A 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod and a manufacturing method thereof

Through the design of high C-Si-Mn-Al-Cr composition and online salt bath strong tempering technology, combined with roller slow cooling, the problems of high material cost, high abnormal tissue risk and complex process in the manufacturing of 15.9-level fasteners are solved. The manufacturing of 15.9-level fastener strips with high plasticity and high material yield is achieved, and the process flow is simplified.

CN118639122BActive Publication Date: 2024-11-19JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411125830.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The prior art is difficult to effectively manufacture high-strength cold-headed steel strips required for grade 15.9 fasteners, which have problems such as high material cost, high risk of abnormal structure, insufficient plasticity and complex processes, especially when avoiding annealing process.

Method used

Using high C-Si-Mn-Al-Cr composition design, combined with online salt bath strong tempering and roller slow cooling technology, the microstructure of the control strip is tempered pearlite and tempered cortexite, and is rolled through high temperature The silk making and spinning process shortens the residence time of the mesh carbon area, uses the high-speed heat exchange ability of molten salt to perform isothermal diffusion phase transformation, and regulates the strong plasticity performance of the matrix.

Benefits of technology

It significantly improves the plasticity and material yield of the strip, reduces the risk of cold work cracking, simplifies the manufacturing process, and achieves the performance level of 15.9 fasteners while saving annealing process, reducing material costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639122B_ABST
    Figure CN118639122B_ABST
Patent Text Reader

Abstract

The invention relates to a 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. The invention discloses a 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod ... 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod is designed to perform online salt bath strong tempering after hot-rolling wire laying into a wire rod based on a high C-Si-Mn-Al-Cr component. The molten salt circulation amount at the front end is controlled to be greater than the molten salt circulation amount at the rear end. The wire rod is cooled to a pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation. The wire rod is controlled to form a troostite structure and a pearlite structure and promote tempering softening. The troostite structure is mainly tempered pearlite and a small amount of tempered troostite, ferrite and fused pearlite are slowly cooled by a roller. The 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod is prepared. The 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod is capable of reducing material cost, avoiding abnormal structures, realizing wire rod structure regulation and matching of strength and plasticity. The 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod has a tensile strength of 1115-1165MPa and a cross-sectional shrinkage of 47%-52%. The 15.9-grade annealing-free fastener is suitable for efficient and green manufacturing. The annealing-free fastener is beneficial to reducing the risk of
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and specifically relates to a 15.9-grade annealing-free hot-rolled high-carbon cold-heading steel wire rod and a manufacturing method thereof. Background Art

[0002] At present, cold heading steels for fasteners of grade 8.8 to 12.9 are widely used, and are generally designed with low carbon, medium carbon and alloying components. In view of the excellent room temperature cold processing performance of cold heading steel, it is often used to make screws, bolts, nuts, self-tapping screws, wall nails and other fasteners. There is an application demand for fasteners with higher strength grades, such as cold heading steel for fasteners of grade 15.9 with tensile strength ≥1500MPa and yield strength ratio ≥0.9. Cold heading steel for fasteners of higher strength grades is often improved by adding a large amount of high hardenability elements, for example:

[0003] Patent CN114058974B discloses a 15.9-grade corrosion-resistant high-strength bolt steel and its production method and heat treatment method. Based on the C-Si-Mn-Cr-Mo-V-Nb-Ti-B-Ni-Cu-Al composition design, the steel is rolled into square billets and then rolled into bars, and then slowly cooled on a cooling bed to obtain a hot-rolled structure of pearlite + ferrite. After the steel is subjected to deformation heat treatment and high-frequency tempering heat treatment, it is adjusted to tempered troostite + dispersed precipitated fine carbides. The 15.9-grade fasteners are processed by annealing → drawing → warm forging → heat treatment → coating. However, in order to achieve lower cost, greener and more efficient 15.9-grade fastener manufacturing, the following problems and technical difficulties still exist:

[0004] (1) In order to achieve the high strength performance level of 15.9 grade fasteners after quenching and tempering heat treatment after cold heading, a large amount of strong hardenability components such as Mn, Cr, Mo and micro-alloy components such as V, Ti, Nb are added to the steel. However, this also brings about the problem that the high hardenability causes an increased risk of abnormal structure during controlled cooling after rolling, and the difficulty of improving plasticity increases. In order to reduce the risk of brittle fracture during wire rod manufacturing and cracking during fastener processing caused by abnormal structure precipitation:

[0005] One situation is that steel is forged or rolled to obtain blanks or bars with larger diameters to avoid the formation of martensite or bainite hard and brittle phases during the Stelmor wire controlled cooling process after rolling in high-wire manufacturing, which in turn causes brittle fracture of coils and adverse effects on yield. This makes it difficult to directly obtain wire rods with smaller diameters by rolling under this process, which is more suitable for the manufacture of fasteners with larger specifications. The manufacture of fasteners with smaller specifications is more difficult or requires more processes.

[0006] Another situation is that the steel adopts low-temperature rolling and insulation cooling to obtain pearlite with larger interlamellar spacing + ferrite soft phase structure with a relatively large proportion, so as to reduce the risk of abnormal tissue precipitation and improve the plasticity of wire rod. However, the stress and dislocation density of the formed pearlite structure are relatively large, and the improvement of the plasticity of wire rod is limited. Increasing the soft phase composition will also excessively deteriorate the strength and drawing performance of wire rod. After that, it is necessary to increase the strength by increasing the surface reduction rate to achieve the strength requirement before quenching and tempering. The loss of plasticity in the process is large, which increases the risk of wire breakage during drawing and cracking during cold heading. For further deformation heat treatment and high-frequency tempering heat treatment of the hot-rolled structure of pearlite + ferrite, it is necessary to raise the cold bar to the austenitizing temperature for further heat treatment, which brings many processes, high energy consumption and cost, affects production efficiency, and is not enough to directly obtain high-plasticity materials. Downstream users also need to further anneal the hot-rolled raw materials after material formation to improve the deformation performance of the bars, which brings energy consumption, cost and efficiency pressure to fastener manufacturing.

[0007] (2) In addition to the increase in process difficulty and process flow, the addition of a large amount of high hardenability elements and micro-alloy components also leads to a significant increase in the cost of steel raw materials. The cheaper high-carbon steel is limited by the cooling control capacity of the Stelmor cooling line after rolling and is not enough to meet the demand for 15.9 grade annealing-free hot-rolled cold heading steel wire rod. The reasons are:

[0008] The existing high-carbon steel used for drawing manufacturing mainly improves the drawing performance by increasing the troostite content in the organization. It will be combined with the heat preservation or low-speed cooling process after wire drawing to extend the incubation time of the wire rod in the troostite phase region to increase the troostite content in the organization. This is also to avoid the excessive difference in air volume and temperature difference on the wire rod surface caused by the increase in air cooling intensity after wire drawing, so as to reduce the risk of abnormal bainite or martensite organization. However, too low a cooling rate will cause the high-temperature wire rod after wire drawing to stay in the secondary cementite precipitation zone for a long time, forming a higher level of network carbide, which seriously deteriorates the plastic toughness of the wire rod. The annealing process cannot be omitted and it is difficult to eliminate the residual network carbide by annealing, causing the risk of cracking during the cold heading process.

[0009] In order to reduce the risk of carbon precipitation in the spinning stage caused by low-temperature spinning, the spinning temperature is appropriately increased. At the same time, in order to reduce the risk of precipitation of hard and brittle abnormal tissues, a heat preservation process is adopted after spinning into wire rods, which not only prolongs the online time of the wire rods, but also is limited by the low insulation cooling rate and the online time should not be too long to affect the production efficiency. Therefore, the spinning temperature cannot be too high, and it is difficult to obtain a large degree of supercooling. The spacing between the troostite lamellae is large, which is not conducive to the drawing performance, and the matrix strength is difficult to control. Although the insulation cooling rate is relatively low, the wire rod is still in a continuous cooling state. The wire rod is in a low temperature state after the troostite phase transformation. The coarsening of cementite also increases the difficulty of softening, making the final dislocation density of the troostite structure high, and the plasticity of the wire rod is difficult to improve, and it is difficult to avoid annealing processing, which will also increase the risk of cracking in the cold heading process. Summary of the invention

[0010] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 15.9-grade annealing-free hot-rolled high-carbon cold heading steel wire rod and a manufacturing method thereof, which can utilize high carbon components to reduce material costs, avoid abnormal structures, achieve wire rod structure regulation and strength-plasticity matching, significantly improve wire rod plasticity, simplify the manufacturing method, and is suitable for efficient and green manufacturing of 15.9-grade fasteners that eliminates the annealing process, which is beneficial to reducing the risk of cold working cracking and improving the yield rate.

[0011] The technical solution adopted by the present invention to solve its technical problem is:

[0012] A 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.82%-0.86%, Si: 0.30%-0.45%, Mn: 0.22%-0.42%, Al: 0.10%-0.30%, Cr: 0.15%-0.35%, P≤0.015%, S≤0.015%, the rest is Fe and unavoidable impurities, and its microstructure includes tempered pearlite accounting for 74%-80% by volume, tempered troostite accounting for 14%-20% by volume, and the rest is a mixed structure consisting of ferrite and fused pearlite.

[0013] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:

[0014] (1) Carbon: As the most economical and effective element for solid solution strengthening and precipitation strengthening, C is the main added element in the present invention to ensure the matrix strength and high hardenability of steel. However, it also increases the decarburization sensitivity and the risk of cementite distribution along the grain boundaries. If the C content is too high, the cementite lamellae will be thicker, which will increase the difficulty of cementite melting and tempering softening, and is not conducive to the control of matrix structure. Therefore, in order to ensure the cold deformation performance of cold heading steel wire rod and meet the final performance level requirements of 15.9 grade fasteners, the mass percentage of C is controlled to be 0.82%~0.86%.

[0015] (2) Silicon: Si is the main deoxidizing element in steel and can be dissolved in austenite to increase the strength of steel. It can inhibit grain coarsening in the early stage of online salt bath strong tempering, which is beneficial to sorbite nucleation and tempering softening. However, excessive silicon will increase non-metallic inclusions and impurity element segregation, increase carbon diffusion in steel, aggravate decarburization of steel, and significantly increase cold heading deformation resistance, which is not conducive to cold heading and cold extrusion. Therefore, the mass percentage of Si is controlled to be 0.30%~0.45%.

[0016] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. As a solid solution strengthening element, it can improve the strength and hardenability of steel. However, too high Mn content will aggravate the segregation during the solidification process of the steel billet, reduce the activity of carbon and the diffusion rate of carbon, increase the difficulty of spheroidizing tempering softening and controlled cooling structure control, and cause deformation resistance. Too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.22%~0.42%.

[0017] (4) Aluminum: Al acts as a deoxidizer during the smelting process, which can reduce the number of non-metallic inclusions in steel. It forms fine precipitates during hot rolling, which is beneficial to inhibit the coarsening of cementite and refine the thickness of cementite lamellae. This is beneficial to the melting of cementite lamellae at high temperature after online salt bath strong tempering, thereby improving the impact toughness of steel and reducing the tendency to cold brittleness. However, too high Al content will promote graphitization of steel and increase the risk of decarburization. Therefore, the mass percentage of Al is controlled to be 0.22%~0.42%.

[0018] (5) Chromium: As a solid solution strengthening element, Cr can greatly improve the hardenability of the material and regulate the matrix phase composition. After online salt bath intensive tempering, fine dispersed carbide particles are precipitated to improve the material strength. However, if the Cr content is too high, the temper brittleness tendency and low-temperature microstructure risk of the steel will increase, making it more difficult to improve plasticity. The precipitation and coarsening of Cr will also significantly deteriorate the strength and plasticity of the wire rod. Therefore, the mass percentage of Cr is controlled to be 0.15%~0.35%.

[0019] (6) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0020] In a preferred embodiment, the interlamellar spacing of the tempered pearlite is 165~205nm, the interlamellar spacing of the tempered bainite is 90~130nm, and the volume percentage of the ferrite is ≤5%. The smaller the interlamellar spacing of the tempered pearlite and the tempered bainite, the higher the strength of the wire rod and the lower the plasticity. The higher the proportion of tempered pearlite and the increase in interlamellar spacing are accompanied by an increase in the ferrite content, the lower the strength of the wire rod and the higher the plasticity.

[0021] The above-mentioned cold heading steel wire rod adopts a high C-Si-Mn-Al-Cr composition design, replacing the addition of strong hardenability elements and micro-alloying elements with lower-priced carbon elements, and has lower Mn and Cr alloy contents, and does not contain expensive Mo, Ti, Nb, V, B and other elements, so that the composition system can meet the 15.9 grade fastener performance level after drawing, cold heading and tempering, reducing material costs, and cooperates with tempered pearlite and tempered troostite in the microstructure to provide matrix strength. The pearlite structure has a coarser interlamellar spacing than the troostite structure, higher plasticity than the troostite, and better strength than the ferrite. After tempering and melting and transforming to spheroidized structure into tempered pearlite and fused pearlite, the moderate strength characteristics of pearlite can be retained, so that the organizational stress and dislocation density are further reduced, and the plasticity is further improved. The tempered pearlite accounts for a large proportion, accompanied by a very small amount of unavoidable soft phase ferrite. The troostite structure has finer interlamellar spacing than the pearlite structure and better plasticity than the hard-brittle phase structure of bainite and martensite. After tempering and transforming into tempered troostite from spheroidized structure, the higher strength of troostite can be retained, so that the dislocation density of troostite group is further reduced, the plasticity is improved, and the drawing hardening is effectively reduced. Compared with the existing hot-rolled wire rod structure of pearlite + ferrite, the excessive deterioration of the strength of the wire rod can be avoided. Compared with the existing hot-rolled structure containing bainite or martensite or high troostitization rate, it has significantly improved plasticity and toughness, which makes up for the adverse effects of high carbon component system on the plasticity and cold deformation properties of wire rod, and thus can improve the yield rate. Smaller wire rods can be obtained quickly and directly through rolling, which reduces the manufacturing difficulty of small-sized fasteners. 15.9-grade fasteners are manufactured by cold heading under annealing-free process to reduce the risk of cracking.

[0022] In a preferred embodiment, the network carbide of the cold heading steel wire rod is level 0, which can eliminate the uncontrollable deterioration factors caused by the network carbide, enhance the strengthening effect of the carbon element, and reduce the risk of cracking.

[0023] In a preferred embodiment, the diameter of the cold heading steel wire rod is 12.0~26.0mm, the tensile strength is 1115~1165MPa, and the cross-sectional shrinkage rate is 47%~52%. The cold heading steel wire rod has high tensile strength and significantly increased cross-sectional shrinkage rate, and can achieve the performance level of 15.9 fasteners through drawing, cold heading and tempering heat treatment without annealing process.

[0024] A method for manufacturing a 15.9 grade annealing-free hot-rolled high-carbon cold-heading steel wire rod, the manufacturing method comprising:

[0025] The wire rod is produced by rolling the chemical composition of the 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to any one of the above items, and after the wire rod is spun into a wire rod at a spinning temperature of ≥960°C, it is subjected to online salt bath strong tempering, and the front end molten salt circulation amount of the online salt bath strong tempering is controlled to be greater than the rear end molten salt circulation amount, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and the wire rod is controlled to form troostite and pearlite structures, and the tempering and softening of the troostite and pearlite structures are promoted at the same time, and finally it is slowly cooled by a roller to obtain a cold heading steel wire rod with a microstructure including 74% to 80% tempered pearlite by volume, 14% to 20% tempered troostite by volume, and the rest is a mixed structure composed of ferrite and fused pearlite.

[0026] The manufacturing method adopts a relatively high spinning temperature, which can make the wire rod austenitized and avoid the precipitation of secondary cementite in the spinning stage. Compared with slow cooling methods such as insulation cooling, online salt bath strong tempering is directly carried out after spinning, which can utilize the high heat exchange capacity of molten salt to control the cooling of the wire rod at a cooling rate significantly higher than the upper limit of the air cooling intensity of 10°C / s. On the one hand, it can quickly skip the precipitation temperature range of secondary cementite and tertiary cementite, avoid the generation of network carbides and deteriorate the mechanical properties of high carbon steel wire rod, especially the plasticity and toughness, and improve the utilization of carbon; on the other hand, the significant increase in cooling rate It also breaks the previous restriction that the spinning temperature cannot be increased due to the online time being too long. A higher spinning temperature can be used, and the molten salt circulation volume at the front end is larger than that at the back end to form a greater degree of supercooling, so that the wire rod can quickly enter the pearlite phase region for isothermal diffusion phase transformation, and the austenite structure of the wire rod is controlled to form a troostite structure with finer interlamellar spacing. Moreover, since the wire rod can pass through the molten salt when passing through the molten salt, the molten salt is evenly coated on the surface of the wire rod, and there is no problem of wind volume difference and temperature difference between the windward side and the leeward side of the wire rod under the strong air cooling process. It can also avoid the wire rod entering the bainite phase region and producing abnormal bainite structure.

[0027] The molten salt circulation volume at the rear end of the online salt bath strong tempering is smaller than that at the front end, which can appropriately reduce the supercooling degree and control the untransformed high-temperature austenite to enter the pearlite phase region for isothermal phase transformation. This allows the wire rod to achieve phase transformation control of troostite and pearlite in an online salt bath strong tempering process, simplifying the process. At the same time, due to the high heat exchange effect, the wire rod can be kept consistent with the molten salt temperature, rather than the continuous cooling of the existing insulation treatment. This allows the wire rod to remain in a high temperature state after the phase transformation is completed. With a longer high-temperature isothermal process, the troostite is promoted to transform into spheroidized troostite and reduce the dislocation density. Al is used to refine the thickness of the cementite lamellae, promote the melting of the pearlite cementite lamellae into fused pearlite, and the pearlite is transformed into a spheroidized structure to form tempered pearlite, reduce the organizational stress and dislocation density, avoid the precipitation and coarsening of Cr, and regulate the strength and plasticity of the matrix.

[0028] After the online salt bath strong tempering, the wire rod undergoes a full phase change in its structure, and also avoids the abnormal structure in the roller slow cooling stage. After the online salt bath strong tempering treatment, the wire rod is in a high temperature state. The roller slow cooling can be used to continue the softening effect of the wire rod in the high temperature state with low-speed cooling, further promoting the softening of the structure and plasticity improvement. Compared with directly extending the time of online salt bath strong tempering, it can also save energy. Finally, a structure mainly composed of tempered pearlite, a small amount of tempered troostite, ferrite and fused pearlite, without bainite and martensite is obtained, realizing structure regulation and strong plasticity matching, which can be smoothly coiled to avoid brittle fracture and improve the material quality. Compared with the existing process, it no longer needs to be reheated and heat treated or annealed before being transported to the downstream for unwinding and drawing, so that the manufacturing process of wire rods and fasteners can be simplified and emissions can be reduced efficiently.

[0029] In a preferred embodiment, during the rolling, the heating furnace temperature is controlled to be ≤1155°C before rolling, the soaking time is 3-4h, and the time in the furnace is ≤6h. A higher heating furnace temperature and a longer soaking time are selected to promote uniform composition of the billet, so that high temperature rolling can be quickly entered, while avoiding the risk of burning and decarburization on the billet surface caused by too long time in the furnace.

[0030] Since the limitation of the existing low-temperature wire spinning on the demand for low-temperature rolling is broken, in a preferred embodiment, high-temperature rolling is adopted during the rolling, the initial rolling temperature is controlled to be 1085~1125℃, and the initial rolling reduction is 33%~38%. The use of a higher initial rolling temperature can reduce the deformation resistance of the steel billet and the wear on the rolling mill, increase the rolling speed, and cooperate with a larger initial rolling reduction to improve the interface bonding strength and refine the original austenite grains.

[0031] In a preferred embodiment, during the rolling, the final rolling temperature is controlled to be ≤1000°C, and the final rolling reduction is 32%~42% to avoid the final rolling temperature being too high to make the austenite grains coarse. A larger final rolling reduction is used to increase the nucleation rate, promote dynamic recrystallization, and avoid the aggravation of local stress concentration.

[0032] In a preferred embodiment, the molten salt temperature of the online salt bath strong tempering is 590~625℃, and the processing time is 490~740s. The lower the molten salt temperature, the finer the interlamellar spacing of the troostite and pearlite tissues formed by the phase transformation, the higher the matrix strength and the lower the plasticity, which is beneficial to melting and transforming the spheroidized tissue into the tempered state for softening. However, if the molten salt temperature is too low, the proportion of tempered troostite increases, which is not conducive to improving the plasticity of the wire rod, and even produces abnormal bainite tissue and significantly increases the brittleness of the wire rod. On the contrary, the higher the molten salt temperature, the larger the interlamellar spacing of the troostite and pearlite formed by the phase transformation, the higher the proportion of ferrite, the lower the matrix strength and the higher the plasticity, which can provide more thermal power for matrix softening. However, if the molten salt temperature is too high, it is difficult to form a large degree of supercooling, which is not conducive to the formation of troostite with finer interlamellar spacing and the inhibition of network carbon, and more ferrite is produced, resulting in matrix strength and The drawing performance decreases; the longer the treatment time, the better the tempering and softening effect after the phase transformation is completed, the lower the organizational stress and dislocation density of the tempered troostite and tempered pearlite, the wire rod strength decreases and the plasticity increases, but if the treatment time is too long, there is a risk of excessive tempering and softening to lose the wire rod strength, and the precipitation and coarsening of Cr significantly reduces the strength and plasticity. On the contrary, the shorter the treatment time, the worse the tempering and softening effect, the wire rod strength increases and the plasticity decreases. If the treatment time is too short, the troostite and pearlite obtained fail to soften, the dislocation density is high, and stress concentration and drawing hardening are prone to cause wire breakage and cold heading cracking risks, which is not conducive to the elimination of the annealing process, and even insufficient phase transformation causes strength loss and even abnormal organization. Therefore, the molten salt temperature and treatment time of online salt bath strong tempering can be further controlled to regulate the proportion of tempered troostite and tempered pearlite, the interlamellar spacing and softening effect.

[0033] In a preferred embodiment, the front-end molten salt circulation volume of the online salt bath strong tempering is 600~900t / h, and the temperature rise of the front-end molten salt is controlled to be ≤10°C. The molten salt circulation pipeline can be set at the front end close to the salt bath tank to control the front-end molten salt circulation volume. A larger front-end molten salt circulation volume is selected to control the molten salt temperature rise and improve the processing accuracy, so that the wire rod can enter the phase zone with a greater degree of supercooling for isothermal diffusion phase transformation, promote a small amount of austenite structure to be transformed into a troostite structure with finer lamellar spacing, and adjust the proportion of tempered troostite.

[0034] In a preferred embodiment, the rear-end molten salt circulation volume of the online salt bath strong tempering is 200~400t / h, and the temperature rise of the rear-end molten salt is controlled to be ≤5°C. The molten salt circulation pipeline can be set at the rear end close to the salt bath tank to control the rear-end molten salt circulation volume. The smaller rear-end molten salt circulation volume is selected to control the low supercooling degree, and the temperature accuracy is further controlled, so that the untransformed high-temperature austenite enters the pearlite phase region for isothermal phase transformation and tempering softening, thereby regulating the strength and plasticity of the matrix.

[0035] In a preferred embodiment, the roller slow cooling adopts closing the insulation cover, controlling the wire rod to be cooled at a cooling rate of 0.2~0.5℃ / s, and the slow cooling time is ≥500s. The wire rod that has been subjected to online salt bath strong tempering treatment can be controlled to be slowly cooled along the roller in the insulation cover at a lower cooling rate, thereby further promoting the softening of tempered pearlite and tempered troostite and regulating the strength and plasticity of the matrix.

[0036] In a preferred embodiment, the roller slow cooling adopts the method of passing the hot air above the salt bath tank of the online salt bath strong tempering into the insulation cover, which can recycle the hot air thermal energy in the online salt bath strong tempering process, reduce the cooling speed of the wire rod for the roller slow cooling insulation, and save energy.

[0037] Compared with the prior art, the beneficial effects of the present invention are at least:

[0038] (1) Cold heading steel for fasteners with higher strength grades is often improved by adding a large amount of high hardenability elements, but this also brings about problems such as high material cost, increased risk of abnormal structure and insufficient plasticity, leading to an increased risk of cold working cracking of the material. The cold heading steel wire rod of the present invention is designed with a high C-Si-Mn-Al-Cr composition, with lower Mn and Cr alloy content, and does not contain expensive elements such as Mo, Ti, Nb, V, B, etc., which can reduce material costs. The microstructure does not contain bainite or martensite hard and brittle phases, and is mainly tempered pearlite. , a small amount of tempered troostite, ferrite and fused pearlite structure, which further reduces the organizational stress and dislocation density, significantly improves the plasticity of the wire rod, and makes up for the adverse effects of the high carbon component system on the plasticity and cold deformation properties of the wire rod, so that the strength and plasticity can be matched, thereby improving the yield rate and reducing drawing hardening, achieving a tensile strength of 1115~1165MPa and a cross-sectional shrinkage rate of 47%~52%. It can achieve the performance level of 15.9 fasteners through direct drawing, cold heading and tempering heat treatment without annealing process, and has good market application prospects.

[0039] (2) In view of the problems that the existing manufacturing process is limited by the controlled abnormal organization and it is difficult to directly obtain small-sized wire rods, the yield rate is low, the plasticity is insufficient or there are too many processes, the manufacturing method of the present invention adopts a high C-Si-Mn-Al-Cr composition design, combines online salt bath strong tempering and roller slow cooling technology, selects a higher wire drawing temperature to increase the supercooling of the wire rod in the subsequent online salt bath strong tempering treatment, and effectively shortens the residence time in the network carbon area, eliminates the uncontrollable deterioration factors of the network carbide, enhances the strengthening effect of the carbon element, and utilizes the high-speed heat exchange capacity of the molten salt. , control the wire rod to undergo isothermal diffusion phase transformation to form troostite, use a front-end molten salt circulation volume greater than a rear-end molten salt circulation volume to make the rear-end undercooling lower, control the untransformed high-temperature austenite to enter the pearlite phase region for isothermal phase transformation, and after the phase transformation is completed, temper and soften it in the subsequent long-term high-temperature isothermal process, use roller slow cooling to further soften the matrix, regulate the strength and plasticity matching of the matrix, can smoothly roll up, avoid brittle fracture, improve the material, no longer need to reheat and heat treatment or annealing, can simplify the manufacture of cold heading steel wire rods and fasteners, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0041] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0042] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0043] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0044] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0045] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.84%, Si: 0.45%, Mn: 0.22%, Al: 0.29%, Cr: 0.27%, P: 0.014%, S: 0.013%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of high temperature rolling → wire laying → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0046] The high temperature rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 22mm through a rolling line. High temperature rolling is used to increase the rolling speed, reduce the deformation resistance of the steel billet and the wear of the rolling line, and a large reduction is used to refine the original austenite grains. Specifically: the heating furnace adopts a preheating, heating, and soaking procedure with sequential temperature increases, and the heating furnace temperature is controlled to be 1150°C, the soaking time is 3h, the furnace time is 5.5h, the initial rolling temperature is 1115°C, the initial rolling reduction is 34%, the final rolling temperature is 995°C, and the final rolling reduction is 35%.

[0047] The spinning process is used to turn the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers. A higher spinning temperature is selected to increase the supercooling of the wire rods in the subsequent online salt bath strong tempering treatment and effectively shorten the residence time in the carbon mesh area. Specifically, the spinning temperature is controlled to be 970°C.

[0048] The online salt bath strong tempering adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. The molten salt circulation volume at the front end of the salt bath tank is controlled to be greater than the molten salt circulation volume at the rear end, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 39°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminating the network carbon deterioration phase caused by excessive carbon element, and improving the use value of carbon element. At the same time, a larger front end molten salt circulation volume is used to form a larger supercooling degree, which promotes a small amount of The austenite structure is transformed into a troostite structure with finer interlamellar spacing, and a smaller rear-end molten salt circulation volume is used to appropriately reduce the undercooling degree, and the untransformed high-temperature austenite is controlled to enter the pearlite phase region for isothermal phase transformation to form pearlite structure, while promoting the tempering and softening of the troostite structure and pearlite structure. Specifically: the molten salt temperature is controlled to be 615℃, the processing time is 565s, the front-end molten salt circulation volume is 700t / h, the temperature rise of the front-end molten salt is ≤10℃, the rear-end molten salt circulation volume is 250t / h, and the temperature rise of the rear-end molten salt is ≤5℃.

[0049] The roller slow cooling process adopts closing the insulation cover, conveying the wire rod from the salt bath tank into the insulation cover by rollers, passing the hot air above the salt bath tank into the insulation cover, and performing slow cooling treatment to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool at a cooling rate of 0.4°C / s, the slow cooling time is 680s, and it is cooled to 343°C; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 1 shown.

[0050] Comparative Example 1:

[0051] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of rolling → spinning → Stelmor insulation slow cooling, specifically: controlling the heating furnace temperature to 1090°C, the soaking time to 4h, the furnace time to 6h, the initial rolling temperature to 1050°C, the final rolling temperature to 950°C, the spinning temperature to 920°C, the Stelmor insulation slow cooling adopts closing all fans and insulation hoods, and conveying the wire rod with rollers, the wire rod completes phase change in the hood at a cooling rate of 1.5°C / s, and the finished wire rod is obtained after coming off the line.

[0052] Comparative Example 2:

[0053] A method for manufacturing a wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of low-temperature rolling → low-temperature wire drawing → Stelmor air cooling → insulation and slow cooling. Specifically: the low-temperature rolling controls the heating furnace temperature to 1010°C, the soaking time is 5h, the furnace time is 6.5h, the initial rolling temperature is 980°C, the final rolling temperature is 880°C, the wire drawing temperature of the low-temperature wire drawing is 850°C, the Stelmor air cooling adopts 10% opening of 1~7# fans to cool the wire rod to 690°C at a cooling rate of 2.3°C / s, the insulation and slow cooling adopts closing all fans and insulation covers to complete the phase change of the wire rod in the cover at a cooling rate of 0.9°C / s, and the finished wire rod is obtained after going offline.

[0054] Comparative Example 3:

[0055] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of rolling → spinning → Stelmor rapid cooling → roller slow cooling, specifically: controlling the heating furnace temperature to 1080°C, the soaking time to 4.5h, the furnace time to 6h, the initial rolling temperature to 1040°C, the final rolling temperature to 940°C, the spinning temperature to 910°C, the Stelmor rapid cooling adopts opening 1~6# fans at 45%, so that the wire rod is cooled to 680°C at a cooling rate of 4.5°C / s, the roller slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 0.9°C / s, and the finished wire rod is obtained after going offline.

[0056] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organizational and performance tests: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization test was conducted according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0057] Table 1. Comparison of wire rod structure and properties by different manufacturing methods

[0058]

[0059] From the comparison results of Example 1 and Comparative Example 1, it can be seen that, compared with the limitation of low insulation cooling rate, the online time should not be too long to affect the production efficiency, the spinning temperature cannot be too high. Although the troostite structure can be obtained under insulation cooling, the level of network carbide is relatively high. The wire rod is in a low temperature state after the troostite phase transformation, the dislocation density is relatively high, and the plasticity of the wire rod is difficult to improve. The present invention can reduce the material cost by utilizing high carbon components, and combines online salt bath strong tempering and roller slow cooling technology to eliminate the uncontrollable deterioration factors of the network carbide, enhance the strengthening effect of the carbon element, and realize tempering softening in a long-term high-temperature isothermal process, which can improve the yield rate and reduce drawing hardening.

[0060] From the comparison results of Example 1 and Comparative Example 2, it can be seen that although the grains are refined compared with low-temperature rolling and spinning, the improvement of the network carbide is limited due to the reduction of the risk of precipitation of hard and brittle abnormal tissues. At the same time, the pearlite tissue formed has large stress and dislocation density, and the improvement of the plasticity of the wire rod is limited. Increasing the soft phase composition will also excessively deteriorate the strength and drawing performance of the wire rod. The present invention controls the wire rod to undergo isothermal diffusion phase transformation to form troostite, and cooperates with the tempered pearlite and tempered troostite in the microstructure to provide matrix strength, enhance the strengthening effect of the carbon element, and regulate the matrix strength-plasticity matching.

[0061] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with the risk of abnormal tissue precipitation under accelerated cooling rate, which in turn causes adverse effects on coil brittle fracture and yield rate, the present invention avoids the wire rod entering the bainite phase region to produce bainite abnormal tissue, has no bainite and martensite tissue, has significantly improved plasticity and toughness, compensates for the adverse effects of the high carbon component system on the plasticity and cold deformation properties of the wire rod, and thus can improve the yield rate, quickly and directly obtain smaller wire rods through rolling, and reduce the difficulty of manufacturing small-sized fasteners. Embodiment 2:

[0062] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.82%, Si: 0.3%, Mn: 0.31%, Al: 0.1%, Cr: 0.32%, P: 0.015%, S: 0.013%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of high temperature rolling → wire laying → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0063] The high temperature rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 12mm through a rolling line. High temperature rolling is used to increase the rolling speed, reduce the deformation resistance of the steel billet and the wear of the rolling line, and a large reduction is used to refine the original austenite grains. Specifically: the heating furnace adopts a preheating, heating, and soaking procedure with sequential temperature increases, and the heating furnace temperature is controlled to be 1140°C, the soaking time is 3h, the furnace time is 5h, the initial rolling temperature is 1080°C, the initial rolling reduction is 38%, the final rolling temperature is 985°C, and the final rolling reduction is 42%.

[0064] The spinning process is used to turn the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers. A higher spinning temperature is selected to increase the supercooling of the wire rods in the subsequent online salt bath strong tempering treatment and effectively shorten the residence time in the carbon mesh area. Specifically, the spinning temperature is controlled to be 960°C.

[0065] The online salt bath strong tempering adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. The molten salt circulation volume at the front end of the salt bath tank is controlled to be greater than the molten salt circulation volume at the rear end, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 41°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminating the network carbon deterioration phase caused by excessive carbon element, and improving the use value of carbon element. At the same time, a larger front end molten salt circulation volume is used to form a larger supercooling degree, which promotes a small amount of The austenite structure is transformed into a troostite structure with finer interlamellar spacing, and a smaller rear-end molten salt circulation volume is used to appropriately reduce the undercooling degree, and the untransformed high-temperature austenite is controlled to enter the pearlite phase region for isothermal phase transformation to form pearlite structure, while promoting the tempering and softening of the troostite structure and pearlite structure. Specifically: the molten salt temperature is controlled to be 590℃, the processing time is 740s, the front-end molten salt circulation volume is 900t / h, the temperature rise of the front-end molten salt is ≤10℃, the rear-end molten salt circulation volume is 400t / h, and the temperature rise of the rear-end molten salt is ≤5℃.

[0066] The roller slow cooling process adopts closing the insulation cover, conveying the wire rod from the salt bath tank into the insulation cover by rollers, passing the hot air above the salt bath tank into the insulation cover, and performing slow cooling treatment to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool at a cooling rate of 0.2°C / s, the slow cooling time is 990s, and it is cooled to 392°C; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 2 shown.

[0067] Comparative Example 4:

[0068] A method for manufacturing a wire rod, which differs from Example 2 in that the heating furnace temperature is controlled to be 1090°C, the soaking time is 4 hours, the furnace time is 6 hours, the initial rolling temperature is 1050°C, the final rolling temperature is 950°C, and the spinning temperature is 920°C. The online salt bath strong tempering controls the wire rod to be cooled at a cooling rate of 35°C / s to the pearlite phase region for isothermal phase transformation, and the finished wire rod is obtained after it comes off the line.

[0069] Comparative Example 5:

[0070] A method for manufacturing a wire rod, which differs from that of Example 2 in that the online salt bath strong tempering controls the wire rod to be cooled at a cooling rate of 35°C / s to the pearlite phase region for isothermal phase transformation, the molten salt temperature is 630°C, and the roller slow cooling process controls the wire rod to be cooled at a cooling rate of 0.2°C / s, the slow cooling time is 1200s, and the wire rod is cooled to 390°C; the finished wire rod is obtained after going offline.

[0071] Comparative Example 6:

[0072] A method for manufacturing a wire rod, which differs from Example 2 in that the online salt bath strong tempering controls the wire rod to be cooled to the pearlite phase region at a cooling rate of 44°C / s for isothermal phase transformation, the molten salt temperature is 560°C, and the finished wire rod is obtained after it comes off the line. Embodiment 3:

[0073] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.83%, Si: 0.4%, Mn: 0.37%, Al: 0.18%, Cr: 0.15%, P: 0.012%, S: 0.015%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of high temperature rolling → wire laying → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0074] The high temperature rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 18mm through a rolling line. High temperature rolling is used to increase the rolling speed, reduce the deformation resistance of the steel billet and the wear of the rolling line, and a large reduction is used to refine the original austenite grains. Specifically: the heating furnace adopts a preheating, heating, and soaking procedure with sequential temperature increases, and the heating furnace temperature is controlled to be 1145°C, the soaking time is 3.5h, the furnace time is 6h, the initial rolling temperature is 1095°C, the initial rolling reduction is 36%, the final rolling temperature is 990°C, and the final rolling reduction is 40%.

[0075] The spinning process is used to convert the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers. A higher spinning temperature is selected to increase the supercooling of the wire rods in the subsequent online salt bath strong tempering treatment and effectively shorten the residence time in the carbon mesh area. Specifically, the spinning temperature is controlled to be 965°C.

[0076] The online salt bath strong tempering adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. The molten salt circulation volume at the front end of the salt bath tank is controlled to be greater than the molten salt circulation volume at the rear end, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 40°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminating the network carbon deterioration phase caused by excessive carbon element, and improving the use value of carbon element. At the same time, a larger front end molten salt circulation volume is used to form a larger supercooling degree, which promotes a small amount of The austenite structure is transformed into a troostite structure with finer interlamellar spacing, and a smaller rear-end molten salt circulation volume is used to appropriately reduce the undercooling degree, and the untransformed high-temperature austenite is controlled to enter the pearlite phase region for isothermal phase transformation to form pearlite structure, while promoting the tempering and softening of the troostite structure and pearlite structure. Specifically: the molten salt temperature is controlled to be 600℃, the processing time is 650s, the front-end molten salt circulation volume is 800t / h, the temperature rise of the front-end molten salt is ≤10℃, the rear-end molten salt circulation volume is 300t / h, and the temperature rise of the rear-end molten salt is ≤5℃.

[0077] The roller slow cooling process adopts closing the insulation cover, conveying the wire rod from the salt bath tank into the insulation cover by rollers, passing the hot air above the salt bath tank into the insulation cover, and performing slow cooling treatment to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool at a cooling rate of 0.3°C / s, the slow cooling time is 790s, and it is cooled to 363°C; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.

[0078] Comparative Example 7:

[0079] A method for manufacturing a wire rod, which differs from the manufacturing method of Example 3 in that the treatment time of the online salt bath strong tempering is 400s, and the finished wire rod is obtained after going offline.

[0080] Comparative Example 8:

[0081] A method for manufacturing a wire rod, which differs from that of Example 3 in that the treatment time of the online salt bath strong tempering is 780s, and the finished wire rod is obtained after going offline. Embodiment 4:

[0082] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.86%, Si: 0.43%, Mn: 0.42%, Al: 0.3%, Cr: 0.35%, P: 0.014%, S: 0.012%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of high temperature rolling → wire laying → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0083] The high temperature rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the steel billet composition and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 26mm through a rolling line. High temperature rolling is used to increase the rolling speed, reduce the deformation resistance of the steel billet and the wear of the rolling line, and a large reduction is used to refine the original austenite grains. Specifically: the heating furnace adopts a preheating, heating, and soaking procedure with sequential temperature increases, and the heating furnace temperature is controlled to be 1155°C, the soaking time is 4h, the time in the furnace is 6h, the initial rolling temperature is 1125°C, the initial rolling reduction is 33%, the final rolling temperature is 1000°C, and the final rolling reduction is 32%.

[0084] The spinning process is used to convert the wire rod coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers. A higher spinning temperature is selected to increase the supercooling of the wire rods in the subsequent online salt bath strong tempering treatment and effectively shorten the residence time in the carbon mesh area. Specifically, the spinning temperature is controlled to be 975°C.

[0085] The online salt bath strong tempering adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature. The molten salt circulation volume at the front end of the salt bath tank is controlled to be greater than the molten salt circulation volume at the rear end, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 38°C / s for isothermal phase transformation, and quickly passes through the precipitation temperature range of secondary cementite, eliminating the network carbon deterioration phase caused by excessive carbon element, and improving the use value of carbon element. At the same time, a larger front end molten salt circulation volume is used to form a larger supercooling degree, which promotes a small amount of The austenite structure is transformed into a troostite structure with finer interlamellar spacing, and a smaller rear-end molten salt circulation volume is used to appropriately reduce the undercooling degree, and the untransformed high-temperature austenite is controlled to enter the pearlite phase region for isothermal phase transformation to form pearlite structure, while promoting the tempering and softening of the troostite structure and pearlite structure. Specifically: the molten salt temperature is controlled to be 625℃, the processing time is 490s, the front-end molten salt circulation volume is 600t / h, the temperature rise of the front-end molten salt is ≤10℃, the rear-end molten salt circulation volume is 200t / h, and the temperature rise of the rear-end molten salt is ≤5℃.

[0086] The roller slow cooling process adopts closing the insulation cover and conveying the wire rod coming out of the salt bath tank into the insulation cover by rollers for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled at a cooling rate of 0.5°C / s, the slow cooling time is 500s, and it is cooled to 375°C; the coiling process is used to coil the wire rod into coils through the coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage.

[0087] Comparative Example 9:

[0088] A method for manufacturing wire rod, which differs from Example 4 in that the front-end molten salt circulation rate of the online salt bath strong tempering is 450t / h, the rear-end molten salt circulation rate is 450t / h, and the finished wire rod is obtained after going offline.

[0089] Comparative Example 10:

[0090] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of high-temperature rolling → wire laying → online salt bath strong tempering → air cooling → coiling. Specifically: the air cooling is performed by opening a heat preservation cover and conveying the wire rod out of a salt bath tank with a roller for air cooling. The wire rod is controlled to cool at a cooling rate of 2°C / s for 125s, cooled to 375°C, and a finished wire rod is obtained after it comes off the line.

[0091] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 10 were subjected to organization and performance testing: the tensile test was conducted according to GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:

[0092] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0093]

[0094] It can be seen from the results of Examples 1 to 4 that the cold heading steel wire rod of the present invention is designed with a high C-Si-Mn-Al-Cr composition, does not contain bainite or martensite hard and brittle phases in its microstructure, is mainly composed of tempered pearlite, a small amount of tempered troostite, ferrite and fused pearlite, can achieve a tensile strength of 1115 to 1165 MPa, and a cross-sectional reduction rate of 47% to 52%. It can achieve the performance level of 15.9 grade fasteners through direct drawing, cold heading and tempering heat treatment without annealing process, and has good market application prospects.

[0095] From the comparison results of Example 2 and Comparative Example 4, it can be seen that a higher spinning temperature is selected to increase the supercooling of the wire rod in the subsequent online salt bath strong tempering treatment, and the high-speed heat exchange capacity of the molten salt is utilized to control the wire rod to undergo isothermal diffusion phase transformation to form troostite, and the uncontrollable deterioration factors of the network carbide can be eliminated; from the comparison results of Example 2 and Comparative Example 5, it can be seen that the higher the molten salt temperature, the larger the interlamellar spacing of the troostite and pearlite formed by the phase transformation, the higher the proportion of ferrite, and more thermal power can be provided for matrix softening, but the molten salt temperature is too high, and it is difficult to form a large supercooling, which is not conducive to the formation of troostite with finer interlamellar spacing and the inhibition of network carbon, resulting in a decrease in matrix strength and drawing performance; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the lower the molten salt temperature, the finer the interlamellar spacing of the troostite and pearlite structure formed by the phase transformation, the matrix strength increases and the plasticity decreases, but the molten salt temperature is too low, the proportion of tempered troostite increases, which is not conducive to the improvement of the plasticity of the wire rod.

[0096] From the comparison results of Example 3 and Comparative Example 7, it can be seen that if the treatment time is too short, the obtained troostite and pearlite fail to soften, the dislocation density is high, which is not conducive to plasticity, and is prone to stress concentration and drawing hardening, causing the risk of wire breakage and cold heading cracking; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the longer the treatment time, the better the tempering softening effect after the phase transformation is completed, the lower the structural stress and dislocation density of the tempered troostite and tempered pearlite, the lower the wire rod strength and the higher the plasticity, but if the treatment time is too long, excessive tempering softening will lose the wire rod strength, and the precipitation and coarsening of Cr will significantly reduce the strength and plasticity properties.

[0097] From the comparison results of Example 4 and Comparative Example 9, it can be seen that the molten salt circulation amount at the front end is consistent with the molten salt circulation amount at the rear end, the formed troostite structure is small, the interlamellar spacing is coarse, and it is not conducive to structure control. The present invention further controls the difference in molten salt circulation amounts at the front and rear ends, and can achieve phase change control of troostite and pearlite in an online salt bath strong tempering process, thereby simplifying the process. From the comparison results of Example 4 and Comparative Example 10, it can be seen that the use of roller slow cooling can continue the high-temperature softening effect of the wire rod by low-speed cooling, thereby further promoting structure softening and plasticity improvement.

[0098] The series of detailed descriptions listed above are only specific descriptions of the feasible embodiments of the present invention, and they are not intended to limit the protection scope of the present invention. For example, the steel billet can be obtained by sequentially performing converter smelting, refining, and continuous casting processes on the steelmaking raw materials; the control of the front-end molten salt circulation amount and the rear-end molten salt circulation amount can be adopted. The high-speed wire rod online heat treatment equipment and process based on energy recycling disclosed in patent CN116287664B can be adopted, wherein the circulation position design of the rapid cooling tank or the isothermal tank, along the conveying direction, the front and rear ends of the salt bath tank for online salt bath strong tempering are respectively provided with molten salt circulation pipelines and temperature detection devices to respectively control the front-end molten salt circulation amount, the rear-end molten salt circulation amount and the molten salt temperature rise. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.82%-0.86%, Si: 0.30%-0.45%, Mn: 0.22%-0.42%, Al: 0.10%-0.30%, Cr: 0.15%-0.35%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities. The microstructure includes tempered pearlite accounting for 74%-80% by volume, tempered troostite accounting for 14%-20% by volume, and the rest is a mixed structure composed of ferrite and fused pearlite. The manufacturing method includes: The wire rod is produced by rolling according to the chemical composition of the 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod. After the wire rod is spun into a wire rod at a spinning temperature of ≥960°C, it is subjected to online salt bath strong tempering, and the front end molten salt circulation amount of the online salt bath strong tempering is controlled to be greater than the rear end molten salt circulation amount, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and the wire rod is controlled to form troostite and pearlite structures, and the tempering and softening of the troostite and pearlite structures are promoted at the same time. Finally, it is slowly cooled through a roller to produce a cold heading steel wire rod with a mixed structure composed of tempered pearlite, tempered troostite, ferrite and fused pearlite; the molten salt temperature of the online salt bath strong tempering is 590-625°C, and the processing time is 490-740s.

2. The 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 165-205 nm, the interlamellar spacing of the tempered bainite is 90-130 nm, the volume percentage of the ferrite is ≤5%, and the network carbide of the cold heading steel wire rod is level 0.

3. The 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 12.0-26.0 mm, a tensile strength of 1115-1165 MPa, and a cross-sectional shrinkage of 47%-52%.

4. A method for manufacturing 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod, characterized in that: The manufacturing method thereof comprises: According to the chemical composition of the 15.9 grade annealing-free hot-rolled high-carbon cold heading steel wire rod as claimed in claim 1, the wire rod is rolled into a wire rod at a spinning temperature of ≥960°C, and then subjected to online salt bath strong tempering, and the front end molten salt circulation amount of the online salt bath strong tempering is controlled to be greater than the rear end molten salt circulation amount, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥38°C / s for isothermal phase transformation, and the wire rod is controlled to form troostite and pearlite structures, and at the same time promotes tempering and softening of the troostite and pearlite structures, and finally is slowly cooled by a roller to obtain a cold heading steel wire rod having a microstructure including 74% to 80% tempered pearlite by volume, 14% to 20% tempered troostite by volume, and the rest being a mixed structure composed of ferrite and fused pearlite, the molten salt temperature of the online salt bath strong tempering is 590 to 625°C, and the processing time is 490 to 740s.

5. The method for manufacturing a 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: Before rolling, the heating furnace temperature is controlled to be ≤1155°C, the soaking time is 3-4h, and the time in the furnace is ≤6h.

6. The method for manufacturing a 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: During the rolling, high temperature rolling is adopted, the initial rolling temperature is controlled to be 1085-1125° C., the initial rolling reduction is 33%-38%, the final rolling temperature is ≤1000° C., and the final rolling reduction is 32%-42%.

7. The method for manufacturing a 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: The front-end molten salt circulation volume of the online salt bath strong tempering is 600-900 t / h, and the temperature rise of the front-end molten salt is controlled to be ≤10°C. The rear-end molten salt circulation volume is 200-400 t / h, and the temperature rise of the rear-end molten salt is controlled to be ≤5°C.

8. The method for manufacturing a 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: The roller slow cooling adopts closing the heat preservation cover, controlling the wire rod to cool at a cooling rate of 0.2-0.5°C / s, and the slow cooling time is ≥500s.

9. The method for manufacturing a 15.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 8, characterized in that: The roller slow cooling adopts the method of passing the hot air above the salt bath tank of the online salt bath strong tempering into the heat preservation cover.

Citation Information

Cited By

  • Non-quenched and tempered cold heading steel wire rod for 16.9-grade high-strength bolt and production method of non-quenched and tempered cold heading steel wire rod

    CN122564416A