A method for preparing microwave absorbing material from ultrafine manganese-zinc ferrite powder
Through ultrasonic co-precipitation method and surface modification technology, manganese-zeb ferrite ultrafine powder was prepared and blended with porous spherical zinc oxide and carbon oxide nanotubes, which solved the easy agglomeration of manganese-zeb ferrite ultrafine powder in traditional methods. The problem is that the preparation of high-performance absorbing materials has been achieved to meet the needs of modern electronic devices for absorbing materials.
Patent Information
- Application Number
- CN202410695868.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-11-02
AI Technical Summary
The traditional method of preparing manganese-zeb ferrite ultrafine powder is prone to agglomeration, has low purity, poor uniformity, and complex process, making it difficult to meet the demand of modern electronic devices for high-performance wave absorbing materials.
Manganese-zeb ferrite ultrafine powder was prepared by ultrasonic co-precipitation method, and the surface modification was made and blended with porous spherical zinc oxide and carbon oxide nanotubes to form a composite wave absorbing material with excellent performance.
The fine particle size distribution of manganese-zeb ferrite ultrafine powder and the preparation of high-performance absorbing materials are realized, which improves the absorption bandwidth, compatibility and lightness of the material, and meets the requirements of modern absorbing materials.
Smart Images

Figure SMS_1
Abstract
Description
[0001] This application is a divisional application with application number 2023114467761, application date November 2, 2023, and invention name “Preparation process and application of manganese-zinc ferrite ultrafine powder”. Technical Field
[0002] The invention relates to the technical field of manganese-zinc ferrite, in particular to a method for preparing a wave-absorbing material from superfine manganese-zinc ferrite powder. Background Art
[0003] Manganese zinc ferrite materials are widely used in electronic information and military fields due to their advantages such as high resistivity, low loss and good dielectric properties. With the continuous development of electronic devices towards ultra-miniaturization, thinness and high performance, manganese zinc ferrite ultrafine powder has excellent nano-size characteristics and potential application value, gradually replacing traditional metal magnetic materials and becoming the focus of people's attention. In recent years, research on manganese zinc ferrite ultrafine powder is in full swing. For example, in the prior art, the solid phase method and coprecipitation method are more commonly used to prepare manganese zinc ferrite ultrafine powder. However, the problems are that the powder obtained by the solid phase method has low purity, poor uniformity, easy to agglomerate, large particle size and requires very high reaction temperature; the precipitate obtained by the traditional coprecipitation reaction is colloidal and difficult to wash and filter, and may even cause segregation of the components, especially for multi-component system ferrite, the coprecipitation is slow and the process turnover time is very long.
[0004] Electromagnetic pollution has become the fourth largest pollution after air pollution, water pollution and noise pollution. Absorbing materials that can effectively resist and weaken electromagnetic radiation have become a research hotspot for new functional materials. Manganese-zinc ferrite has excellent magnetic properties and is widely used in the field of electromagnetic wave absorbing materials. However, a single ferrite material can no longer meet today's usage requirements. Ferrite, as a traditional absorbing material, has disadvantages such as high density and narrow absorption band, and is not suitable for practical applications. Therefore, nano-ferrite composites provide a new way to develop high-performance new materials and improve the performance of existing materials, and become an important direction for new material research.
[0005] Due to the special structure and dielectric properties of carbon nanotubes, the wave absorbing performance of composite materials synthesized from carbon nanotubes and other materials has shown good application prospects. Some nanomaterials have excellent wave absorbing properties, quantum size effects and tunnel effects. For example, nano zinc oxide as a wave absorbing material can not only evade radar detection within a wide frequency band, but also has the characteristics of good compatibility, small mass and thin thickness. The present invention prepares manganese zinc ferrite ultrafine powder by adopting ultrasonic coprecipitation method, and modifies its surface. The obtained modified manganese zinc ferrite ultrafine powder is blended with porous spherical zinc oxide and oxidized carbon nanotubes to obtain a composite wave absorbing material with excellent performance. The process is simple and easy to implement. Summary of the invention
[0006] The technical problem solved by the invention is to provide a method for preparing wave-absorbing materials from ultrafine manganese-zinc ferrite powder, solve the problem of easy agglomeration of ultrafine powder prepared by traditional methods, and prepare composite wave-absorbing materials with excellent comprehensive performance.
[0007] The technical solution of the present invention is as follows:
[0008] A preparation process of manganese-zinc ferrite ultrafine powder, the preparation process is carried out according to the following steps:
[0009] (1) Add FeCl3, MnCl2, ZnCl2 and deionized water to a reaction bottle, stir and disperse, add dispersant oleic acid under nitrogen protection, stir at 40-60°C for 10-30 minutes, add ammonia water to control the pH of the system to 7-9, then dropwise add a coprecipitant, stir and disperse, place the mixed solution in an ultrasonic generator, and perform an ultrasonic-assisted reaction. After the reaction is completed, filter, wash the filter cake with ethanol and deionized water, and dry to obtain a manganese zinc ferrite precursor.
[0010] (2) Add the manganese zinc ferrite precursor into a high temperature furnace, raise the temperature of the high temperature furnace to 350-500°C at a rate of 3-5°C / min, keep it at that temperature for 1-2 hours, and then keep it at 800-900°C for 2-4 hours. After natural cooling, obtain manganese zinc ferrite ultrafine powder.
[0011] Furthermore, in step (1), the ratio of FeCl3, MnCl2, ZnCl2, oleic acid and coprecipitant is: 4 mol: 1 mol: 1 mol: 0.1-0.35 mol: 0.01-0.03 mol.
[0012] Furthermore, in step (1), the co-precipitant is any one of ammonium oxalate and ammonium bicarbonate.
[0013] Furthermore, in step (1), the power of the ultrasonic generator is 50-300 W, the ultrasonic-assisted temperature is 30-45° C., and the time is 10-50 min.
[0014] Further, S1, add a mixed solvent of manganese zinc ferrite ultrafine powder, ethanol and deionized water into a reaction bottle, stir evenly, add KH550, stir to react, after the reaction is completed, filter, wash with acetone and deionized water, and dry to obtain modified manganese zinc ferrite ultrafine powder.
[0015] S2. Add zinc sulfate, ammonium carbonate and deionized water to a reaction bottle, stir evenly at room temperature, add dispersant polyethylene glycol, stir at 20-35°C for 8-16h, then place the mixed solution in a tubular furnace, and heat it to 400-500°C at a heating rate of 4-8°C / min in a nitrogen atmosphere, react at a constant temperature for 5-10h, and obtain porous spherical zinc oxide after natural cooling.
[0016] S3. Add modified manganese zinc ferrite ultrafine powder, porous spherical zinc oxide and ethanol into a reaction bottle, stir and disperse, add oxidized carbon nanotubes, ultrasonically disperse at 20-35° C. for 20-40 minutes, wash with deionizer, and dry to obtain manganese zinc ferrite ultrafine powder absorbing material.
[0017] Furthermore, in step S1, the ratio of ultrafine manganese zinc ferrite powder to KH550 is 1g:0.5-1g.
[0018] Furthermore, in step S1, the reaction temperature is 60-80° C., and the reaction time is 4-8 h.
[0019] Furthermore, in step S2, the ratio of zinc sulfate, ammonium carbonate and polyethylene glycol is: 1 mol: 1-3 mol: 15-25 g.
[0020] Furthermore, in step S3, the ratio of modified manganese zinc ferrite ultrafine powder, porous spherical zinc oxide, and oxidized carbon nanotubes is: 1g: 1-5g: 0.05-0.25g.
[0021] The beneficial technical effects of the present invention are as follows:
[0022] The invention allows FeCl3, MnCl2, ZnCl2 and dispersant oleic acid and coprecipitant ammonium oxalate or ammonium bicarbonate to undergo coprecipitation reaction in an ultrasonic generator, obtains a manganese zinc ferrite precursor by controlling the ultrasonic frequency, and obtains manganese zinc ferrite ultrafine powder with a nanometer particle size after the precursor is calcined at high temperature; KH550 is used to modify the surface of the manganese zinc ferrite ultrafine powder to avoid powder agglomeration, and then zinc sulfate, ammonium carbonate and dispersant polyethylene glycol are reacted in a reactor to obtain porous spherical zinc oxide; finally, the modified manganese zinc ferrite ultrafine powder, the porous spherical zinc oxide and oxidized carbon nanotubes are blended to obtain a manganese zinc ferrite ultrafine powder wave absorbing material.
[0023] In the manganese zinc ferrite ultrafine powder prepared by ultrasonic co-precipitation, oleic acid improves the dispersibility and particle size distribution of nanoparticles; the cavitation effect and impact effect of ultrasound are used to crush the precipitate and refine the grains, thereby increasing the rate of crystal nucleus generation during the precipitation process. At the same time, a large number of bubbles will be generated during the ultrasonic-assisted process, and these bubbles will adhere to the surface of the precipitate to reduce the surface energy of the precipitate, making it more difficult to aggregate the crystal nuclei and making the particle size of the prepared material smaller.
[0024] Porous spherical zinc oxide has a quantum size effect and an antenna-like structure. Charges gather at the tip of the needle to form multiple polarization centers, which cause electromagnetic waves to be dispersed and reflected, and the microwave absorption capacity is enhanced. The carbon nanotube lumen is small and narrow, and the capillary effect is strong. Magnetic particles can be sucked into the lumen and densely arranged, resulting in a certain magnetic loss, thus having microwave absorption performance. The modified manganese zinc ferrite ultrafine powder has a large specific surface area and nanometer size. The reduction in particle size increases the roughness of the material surface, which is beneficial to the attenuation of microwaves. At the same time, the surface atoms lack coordination and the number of dangling bonds increases, so interface polarization and multiple scattering become important wave absorption channels. The three are combined to produce a synergistic wave absorption effect, which improves the wave absorption performance of the material and meets the requirements of the absorption bandwidth, good compatibility, light weight and thin thickness of the wave absorbing material. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Preparation of oxidized carbon nanotubes: Weigh 5 g of carbon nanotubes, calcine at 520°C for 2 h, add to a mixture of 100 mL of concentrated sulfuric acid and 10 mL of concentrated nitric acid, ultrasonically disperse for 30 min, stir at 80°C for 2 h, cool, add 600 mL of deionized water to dilute, place at room temperature for 6 h, filter, wash with deionized water, and dry to obtain oxidized carbon nanotubes.
[0027] Preparation of ultrafine manganese zinc ferrite powder:
[0028] (1) Add 4 mol of FeCl3, 1 mol of MnCl2, 1 mol of ZnCl2 and deionized water to a reaction bottle, stir and disperse, add 0.1-0.35 mol of dispersant oleic acid under nitrogen protection, stir at 40-60°C for 10-30 min, add ammonia water to control the pH of the system to 7-9, then dropwise add 0.01-0.03 mol of coprecipitant ammonium oxalate or ammonium bicarbonate, stir and disperse, place the mixed solution in an ultrasonic generator with a power of 50-300 W, ultrasonically assist at 30-45°C for 10-50 min, filter, wash the filter cake with ethanol and deionized water, and obtain a manganese zinc ferrite precursor after drying.
[0029] (2) Add the manganese zinc ferrite precursor into a high temperature furnace, raise the temperature of the high temperature furnace to 350-500°C at a rate of 3-5°C / min, keep it at that temperature for 1-2 hours, and then keep it at 800-900°C for 2-4 hours. After natural cooling, obtain manganese zinc ferrite ultrafine powder.
[0030] Preparation of manganese zinc ferrite ultrafine powder absorbing material:
[0031] S1. Add 1g of manganese zinc ferrite ultrafine powder, a mixed solvent of ethanol and deionized water into a reaction bottle, stir evenly, add 0.5-1g of KH550, stir to react, react at 60-80°C for 4-8h, filter, wash with acetone and deionized water, and dry to obtain modified manganese zinc ferrite ultrafine powder.
[0032] S2. Add 1 mol of zinc sulfate, 1-3 mol of ammonium carbonate and deionized water to a reaction bottle, stir evenly at room temperature, add 15-25 g of dispersant polyethylene glycol, stir at 20-35 ° C for 8-16 hours, then place the mixed solution in a tubular furnace, and heat it to 400-500 ° C at a heating rate of 4-8 ° C / min in a nitrogen atmosphere, react at a constant temperature for 5-10 hours, and obtain porous spherical zinc oxide after natural cooling.
[0033] S3. Add 1g of modified manganese zinc ferrite ultrafine powder, 1-5g of porous spherical zinc oxide and ethanol into a reaction bottle, stir and disperse, add 0.05-0.25g of oxidized carbon nanotubes, ultrasonically disperse at 20-35°C for 20-40min, deionize and wash, and dry to obtain manganese zinc ferrite ultrafine powder absorbing material.
[0034] Example 1
[0035] (1) Add 10 mmol of FeCl3, 2.5 mmol of MnCl2, 2.5 mmol of ZnCl2 and deionized water to a reaction flask, stir and disperse, add 2.8 mmol of dispersant oleic acid under nitrogen protection, stir at 55 ° C for 15 min, add ammonia water to control the pH of the system at 7, then add 0.2 mmol of coprecipitant ammonium bicarbonate dropwise, stir and disperse, place the mixed solution in an ultrasonic generator with a power of 50 W, ultrasonically assist at 40 ° C for 20 min, filter, wash the filter cake with ethanol and deionized water, and obtain a manganese zinc ferrite precursor after drying.
[0036] (2) The manganese zinc ferrite precursor is added into a high temperature furnace, and the temperature of the high temperature furnace is raised to 450°C at a rate of 4°C / min, kept at that temperature for 1 hour, and then kept at 800°C for 4 hours. After natural cooling, ultrafine manganese zinc ferrite powder is obtained.
[0037] Example 2
[0038] (1) Add 2 mmol of FeCl3, 0.5 mmol of MnCl2, 0.5 mmol of ZnCl2 and deionized water to a reaction flask, stir and disperse, add 0.1 mmol of dispersant oleic acid under nitrogen protection, stir at 50 ° C for 20 min, add ammonia water to control the pH of the system at 8, then add 0.015 mmol of coprecipitant ammonium oxalate dropwise, stir and disperse, place the mixed solution in an ultrasonic generator with a power of 130 W, ultrasonically assist at 30 ° C for 15 min, filter, wash the filter cake with ethanol and deionized water, and obtain a manganese zinc ferrite precursor after drying.
[0039] (2) The manganese zinc ferrite precursor is added into a high temperature furnace, and the temperature of the high temperature furnace is raised to 450°C at a rate of 5°C / min, kept at this temperature for 2 hours, and then kept at 850°C for 3 hours. After natural cooling, ultrafine manganese zinc ferrite powder is obtained.
[0040] Example 3
[0041] (1) Add 4 mmol of FeCl3, 1 mmol of MnCl2, 1 mmol of ZnCl2 and deionized water to a reaction flask, stir and disperse, add 0.35 mmol of dispersant oleic acid under nitrogen protection, stir at 60 ° C for 30 min, add ammonia water to control the pH of the system at 9, then add 0.03 mmol of coprecipitant ammonium bicarbonate dropwise, stir and disperse, place the mixed solution in an ultrasonic generator with a power of 210 W, ultrasonically assist at 35 ° C for 30 min, filter, wash the filter cake with ethanol and deionized water, and obtain a manganese zinc ferrite precursor after drying.
[0042] (2) The manganese zinc ferrite precursor is added into a high temperature furnace, and the temperature of the high temperature furnace is raised to 350°C at a rate of 3°C / min, kept at this temperature for 2 hours, and then kept at 900°C for 4 hours. After natural cooling, ultrafine manganese zinc ferrite powder is obtained.
[0043] Example 4
[0044] (1) Add 8 mmol of FeCl3, 2 mmol of MnCl2, 2 mmol of ZnCl2 and deionized water to a reaction flask, stir and disperse, add 0.2 mmol of dispersant oleic acid under nitrogen protection, stir at 40 ° C for 10 min, add ammonia water to control the pH of the system at 9, then add 0.02 mmol of coprecipitant ammonium oxalate dropwise, stir and disperse, place the mixed solution in an ultrasonic generator with a power of 300 W, ultrasonically assist at 35 ° C for 40 min, filter, wash the filter cake with ethanol and deionized water, and obtain a manganese zinc ferrite precursor after drying.
[0045] (2) The manganese zinc ferrite precursor is added into a high temperature furnace, and the temperature of the high temperature furnace is raised to 500°C at a rate of 5°C / min, kept at this temperature for 2 hours, and then kept at 900°C for 3 hours. After natural cooling, ultrafine manganese zinc ferrite powder is obtained.
[0046] Particle size test: Powder particle size test is carried out using a laser particle size analyzer.
[0047] Magnetic property test: A vibrating sample magnetometer is used to test the saturation magnetization intensity of the sample.
[0048]
[0049] It can be seen from the test results in the above table that with the increase of ultrasonic power, the particle size of manganese-zinc ferrite gradually decreases. When the ultrasonic power of Example 2 is 130W, the average particle size is 10.35nm, indicating that the ultrafine powder prepared by the ultrasonic method combined with the co-precipitation method has a small particle size and meets the requirements of nanoparticles; this is because the impact effect and cavitation effect of ultrasound can crush the precipitate and refine the grains, so that the generation rate of crystal nuclei during the precipitation process is greatly improved, thereby making the particle size of the precipitate smaller; and a large number of bubbles will be generated in the ultrasonic-assisted process, and these bubbles will adhere to the surface of the precipitate to reduce the surface energy of the precipitate, which makes the aggregation of crystal nuclei more difficult and reduces the agglomeration of particles; the average particle size of Example 3 is 11.21nm, the saturation magnetization intensity is 77.45emu / g, and the comprehensive performance is excellent, so the subsequent sample preparation is carried out with a microwave power of 210W.
[0050] Example 5
[0051] S1. Add 2 g of manganese zinc ferrite ultrafine powder (prepared by Example 3), 200 mL of a mixed solvent of ethanol and 200 mL of deionized water into a reaction bottle, stir evenly, add 3 g of KH550, stir to react, react at 70 ° C for 5 h, filter, wash with acetone and deionized water, and dry to obtain modified manganese zinc ferrite ultrafine powder.
[0052] S2. Add 1 mmol zinc sulfate, 2 mmol ammonium carbonate and deionized water to a reaction bottle, stir evenly at room temperature, add 0.02 g dispersant polyethylene glycol, stir at 25°C for 12 h, then place the mixed solution in a tubular furnace, and heat to 450°C at a heating rate of 5°C / min in a nitrogen atmosphere, react at a constant temperature for 8 h, and obtain porous spherical zinc oxide after natural cooling.
[0053] S3. Add 1 g of modified manganese zinc ferrite ultrafine powder, 2 g of porous spherical zinc oxide and ethanol into a reaction bottle, stir and disperse, add 0.2 g of oxidized carbon nanotubes, ultrasonically disperse at 30°C for 30 min, deionize and wash, and dry to obtain a manganese zinc ferrite ultrafine powder absorbing material.
[0054] Example 6
[0055] S1. Add 5 g of manganese zinc ferrite ultrafine powder (prepared by Example 3), 500 mL of ethanol and 500 mL of deionized water into a reaction bottle, stir evenly, add 4.5 g of KH550, stir to react, react at 80 ° C for 4 h, filter, wash with acetone and deionized water, and dry to obtain modified manganese zinc ferrite ultrafine powder.
[0056] S2. Add 3 mmol zinc sulfate, 8 mmol ammonium carbonate and deionized water to the reaction bottle, stir evenly at room temperature, add 0.06 g dispersant polyethylene glycol, stir at 20 ° C for 16 hours, and then place the mixed solution in a tubular furnace, and heat it to 500 ° C at a heating rate of 8 ° C / min in a nitrogen atmosphere. React at a constant temperature for 10 hours, and obtain porous spherical zinc oxide after natural cooling.
[0057] S3. Add 1 g of modified manganese zinc ferrite ultrafine powder, 3 g of porous spherical zinc oxide and ethanol into a reaction bottle, stir and disperse, add 0.15 g of oxidized carbon nanotubes, ultrasonically disperse at 25°C for 40 min, deionize and wash, and dry to obtain a manganese zinc ferrite ultrafine powder absorbing material.
[0058] Example 7
[0059] S1. Add 10 g of manganese zinc ferrite ultrafine powder (prepared by Example 3), 1000 mL of a mixed solvent of ethanol and 1000 mL of deionized water into a reaction bottle, stir evenly, add 8 g of KH550, stir to react, react at 65 ° C for 8 h, filter, wash with acetone and deionized water, and dry to obtain modified manganese zinc ferrite ultrafine powder.
[0060] S2. Add 1 mmol zinc sulfate, 3 mmol ammonium carbonate and deionized water to a reaction bottle, stir evenly at room temperature, add 0.025 g dispersant polyethylene glycol, stir at 35 ° C for 15 hours, and then place the mixed solution in a tubular furnace, and heat it to 400 ° C at a heating rate of 6 ° C / min in a nitrogen atmosphere, react at a constant temperature for 6 hours, and obtain porous spherical zinc oxide after natural cooling.
[0061] S3. Add 1 g of modified manganese zinc ferrite ultrafine powder, 4 g of porous spherical zinc oxide and ethanol into a reaction bottle, stir and disperse, add 0.1 g of oxidized carbon nanotubes, ultrasonically disperse at 30°C for 35 min, deionize and wash, and dry to obtain a manganese zinc ferrite ultrafine powder absorbing material.
[0062] Comparative Example 1
[0063] 2 g of porous spherical zinc oxide and ethanol were added to a reaction bottle, stirred and dispersed, 0.2 g of oxidized carbon nanotubes were added, ultrasonically dispersed at 30° C. for 30 min, washed with deionizers, and dried to obtain an absorbing material.
[0064] Comparative Example 2
[0065] Add 1 g of modified manganese zinc ferrite ultrafine powder and ethanol into a reaction bottle, stir and disperse, add 0.2 g of oxidized carbon nanotubes, ultrasonically disperse at 30° C. for 30 min, wash with deionizer, and dry to obtain an absorbing material.
[0066] Comparative Example 3
[0067] 1 g of modified manganese-zinc ferrite ultrafine powder, 2 g of porous spherical zinc oxide and ethanol were added into a reaction bottle, ultrasonically dispersed at 30° C. for 30 min, washed with deionizers, and dried to obtain a wave absorbing material.
[0068] Comparative Example 4
[0069] In this comparative example, the porous spherical zinc oxide prepared in Example 5 alone constitutes the absorbing material.
[0070] Comparative Example 5
[0071] In this comparative example, the oxidized carbon nanotubes alone constitute the absorbing material.
[0072] Comparative Example 6
[0073] In this comparative example, the modified manganese-zinc ferrite ultrafine powder prepared in Example 5 is used alone to form the absorbing material.
[0074] Wave absorption performance test: The samples prepared in Examples 5-7 and Comparative Examples 1-6 were respectively mixed with paraffin wax at a mass ratio of 7:3 to prepare circular samples with an outer diameter of 10 mm, an inner diameter of 5 mm, and a height of 2 mm. The wave absorption performance of the materials in the frequency range of 2-18 GHz was tested using a network analyzer.
[0075] .
[0076] Reflection loss refers to the ratio of the energy lost when electromagnetic waves are reflected on the surface of a material to the incident energy. The smaller the reflection loss, the stronger the material's ability to absorb electromagnetic waves. It can be seen from the test data in the above table that the reflection loss values of Examples 5-7 are in the range of -32.3 to -46.5 dB, and the wave absorption performance is good. This is because the modified manganese zinc ferrite ultrafine powder, porous spherical zinc oxide and oxidized carbon nanotubes all have wave absorption performance: the modified manganese zinc ferrite ultrafine powder has a large specific surface area and nanometer size. The reduction in particle size increases the roughness of the material surface, which is beneficial to the attenuation of microwaves. At the same time, the surface atoms lack coordination and the number of dangling bonds increases, so that interface polarization and multiple scattering become important wave absorption channels; the porous spherical zinc oxide has a rich pore structure and an antenna-like structure, and the charge gathers at the needle tip to form multiple polarization centers, which causes the electromagnetic waves to be dispersed and reflected, and the microwave receiving ability is enhanced; the carbon nanotube cavity is small and narrow, and the capillary effect is strong. The magnetic particles can be sucked into the cavity and densely arranged, resulting in a certain magnetic loss, thereby having microwave absorption performance, and the three are combined to produce a synergistic wave absorption effect.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an absorbing material from ultrafine manganese-zinc ferrite powder, characterized in that: S1. Add a mixed solvent of manganese zinc ferrite ultrafine powder, ethanol and deionized water into a reaction bottle, stir evenly, add KH550, stir to react, filter after the reaction is completed, wash with acetone and deionized water, and dry to obtain modified manganese zinc ferrite ultrafine powder; S2. Add zinc sulfate, ammonium carbonate and deionized water to a reaction bottle, stir evenly at room temperature, add dispersant polyethylene glycol, stir at 20-35°C for 8-16h, then place the mixed solution in a tube furnace, heat to 400-500°C at a heating rate of 4-8°C / min in a nitrogen atmosphere, react at a constant temperature for 5-10h, and naturally cool to obtain porous spherical zinc oxide; S3, adding modified manganese zinc ferrite ultrafine powder, porous spherical zinc oxide and ethanol to a reaction bottle, stirring and dispersing, adding oxidized carbon nanotubes, ultrasonically dispersing at 20-35° C. for 20-40 min, deionizing washing, and drying to obtain manganese zinc ferrite ultrafine powder absorbing material; The preparation process of the manganese-zinc ferrite ultrafine powder is: (1) Add FeCl3, MnCl2, ZnCl2 and deionized water to a reaction bottle, stir and disperse, add dispersant oleic acid under nitrogen protection, stir at 40-60°C for 10-30 minutes, add ammonia water to control the pH of the system to 7-9, then dropwise add a coprecipitant, stir and disperse, place the mixed solution in an ultrasonic generator, and perform an ultrasonic-assisted reaction. After the reaction is completed, filter, wash the filter cake with ethanol and deionized water, and dry to obtain a manganese zinc ferrite precursor; (2) adding the manganese zinc ferrite precursor into a high temperature furnace, raising the temperature of the high temperature furnace to 350-500°C at a rate of 3-5°C / min, maintaining the temperature for 1-2 hours, and then maintaining the temperature at 800-900°C for 2-4 hours. After natural cooling, ultrafine manganese zinc ferrite powder is obtained; In step (1), the ratio of FeCl3, MnCl2, ZnCl2, oleic acid and coprecipitant is: 4 mol: 1 mol: 1 mol: 0.1-0.35 mol: 0.01-0.03 mol; in step (1), the coprecipitant is any one of ammonium oxalate and ammonium bicarbonate; in step (1), the power of the ultrasonic generator is 50-300 W, the ultrasonic auxiliary temperature is 30-45° C., and the time is 10-50 min; In step S1, the ratio of ultrafine manganese zinc ferrite powder and KH550 is: 1g:0.5-1g; the reaction temperature in step S1 is 60-80°C, and the reaction time is 4-8h; in step S2, the ratio of zinc sulfate, ammonium carbonate and polyethylene glycol is: 1mol:1-3mol:15-25g.
2. The method for preparing an absorbing material from ultrafine manganese-zinc ferrite powder according to claim 1, characterized in that: In step S3, the ratio of modified manganese zinc ferrite ultrafine powder, porous spherical zinc oxide, and oxidized carbon nanotubes is: 1g: 1-5g: 0.05-0.25g.
Citation Information
Patent Citations
Method for preparing manganese zinc ferrite-coated carbon nano tube magnetic material
CN101834044A
Preparation method of coaxial cable structure MWCNT / Fe3O4 / ZnO / PANI microwave absorbant
CN103113580A
Method for preparing porous zinc oxide with three-dimensional structure
CN105565366A
Wave-absorbing material compounded by barium ferrite and carbon nanotubes and preparation method thereof
CN109850950A
Preparation method of centimeter wave / millimeter wave compatible broadband composite wave-absorbing material
CN114956033A