast absorption and prevent reverse osmosis at a fixed point, and achieves rapid absorption and skin care effects of liquids. It is suitable for Diaper products and reduce production costs and environmental pollution.
Patent Information
- Application Number
- CN202410999047.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
It is difficult to achieve fast absorption and prevention of reverse osmosis on the surface of existing sanitary products.
The preparation method of a modified liquid-permeable surface layer includes a hydrophobic layer, a hydrophilic layer and a skin care layer arranged from top to bottom, and the hydrophobic material is applied through a first roller coating mechanism and a second roller coating mechanism is applied to the skin care material. , a hydrophobic area and a skin care area are formed that are connected in intervals, and a modified liquid-permeable surface layer is formed by drying hot air.
It realizes fast absorption of liquid at a fixed point and prevents reverse osmosis, keeps it dry and comfortable, and provides skin care effects. It is suitable for diaper products, reducing production costs and environmental pollution.
Smart Images

Figure CN118542779B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sanitary products, and in particular to a method for preparing a modified liquid-permeable surface layer. Background Art
[0002] Chinese patent publication number CN116999246A discloses a composite surface layer of sanitary products, which is composed of a surface layer, a guide layer, a water absorption layer and a diffusion layer from top to bottom, the guide layer and the diffusion layer are both composed of mixed fibers of ES fiber and wood pulp, the water absorption layer is composed of a polymer water-absorbing resin, and the guide layer is evenly permeated with the polymer water-absorbing resin; the surface layer is made of hot air non-woven fabric or ES fiber. The composite surface layer is a four-layer structure, and its guide layer is made of mixed fibers of ES fiber and wood pulp according to the weight ratio, which cannot achieve fixed-point rapid absorption and has limited ability to prevent reverse osmosis. Summary of the invention
[0003] Therefore, in view of the above problems, the present invention provides a method for preparing a modified liquid-permeable surface layer to solve the problem that the existing method for preparing the surface layer of sanitary products is difficult to achieve fast absorption at a fixed point and prevent reverse osmosis.
[0004] To achieve the above object, the present invention is implemented by the following technical solutions:
[0005] A method for preparing a modified liquid-permeable surface layer, the modified liquid-permeable surface layer comprising a hydrophobic layer, a hydrophilic layer and a skin-care layer arranged in sequence from top to bottom, the hydrophilic layer adopts a bamboo fiber spunlace non-woven fabric, the hydrophobic layer comprises a plurality of mutually spaced and connected hydrophobic regions, the skin-care layer comprises a plurality of mutually spaced and connected skin-care regions, and each of the skin-care regions is respectively arranged below each of the hydrophobic regions;
[0006] The method for preparing the modified liquid-permeable surface layer comprises the following steps:
[0007] S1, coating a hydrophobic material on the upper surface of the hydrophilic layer by a first roller coating mechanism;
[0008] S2, drying the hydrophobic material applied in step S1 to form the hydrophobic layer on the upper surface of the hydrophilic layer;
[0009] S3, coating the skin care material on the lower surface of the hydrophilic layer by a second roller coating mechanism;
[0010] S4, drying the skin care material applied in step S3 to form the skin care layer on the lower surface of the hydrophilic layer;
[0011] The first roller coating mechanism comprises a first rolling shaft, a first rotating shaft, a second rotating shaft and a first liquid storage tank, the first rotating shaft is arranged on one side of the first rolling shaft, the second rotating shaft is arranged on the other side of the first rotating shaft, the first liquid storage tank is arranged below the second rotating shaft, a sponge layer is arranged on the outer sleeves of the first rotating shaft and the second rotating shaft, a plurality of first protrusions are arranged on the surface of the first rolling shaft, and a first sponge sheet is arranged on the top of each of the first protrusions;
[0012] The second roller coating mechanism comprises a second rolling shaft and a second liquid storage tank, a plurality of second protrusions are arranged on the surface of the second rolling shaft, and a second sponge sheet is arranged on the top of each second protrusion;
[0013] The first rolling axis has a radius smaller than that of the second rolling axis.
[0014] Furthermore, hot air penetration drying is adopted in step S2 and step S4.
[0015] Furthermore, the hydrophobic material is composed of the following components in parts by weight: 10-15 parts of diethylene glycol monobutyl ether; 8-12 parts of dimethyl silicone oil; 5-10 parts of distearic acid glyceryl; 0.5-2 parts of glycerol; 0.5-2 parts of distearyl dimethyl ammonium chloride; and 60-70 parts of deionized water.
[0016] Furthermore, the preparation of the skin care material comprises the following steps:
[0017] 1) Take 1 part of pullulan, 1 part of carboxymethyl cellulose, 40 parts of aloe vera gel and 200 parts of deionized water;
[0018] 2) dissolving a formulated amount of pullulan in a formulated amount of deionized water to form a pullulan solution;
[0019] 3) adding the formulated amount of aloe vera gel and carboxymethyl cellulose to the pullulan solution and stirring to mix evenly to obtain a mixed solution;
[0020] 4) The pH of the mixed solution is adjusted to 4.5-5.5 using lactic acid to obtain a skin care material.
[0021] Furthermore, the thickness of the first sponge sheet is smaller than the thickness of the sponge layer.
[0022] Furthermore, the liquid surface in the first liquid storage tank is in contact with the sponge layer sleeved on the surface of the second rotating shaft.
[0023] Furthermore, the liquid surface in the second liquid storage tank contacts the second sponge sheet on the surface of the second protrusion.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention makes the hydrophilic layer have the characteristics of hydrophilic and hydrophobic zoning through the coating of hydrophobic materials. When the surface layer contacts the liquid, the liquid can only gather between the intervals of each hydrophobic area and be quickly penetrated by the hydrophilic layer. When used in diaper products, the product can have the characteristics of fixed-point rapid absorption, achieving the characteristics of dryness and comfort. At the same time, it can also avoid the phenomenon of reverse osmosis and maintain dryness; through the coating of skin care materials, since the skin care area is arranged below the hydrophobic area, the liquid diffuses through the intervals between the hydrophobic areas to the skin care layer at the bottom of the hydrophilic layer, and then diffuses the skin care material in the skin care area to the intervals between the hydrophobic areas. If it comes into contact with the skin, it has a skin care effect.
[0026] 2. The present invention can continuously coat the upper surface of the hydrophilic layer through the first roller coating mechanism to form hydrophobic areas that are spaced apart and interconnected, and can continuously coat the lower surface of the hydrophilic layer through the second roller coating mechanism to form skin care areas that are spaced apart and interconnected.
[0027] 3. The present invention simplifies the structure by setting up a second roller coating mechanism whose structural composition is different from the first roller coating mechanism. By setting the radius of the first rolling axis to be smaller than that of the second rolling axis, the linear speed of the second protrusion on the surface of the second rolling axis in continuous production is reduced to avoid dragging up the liquid in the second liquid storage tank. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic structural diagram of a first roller coating mechanism and a second roller coating mechanism according to a first embodiment of the present invention;
[0029] Figure 2 This is a schematic diagram of the decomposed structure of each structural layer in the first embodiment of the present invention;
[0030] Figure 3 This is a schematic diagram of the first protrusion structure of Embodiment 1 of the present invention;
[0031] Figure 4 This is a schematic diagram of the shape structure of the hydrophobic area in Example 1 of the present invention;
[0032] Figure 5 This is a schematic diagram of the shape structure of the hydrophobic area in a preferred embodiment of the present invention;
[0033] Figure 6 for Figure 1 The enlarged structural diagram at A in the middle;
[0034] Figure 7 for Figure 1 The enlarged structural diagram at B in the middle;
[0035] Figure 8 It is a schematic diagram of the structure of the first rotating shaft and the second rotating shaft according to the second embodiment of the present invention.
[0036] Description of Figure Numbers
[0037] Hydrophobic layer 1; Hydrophobic region 11;
[0038] Hydrophilic layer 2;
[0039] Skin care layer 3; Skin care area 31;
[0040] First roller coating mechanism 4; first rolling shaft 41; first rotating shaft 42; second rotating shaft 43; first liquid storage tank 44; sponge layer 45; first protrusion 46; first sponge sheet 47; first liquid leakage port 48;
[0041] The second roller coating mechanism 5 ; the second rolling shaft 51 ; the second liquid storage tank 52 ; the second protrusion 53 ; the second sponge sheet 54 ; and the second liquid leakage port 55 . DETAILED DESCRIPTION
[0042] The following will describe the implementation methods of the present invention in detail in conjunction with specific embodiments, so that the implementation process of how the present invention applies technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly. Embodiment 1
[0043] like Figures 1 to 7 As shown, a method for preparing a modified liquid-permeable surface layer, the modified liquid-permeable surface layer comprises a hydrophobic layer 1, a hydrophilic layer 2 and a skin-care layer 3 arranged in sequence from top to bottom, the hydrophilic layer 2 is made of bamboo fiber spunlace non-woven fabric, the hydrophobic layer 1 comprises a plurality of mutually spaced and connected hydrophobic regions 11, the skin-care layer 3 comprises a plurality of mutually spaced and connected skin-care regions 31, and each of the skin-care regions 31 is respectively arranged below each of the hydrophobic regions 11;
[0044] Bamboo fiber spunlace nonwoven fabric is not only skin-friendly and environmentally friendly, but also has a natural antibacterial effect. Natural bamboo fiber has better hypoallergenicity, and its raw material comes from bamboo that is widely planted in my country. It has a short growth cycle, is environmentally friendly and easy to plant, and the material can be degraded after use, which can effectively reduce environmental pollution.
[0045] The method for preparing the modified liquid-permeable surface layer comprises the following steps:
[0046] S1, coating a hydrophobic material on the upper surface of the hydrophilic layer 2 by a first roller coating mechanism 4;
[0047] S2, drying the hydrophobic material applied in step S1 to form the hydrophobic layer 1 on the upper surface of the hydrophilic layer 2;
[0048] S3, coating the skin care material on the lower surface of the hydrophilic layer 2 by the second roller coating mechanism 5;
[0049] S4, drying the skin care material applied in step S3 to form the skin care layer 3 on the lower surface of the hydrophilic layer 2;
[0050] The first roller coating mechanism 4 comprises a first rolling shaft 41, a first rotating shaft 42, a second rotating shaft 43 and a first liquid storage tank 44. The first rotating shaft 42 is arranged on one side of the first rolling shaft 41, and the second rotating shaft 43 is arranged on the other side of the first rotating shaft 42. The first liquid storage tank 44 is arranged below the second rotating shaft 43. The first rotating shaft 42 and the second rotating shaft 43 are covered with a sponge layer 45. The surface of the first rolling shaft 41 is provided with a plurality of first protrusions 46, and the top of each of the first protrusions 46 is provided with a first sponge sheet 47.
[0051] The second roller coating mechanism 5 comprises a second rolling shaft 51 and a second liquid storage tank 52. The surface of the second rolling shaft 51 is provided with a plurality of second protrusions 53. The top of each second protrusion 53 is provided with a second sponge sheet 54.
[0052] The radius of the first rolling axis 41 is smaller than that of the second rolling axis 51;
[0053] The present application does not specifically limit the number of the first protrusions 46 and the second protrusions 53, which can be adjusted according to actual conditions. To ensure that each skin care layer 3 is formed under each hydrophobic layer 1, the arrangement of the first protrusions 46 and the second protrusions 53 and the distance between the first rolling shaft 41 and the second rolling shaft 51 can be adjusted, which will not be described in detail here.
[0054] The hydrophobic area 11 and the skin care area 31 formed in the present application are rectangular. In other preferred embodiments, the hydrophobic area 11 and the skin care area 31 can also be other geometric shapes, such as honeycomb, triangle, etc., and the first protrusions 46 and the second protrusions 53 of corresponding shapes can be provided;
[0055] By coating with hydrophobic material, the hydrophilic layer 2 has the characteristics of hydrophilic and hydrophobic partitions. When the surface layer contacts the liquid, the liquid can only gather between the intervals of the hydrophobic areas 11 and be quickly penetrated by the hydrophilic layer 2. When used in diaper products, the product can have the characteristics of fixed-point rapid absorption, achieving the characteristics of dryness and comfort. At the same time, it can also avoid the phenomenon of reverse osmosis and keep dryness. By coating with skin care material, since the skin care area 31 is arranged below the hydrophobic area 11, the liquid diffuses through the intervals between the hydrophobic areas 11 to the skin care layer 3 at the bottom of the hydrophilic layer 2, and then the skin care material in the skin care area 31 is diffused to the intervals between the hydrophobic areas 11. If it contacts the skin, it has a skin care effect. Due to the barrier of the hydrophobic layer 1, the liquid penetrates the hydrophilic layer 2 without causing all the skin care materials to diffuse. The diaper product made of this surface layer has a long-lasting skin care function.
[0056] The upper surface of the hydrophilic layer 2 can be continuously coated by the first roller coating mechanism 4 to form the hydrophobic areas 11 which are spaced apart and interconnected, and the lower surface of the hydrophilic layer can be continuously coated by the second roller coating mechanism 5 to form the skin care areas 31 which are spaced apart and interconnected; the second roller coating mechanism 5 is provided with a structural component different from the first roller coating mechanism 4 to simplify the structure, and the radius of the first rolling shaft 41 is provided to be smaller than the second rolling shaft 51 to reduce the linear speed of the second protrusion 53 on the surface of the second rolling shaft 51 during continuous production, so as to avoid carrying up the liquid in the second liquid storage tank 52;
[0057] In step S2 and step S4, hot air penetration drying is adopted, wherein hot air penetration drying is a conventional technical means in the art and will not be described in detail here;
[0058] The hydrophobic material is composed of the following components in parts by weight: 13 parts of diethylene glycol monobutyl ether; 11 parts of dimethyl silicone oil; 7 parts of distearic acid glyceryl; 1 part of glycerol; 1 part of distearyl dimethyl ammonium chloride; and 67 parts of deionized water.
[0059] The modified liquid-permeable surface layer obtained by coating with a hydrophobic material has a unidirectional moisture conduction function, and the diapers prepared with the modified liquid-permeable surface layer have a lower slip and back-seepage amount, thereby achieving the effect of fast urine transmission, strong water lock and no back-seepage;
[0060] The preparation of the skin care material comprises the following steps:
[0061] 1) Take 1 part of pullulan, 1 part of carboxymethyl cellulose, 40 parts of aloe vera gel and 200 parts of deionized water;
[0062] 2) dissolving a formulated amount of pullulan in a formulated amount of deionized water to form a pullulan solution;
[0063] 3) adding the formulated amount of aloe vera gel and carboxymethyl cellulose to the pullulan solution and stirring to mix evenly to obtain a mixed solution;
[0064] 4) adjusting the pH of the mixed solution to 5 using lactic acid to obtain a skin care material;
[0065] The skin care material is attached to the lower surface of the hydrophilic layer by coating, the raw material loss is low in the production process, the environment is friendly, and the production cost is low. The aloe vera gel is coated with pullulan as a biofilm, and the high activity of the aloe vera gel can be ensured by hot air drying and evaporating water.
[0066] The thickness of the first sponge sheet 47 is smaller than that of the sponge layer 45, so as to ensure that when the first sponge sheet 47 contacts the sponge layer 45, the first sponge sheet 47 can absorb sufficient liquid from the sponge layer 45;
[0067] The liquid level in the first liquid storage tank 44 contacts the sponge layer 45 sleeved on the surface of the second rotating shaft 43; the liquid level in the second liquid storage tank 52 contacts the second sponge sheet 54 on the surface of the second protrusion 53;
[0068] In order to ensure that the liquid level in the first liquid storage tank 44 can always contact the sponge layer 45, it is necessary to continuously transport hydrophobic material into the first liquid storage tank 44. At the same time, a first liquid leakage port 48 for limiting the liquid level height is set on the side of the first liquid storage tank 44. Similarly, a second liquid leakage port 55 is set on the side of the second liquid storage tank 52, which will not be repeated here. Embodiment 2
[0069] like Figure 8 As shown, different from the first embodiment, the diameter of the second rotating shaft 43 is larger than the diameter of the first rotating shaft 42 to prevent the second sponge sheet 54 from bringing up the liquid in the second liquid storage tank 52 due to an excessively fast rotation speed of the second rotating shaft 43 .
[0070] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A method for preparing a modified liquid-permeable surface layer, characterized in that: The modified liquid-permeable surface layer comprises a hydrophobic layer, a hydrophilic layer and a skin care layer arranged in sequence from top to bottom, the hydrophilic layer is made of bamboo fiber spunlace non-woven fabric, the hydrophobic layer comprises a plurality of mutually spaced and connected hydrophobic areas, the skin care layer comprises a plurality of mutually spaced and connected skin care areas, and each of the skin care areas is respectively arranged below each of the hydrophobic areas; The method for preparing the modified liquid-permeable surface layer comprises the following steps: S1, coating a hydrophobic material on the upper surface of the hydrophilic layer by a first roller coating mechanism; S2, drying the hydrophobic material applied in step S1 to form the hydrophobic layer on the upper surface of the hydrophilic layer; S3, coating the skin care material on the lower surface of the hydrophilic layer by a second roller coating mechanism; S4, drying the skin care material applied in step S3 to form the skin care layer on the lower surface of the hydrophilic layer; The first roller coating mechanism comprises a first rolling shaft, a first rotating shaft, a second rotating shaft and a first liquid storage tank, the first rotating shaft is arranged on one side of the first rolling shaft, the second rotating shaft is arranged on the other side of the first rotating shaft, the first liquid storage tank is arranged below the second rotating shaft, a sponge layer is arranged on the outer sleeves of the first rotating shaft and the second rotating shaft, a plurality of first protrusions are arranged on the surface of the first rolling shaft, and a first sponge sheet is arranged on the top of each of the first protrusions; The second roller coating mechanism comprises a second rolling shaft and a second liquid storage tank, a plurality of second protrusions are arranged on the surface of the second rolling shaft, and a second sponge sheet is arranged on the top of each second protrusion; The first rolling axis has a radius smaller than that of the second rolling axis.
2. The method for preparing a modified liquid-permeable surface layer according to claim 1, characterized in that: In step S2 and step S4, hot air penetration drying is adopted.
3. The method for preparing a modified liquid-permeable surface layer according to claim 1, characterized in that: The hydrophobic material is composed of the following components in parts by weight: 10-15 parts of diethylene glycol monobutyl ether; 8-12 parts of dimethyl silicone oil; 5-10 parts of distearic acid glyceryl; 0.5-2 parts of glycerol; 0.5-2 parts of distearyl dimethyl ammonium chloride; and 60-70 parts of deionized water.
4. The method for preparing a modified liquid-permeable surface layer according to claim 1, characterized in that: The preparation of the skin care material comprises the following steps: 1) Take 1 part of pullulan, 1 part of carboxymethyl cellulose, 40 parts of aloe vera gel and 200 parts of deionized water; 2) dissolving a formulated amount of pullulan in a formulated amount of deionized water to form a pullulan solution; 3) adding the formulated amount of aloe vera gel and carboxymethyl cellulose to the pullulan solution and stirring to mix evenly to obtain a mixed solution; 4) The pH of the mixed solution is adjusted to 4.5-5.5 using lactic acid to obtain a skin care material.
5. The method for preparing a modified liquid-permeable surface layer according to claim 1, characterized in that: The thickness of the first sponge sheet is smaller than the thickness of the sponge layer.
6. The method for preparing a modified liquid-permeable surface layer according to claim 1, characterized in that: The liquid surface in the first liquid storage tank contacts the sponge layer sleeved on the surface of the second rotating shaft.
7. The method for preparing a modified liquid-permeable surface layer according to claim 1, characterized in that: The liquid surface in the second liquid storage tank contacts the second sponge sheet on the surface of the second protrusion.
Citation Information
Cited By
A non-caking polymer water-absorbing resin, its preparation method and use
CN122685914A