A method for preparing a graphite bipolar plate with high sealing performance

By plasma treatment of activated graphite plates and using a combination of polytetrafluoroethylene and γ-aminopropyltriethoxysilane, combined with negative pressure impregnation and high pressure curing technology, the pore problem of graphite bipolar plates is solved, realizing the effect of pores on the graphite bipolar plates. The high sealing and low cost graphite bipolar plate preparation meets the airtightness and conductivity requirements of fuel cells.

CN118553944BActive Publication Date: 2024-11-08ZHEJIANG HAROG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411025870.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing graphite bipolar plates have pore problems during the preparation process, resulting in a decrease in airtightness. Commonly used resins and other materials have poor weather resistance under harsh environments, which increases processing costs and complexity.

Method used

The surface of activated graphite plates is treated with plasma, and a combination of polytetrafluoroethylene and γ-aminopropyltriethoxysilane is used to achieve microporous surface of graphite bipolar plates through negative pressure impregnation and high pressure curing technology. High sealing of holes.

Benefits of technology

Significantly reduces the airtightness of graphite bipolar plates from 2.560 sccm to 0.001 sccm, improves sealing while maintaining conductivity, simplifying process flow and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118553944B_ABST
    Figure CN118553944B_ABST
Patent Text Reader

Abstract

The present invention relates to a fuel cell preparation technology, and aims to provide a method for preparing a highly sealed graphite bipolar plate. The method comprises: fully mixing a polytetrafluoroethylene concentrated dispersion and γ-aminopropyltriethoxysilane, and obtaining a micropore plugging liquid after standing; immersing the graphite bipolar plate after plasma treatment in the micropore plugging liquid, and performing an immersion treatment under vacuum conditions; washing and drying after taking out, and obtaining a highly sealed graphite bipolar plate with blocked surface micropores through pressurization treatment. In the present invention, the surface of the graphite bipolar plate is treated with plasma to provide a good grafting environment for the subsequent micropore plugging agent; γ-aminopropyltriethoxysilane is used to improve the affinity between polytetrafluoroethylene and the graphite plate; the graphite plate is completely plugged by a method of negative pressure impregnation and high pressure curing, and complete sealing can be achieved by only one impregnation; the method of the present invention is simple to operate, has low equipment requirements, and has low comprehensive costs, and the obtained graphite bipolar plate has a good plugging effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fuel cell preparation technology, and in particular to a preparation method of a highly sealed graphite bipolar plate. Background Art

[0002] As one of the eight core materials of fuel cells, bipolar plates are called the "skeleton" of fuel cells. As a key component of hydrogen fuel cells, bipolar plates have the functions of providing electrical connections, transporting reaction gases, dissipating reaction heat, and removing by-products. Generally speaking, bipolar plates account for more than 80% of the total mass of the stack and about 30% of the total cost, while the volume of the stack is basically occupied by bipolar plates. Improving the efficiency of bipolar plates and reducing costs have become technical directions of concern in the entire hydrogen energy field.

[0003] The bipolar plates used in existing fuel cells mainly include metal, conductive plastic and graphite. Among them, metal bipolar plates have good formability and obvious volume advantages, but their corrosion resistance needs to be further improved, and they do not have the prospect of large-scale application. The contradiction between the conductivity and mechanical strength of conductive plastic bipolar plates is difficult to balance, which limits their application in high-power battery packs.

[0004] In the current proton exchange membrane fuel cells, the widely used bipolar plates are graphite bipolar plates. Graphite bipolar plates are usually prepared by molding graphite powder. This method will cause many microscopic pores on the graphite bipolar plates, resulting in reduced air tightness of the graphite bipolar plates and causing mutual penetration of fuels. Therefore, after being molded into bipolar plates, they need to undergo an impregnation process to improve the performance of the bipolar plates. Through the impregnation process, the graphite bipolar plates can have excellent air tightness, chemical resistance and temperature stability. Now, researchers in the industry are more likely to use phenolic resins, paraffin wax, asphalt, polycarbosilane, etc. to fill the holes in the graphite plates to reduce the porosity and achieve the purpose of sealing the graphite plates. The advantages of these materials are large molecular weight, long molecular chain, and good deformation performance, so they can seal the graphite plates well. However, due to the poor weather resistance of some resins and other materials themselves, they are limited in harsh application environments. In addition, the introduction of materials such as resins makes it time-consuming to machine the flow channel, which also leads to increased processing costs.

[0005] Therefore, it is in line with actual needs to propose a new graphite bipolar plate micropore plugging technology to prepare sealed graphite plates. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a graphite bipolar plate with high sealing performance.

[0007] To solve the technical problem, the solution of the present invention is:

[0008] A method for preparing a high-sealing graphite bipolar plate is provided, comprising the following steps:

[0009] (1) Clean and dry the graphite bipolar plate, move it into a plasma generator for plasma treatment, and keep it ready for use;

[0010] (2) Adding concentrated polytetrafluoroethylene dispersion and γ-aminopropyltriethoxysilane into a container in sequence, stirring and mixing them evenly, and letting them stand for a long time to obtain a micropore plugging liquid with bubbles removed;

[0011] The mass concentration of the polytetrafluoroethylene concentrated dispersion is 20% to 60%, and the mass ratio of γ-aminopropyltriethoxysilane to the polytetrafluoroethylene concentrated dispersion is 1:8 to 20;

[0012] (3) Immersing the graphite bipolar plate in a micropore plugging liquid and performing an immersion treatment under vacuum conditions;

[0013] (4) The graphite plate is taken out, cleaned, dried, and then placed in an autoclave for pressure treatment to obtain a highly sealed graphite bipolar plate with blocked surface micropores.

[0014] As a preferred embodiment of the present invention, the cleaning in step (1) refers to: firstly immersing the graphite bipolar plate in acetone to remove organic matter on the surface; then taking it out and immersing it in deionized water to wash it under ultrasonic conditions to remove dust on the surface.

[0015] As a preferred embodiment of the present invention, the ultrasonic condition refers to controlling the power of the ultrasonic equipment to 1440W and the processing time to 10 to 30 minutes.

[0016] As a preferred embodiment of the present invention, the drying in step (1) refers to moving the cleaned graphite bipolar plate into an oven and controlling the drying temperature to 60 to 150° C. for 3 to 6 hours.

[0017] As a preferred embodiment of the present invention, during the plasma treatment in step (1), the power of the plasma generator is controlled to be 10-15 W, and the treatment time is 5-30 min.

[0018] As a preferred embodiment of the present invention, the polytetrafluoroethylene concentrated dispersion in step (2) has an average particle size of 0.17 to 0.45 μm and a viscosity of (16 to 40) × 10 -3 Pa•s.

[0019] As a preferred embodiment of the present invention, in the step (2), the stirring time during mixing is 10 to 30 minutes.

[0020] As a preferred embodiment of the present invention, the vacuum condition in step (3) refers to placing the container containing the graphite bipolar plate and the micropore plugging liquid in a vacuum impregnation kettle, maintaining the vacuum pressure at -0.1 to 0.3 MPa for 12 to 24 hours.

[0021] As a preferred embodiment of the present invention, the cleaning in step (4) refers to cleaning with deionized water, and the drying refers to natural drying at room temperature for 2 hours.

[0022] As a preferred embodiment of the present invention, the conditions for the pressure treatment in step (4) are: pressure 0.4 to 0.7 MPa, and pressure holding time 3 to 6 h.

[0023] Description of the invention principle:

[0024] In the technical solution of the present invention, the combination of "polytetrafluoroethylene concentrated dispersion liquid + γ-aminopropyltriethoxysilane" is used as a micropore plugging liquid. The γ-aminopropyltriethoxysilane and the polytetrafluoroethylene slurry are stirred evenly to make the amino groups therein combine with the organic groups in the polytetrafluoroethylene. The mixed slurry is then used for impregnation of the graphite plate, so that the ethoxy groups in the γ-aminopropyltriethoxysilane are fully combined with the graphite plate to firmly lock the polytetrafluoroethylene in the pores to achieve sealing.

[0025] Polytetrafluoroethylene has excellent chemical properties due to its high-energy CF bond and its unique helical structure, but its self-lubricating property prevents it from combining with other substrates. The present invention uses γ-aminopropyltriethoxysilane to build a "bridge" between polytetrafluoroethylene and graphite material, thereby connecting the two incompatible parts together to achieve a plugging effect.

[0026] (1) Polytetrafluoroethylene is polymerized from its monomer tetrafluoroethylene, and the molecule presents a helical conformation, that is, the CC skeleton is completely wrapped by the surrounding F atoms. At the same time, because the bond energy of CF is very high and not easy to break, PTFE can resist corrosion from strong acids, strong alkalis, oils, pure oxidants and organic agents. However, due to its own self-lubricating property, polytetrafluoroethylene has a weak bonding force with graphite bipolar plates and cannot seal graphite bipolar plates, which greatly limits the application of polytetrafluoroethylene in graphite bipolar plates.

[0027] To solve this problem, the present invention first uses plasma to treat the surface of the graphite plate, and bombards the surface of the substrate with high-energy plasma to activate the surface of the graphite plate to form a hydrophilic surface, and the surface roughness is further improved. More importantly, after the oxygen plasma surface treatment, the surface morphology of the graphite has changed significantly; and under the oxidation of oxygen plasma, some CC bonds are broken, and various oxygen-containing groups such as C-OH, COC, O=C-OH are introduced, which increases the surface activity. Based on the above treatment, the graphite surface is transformed from non-polar and difficult to stick to a certain polarity, easy to stick and hydrophilic, which is conducive to combining with foreign substances and increasing the bonding and coating performance. Therefore, when the graphite plate is immersed in the micropore plugging liquid, the modified graphite plate is easier to combine with foreign substances. Therefore, the present invention innovatively proposes plasma treatment measures to provide a good grafting environment for the subsequent use of micropore plugging agents.

[0028] (2) A further innovation of the present invention is to introduce γ-aminopropyltriethoxysilane into the micropore plugging agent. The structure of this organic substance contains two different active groups, ethoxy and amino. The ethoxy is an inorganic-philic group that can undergo hydrolysis and generate Si-OH groups, which polymerize with the free radicals generated in the graphite plate; the amino group is a non-hydrolyzable organic group and an organic-philic group that can combine with polytetrafluoroethylene.

[0029] (3) The present invention uses negative pressure impregnation and high pressure curing to allow the components of the micropore plugging agent to evenly enter the internal pores of the graphite bipolar plate, which can reduce the sealing performance of the bipolar plate from the initial 2.560 sccm to 0.001 sccm; this airtightness data is much lower than that of the bipolar plates sold on the market, achieving a high sealing effect.

[0030] Compared with the prior art, the technical effects of the present invention are:

[0031] 1. In the present invention, plasma surface treatment is first used to improve the performance of graphite plates from three aspects: activating the surface of the graphite plate to form a hydrophilic surface, improving the surface roughness of the graphite plate, and generating free radicals for initiating polymerization. Therefore, plasma treatment can provide a good grafting environment for the subsequent micropore plugging agent.

[0032] 2. The main plugging materials used in the present invention are polytetrafluoroethylene and γ-aminopropyltriethoxysilane; after the introduction of γ-aminopropyltriethoxysilane, since its structure mainly contains two groups, one group is inorganic-friendly and can be tightly combined with the graphite bipolar plate, and the other group is organic-friendly and can be tightly combined with polytetrafluoroethylene. The present invention uses γ-aminopropyltriethoxysilane to improve the affinity between polytetrafluoroethylene and the graphite plate, so that the polytetrafluoroethylene, which mainly plays a plugging role, is firmly combined with the substrate, thereby achieving high sealing plugging of the micropores on the surface of the graphite bipolar plate.

[0033] 3. In the present invention, the graphite plate is completely sealed by negative pressure impregnation and high pressure curing. The slurry is evenly pressed into the graphite plate by negative pressure. In the process of drying and curing, the slurry is prevented from overflowing due to incomplete drying. Therefore, high pressure curing is adopted. This process combined with the sealant enables the bipolar plate to be completely sealed with only one impregnation.

[0034] 4. The main plugging material used in the present invention is polytetrafluoroethylene, which has many excellent properties, such as excellent heat resistance and cold resistance, and can be used for a long time at -180 to 260°C. This material is resistant to acids, alkalis, and various organic solvents, and is almost insoluble in all solvents. The graphite bipolar plate prepared by the sealant can fully meet the use environment of the bipolar plate.

[0035] 5. The method of the present invention is simple to operate, has low equipment requirements, low comprehensive cost, and the obtained graphite bipolar plate has good plugging effect. The prepared graphite bipolar plate will not increase the machining cost and will not have any impact on the performance of the bipolar plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The present invention is a flow chart for preparing the sealant and applying it to graphite plates.

[0037] Figure 2 This is a scanning electron microscope image of the graphite plate before sealing in Example 1 of the present invention.

[0038] Figure 3 This is a scanning electron microscope image of the sealed graphite plate in Example 1 of the present invention. DETAILED DESCRIPTION

[0039] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings.

[0040] Part I Implementation of the Invention

[0041] The method for preparing the high-sealing graphite bipolar plate of the present invention comprises the following steps:

[0042] (1) Clean and dry the graphite bipolar plate, move it into a plasma generator for plasma treatment, and keep it ready for use;

[0043] Wherein, the cleaning means: first soaking the graphite bipolar plate in acetone to remove the organic matter on the surface; taking it out and immersing it in deionized water, washing it under ultrasonic conditions to remove the surface dust. The ultrasonic conditions mean that the power of the ultrasonic equipment is controlled to be 1440W, and the treatment time is 10 to 30min. The drying means that the cleaned graphite bipolar plate is moved to an oven, and the drying temperature is controlled to be 60 to 150℃, and the time is 3 to 6h. During plasma treatment, the power of the plasma generator is controlled to be 10 to 15W, and the treatment time is 5 to 30min.

[0044] (2) Adding concentrated polytetrafluoroethylene dispersion and γ-aminopropyltriethoxysilane into a container in sequence, stirring and mixing them evenly, and letting them stand for a long time to obtain a micropore plugging liquid with bubbles removed;

[0045] The mass concentration of the polytetrafluoroethylene concentrated dispersion is 20% to 60%, the mass ratio of γ-aminopropyltriethoxysilane to the polytetrafluoroethylene concentrated dispersion is 1:8 to 20; the average particle size of the polytetrafluoroethylene concentrated dispersion is 0.17 to 0.45 μm, and the viscosity is (16 to 40)×10 -3 Pa•s. The stirring time during mixing is 10 ~ 30min.

[0046] (3) Immersing the graphite bipolar plate in a micropore plugging liquid and performing an immersion treatment under vacuum conditions;

[0047] The vacuum condition refers to placing the container containing the graphite bipolar plate and the micropore plugging liquid in a vacuum impregnation kettle, maintaining the vacuum pressure at -0.1 to 0.3 MPa, and maintaining the pressure for 12 to 24 hours.

[0048] (4) The graphite plate is taken out, cleaned, dried, and then placed in an autoclave for pressure treatment to obtain a highly sealed graphite bipolar plate with blocked surface micropores.

[0049] The cleaning refers to cleaning with deionized water, and the drying refers to natural drying at room temperature for 2 hours; the conditions for the pressure treatment are: pressure 0.4 ~ 0.7 Mpa, and pressure holding time 3 ~ 6 hours.

[0050] The polytetrafluoroethylene aqueous dispersion and γ-aminopropyltriethoxysilane described in the present invention can be commercially available products.

[0051] Part II Specific Examples and Comparative Examples

[0052] Embodiment 1:

[0053] (1) Clean and dry the graphite bipolar plate:

[0054] First, the graphite bipolar plate was soaked in acetone to remove the organic matter on the surface; then, it was taken out and immersed in deionized water, and washed for 10 min under ultrasonic conditions with a power of 1440 W to remove the surface dust; then, the cleaned graphite bipolar plate was moved to an oven, and the drying temperature was controlled at 60°C for 6 hours.

[0055] (2) The dried graphite plate was subjected to plasma treatment for 5 min, and the power of the plasma generator was controlled to 15 W.

[0056] (3) Add a 20% mass concentration, an average particle size of 0.17 μm, and a viscosity of 16×10 -3 100 g of Pa•s polytetrafluoroethylene concentrated dispersion was stirred evenly; then 5 g of γ-aminopropyltriethoxysilane was added and stirred for 10 min to make it evenly mixed. After standing still, the micropore plugging liquid with bubbles removed was obtained.

[0057] (4) The pretreated graphite bipolar plate is immersed in a micropore plugging liquid, and then the container in which the graphite bipolar plate is immersed is placed in a vacuum impregnation kettle for impregnation treatment, maintaining the vacuum pressure at -0.1 MPa for 12 h.

[0058] (5) Take out the impregnated graphite plate, wash it with deionized water, and dry it naturally at room temperature for 2 hours. Then place it in a pressure autoclave for pressure treatment, control the pressure in the autoclave to 0.4 MPa, and keep the pressure for 6 hours. Finally, a highly sealed graphite bipolar plate with blocked surface micropores is obtained.

[0059] Embodiment 2:

[0060] (1) Clean and dry the graphite bipolar plate:

[0061] First, the graphite bipolar plate was soaked in acetone to remove the organic matter on the surface; then, it was taken out and immersed in deionized water, and washed under ultrasonic conditions with a power of 1440W for 20 minutes to remove the surface dust; then, the cleaned graphite bipolar plate was moved to an oven, and the drying temperature was controlled to 80℃ for 4 hours.

[0062] (2) The dried graphite plate was subjected to plasma treatment for 15 min, and the power of the plasma generator was controlled to 12 W.

[0063] (3) Add a 40% mass concentration, an average particle size of 0.25 μm, and a viscosity of 27×10 -3 100 g of Pa•s polytetrafluoroethylene concentrated dispersion was stirred evenly; then 10 g of γ-aminopropyltriethoxysilane was added and stirred for 20 minutes to make it evenly mixed. After standing still, the micropore plugging liquid with bubbles removed was obtained.

[0064] (4) The pretreated graphite bipolar plate is immersed in a micropore plugging liquid, and then the container in which the graphite bipolar plate is immersed is placed in a vacuum impregnation kettle for impregnation treatment, maintaining the vacuum pressure at 0.1 MPa for 18 h.

[0065] (5) Take out the impregnated graphite plate, wash it with deionized water, and dry it naturally at room temperature for 2 hours. Then place it in a pressure autoclave for pressure treatment, control the pressure in the autoclave to 0.6 MPa, and keep the pressure for 4 hours. Finally, a highly sealed graphite bipolar plate with blocked surface micropores is obtained.

[0066] Embodiment 3:

[0067] (1) Clean and dry the graphite bipolar plate:

[0068] First, the graphite bipolar plate was soaked in acetone to remove organic matter on the surface; then, it was taken out and immersed in deionized water, and washed for 30 minutes under ultrasonic conditions with a power of 1440W to remove surface dust; then, the cleaned graphite bipolar plate was moved to an oven, and the drying temperature was controlled at 150°C for 3 hours.

[0069] (2) The dried graphite plate was subjected to plasma treatment for 30 min, and the power of the plasma generator was controlled to 10 W.

[0070] (3) Add a 60% mass concentration, an average particle size of 0.45 μm, and a viscosity of 40×10 -3 100 g of Pa•s polytetrafluoroethylene concentrated dispersion was stirred evenly; then 12.5 g of γ-aminopropyltriethoxysilane was added and stirred for 30 min to mix evenly. After standing still, the micropore plugging liquid with bubbles removed was obtained.

[0071] (4) The pretreated graphite bipolar plate is immersed in a micropore plugging liquid, and then the container in which the graphite bipolar plate is immersed is placed in a vacuum impregnation kettle for impregnation treatment, maintaining the vacuum pressure at 0.3 MPa for 24 h.

[0072] (5) Take out the impregnated graphite plate, wash it with deionized water, and dry it naturally at room temperature for 2 hours. Then place it in a pressure autoclave for pressure treatment, control the pressure in the autoclave to 0.7 MPa, and maintain the pressure for 3 hours. Finally, a highly sealed graphite bipolar plate with blocked surface micropores is obtained.

[0073] Comparative Example 1

[0074] Referring to the technical solution disclosed in the patent document "A modified phenolic resin / graphite-based conductive composite material and its preparation process" (CN 1927936A), the surface of the graphite bipolar plate is sealed by using modified solid phenolic resin.

[0075] Comparative Example 2

[0076] Referring to the technical solution disclosed in the journal document “Liquid resin for preparing graphite bipolar plate and graphite bipolar plate” (CN 110204669), phenolic liquid resin is used to perform surface plugging treatment on the graphite bipolar plate.

[0077] Part III Product Testing and Result Analysis

[0078] With reference to the provisions of GB / T 20042.6-2011 standard, the air permeability (air tightness) test was performed on the graphite bipolar plates in each embodiment and comparative example using a monopolar plate air tightness test platform.

[0079] Referring to the record of the patent "A graphite plate manufacturing process", the conductivity of the graphite bipolar plates in each embodiment and comparative example was tested using a four-probe low-resistance measuring instrument.

[0080] The resistivity of the graphite bipolar plates in each embodiment and comparative example was tested using a four-probe low-resistance measuring instrument method with reference to the document “Preparation and Performance of Phenolic Resin / Graphite Compression Molded Composite Bipolar Plates”.

[0081] 1. The graphite bipolar plates in the three embodiments were tested before and after micropore plugging. The test results are shown in Table 1.

[0082] Table 1 Comparison of air tightness before and after plugging

[0083] Unsealed graphite plate Embodiment 1 Embodiment 2 Embodiment 3 Air permeability sccm 2.560 0.037 0.017 0.001 Conductivity KS / mm 0.10 0.10 0.10 0.10 Resistivity mΩ.mm 9.22 9.87 9.45 9.27

[0084] As can be seen from the table, the air tightness drops from 2.560 sccm to below 0.05 sccm. Therefore, the preparation method of the present invention is used to block the micropores of the graphite bipolar plate, which can not only achieve the blocking of the graphite bipolar plate, but also does not reduce its conductivity, and can meet the requirements of the fuel cell production and assembly process for the air tightness and conductivity of the bipolar plate.

[0085] contrast Figure 2 , 3 It can be seen from the surface microscopic images before and after the sealing treatment that the surface of the graphite bipolar plate treated by the present invention is smooth and the original microporous structure is basically non-existent, which can also confirm the results of the above airtightness experiment.

[0086] 2. The graphite bipolar plates in each comparative example were tested respectively, and the test results are shown in Table 2.

[0087] Table 2 Data comparison between the examples of the present invention and the comparative examples

[0088] Comparative Example 1 Comparative Example 2 Embodiment 1 Embodiment 2 Embodiment 3 Air permeability sccm 1kg negative pressure, airtight 1kg negative pressure, airtight 0.037 0.017 0.001 Conductivity KS / mm 0.016 0.012 0.10 0.10 0.10 Resistivity mΩ.mm 62.5 83.3 9.87 9.45 9.27

[0089] It can be seen from the table that, whether it is sealed by liquid resin or solid resin, the air tightness is good, but the conductivity is at a low level. Bipolar plate products treated by the prior art are prone to fuel leakage after being assembled and applied in fuel cells due to the poor weather resistance of the resin. Therefore, the preparation method of the present invention is used to seal the micropores of the graphite bipolar plate. Compared with the products after various types of sealing in the prior art, it can simultaneously meet the requirements of achieving complete sealing and meeting the conductivity requirements.

Claims

1. A method for preparing a highly sealed graphite bipolar plate, characterized in that: The following steps are involved: (1) Clean and dry the graphite bipolar plate, move it into a plasma generator for plasma treatment, and keep it ready for use; During plasma treatment, the power of the plasma generator is controlled to be 10~15W, and the treatment time is 5~30min; (2) Adding concentrated polytetrafluoroethylene dispersion and γ-aminopropyltriethoxysilane into a container in sequence, stirring and mixing them evenly, and letting them stand for a long time to obtain a micropore plugging liquid with bubbles removed; The mass concentration of the polytetrafluoroethylene concentrated dispersion is 20% to 60%, and the mass ratio of γ-aminopropyltriethoxysilane to the polytetrafluoroethylene concentrated dispersion is 1:8 to 20; (3) Immersing the graphite bipolar plate in a micropore plugging liquid and performing an immersion treatment under vacuum conditions; The vacuum condition refers to placing the container containing the graphite bipolar plate and the micropore plugging liquid in a vacuum impregnation kettle, maintaining the vacuum pressure at -0.1 to 0.3 MPa for 12 to 24 hours; (4) taking out the graphite plate, cleaning and drying it, and then placing it in an autoclave for pressure treatment to obtain a highly sealed graphite bipolar plate with blocked surface micropores; The conditions of the pressure treatment are: pressure 0.4 ~ 0.7 Mpa, and pressure holding time 3 ~ 6 h.

2. The method according to claim 1, characterized in that: The cleaning in step (1) refers to: firstly immersing the graphite bipolar plate in acetone to remove organic matter on the surface; then taking it out and immersing it in deionized water to wash it under ultrasonic conditions to remove dust on the surface.

3. The method according to claim 2, characterized in that The ultrasonic conditions refer to controlling the power of the ultrasonic equipment to 1440W and the processing time to 10 to 30 minutes.

4. The method according to claim 1, characterized in that: The drying in step (1) refers to moving the cleaned graphite bipolar plate into an oven and controlling the drying temperature to 60 to 150° C. for 3 to 6 hours.

5. The method according to claim 1, characterized in that The polytetrafluoroethylene concentrated dispersion in step (2) has an average particle size of 0.17 to 0.45 μm and a viscosity of (16 to 40) × 10 -3 Pa•s.

6. The method according to claim 1, characterized in that In the step (2), the stirring time during mixing is 10 to 30 minutes.