Regeneration and volume correction technology of false particles of used carbon-containing magnesium refractory materials
Through micro-spiral low-temperature nitrogen-oxygen suspension roasting, low-temperature ethanol cold-punching and high-efficiency milling technology, the problems of low removal rate and high energy consumption in carbon-magnesium-containing refractory materials after use are solved, and efficient graphite component retention is achieved The morphology of the magnesium sand particles is restored, which improves the recycling value of the material and the performance of recycled bricks.
Patent Information
- Application Number
- CN202410745252.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-11
AI Technical Summary
In the prior art, when the carbon-magnesium-containing refractory material is used for treatment, the removal rate of fake particles is low, the energy consumption is high, and the utilization value of graphite components is not high, which affects the recycling value of the material.
Using micro-spiral low-temperature nitrogen-oxygen suspension roasting, low-temperature ethanol cold-punching and high-efficiency milling technology, through selective oxidation roasting and mechanical milling, the bonded carbon layer on the surface of fake particles is quickly oxidized, the graphite components are retained, and the magnesium sand particles are improved. the true form and recycled value.
It significantly improves the false particle elimination rate and treatment efficiency, reduces energy consumption, retains graphite components, improves the recycling value of the material and the performance indicators of recycled bricks.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_7
Abstract
Description
Technical Field
[0001] The invention relates to a pseudo-particle volume correction process for regenerating used carbon-containing magnesium refractory materials, belonging to the technical field of recycled material processing for recycling refractory solid waste. Background Art
[0002] In recent years, more and more domestic magnesium refractory companies are gradually increasing their research efforts on the recycling and treatment technology of used carbon-containing magnesium refractory materials. However, under the binding effect of the residual carbon (bound carbon layer) of the resin, after the used carbon-containing magnesium refractory materials are crushed and screened, the surface of the magnesium sand particles is evenly coated with a layer of graphite carbon layer, forming the so-called pseudo-particle morphology.
[0003] Since the magnesium-carbon pseudo-particles have been used at high temperatures, the residual carbon after the resin is cured is in a glassy state, showing obvious brittleness. The surface coating is loose and porous honeycomb and relatively poorly combined with the magnesium oxide particles. If it is not treated and directly produced into recycled bricks, it will seriously affect the key performance indicators of the new product, such as volume density, apparent porosity, medium and high temperature strength, and corrosion resistance. It is precisely because of the existence of pseudo-particles that the proportion of carbon-containing magnesium recycled materials used in the production of new refractory materials in the industry is currently less than 60%.
[0004] In order to reduce the negative effects of fake particles, the industry mostly uses the following two technologies to deal with the above problems:
[0005] The first is to use a mud mill for rolling. After the used carbon-containing magnesium refractory materials are crushed, they are all put into the mud mill for rolling. With the help of mechanical force, the adhesion layer on the surface of the particles is crushed and separated from the particles. Although this technology can reduce some false particles, there are still many technical problems: first, the removal rate of false particles is low. According to actual surveys, the removal rate is estimated to be about 30%, and nearly 70% of false particles still exist; second, due to the need for long-term cyclic rolling, some of the better real particles are damaged due to rolling; third, the work efficiency is low.
[0006] The second is to use the oxidation-reduction magnesia technology. After the used carbon-containing magnesia refractory material is crushed, it is put into the furnace for high-temperature oxidation roasting. The roasting temperature is generally set at above 800°C. With the help of oxidation reaction, the carbon layer and graphite carbon layer on the surface of the pseudo-particles are completely burned out, thereby obtaining reduced magnesia. This technology has the following problems: First, the oxidation reaction completely oxidizes the graphite components in the attachment layer, loses the beneficial components, and reduces the utilization value of the recycled material; second, the roasting temperature is high, the energy consumption is large, and the cost of recycling and regenerating the used carbon-containing magnesia refractory material is high. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a pseudo-particle volume correction process for regenerating used carbon-containing magnesium refractory materials. This process not only approaches the real morphology of magnesium oxide particles to the greatest extent and completes the volume correction optimization of the pseudo-particle surface structure, but also can 100% retain high-value graphite components, thereby greatly improving the intrinsic value of the recycling of used carbon-containing magnesium refractory materials.
[0008] To solve the above problems, the specific technical scheme of the present invention is as follows: A process for regenerating pseudo particles and correcting the volume of carbon-containing magnesium refractory materials, comprising the following steps:
[0009] Step 1-Preparation of carbon-containing magnesium regenerated granular material: The recovered, purified and selected used carbon-containing magnesium refractory material is treated by conventional process, and then crushed to prepare 5-0 mm carbon-containing magnesium regenerated granular material;
[0010] Step 2-primary screening: The carbon-containing magnesium recycled granular material obtained in step 1 is screened for the first time, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, and the 5-0.5 mm part is called the first aggregate to be corrected;
[0011] Step 3 - Micro-spiral low-temperature nitrogen-oxygen suspension tumbling roasting: The first aggregate to be corrected in step 2 is fed into the inlet of the micro-spiral suspension roasting furnace, and fully fused with the compressed nitrogen-oxygen mixed gas with a temperature of 350°C to 380°C after preheating to form a gas-material suspension. The carbon layer of the first aggregate to be corrected is rapidly selectively preferentially oxidized with oxygen to disintegrate and disperse, and runs to the tail section of the furnace. The gas-material separation is achieved under the conditions of obstruction and filtration of a 325-mesh vibrating screen. The gas is sucked into the negative pressure outlet and collected after dust removal, and the material separated by the vibrating screen is discharged from the outlet to obtain the primary corrected material;
[0012] Step 4-Secondary Screening: The primary aggregate obtained in step 3 is screened again to screen out two parts, 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, and the 5-0.5 mm part is called the secondary aggregate to be screened;
[0013] Step 5-Rapid low-temperature ethanol cold shock treatment: put the secondary aggregate to be corrected into the mixer, then turn on the mixer switch, start the auxiliary heating device at the bottom of the mixer, the temperature is 80-100°C, and quickly inject low-temperature ethanol into the mixer in a spraying state, so that the secondary aggregate to be corrected is subjected to a negative temperature difference of -(200±5°C), and stir at this speed for 10-15 minutes to fully blend the secondary aggregate to be corrected with the low-temperature ethanol; after the stirring is completed, keep it in a static state for 10-15 minutes and then discharge it to obtain the cold shock material;
[0014] Step 6 - tertiary screening: The cold-shocked material obtained in step 5 is sent to the screening system to screen out two parts, 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called the tertiary aggregate to be corrected;
[0015] Step 7-High-efficiency grinding treatment: The tertiary aggregates screened in step 6 are sent to the grinding machine for high-efficiency grinding treatment for 20 to 30 minutes. The surface of the tertiary aggregates undergoes mechanical grinding and grinding, which causes the remaining coating layer to be crushed and deeply removed, achieving the ultimate correction and restoration. After the grinding treatment is completed, the ground material is obtained;
[0016] Step 8 - Four-time screening: Send the milled material obtained in step 7 to the screening system, screen out two parts, 5-0.5 mm and 0.5-0 mm, of which the 0.5-0 mm part directly enters the finished product regenerated fine particle silo for standby use; the 5-0.5 mm part is called the regenerated and reduced particle material, which is very close to the original magnesia particle morphology and will enter the regenerated and reduced particle material silo for standby use.
[0017] The conventional process treatment in step 1 includes any one of the processes of hydration, non-hydration or regeneration of waste refractory materials.
[0018] In the step 3, the micro-spiral suspension roasting furnace is horizontally distributed and is divided into three sections: a furnace head, a furnace body and a furnace tail; the optimal diameter of the furnace is 200-300 mm and the length is 10-12 m; the spiral diameter is 420-500 mm and the pitch is 1000-1500 mm; the air inlet is arranged on the end face of the furnace head, the feed port is arranged directly above the furnace head, and the center lines of the two intersect vertically, the ratio of the diameter of the air inlet to the feed port is (1-1.5): 1, and the diameter of the feed port is 50-100 mm; the diameter of the negative pressure air outlet is 100-150 mm, one end of which is arranged on the end face of the furnace tail section, and the other end is installed with a negative pressure fan, and the static pressure of the negative pressure fan is 1200-2000 Pa; the 325 mesh vibrating screen is arranged on a cross section 400-500 mm away from the end face of the furnace tail, and the screen area should account for more than 80% of the cross section; the diameter of the discharge port is 200-250 mm.
[0019] In step 3, the pressure of the compressed nitrogen-oxygen mixed gas is 1.2-1.5 MPa, and the optimal volume ratio of nitrogen and oxygen in the mixed gas is (15%-20%): (80%-85%).
[0020] In step 5, the mixer speed is set to 70-80 r / min, the effective working capacity is not less than 1000 L, and the heating method is water bath or electric heating.
[0021] In step 5, the weight ratio of low-temperature ethanol to secondary aggregate to be corrected should be 1: (8-12).
[0022] In step 7, the mill is a three-wheel variable speed mill, which consists of a variable frequency motor, a vertical spindle, an iron bowl-shaped grinding disc and three wide millstones, and each millstone is connected to the vertical spindle by a horizontal axis, and the vertical spindle is driven by the variable frequency motor to rotate at a variable speed around the center line of the grinding disc, thereby driving the millstone to rotate at a variable speed around the spindle; during the rotation process, since the distances of various points on the width direction of the millstone from the rotation center line are different, the linear speeds are also different; the wide millstone is a circular stone wheel with a diameter of 500-600mm, an effective width of 300-350mm, and a weight of 250-350kg. A layer of SiC abrasive particles with a thickness of about 20mm is solidified on the tread of the millstone, wherein the SiC particle size is 60-80 mesh; the gap between the wide millstone and the grinding disc is 15-20mm.
[0023] Compared with the common processes traditionally used to deal with the false particle effect, the particle correction process of this application has the following significant advantages:
[0024] 1. The processing efficiency is greatly improved: Since the volume correction technology provided by the present invention is always aimed at particles with a particle size greater than 0.5 mm, it effectively eliminates the interference effects of fine powder packaging and fine powder cushioning. In addition, the present application also uses low-temperature chemical roasting method (micro-spiral low-temperature nitrogen and oxygen suspension furnace roasting treatment), physical method (low-temperature ethanol cold shock treatment), and mechanical method (selective particle efficient grinding) to work together, so that the combined carbon layer of the false particles is quickly oxidized and removed, and the coating layer is quickly broken, and the true appearance of the particles is efficiently restored. According to calculations, the present invention improves efficiency by nearly 50% compared with traditional treatment processes, and the elimination rate of false particles is as high as nearly 100%.
[0025] 2. The energy consumption of the treatment process is greatly reduced: Due to the capacity correction method provided by this application, only low-temperature oxidation roasting at 350℃ to 380℃ is required, which not only has a low temperature but also a short treatment time. Compared with the traditional pure redox magnesia technology using more than 800℃, it can greatly save energy consumption. Summarizing the energy consumption of the entire capacity correction process, the comprehensive energy consumption is reduced by 45% to 60% compared with the traditional pure redox magnesia process.
[0026] 3. Greatly improve the recycling value of used carbon-containing magnesium refractory materials: Due to the use of selective low-temperature oxidation roasting treatment process, oxidation and burning only act on the bonding carbon layer, while the graphite carbon layer in the regenerated particles is well preserved. When using it to produce regenerated refractory materials, the amount of flake graphite added can be reduced, the production cost is reduced, and the recycling value of used carbon-containing magnesium refractory materials is improved.
[0027] 4. The morphological integrity of the recycled magnesium oxide particles is well guaranteed. The traditional process of eliminating false particles uses a mud mill rolling technology for rolling the entire material. Under the influence of the coating and shock-absorbing efficiency of the fine powder, the rolling effect is poor. However, in order to further reduce the proportion of false particles, a large millstone and a long-term cycle rolling method are often used. This will cause some of the better true particles to be severely damaged due to rolling, thereby affecting the quality of the recycled material. The present invention utilizes selective and efficient grinding technology, and at the same time uses low-temperature oxidation and low-temperature ethanol cold shock technology to weaken the bonded carbon layer by burning, thermal shock and other treatments before grinding, so that the magnesium oxide particles and the coating layer can be quickly separated during mechanical grinding, which well protects the integrity of the true particles. DETAILED DESCRIPTION
[0028] A method for regenerating false particles and correcting the volume of used carbon-containing magnesia refractory materials comprises the following steps:
[0029] Step 1 - Preparation of carbon-containing magnesium regenerated granular material: The recovered, purified and sorted used carbon-containing magnesium refractory material is treated by conventional process, and then crushed and screened to prepare 5-0 mm carbon-containing magnesium regenerated granular material.
[0030] Furthermore, the conventional process treatment described in this step is any one of the processes for hydration, hydration-free or other regeneration treatment of other mature waste refractory materials after use.
[0031] Step 2 - primary screening: the carbon-containing magnesium recycled granular material obtained in step 1 is screened for the first time, and two parts of 5-0.5 mm and 0.5-0 mm are screened out, of which the 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, and the 5-0.5 mm part is called the first aggregate to be corrected and will enter step 3.
[0032] Furthermore, the present invention uses 0.5 mm as the critical particle size to screen the carbon-containing magnesium recycled granular material into two parts to achieve selective particle correction. This is because the inventors found through experiments that the false particle phenomenon mainly occurs in aggregates with a particle size of >0.5 mm, while the part with a particle size of ≤0.5 mm is not obvious, which can be supported by the data in Table 1. As can be seen from Table 1, with the continuous increase in the proportion of 0.5-0 mm recycled granular material added, the key properties of the recycled magnesium carbon bricks prepared therefrom, such as the volume density and high-temperature flexural strength, are comparable to those of the new magnesium carbon bricks prepared from the same grade of fused magnesia sand, and will not significantly reduce the quality of the recycled magnesium carbon bricks.
[0033] Table 1 Performance comparison between recycled magnesia carbon bricks prepared by adding different proportions of recycled particles (≤0.5 mm) and new magnesia carbon bricks
[0034]
[0035] Step 3-micro-spiral low-temperature nitrogen-oxygen suspension tumbling roasting: The first aggregate to be corrected screened out in step 2 is conveyed to the feed port of the micro-spiral suspension roasting furnace via a belt conveyor. After the air inlet valve is opened, the compressed nitrogen-oxygen mixed gas with a temperature of 350°C to 380°C after preheating enters the furnace of the roasting furnace from the air inlet, and then the feed port valve is quickly opened. At this time, under the strong push of the high-pressure mixed airflow, the first aggregate to be corrected and the argon-oxygen mixed gas are quickly and fully fused to form a gas suspension. Because the bound carbon is an amorphous carbon and the oxidation start temperature is low, the bound carbon layer in the first aggregate to be corrected quickly undergoes selective preferential oxidation with oxygen and disintegrates and disperses (while the graphite carbon layer has a high oxidation start temperature and has not yet oxidized). In addition, due to the unique spiral furnace design of the roasting furnace, the gas suspension always maintains a fluctuating and tumbling flow state during the process of running from the furnace head to the furnace tail, which can effectively accelerate the oxidation and decarbonization of the bound carbon layer in the first aggregate to be corrected and the disintegration and dispersion of its binding structure. When the gas-material suspension runs to the tail section of the furnace, gas-material separation is achieved under the conditions of obstruction and filtration by the 325-mesh vibrating screen. The gas is sucked into the negative pressure air outlet and collected after dust removal. The material blocked and separated by the vibrating screen is called primary material. The primary material falls through the discharge port to the belt conveyor and is transported by the belt to step 4.
[0036] Furthermore, the micro-spiral suspension roasting furnace is horizontally distributed and is divided into three sections: the furnace head, the furnace body and the furnace tail. In order to minimize the temperature drop of the nitrogen-oxygen mixed gas to ensure a better oxidation roasting effect, the optimal diameter of the furnace is designed to be 200-300mm and the optimal length is 10-12m; in order to obtain the best fluctuation and tumbling effect of the gas-material suspension and minimize the kinetic energy loss of the suspension, the spiral diameter is required to be 420-500mm and the pitch is 1000-1500mm to form a micro-spiral effect; the air inlet is set on the end face of the furnace head, and the feed port is set directly above the furnace head, and the center lines of the two intersect vertically. In order to obtain the best gas-material mixture, the optimal diameter ratio of the air inlet to the feed port is (1-1.5):1. In order to further reduce the processing energy efficiency, the optimal diameter of the feed port is 50-100mm.
[0037] Table 2 Loss on ignition of phenolic resin residues treated with 1700℃ reduction at 380℃×5min in different nitrogen and oxygen atmospheres
[0038]
[0039] Furthermore, the pressure of the compressed nitrogen-oxygen mixed gas is 1.2-1.5 MPa, and it needs to be fully preheated, and its temperature should reach 350°C-380°C after preheating. In order to control the gas suspension to better complete the selective oxidation decarbonization at a temperature of 350°C-380°C, the optimal volume ratio of nitrogen and oxygen in the mixed gas is (15%-20%): (80%-85%). This is because the density of nitrogen is smaller than that of O2 and CO2. With the help of the wave tumbling effect described above, its addition can greatly reduce the atmosphere pressure of the reaction products at the carbon-oxygen interface (i.e., the partial pressure of CO2), thereby accelerating the selective oxidation process of the carbon bound to the surface of the pseudo-particles from a kinetic point of view. However, if the proportion of nitrogen is too high, the oxidation reaction of the pseudo-particles combined with the carbon layer will be slowed down due to the reduction of the oxidizing atmosphere in the furnace, which can be effectively verified from the data in Table 2. The data in Table 2 are obtained by treating the phenolic resin (commonly used binder for carbon-containing magnesium refractory materials) under a reducing atmosphere at 1700°C to obtain a residue, and then quickly placing the residue in a calcining furnace under different nitrogen and oxygen mixed atmospheres for 380°C×5min treatment, and then testing the oxidation loss rate obtained. As can be seen from Table 2, when the volume ratio of nitrogen in the mixed gas is greater than 20%, the oxidation loss rate of the residue after burning the phenolic resin is greatly reduced. It is not difficult to predict that in this mixed atmosphere, the selective oxidation reaction of the carbon-containing magnesium pseudo-particles combined with the carbon layer will be greatly slowed down. In addition, when the volume ratio of nitrogen is less than 15%, although the oxidation reaction process can be accelerated, the micro-spiral suspension calcining furnace and its supporting equipment are required to be relatively high, which will increase the process complexity and comprehensive cost of the implementation of the present application scheme, which is very unfavorable for industrial promotion. Therefore, the present invention requires that the optimal volume ratio of nitrogen in the mixed gas is 15% to 20%.
[0040] Furthermore, the diameter of the negative pressure air outlet is 100-150mm, one end of which is arranged on the end face of the furnace tail section, and a negative pressure fan is installed on the other end. The static pressure of the negative pressure fan is 1200-2000Pa. A negative pressure state is formed by the negative pressure fan to suck the gas in the furnace tail area to the air outlet; the 325-mesh vibrating screen has a sieve hole size of 0.045mm, which is arranged on a cross section 400-500mm away from the furnace tail end face, and the screen area should account for more than 80% of the cross section; the optimal diameter of the discharge port is 200-250mm, and the discharge port should be arranged directly below the front end of the vibrating screen, and the distance from the screen surface should be less than 80mm to ensure that the initial material quickly enters the discharge port without being obstructed by the screen and falls into the belt conveyor.
[0041] Step 4 - Secondary screening: The primary aggregate obtained in step 3 is sent to the screening system again through the conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part also directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called secondary aggregate to be corrected and will enter step 5.
[0042] Step 5-Rapid low-temperature ethanol cold shock treatment: The secondary aggregate to be corrected screened out in step 4 is quickly put into the mixer through the conveyor belt, then the mixer switch is turned on, the speed is set to 70-80 r / min, and low-temperature ethanol is quickly injected into the mixer in a spraying state, and stirred at this speed for 10-15 minutes to fully blend the secondary aggregate to be corrected with the low-temperature ethanol. After the stirring is completed, the switch is turned off, and the static state is maintained for another 10-15 minutes. Under the continuous action of the auxiliary heating device at the bottom of the mixer, the internal temperature of the mixer is always controlled at 80-100°C to ensure that the ethanol can be completely evaporated after the cold shock effect is completed. After the static state is completed, all the materials that have been cold-shocked are discharged through the discharge port to obtain cold-shocked materials, which will enter step 6.
[0043] It should be noted that the purpose of this step is to make full use of the significant feature of the combined carbon layer of the secondary aggregate to be corrected, which is in a relatively brittle glassy state, and to use the large negative temperature difference brought about by low-temperature ethanol to form a cold shock effect, so that cracks or separations quickly occur at the interface between the combined carbon and the magnesium oxide particles, laying a solid foundation for the next step of achieving efficient grinding, thereby further improving the pseudo-particle correction effect.
[0044] Furthermore, the mixer is a sand mixer with dual functions of electric-driven forced stirring and bottom auxiliary heating, with an effective working capacity of not less than 1000L and a minimum rotation speed of ≥30r / min. The bottom auxiliary heating can be passively heated by high-temperature fluid heat exchange, such as a water bath, or can be actively heated by electric heating, so as to achieve the purpose of maintaining the temperature of the mixer at 80-100°C.
[0045] Furthermore, the low-temperature ethanol is industrial ethanol with a purity of more than 95% after refrigeration. In order to obtain the best cold shock effect and process operability, the inventors found through experiments that the best negative temperature difference that the secondary aggregate to be corrected needs to withstand is -(200±5°C). The secondary aggregate to be corrected absorbs heat during the roasting in step 3, and the residual temperature is still 140-150°C in this step. Therefore, the temperature of the low-temperature ethanol in the present invention is required to be within the range of -60 to -50°C. Further, considering the cold shock effect and the subsequent efficient volatilization and removal, the weight ratio of the low-temperature ethanol to the secondary aggregate to be corrected should be 1: (8-12).
[0046] Step 6 - tertiary screening: The cold-shocked material obtained in step 5 is sent to the screening system through a conveyor belt, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part also directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called the tertiary aggregate to be corrected and will enter step 7.
[0047] Step 7-High-efficiency grinding treatment: The tertiary aggregates screened in step 6 are conveyed to a three-wheel variable-speed mill through a belt for high-efficiency grinding treatment for 20 to 30 minutes. The relative movement between the millstone and the mill plate produces a mechanical action of crushing and grinding the surface of the tertiary aggregates to be corrected, causing the remaining coating layer to be crushed and deeply removed, achieving the ultimate correction and restoration. After the grinding treatment is completed, the milled material is obtained, and the milled material enters the conveyor belt through the mill outlet and is conveyed to step 8 through the belt.
[0048] Furthermore, the mill is composed of a variable frequency motor, a vertical spindle, an iron bowl-shaped milling disc and three wide milling wheels, and each milling wheel is connected to the vertical spindle by a horizontal axis. The vertical spindle is driven by the variable frequency motor to rotate at a variable speed around the center line of the milling disc, thereby driving the milling wheel to rotate at a variable speed around the spindle. During the rotation process, since the distances of each point in the width direction of the milling wheel from the rotation center line are different, the linear speed is also different, so on the contact surface between the milling wheel and the milling disc, a large sliding friction will occur in the radial direction, thereby forming a friction and rolling effect on the tertiary aggregate to be corrected located on this contact surface. Further, the wide milling wheel is a circular stone wheel with a diameter of 500 to 600 mm. In order to maximize the contact surface with the milling disc and the sliding friction action area, and to increase the friction and rolling force on the tertiary aggregate to be corrected, the effective width of the milling wheel designed by the present invention is 300 to 350 mm, and the weight is 250 to 350 kg. In addition, to enhance the above-mentioned sliding friction effect, a layer of SiC abrasive particles with a thickness of about 20 mm is solidified on the tread of the roller, wherein the SiC particle size is preferably 60-80 mesh, which can effectively improve the sliding friction coefficient. In order to prevent the reduction particles from being over-extruded and crushed, the wide roller and the roller disc are not in direct contact, and a buffer gap design is adopted between them, and the gap size is 15-20 mm.
[0049] The inventors have found through research that if the mill adopts variable speed rotation, in addition to the sliding friction caused by the linear velocity difference of each point in the width direction of the millstone as mentioned above, a certain dragging friction effect will be generated on the aggregate to be corrected in the tangential direction of the millstone rotation. Furthermore, the frequency of the variable frequency motor is set to a sinusoidal mode change, and when the speed N of the millstone around the main shaft changes sinusoidally with time t as shown in formula (1), the dragging friction effect is best when it is at the peak or trough of the speed.
[0050] Formula (1)
[0051] Where N is the mill speed, unit is r / min; K is the period constant of the mill variable frequency motor, generally ranging from 20 to 30.
[0052] Furthermore, in order to obtain the best grinding efficiency, reduce energy consumption, and maximize energy utilization, the present invention adopts a method of connecting three grinding wheels to the vertical main shaft through a horizontal axis to achieve coaxial symmetrical linkage rotation. In order to obtain the best linkage effect, the present invention further designs the three horizontal axes to be evenly distributed at an angle of 120º.
[0053] Step 8 - Four-time screening: The milled material obtained in step 7 is sent to the screening system through a conveyor belt, and two parts of 5-0.5mm and 0.5-0mm are screened out. The 0.5-0mm part also directly enters the finished product regenerated fine particle silo for standby use. The 5-0.5mm part is called regenerated and reduced particle material, which is very close to the original magnesia particle morphology and will enter the regenerated and reduced particle material silo for standby use.
[0054] Through steps 1 to 8, the recycled material particles are always classified, and the coarse particles (5-0.5mm) that are prone to false particles are deeply treated by chemical, physical and mechanical methods. The true appearance of the magnesia particles is restored to the greatest extent, the purpose of correcting the false particles is achieved, and the volume density and resistance to slag erosion of the recycled particles are improved. It is not difficult to predict that the performance of the recycled bricks prepared by it will not be lower than that of the new magnesia-carbon bricks prepared with the same grade of magnesia.
[0055] The following will combine the application scenarios of the pseudo-particle correction process of used carbon-containing magnesium refractory materials of different materials, and explain the technical solution of the present invention in detail through specific examples. However, it is worth noting that these examples are only the best implementation schemes for a specific application scenario and do not limit the scope of the present invention.
[0056] Regeneration particle capacity correction technology of used MgO-C refractory
[0057] The treatment object of this embodiment is the spent MgO-C bricks obtained by dismantling the residual lining of the working layer of a domestic large-scale steel company's converter after 10,000 furnaces in service. After classification, sorting and recycling, they will be recycled and used. The following regenerated particle correction method is specifically used in the treatment process:
[0058] Step 1: Preparation of MgO-C regenerated granular material: The above-mentioned used MgO-C bricks that have been recovered, purified and sorted are regenerated by a water-free treatment process, and MgO-C regenerated granular materials of 5 to 0 mm are obtained by crushing and screening.
[0059] Step 2: Primary screening. The MgO-C regenerated granular material obtained in step 1 is screened for the first time, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part directly enters the finished product regenerated fine granular material bin for standby use, while the 5-0.5 mm part is called the first aggregate to be corrected and will enter step 3.
[0060] Step 3: Micro-spiral low-temperature nitrogen-oxygen suspension tumbling roasting. The first aggregate to be corrected screened in step 2 is conveyed to the feed port of the micro-spiral suspension roasting furnace via a belt conveyor. First, open the air inlet valve and inject 350°C compressed nitrogen-oxygen mixed gas into the furnace of the roasting furnace. Then open the feed port valve. At this time, under the strong push of the high-pressure mixed airflow, the first aggregate to be corrected and the argon-oxygen mixed gas are quickly and fully fused to form a gas-material suspension. Under the unique spiral furnace design of the roasting furnace, the gas-material suspension runs from the furnace head to the furnace tail in a fluctuating and tumbling flow state. When the gas-material suspension runs to the furnace tail section, it is filtered and blocked by a 325-mesh vibrating screen to achieve gas-material separation. The mixed gas is then sucked into the negative pressure outlet and collected after dust removal. The material separated by the vibration screen is called the initial correction material. The initial correction material falls to the belt conveyor through the discharge port and is conveyed by the belt to step 4.
[0061] Furthermore, the structural shape characteristics of the micro-spiral suspension roasting furnace are as follows: horizontal distribution, divided into three sections: furnace head, furnace body and furnace tail, the furnace hearth diameter is designed to be 200mm and the length is 10m; the spiral diameter is 420mm and the pitch is 1000mm, forming a micro-spiral effect; the air inlet is arranged on the end face of the furnace head, the feed port is arranged directly above the furnace head, and the center lines of the two intersect vertically, the diameters of the air inlet and the feed port are designed to be 50mm and 50mm respectively, and the ratio of the two is 1:1, so as to obtain the best mixed gas flow and minimize the operating energy consumption; the negative pressure air outlet diameter is 100mm, one end of the air outlet is arranged on the end face of the furnace tail section, and the other end is equipped with a static pressure of 1200 Pa of negative pressure fan forms a good negative pressure state, which can quickly suck the mixed gas in the tail area of the furnace to the outlet; the 325-mesh vibrating screen is 400mm away from the cross-section of the tail end face of the furnace, and the screen area accounts for 80% of the cross-sectional area; a discharge port is set directly below 80mm from the front end of the vibrating screen, and the discharge port diameter is 200mm.
[0062] Furthermore, the 360° C. compressed nitrogen-oxygen mixed gas pressure used in this embodiment is 1.2 MPa, and the nitrogen-oxygen mixed gas volume ratio is 15%:85%.
[0063] Step 4: Secondary screening. The primary aggregate obtained in step 3 is sent to the screening system again through the conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part is also directly sent to the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called secondary aggregate to be screened and will enter step 5.
[0064] Step 5: Rapid low-temperature ethanol cold shock treatment. The secondary aggregate to be corrected screened out in step 4 is quickly put into the mixer through the conveyor belt, then the mixer switch is turned on, the speed is set to 70 r / min, and low-temperature ethanol is quickly injected into the mixer in a spray state. Stir at this speed for 10 minutes to fully blend the secondary aggregate to be corrected with the low-temperature ethanol. After the stirring is completed, turn off the switch and keep it in a static state for another 10 minutes. The temperature in the mixer is kept constant at 80°C to ensure that the ethanol can be completely evaporated after the cold shock effect is completed. After the static state is completed, all the materials that have been cold-shocked are discharged through the discharge port to obtain cold-shocked materials, which will enter step 6.
[0065] Furthermore, the mixer is a sand mixer with dual functions of electric driven forced stirring and bottom auxiliary heating, with an effective working capacity of 1000 liters and a rated loading capacity of 3 tons. The bottom auxiliary heating is carried out in a water bath to achieve the purpose of temperature control of maintaining the internal temperature of the mixer at 80°C.
[0066] Furthermore, the low-temperature ethanol is refrigerated 98% grade industrial ethanol. In order to obtain the best cold shock effect and process operability, the industrial ethanol is cooled to -60°C in this embodiment. Furthermore, in order to obtain the best cold shock effect and subsequent efficient volatilization and removal, the weight ratio of low-temperature ethanol to secondary aggregate to be corrected is controlled to 1:8 in this embodiment, that is, 375 kg of low-temperature ethanol needs to be sprayed for each mixing (3 tons) of secondary aggregate to be corrected.
[0067] Step 6: Tertiary screening. The cold-shocked material obtained in step 5 is sent to the screening system through a conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part also directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called the tertiary aggregate to be corrected and will enter step 7.
[0068] Step 7: High-efficiency grinding treatment. The tertiary aggregates screened in step 6 are conveyed to a three-wheel variable speed mill through a belt for high-efficiency grinding treatment for 20 minutes. After the grinding treatment, the ground material is obtained, and the ground material enters the conveyor belt through the mill outlet and is conveyed to step 8 through the belt.
[0069] In this embodiment, the wide roller has a diameter of 500 mm, an effective width of 300 mm, and a weight of 250 kg. A layer of SiC abrasive particles (60 mesh) with a thickness of about 20 mm is solidified on its tread, which can effectively improve the sliding friction coefficient. In order to prevent the reduction particles from being over-extruded and crushed, the gap between the wide roller and the roller disc is designed to be 15 mm in this embodiment.
[0070] In this embodiment, the motor of the mill is set to sinusoidal frequency conversion, so that the speed N of the mill stone around the main shaft changes with time t according to The sinusoidal periodic changes can maximize the dragging and friction effect of the roller on the aggregate to be corrected when the speed reaches the peak or trough.
[0071] Step 8: Four-time screening. The milled material obtained in step 7 is sent to the screening system through a conveyor belt, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part also directly enters the finished product regenerated fine particle silo for standby use. The 5-0.5 mm part is called regenerated and reduced particle material, which will enter the regenerated and reduced particle material silo for standby use.
[0072] This embodiment adopts the above steps 1 to 8 to correct the volume of the regenerated particles of the used MgO-C refractory material, thereby eliminating the surface coating layer to a large extent, making it infinitely close to the morphology of the original magnesia sand particles (true particles).
[0073] The treatment objects, post-use sorting, collection and water-free treatment process adopted are completely consistent with Example 1. The difference is that Example 1 does not perform any volume correction treatment, but is directly used as recycled material after water-free treatment.
[0074] Example 2: Regeneration of MgO-Al2O3-C refractory particles
[0075] The treatment object of this embodiment is the used MgO-Al2O3-C bricks obtained by dismantling the residual lining of the ladle wall of a 120-ton refining ladle of a domestic steel plant after it has been in service for 150 times. After sorting and recycling, it will be regenerated and used. The following specific regenerated particle correction method is used in its treatment process:
[0076] Step 1: Preparation of MgO-Al2O3-C recycled granules. The recycled, purified and selected used MgO-Al2O3-C bricks are recycled using a water-free treatment process, and 5-0 mm MgO-Al2O3-C recycled granules are obtained by crushing and screening.
[0077] Step 2: Primary screening. The MgO-Al2O3-C recycled granular material obtained in step 1 is screened for the first time, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part directly enters the finished product recycled fine granular material bin for standby use, while the 5-0.5 mm part is called the first aggregate to be corrected and will enter step 3.
[0078] Step 3: Micro-spiral low-temperature nitrogen-oxygen suspension tumbling roasting. The first aggregate to be corrected screened in step 2 is conveyed to the feed port of the micro-spiral suspension roasting furnace via a belt conveyor. First, open the air inlet valve and inject 370°C compressed nitrogen-oxygen mixed gas into the furnace of the roasting furnace. Then open the feed port valve. At this time, under the strong push of the high-pressure mixed airflow, the first aggregate to be corrected and the argon-oxygen mixed gas are quickly and fully fused to form a gas-material suspension. Under the unique spiral furnace design of the roasting furnace, the gas-material suspension runs from the furnace head to the furnace tail in a fluctuating and tumbling flow state. When the gas-material suspension runs to the furnace tail section, it is filtered and blocked by a 325-mesh vibrating screen to achieve gas-material separation. The mixed gas is then sucked into the negative pressure outlet and collected after dust removal. The material separated by the vibration screen is called the initial correction material. The initial correction material falls to the belt conveyor through the discharge port and is conveyed by the belt to step 4.
[0079] Furthermore, the structural shape characteristics of the micro-spiral suspension roasting furnace are as follows: horizontal distribution, divided into three sections: furnace head, furnace body and furnace tail, the furnace hearth diameter is designed to be 250mm and the length is 11m; the spiral diameter is 460mm and the pitch is 1300mm, forming a micro-spiral effect; the air inlet is arranged on the end face of the furnace head, the feed port is arranged directly above the furnace head, and the center lines of the two intersect vertically, the diameters of the air inlet and the feed port are designed to be 91mm and 65mm respectively, and the ratio of the two is 1.4:1, so as to obtain the best mixed gas flow and minimize the operating energy consumption; the negative pressure air outlet has a diameter of 120mm, one end of the air outlet is arranged on the end face of the furnace tail section, and the other end is equipped with a static pressure of 1500 Pa of negative pressure fan forms a good negative pressure state, which can quickly suck the mixed gas in the tail area of the furnace to the outlet; the 325-mesh vibrating screen is 450mm away from the cross-section of the tail end face of the furnace, and the screen area accounts for 85% of the cross-sectional area; a discharge port is set directly below 70mm from the front end of the vibrating screen, and the discharge port diameter is 225mm.
[0080] Furthermore, the 370° C. compressed nitrogen-oxygen mixed gas pressure used in this embodiment is 1.3 MPa, and the nitrogen-oxygen mixed gas volume ratio is 17%:83%.
[0081] Step 4: Secondary screening. The primary aggregate obtained in step 3 is sent to the screening system again through the conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part is also directly sent to the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called secondary aggregate to be screened and will enter step 5.
[0082] Step 5: Rapid low-temperature ethanol cold shock treatment. The secondary aggregate to be corrected screened out in step 4 is quickly put into the mixer through the conveyor belt, then the mixer switch is turned on, the speed is set to 75 r / min, and low-temperature ethanol is quickly injected into the mixer in a spray state. Stir at this speed for 12 minutes to fully blend the secondary aggregate to be corrected with the low-temperature ethanol. After the stirring is completed, turn off the switch and keep it in a static state for 13 minutes. The temperature in the mixer is kept constant at 90°C to ensure that the ethanol can be completely evaporated after the cold shock effect is completed. After the static state is completed, all the materials that have been cold-shocked are discharged through the discharge port to obtain cold-shocked materials, which will enter step 6.
[0083] Furthermore, the mixer is a sand mixer with dual functions of electric-driven forced stirring and bottom auxiliary heating, with an effective working capacity of 1,200 liters and a rated loading capacity of 3.6 tons. The bottom auxiliary heating is carried out by active electric heating to achieve the purpose of temperature control of maintaining the internal temperature of the mixer at 90°C.
[0084] Furthermore, the low-temperature ethanol is refrigerated 96% grade industrial ethanol. In order to obtain the best cold shock effect and process operability, the industrial ethanol is cooled to -55°C in this embodiment. Furthermore, in order to obtain the best cold shock effect and subsequent efficient volatilization and removal, the weight ratio of low-temperature ethanol to secondary aggregate to be corrected is controlled to 1:10 in this embodiment, that is, 360 kg of low-temperature ethanol needs to be sprayed for each mixing (3.6 tons) of secondary aggregate to be corrected.
[0085] Step 6: Tertiary screening. The cold-shocked material obtained in step 5 is sent to the screening system through a conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part also directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called the tertiary aggregate to be corrected and will enter step 7.
[0086] Step 7: High-efficiency grinding. The aggregates to be corrected after the screening in step 6 are conveyed to a three-wheel variable-speed mill through a belt for high-efficiency grinding for 30 minutes. After the grinding, the grinding material is obtained. The grinding material enters the conveyor belt through the mill outlet and is conveyed to step 8 through the belt.
[0087] In this embodiment, the wide roller has a diameter of 550 mm, an effective width of 320 mm, and a weight of 300 kg. A layer of SiC abrasive particles (70 mesh) with a thickness of about 20 mm is solidified on its tread, which can effectively improve the sliding friction coefficient. In order to prevent the reduction particles from being over-extruded and crushed, the gap between the wide roller and the roller disc is designed to be 18 mm in this embodiment.
[0088] In this embodiment, the motor of the mill is set to sinusoidal frequency conversion, so that the speed N of the mill stone around the main shaft changes with time t according to The sinusoidal periodic changes can maximize the dragging and friction effect of the roller on the aggregate to be corrected when the speed reaches the peak or trough.
[0089] Step 8: Four-time screening. The milled material obtained in step 7 is sent to the screening system through a conveyor belt, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part also directly enters the finished product regenerated fine particle silo for standby use. The 5-0.5 mm part is called regenerated and reduced particle material, which will enter the regenerated and reduced particle material silo for standby use.
[0090] This embodiment adopts the above steps 1 to 8 to correct the volume and remove the pseudo particles regenerated from the used MgO-Al2O3-C refractory material, thereby eliminating the surface coating layer to a large extent and making it infinitely close to the morphology of the original MgO (or Al2O3) particles (true particles).
[0091] Comparative Example 2: Regenerated particles of MgO-Al2O3-C refractory material are not subjected to volume correction treatment
[0092] The treatment objects, post-use sorting, collection and traditional hydration treatment process adopted are completely consistent with Example 2. The difference is that Example 2 does not perform any volume correction treatment, but is directly used as recycled material after adopting hydration-free treatment.
[0093] Example 3: Regeneration of Al2O3-MgO-C refractory particles after use
[0094] The treatment object of this embodiment is the spent Al2O3-MgO-C bricks obtained by dismantling the residual lining of the impact zone of the bottom of a 260-ton refining ladle of a domestic steel plant after it has been in service for 120 times. After sorting and recycling, it will be regenerated and used. The following specific regenerated particle correction method is used in its treatment process:
[0095] Step 1: Preparation of Al2O3-MgO-C recycled granules. The recycled, purified and selected Al2O3-MgO-C bricks are recycled using a conventional hydration process, and 5-0 mm Al2O3-MgO-C recycled granules are obtained by crushing and screening.
[0096] Step 2: Primary screening. The Al2O3-MgO-C recycled granular material obtained in step 1 is screened for the first time, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part directly enters the finished product recycled fine granular material bin for standby use, while the 5-0.5 mm part is called the first aggregate to be corrected and will enter step 3.
[0097] Step 3: Micro-spiral low-temperature nitrogen-oxygen suspension tumbling roasting. The first aggregate to be corrected screened in step 2 is conveyed to the feed port of the micro-spiral suspension roasting furnace via a belt conveyor. First, open the air inlet valve and inject 380°C compressed nitrogen-oxygen mixed gas into the furnace of the roasting furnace. Then open the feed port valve. At this time, under the strong push of the high-pressure mixed airflow, the first aggregate to be corrected and the argon-oxygen mixed gas are quickly and fully fused to form a gas-material suspension. Under the unique spiral furnace design of the roasting furnace, the gas-material suspension runs from the furnace head to the furnace tail in a fluctuating and tumbling flow state. When the gas-material suspension runs to the furnace tail section, it is filtered and blocked by a 325-mesh vibrating screen to achieve gas-material separation. The mixed gas is then sucked into the negative pressure outlet and collected after dust removal. The material separated by the vibration screen is called the initial correction material. The initial correction material falls to the belt conveyor through the discharge port and is conveyed by the belt to step 4.
[0098] Furthermore, the structural shape characteristics of the micro-spiral suspension roasting furnace are as follows: horizontal distribution, divided into three sections: furnace head, furnace body and furnace tail, the furnace hearth diameter is designed to be 300mm and the length is 12m; the spiral diameter is 500mm and the pitch is 1500mm, forming a micro-spiral effect; the air inlet is arranged on the end face of the furnace head, the feed port is arranged directly above the furnace head, and the center lines of the two intersect vertically, the diameters of the air inlet and the feed port are designed to be 150mm and 100mm respectively, and the ratio of the two is 1.5:1, so as to obtain the best mixed gas flow and minimize the operating energy consumption; the negative pressure air outlet has a diameter of 150mm, one end of the air outlet is arranged on the end face of the furnace tail section, and the other end is equipped with a static pressure of 2000 Pa of negative pressure fan forms a good negative pressure state, which can quickly suck the mixed gas in the tail area of the furnace to the outlet; the 325-mesh vibrating screen is 500mm away from the cross-section of the tail end face of the furnace, and the screen area accounts for 90% of the cross-sectional area; a discharge port is set just below 60mm from the front end of the vibrating screen, and the discharge port diameter is 250mm.
[0099] Furthermore, the 380° C. compressed nitrogen-oxygen mixed gas pressure used in this embodiment is 1.5 MPa, and the nitrogen-oxygen mixed volume ratio is 20%:80%.
[0100] Step 4: Secondary screening. The primary aggregate obtained in step 3 is sent to the screening system again through the conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part is also directly sent to the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called secondary aggregate to be screened and will enter step 5.
[0101] Step 5: Rapid low-temperature ethanol cold shock treatment. The secondary aggregate to be corrected screened out in step 4 is quickly put into the mixer through the conveyor belt, then the mixer switch is turned on, the speed is set to 80 r / min, and low-temperature ethanol is quickly injected into the mixer in a spraying state. Stir at this speed for 15 minutes to fully blend the secondary aggregate to be corrected with the low-temperature ethanol. After the stirring is completed, turn off the switch and keep it in a static state for another 15 minutes. The temperature in the mixer is kept constant at 100°C to ensure that the ethanol can be completely evaporated after the cold shock effect is completed. After the static state is completed, all the materials that have been cold-shocked are discharged through the discharge port to obtain cold-shocked materials, which will enter step 6.
[0102] Furthermore, the mixer is a sand mixer with dual functions of electric driven forced stirring and bottom auxiliary heating, with an effective working capacity of 1500 liters and a rated loading capacity of 4 tons. The bottom auxiliary heating is carried out by electric heating to achieve the purpose of temperature control of maintaining the internal temperature of the mixer at 100°C.
[0103] Furthermore, the low-temperature ethanol is refrigerated 95% grade industrial ethanol. In order to obtain the best cold shock effect and process operability, the industrial ethanol is cooled to -50°C in this embodiment. Furthermore, in order to obtain the best cold shock effect and subsequent efficient volatilization and removal, the weight ratio of low-temperature ethanol to secondary aggregate to be corrected is controlled to 1:12 in this embodiment, that is, 333 kg of low-temperature ethanol needs to be sprayed for each mixing (4 tons) of secondary aggregate to be corrected.
[0104] Step 6: Tertiary screening. The cold-shocked material obtained in step 5 is sent to the screening system through a conveyor belt to screen out two parts: 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part also directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called the tertiary aggregate to be corrected and will enter step 7.
[0105] Step 7: High-efficiency grinding. The aggregates to be corrected after the screening in step 6 are conveyed to a three-wheel variable-speed mill through a belt for high-efficiency grinding for 30 minutes. After the grinding, the grinding material is obtained. The grinding material enters the conveyor belt through the mill outlet and is conveyed to step 8 through the belt.
[0106] In this embodiment, the wide roller has a diameter of 600 mm, an effective width of 350 mm, and a weight of 350 kg. A layer of SiC abrasive particles (80 mesh) with a thickness of about 20 mm is fixed on its tread, which can effectively improve the sliding friction coefficient. In order to prevent the reduction particles from being over-extruded and crushed, the gap between the wide roller and the roller disc is designed to be 20 mm in this embodiment.
[0107] In this embodiment, the motor of the mill is set to sinusoidal frequency conversion, so that the speed N of the mill stone around the main shaft changes with time t according to The sinusoidal periodic changes can maximize the dragging and friction effect of the roller on the aggregate to be corrected when the speed reaches the peak or trough.
[0108] Step 8: Four-time screening. The milled material obtained in step 7 is sent to the screening system through a conveyor belt, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part also directly enters the finished product regenerated fine particle silo for standby use. The 5-0.5 mm part is called regenerated and reduced particle material, which will enter the regenerated and reduced particle material silo for standby use.
[0109] This embodiment adopts the above steps 1 to 8 to correct the volume and remove the pseudo particles regenerated from the used Al2O3-MgO-C refractory material, thereby eliminating the surface coating layer to a large extent and making it infinitely close to the morphology of the original MgO (or Al2O3) particles (true particles).
[0110] Comparative Example 3: Used Al2O3-MgO-C refractory material regeneration particles are not subjected to volume correction treatment
[0111] The treatment objects, post-use sorting, collection and the traditional hydration treatment process adopted are completely consistent with Example 3. The difference is that Example 3 does not perform any volume correction treatment, but is directly used as recycled material after adopting traditional hydration treatment.
[0112] Test and comparison method: (1) According to GB / T2999 "Test Method for Bulk Density of Refractory Particles", the carbon-containing magnesium regenerated particles obtained by each embodiment and comparative example were tested for bulk density, and the results are shown in Table 3; (2) All particles were used from the carbon-containing magnesium regenerated particles obtained by each embodiment and comparative example, and were mixed with an appropriate amount of -194 flaky graphite, and thermosetting phenolic resin was added as a binder. After mixing, molding, heat treatment and other processes, regenerated bricks with the chemical composition shown in Table 3 (the embodiment and the comparative example are the same) were prepared, and the apparent porosity after heat treatment at 200℃×24h and the high-temperature flexural strength at 1400℃×0.5h were tested according to GB / T2997 "Test Method for Bulk Density, Apparent Porosity and True Porosity of Dense Shaped Refractory Products" and GB / T13473 "Test Method for High-Temperature Flexural Strength of Carbon-Containing Refractory Materials", and the test results are shown in Table 3. Note: The above national standards without year numbers are quoted in the latest version in actual operation.
[0113] Table 3 Data related to the examples and comparative examples
[0114]
[0115] From Table 3, we can see that:
[0116] (1) It is not difficult to see from the volume density test results of the regenerated particles that after the volume correction process provided by the present application is adopted, the volume density of the regenerated particles of the embodiment is greatly improved compared with the comparative example, that is, the volume densities of the regenerated particles of Examples 1, 2, and 3 are increased by 8.3%, 9.6%, and 9.1% compared with the comparative examples 1, 2, and 3, respectively. This indicates that the volume correction process provided by the present application can obtain an excellent pseudo-particle morphology finishing effect, can basically eliminate the carbon coating layer on the surface of the particles, and restore the structural characteristics of the original magnesium oxide particles (true particles) to a great extent, which can greatly increase the recycling rate of the used carbon-containing magnesium refractory materials.
[0117] (2) Because the loose carbon coating on the surface of the particles treated with the correction volume is basically eliminated, all particles are recycled particles and are prepared according to the principle of the same chemical composition. Compared with the spent carbon-containing magnesium refractory material without correction volume treatment (comparative example), the recycled bricks produced by the spent carbon-containing magnesium refractory material obtained by the correction volume process provided by the present invention have lower apparent porosity and higher high-temperature flexural strength. It is not difficult to see from the data in Table 3 that for the apparent porosity index, the embodiment is reduced by 40.5%, 37.5%, and 33.3% respectively compared with the comparative example; while in terms of high-temperature flexural strength, the embodiment is increased by 50%, 43.5%, and 25.4% respectively compared with the comparative example. It can be seen that the technical solution of the present invention can make the key performance indicators of recycled bricks achieve a qualitative leap, and it is far higher than the requirements of the corresponding national standard grades, which will greatly improve the performance of recycled bricks in service again.
Claims
1. A process for regenerating pseudo-particles and rectifying the volume of used carbon-containing magnesium refractory materials, characterized in that The following steps are involved: Step 1-Preparation of carbon-containing magnesium regenerated granular material: The recovered, purified and selected used carbon-containing magnesium refractory material is treated by conventional process, and then crushed to prepare 5-0 mm carbon-containing magnesium regenerated granular material; Step 2-primary screening: The carbon-containing magnesium recycled granular material obtained in step 1 is screened for the first time, and two parts of 5-0.5 mm and 0.5-0 mm are screened out. The 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, and the 5-0.5 mm part is called the first aggregate to be corrected; Step 3 - Micro-spiral low-temperature nitrogen-oxygen suspension tumbling roasting: The first aggregate to be corrected in step 2 is fed into the inlet of the micro-spiral suspension roasting furnace, and fully fused with the compressed nitrogen-oxygen mixed gas with a temperature of 350°C to 380°C after preheating to form a gas-material suspension. The carbon layer of the first aggregate to be corrected is rapidly selectively preferentially oxidized with oxygen to disintegrate and disperse, and runs to the tail section of the furnace. The gas-material separation is achieved under the conditions of obstruction and filtration of a 325-mesh vibrating screen. The gas is sucked into the negative pressure outlet and collected after dust removal, and the material separated by the vibrating screen is discharged from the outlet to obtain the primary corrected material; Step 4-Secondary Screening: The primary aggregate obtained in step 3 is screened again to screen out two parts, 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, and the 5-0.5 mm part is called the secondary aggregate to be screened; Step 5-Rapid low-temperature ethanol cold shock treatment: put the secondary aggregate to be corrected into the mixer, set the mixer speed to 70-80 r / min, then turn on the mixer switch, start the auxiliary heating device at the bottom of the mixer, the temperature is 80-100℃, and quickly inject low-temperature ethanol into the mixer in a spraying state, so that the secondary aggregate to be corrected is subjected to a negative temperature difference of -(200±5℃), and stir at this speed for 10-15 minutes to fully blend the secondary aggregate to be corrected with the low-temperature ethanol; after the stirring is completed, keep it in a static state for 10-15 minutes and then discharge it to obtain the cold shock material; Step 6 - tertiary screening: The cold-shocked material obtained in step 5 is sent to the screening system to screen out two parts, 5-0.5 mm and 0.5-0 mm. The 0.5-0 mm part directly enters the finished product recycled fine particle silo for standby use, while the 5-0.5 mm part is called the tertiary aggregate to be corrected; Step 7-high-efficiency grinding treatment: the tertiary aggregate to be corrected screened out in step 6 is sent to a grinding machine for high-efficiency grinding treatment for 20 to 30 minutes. The surface of the tertiary aggregate to be corrected produces a mechanical action of crushing and grinding, which causes the remaining coating layer to be crushed and deeply removed, achieving ultimate correction and restoration. After the grinding treatment, the ground material is obtained; Step 8 - Four-time screening: Send the milled material obtained in step 7 to the screening system, screen out two parts, 5-0.5 mm and 0.5-0 mm, of which the 0.5-0 mm part directly enters the finished product regenerated fine particle silo for standby use; the 5-0.5 mm part is called the regenerated and reduced particle material, which is very close to the original magnesia particle morphology and will enter the regenerated and reduced particle material silo for standby use.
2. The process for regenerating pseudo particles and correcting the volume of used carbon-containing magnesium refractory materials according to claim 1 is characterized in that: The conventional process treatment in step 1 includes one of the following processes: hydration or hydration-free regeneration treatment of the carbon-containing magnesium refractory material.
3. The process for regenerating pseudo particles and correcting the volume of used carbon-containing magnesium refractory materials according to claim 1 is characterized in that: In the step 3, the micro-spiral suspension roasting furnace is horizontally distributed and is divided into three sections: a furnace head, a furnace body and a furnace tail; the optimal diameter of the furnace is 200-300 mm and the length is 10-12 m; the spiral diameter is 420-500 mm and the pitch is 1000-1500 mm; the air inlet is arranged on the end face of the furnace head, the feed port is arranged directly above the furnace head, and the center lines of the two intersect vertically, the ratio of the diameter of the air inlet to the feed port is (1-1.5): 1, and the diameter of the feed port is 50-100 mm; the diameter of the negative pressure air outlet is 100-150 mm, one end of which is arranged on the end face of the furnace tail section, and the other end is installed with a negative pressure fan, and the static pressure of the negative pressure fan is 1200-2000 Pa; the 325 mesh vibrating screen is arranged on a cross section 400-500 mm away from the end face of the furnace tail, and the screen area should account for more than 80% of the cross section; the diameter of the discharge port is 200-250 mm.
4. The process for regenerating pseudo particles and correcting the volume of used carbon-containing magnesium refractory materials according to claim 1 is characterized in that: In step 3, the pressure of the compressed nitrogen-oxygen mixed gas is 1.2-1.5 MPa, and the optimal volume ratio of nitrogen and oxygen in the mixed gas is (15%-20%): (80%-85%).
5. The process for regenerating pseudo particles and correcting the volume of used carbon-containing magnesium refractory materials according to claim 1 is characterized in that: In step 5, the effective working capacity of the mixer is not less than 1000 L, and the heating method is a water bath or electric heating method.
6. The process for regenerating pseudo particles and correcting the volume of used carbon-containing magnesia refractory materials according to claim 1 is characterized in that: In step 5, the weight ratio of low-temperature ethanol to secondary aggregate to be corrected should be 1: (8-12).
7. The process for regenerating pseudo particles and correcting the volume of used carbon-containing magnesia refractory materials according to claim 1 is characterized in that: In step 7, the mill is a three-wheel variable speed mill, which consists of a variable frequency motor, a vertical spindle, an iron bowl-shaped grinding disc and three wide millstones, and each millstone is connected to the vertical spindle by a horizontal axis, and the vertical spindle is driven by the variable frequency motor to rotate at a variable speed around the center line of the grinding disc, thereby driving the millstone to rotate at a variable speed around the spindle; during the rotation process, since the distances of various points on the width direction of the millstone from the rotation center line are different, the linear speeds are also different; the wide millstone is a circular stone wheel with a diameter of 500-600mm, an effective width of 300-350mm, and a weight of 250-350kg. A layer of SiC abrasive particles with a thickness of about 20mm is solidified on the tread of the millstone, wherein the SiC particle size is 60-80 mesh; the gap between the wide millstone and the grinding disc is 15-20mm.
Citation Information
Patent Citations
Method for improving microscopic structure and thermal shock resistance of ultralow-carbon magnesium-carbon material
CN109206122A
Preparation method for composite powder used for low-carbon magnesia-carbon rod head
CN110790575A
Cited By
Method for preparing magnesium refractory material from magnesium-rich tailings
CN119263857A