A high chromium cast iron reinforced carbon steel wear-resistant composite material and preparation method thereof

By preparing cylindrical through holes in carbon steel slabs and pouring high chromium cast iron, combined with hot rolling and diffusion heat treatment, the problem of uncontrollable distribution and stress damage of high chromium cast iron in carbon steel is solved, and the wear resistance of composite materials is improved. and impact toughness.

CN118668045BActive Publication Date: 2024-10-22JINZHONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411154877.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-22
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In the existing preparation method of high chromium cast iron/carbon steel composite materials, the distribution of high chromium cast iron in carbon steel is uncontrollable, and the stress damage of hard and brittle high chromium cast iron is serious, which is difficult to effectively overcome.

Method used

Regularly arranged cylindrical through holes are prepared on the carbon steel slab, the high chromium cast iron melt is poured, the carbon steel composite plate is welded, and through hot rolling and diffusion heat treatment, the controllable combination of high chromium cast iron and carbon steel and the uniform distribution of stress are achieved .

Benefits of technology

It achieves controllable and regular distribution of high chromium cast iron in carbon steel, reduces stress damage, and improves the wear resistance and impact toughness of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118668045B_ABST
    Figure CN118668045B_ABST
Patent Text Reader

Abstract

The present invention provides a high-chromium cast iron reinforced carbon steel wear-resistant composite material and a preparation method thereof, and belongs to the technical field of composite materials. The preparation method of the high-chromium cast iron reinforced carbon steel wear-resistant composite material provided by the present invention comprises the following steps: (1) regularly arranged cylindrical through holes are prepared on a carbon steel slab to obtain an intermediate substrate; (2) high-chromium cast iron melt is poured into the cylindrical through holes in the intermediate substrate obtained in step (1) to obtain an intermediate slab; (3) a layer of carbon steel composite plate is respectively welded on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab; (4) the composite slab obtained in step (3) is sequentially hot-rolled and diffusion-heat-treated to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a high-chromium cast iron reinforced carbon steel wear-resistant composite material and a preparation method thereof. Background Art

[0002] High chromium cast iron has high hardness and excellent wear resistance, and is widely used in industrial processes that require high wear-resistant parts, such as mining, transportation, and processing and manufacturing. However, the poor impact toughness of high chromium cast iron is a significant disadvantage. By metallurgically combining high chromium cast iron with carbon steel with good toughness to prepare a composite material, the impact toughness of high chromium cast iron can be improved without changing its hardness and wear resistance. The existing preparation methods of high chromium cast iron / steel composite materials mainly include liquid-liquid composite casting, solid-liquid composite casting, explosive welding, and casting combined with rolling, etc. However, the above methods currently have various defects. For example, the Chinese invention patent application with patent number CN 111715691 A discloses a preparation method of a high chromium cast iron dispersed distribution wear-resistant composite material. During the preparation process, a multi-layer blanking method of 7 to 15 layers is required to alternately overlap carbon steel plates and high chromium cast iron plates to prepare the composite material. Although this method improves production efficiency and shortens production cycle, it will lead to uncontrollable distribution of high chromium cast iron materials in carbon steel, and high chromium cast iron will suffer from severe stress damage; the Chinese invention patent application with patent number CN108480398 A discloses a method for blanking and rolling of high chromium cast iron / low carbon steel plates. By separating the casting process from the rolling process, the rapid preparation of high chromium cast iron / low carbon steel composite plates can be achieved, and the prepared composite plates are in the shape of straight plates, which improves production efficiency and is suitable for mass production, but this method still cannot effectively overcome the problem of severe damage to high chromium cast iron.

[0003] The existing preparation methods of high chromium cast iron / carbon steel composite materials mainly have the disadvantages of uncontrollable distribution of high chromium cast iron materials in carbon steel and serious damage to hard and brittle high chromium cast iron. Therefore, how to achieve controllable and regular distribution of high chromium cast iron materials in carbon steel and reduce stress damage of hard and brittle high chromium cast iron has become a technical problem to be solved in this field. Summary of the invention

[0004] The purpose of the present invention is to provide a high-chromium cast iron reinforced carbon steel wear-resistant composite material and a preparation method thereof. The high-chromium cast iron reinforced carbon steel wear-resistant composite material provided by the present invention realizes the controllable regular distribution of the high-chromium cast iron material in the carbon steel, and the stress damage degree of the high-chromium cast iron after rolling is low.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a high-chromium cast iron reinforced carbon steel wear-resistant composite material, comprising the following steps:

[0007] (1) Regularly arranged cylindrical through holes are prepared on a carbon steel slab to obtain an intermediate substrate;

[0008] (2) pouring high chromium cast iron melt into the cylindrical through hole in the intermediate substrate obtained in step (1) to obtain an intermediate slab;

[0009] (3) welding a layer of carbon steel composite plate on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab;

[0010] (4) The composite slab obtained in step (3) is subjected to hot rolling and diffusion heat treatment in sequence to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material.

[0011] Preferably, the size of the cylindrical through hole in step (1) and the size of the carbon steel slab satisfy the following relationship: H / D<2, 1.5D<E<2D, D<T<1.5D, wherein H is the thickness of the carbon steel slab, D is the diameter of the cylindrical through hole, E is the center distance between two adjacent cylindrical through holes, and T is the distance between the center of the cylindrical through hole and the edge of the carbon steel slab.

[0012] Preferably, in the step (2), the intermediate substrate is preheated before pouring, the preheating temperature is 400-500° C., and the preheating time is 20-30 min.

[0013] Preferably, the pouring temperature in step (2) is 1400-1500° C., and the pouring method is bottom pouring.

[0014] Preferably, the relationship between the thickness h of the carbon steel composite plate in step (3) and the thickness H of the carbon steel slab in step (1) is: 0.2H<h<H.

[0015] Preferably, the welding method in step (3) is as follows: the intermediate slab and the surfaces to be joined of the carbon steel composite plate are placed opposite to each other, followed by sealing and welding on all sides, vacuuming the reserved pipe, and finally heat-sealing the reserved pipe.

[0016] Preferably, in step (4), the starting temperature of hot rolling is 1150-1200°C, and the final temperature of hot rolling is ≥1100°C.

[0017] Preferably, in step (4), the hot rolling reduction per pass is ≤10%, and the hot rolling speed is 0.5-2 m / s.

[0018] Preferably, the temperature of the diffusion heat treatment in step (4) is 600-800° C., and the holding time of the diffusion heat treatment is 20-60 min.

[0019] The invention provides a high-chromium cast iron reinforced carbon steel wear-resistant composite material prepared by the preparation method described in the above technical scheme.

[0020] The present invention provides a method for preparing a high-chromium cast iron reinforced carbon steel wear-resistant composite material, comprising the following steps: (1) preparing regularly arranged cylindrical through holes on a carbon steel slab to obtain an intermediate substrate; (2) pouring a high-chromium cast iron melt into the cylindrical through holes in the intermediate substrate obtained in step (1) to obtain an intermediate slab; (3) welding a layer of carbon steel composite plate on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab; and (4) sequentially hot rolling and diffusion heat treating the composite slab obtained in step (3) to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material.

[0021] The present invention adopts high chromium cast iron as the substrate reinforcement material. High chromium cast iron has excellent wear resistance but poor toughness, while carbon steel has good impact toughness but poor wear resistance and hardness. Through the combination of the two, their respective performance advantages can be brought into play, and the wear resistance of the composite material can be comprehensively improved on the basis of maintaining the good toughness of carbon steel.

[0022] The present invention can achieve initial solid-liquid composite of carbon steel and high chromium cast iron by first prefabricating regularly arranged cylindrical through holes in the middle carbon steel plate and then pouring high chromium cast iron melt into the cylindrical through holes, and then further high-quality metallurgical bonding between the two metals is achieved through cladding hot rolling.

[0023] The cylindrical through hole adopted in the present invention can avoid the problem of stress concentration at the hole wall of the high chromium cast iron after solidification to the greatest extent, so that the stress distribution inside the high chromium cast iron is uniform; after the high chromium cast iron in the cylindrical hole solidifies, the surrounding carbon steel can form a canning effect on the high chromium cast iron, so that the high chromium cast iron is in a triaxial compressive stress state during the subsequent rolling process, thereby reducing stress damage; through the regularly arranged cylindrical through holes, the high-hardness high chromium cast iron material can be controllably and regularly distributed in the carbon steel, thereby enhancing the hardness and wear resistance of the carbon steel plate.

[0024] The present invention can make carbon steel form a support and stress buffer for brittle high-chromium cast iron materials that are more sensitive to stress by welding carbon steel composite plates. A carbon steel layer is formed on the upper and lower surfaces of the composite material. The carbon steel layer is first used as a working surface. After the surface is worn, the high-chromium cast iron reinforcement layer with excellent wear resistance is exposed, and its wear resistance is further exerted, thereby achieving the purpose of improving the overall wear resistance of the composite material while maintaining the excellent toughness of carbon steel. At the same time, the presence of the carbon steel composite plate can also avoid direct contact between the brittle high-chromium cast iron and the rolling rollers during subsequent hot rolling, further reducing the probability of cracks in the high-chromium cast iron during thermal deformation.

[0025] The present invention can make carbon steel and high chromium cast iron tightly bonded together under the action of external force through hot rolling treatment. Since the hard and brittle high chromium cast iron is thermally deformed when surrounded by carbon steel during the hot rolling process, the high chromium cast iron is overall coordinated thermoplastic deformation under triaxial compressive stress, which helps to inhibit the initiation and expansion of cracks in the high chromium cast iron during thermal deformation, reduces the stress damage degree of the high chromium cast iron, ensures the orderly and regular distribution of the high chromium cast iron material, and improves the problems of low bonding strength between the bimetals and serious damage to the high chromium cast iron caused by direct compounding.

[0026] The present invention performs diffusion heat treatment on the rolled slab, which can reduce the internal stress after rolling on the one hand, and can make the chemical components between carbon steel and high chromium cast iron diffuse with each other on the other hand, thereby further improving the bonding strength between carbon steel and high chromium cast iron.

[0027] The results of the embodiment show that the high chromium cast iron reinforced carbon steel wear-resistant composite material provided by the present invention realizes the controllable regular distribution of high chromium cast iron material in carbon steel, and the stress damage degree of high chromium cast iron after rolling is low, while also avoiding the problem of low bonding strength between carbon steel and high chromium cast iron layers. After testing, the impact toughness of the high chromium cast iron reinforced carbon steel wear-resistant composite material provided by the present invention is ≥8.9J / cm 2 , the mass loss under friction and wear test conditions is ≤6.1mg. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of regularly arranged cylindrical through holes provided by the present invention, Figure 1 In the figure, 1 is the carbon steel slab, H is the thickness of the carbon steel slab, D is the diameter of the cylindrical through hole, E is the center distance between two adjacent cylindrical through holes, and T is the distance between the center of the cylindrical through hole and the edge of the carbon steel slab;

[0029] Figure 2 A schematic diagram of a carbon steel composite plate provided by the present invention, Figure 2 In, 3 and 3' are carbon steel double plates, and h is the thickness of the carbon steel double plates;

[0030] Figure 3 A schematic diagram of welding a layer of carbon steel composite plate to the upper and lower sides of the intermediate slab provided by the present invention, Figure 3 In the figure, 2 is the middle base plate, 3 and 3' are carbon steel double plates, 4 is the reserved pipe, and 5 is the composite slab;

[0031] Figure 4 A schematic diagram of the deformation of the composite slab provided by the present invention after hot rolling, Figure 4 Among them, 5 is a composite slab, and 6 is a high chromium cast iron reinforced carbon steel wear-resistant composite material. DETAILED DESCRIPTION

[0032] The present invention provides a method for preparing a high-chromium cast iron reinforced carbon steel wear-resistant composite material, comprising the following steps:

[0033] (1) Regularly arranged cylindrical through holes are prepared on a carbon steel slab to obtain an intermediate substrate;

[0034] (2) pouring high chromium cast iron melt into the cylindrical through hole in the intermediate substrate obtained in step (1) to obtain an intermediate slab;

[0035] (3) welding a layer of carbon steel composite plate on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab;

[0036] (4) The composite slab obtained in step (3) is subjected to hot rolling and diffusion heat treatment in sequence to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material.

[0037] In the present invention, unless otherwise specified, the metal materials used are commercially available products well known to those skilled in the art.

[0038] The present invention prepares regularly arranged cylindrical through holes on a carbon steel slab to obtain an intermediate substrate.

[0039] The present invention has no particular limitation on the specific method for preparing the cylindrical through-holes, and a method for preparing through-holes on a steel plate well known to those skilled in the art may be used. The present invention prepares cylindrical through holes on the carbon steel slab, and high-chromium cast iron melt can be poured into the through holes, thereby achieving preliminary solid-liquid composite of carbon steel and high-chromium cast iron, and then further high-quality metallurgical bonding between the two metals is achieved through cladding hot rolling; the use of cylindrical through holes instead of rectangular, triangular or other angled through holes can avoid the problem of stress concentration at the hole wall of the high-chromium cast iron after solidification to the greatest extent, so that the stress distribution inside the high-chromium cast iron is uniform, and after the high-chromium cast iron in the cylindrical hole solidifies, the surrounding carbon steel can form a canning effect on the high-chromium cast iron, so that the high-chromium cast iron is in a triaxial compressive stress state during the subsequent rolling process, thereby reducing stress damage; through the regularly arranged cylindrical through holes, high-hardness high-chromium cast iron materials can be controllably and regularly distributed in the carbon steel, thereby enhancing the hardness and wear resistance of the carbon steel plate, and at the same time, the carbon steel composite plate forms a support and stress buffering effect on the brittle high-chromium cast iron material that is more sensitive to stress.

[0040] In the present invention, the carbon steel slab is preferably Q235 carbon steel. The present invention has no special limitation on the specific size of the carbon steel slab, which can be selected according to the size of the required composite material and the technical common sense of those skilled in the art. The present invention adopts Q235 carbon steel as the carbon steel slab, which not only has good impact toughness, but also has low deformation resistance at 1150°C, which is convenient for subsequent hot rolling deformation treatment.

[0041] In the present invention, the regularly arranged cylindrical through holes are preferably regularly arranged cylindrical through holes at equal intervals. In the present invention, the schematic diagram of the regularly arranged cylindrical through holes is as follows: Figure 1 The present invention arranges multiple groups of cylindrical through holes in a regular pattern on the carbon steel slab, thereby ensuring that the subsequently cast high chromium cast iron can be regularly arranged on the carbon steel slab, so that the high chromium cast iron is evenly distributed in the carbon steel plate, thus avoiding the problem of unstable quality caused by uncontrollable distribution of high chromium cast iron in carbon steel.

[0042] In the present invention, the size of the cylindrical through hole and the size of the carbon steel slab preferably satisfy the following relationship: H / D<2, 1.5D<E<2D, D<T<1.5D, wherein H is the thickness of the carbon steel slab, D is the diameter of the cylindrical through hole, E is the center distance between two adjacent cylindrical through holes, and T is the distance between the center of the cylindrical through hole and the edge of the carbon steel slab. The present invention can evenly distribute the cylindrical through holes on the carbon steel slab by controlling the size relationship of the cylindrical through holes.

[0043] After the intermediate substrate is obtained, the present invention pours high-chromium cast iron melt into the cylindrical through hole in the intermediate substrate to obtain the intermediate slab.

[0044] Before pouring the high chromium cast iron melt, the present invention preferably performs grinding, cleaning and preheating treatment on the intermediate substrate in sequence.

[0045] In the present invention, the polishing and cleaning preferably includes polishing and cleaning the upper surface, the lower surface and the inner wall of the cylindrical through hole of the intermediate substrate. The present invention has no special limitation on the specific operation of the polishing and cleaning, and the operation of polishing and cleaning the carbon steel plate well known to those skilled in the art can be used. The present invention can remove the oxide layer and pollutants on the surface of the intermediate substrate by polishing and cleaning, ensuring that the surface to be bonded is not contaminated.

[0046] In the present invention, the temperature of the preheating treatment is preferably 400-500°C, more preferably 450°C; the holding time of the preheating treatment is preferably 20-30 minutes. The present invention can avoid rapid cooling of the high chromium cast iron melt during the pouring process, thereby affecting its mechanical properties, by preheating the intermediate substrate.

[0047] In the present invention, the high chromium cast iron melt is preferably KmTBCr26 high chromium cast iron melt. The present invention uses the above high chromium cast iron as the substrate reinforcement material. The high chromium cast iron has excellent wear resistance, but poor toughness, while the carbon steel material has good impact toughness, but poor wear resistance and hardness. Through the combination of the two, their respective performance advantages can be brought into play, and the wear resistance of the composite material can be comprehensively improved on the basis of maintaining the good toughness of carbon steel.

[0048] In the present invention, the pouring temperature is preferably 1400-1500°C, more preferably 1450°C; the pouring method is preferably bottom pouring; the equipment used for the pouring is preferably vacuum casting equipment. The present invention has no special restrictions on the specific model and source of the vacuum casting equipment, and commercially available products familiar to those skilled in the art can be used. The present invention can make the high chromium cast iron melt have good fluidity by controlling the pouring temperature; by adopting the bottom pouring method, the probability of defects such as shrinkage cavities, shrinkage and insufficient pouring during pouring can be reduced.

[0049] In the present invention, the pouring is preferably performed in a vacuum environment, and the vacuum degree of the vacuum environment is preferably 0.001-0.003 Pa. The present invention can prevent oxidation of the molten metal and reduce the influence of oxygen by pouring in a vacuum environment.

[0050] After the pouring is completed, the present invention preferably cools the poured product naturally to room temperature to obtain an intermediate slab. The present invention forms a preliminary solid-liquid metallurgical bond between the inner wall of the through hole of the carbon steel plate and the high chromium cast iron by pouring high chromium cast iron melt into the cylindrical through hole on the carbon steel slab.

[0051] After obtaining the intermediate slab, the present invention welds a layer of carbon steel composite plate on the upper and lower sides of the intermediate slab to obtain a composite slab. The present invention can form a carbon steel layer on the upper and lower surfaces of the composite material by welding the carbon steel composite plate. The carbon steel layer is first used as a working surface. After the surface is worn, the high-chromium cast iron reinforcement layer with excellent wear resistance is exposed, and its wear resistance is further exerted, thereby achieving the purpose of improving the overall wear resistance of the composite material while maintaining the excellent toughness of carbon steel; at the same time, the presence of the carbon steel composite plate can also avoid direct contact between the brittle high-chromium cast iron and the roller during subsequent hot rolling, further reducing the probability of cracks in the high-chromium cast iron during thermal deformation.

[0052] In the present invention, the composition of the carbon steel duplex plate is preferably the same as that of the carbon steel slab. The present invention uses carbon steel of the same material as the carbon steel slab as the duplex plate, which can improve the bonding strength of the two in the subsequent rolling process.

[0053] In the present invention, the schematic diagram of the carbon steel composite plate is as follows Figure 2 As shown. In the present invention, the relationship between the thickness h of the carbon steel double plate and the thickness H of the carbon steel slab is preferably: 0.2H<h<H; the length and width of the carbon steel double plate are preferably the same as the length and width of the carbon steel slab. By controlling the thickness of the carbon steel double plate, the present invention can form a thinner carbon steel layer on the surface of the composite material, thereby improving the toughness of the composite material; by controlling the length and width of the carbon steel double plate, the size of the surface to be combined with the intermediate slab can be made to match, so as to achieve symmetry of the deformation resistance of the composite material and obtain a high-quality plate-shaped high-chromium cast iron / carbon steel composite material.

[0054] Before welding, the present invention preferably grinds and cleans the surface to be joined of the carbon steel double plate. The present invention has no special limitation on the specific operation of the grinding and cleaning, and the grinding and cleaning operation well known to those skilled in the art can be used to remove the oxide layer and contaminants on the surface to be joined. The present invention can remove the oxide layer and contaminants on the surface to be joined by grinding and cleaning, thereby avoiding the contaminants from negatively affecting the interface bonding performance of the carbon steel double plate and the intermediate slab.

[0055] In the present invention, the welding method is preferably as follows: the intermediate slab and the carbon steel composite plate to be joined are placed opposite to each other, then the four sides are sealed and welded, and then a vacuum is drawn from the reserved pipe, and finally the reserved pipe is heat-sealed. In the present invention, the vacuum degree of the vacuum drawing is preferably ≤0.003Pa. In the present invention, a layer of carbon steel composite plate is welded on the upper and lower sides of the intermediate slab, respectively. Figure 3 The present invention adopts the above-mentioned method for welding to avoid air from forming pores inside the composite material, thereby further improving the bonding strength of high chromium cast iron and carbon steel.

[0056] After obtaining the composite slab, the present invention sequentially performs hot rolling and diffusion heat treatment on the composite slab to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material.

[0057] In the present invention, the starting temperature of the hot rolling is preferably 1150~1200℃; the final rolling temperature of the hot rolling is preferably ≥1100℃; the heating rate to the starting temperature is preferably 5~8℃ / min, more preferably 6~7℃ / min; the hot rolling is preferably carried out on a flat rolling mill. In the present invention, when the temperature during the hot rolling is less than 1100℃, it is preferred to first heat the composite slab to the starting temperature and then perform hot rolling. In the present invention, the deformation diagram of the composite slab after hot rolling is as follows Figure 4 As shown. The present invention can make carbon steel and high chromium cast iron tightly bonded together under the action of external force through hot rolling treatment, thereby improving their bonding strength; by controlling the hot rolling temperature not lower than the plastic deformation temperature of high chromium cast iron, both carbon steel and high chromium cast iron can have low deformation resistance, thereby facilitating rolling; in the hot rolling process, since the high chromium cast iron is surrounded by carbon steel, the hard and brittle high chromium cast iron can be thermally deformed when surrounded by carbon steel. At this time, the high chromium cast iron realizes overall coordinated thermoplastic deformation under triaxial compressive stress, which helps to inhibit the initiation and expansion of cracks in the high chromium cast iron during thermal deformation, reduces the stress damage degree of the high chromium cast iron, and ensures the orderly and regular distribution of the high chromium cast iron material, thereby improving the problems of low bonding strength between bimetals and serious damage of the high chromium cast iron in direct layered composite.

[0058] In the present invention, the single pass reduction of the hot rolling is preferably ≤10%, more preferably 5-8%; the number of hot rolling passes is preferably 2-8, more preferably 3-5; the total deformation of the hot rolling is preferably ≤80%, more preferably ≤60%; the rolling speed of the hot rolling is preferably 0.5-2m / s, more preferably 1-1.5m / s. The present invention can achieve a metallurgical bond with high bonding strength by adopting a rolling method with a small reduction, so as to reduce the stress damage of the brittle high-chromium cast iron caused by the large rolling force; and the thickness of the composite material can be regulated by controlling the total deformation of the rolling.

[0059] In the present invention, the temperature of the diffusion heat treatment is preferably 600-800°C, more preferably 650-750°C, and further preferably 700°C; the holding time of the diffusion heat treatment is preferably 20-60 minutes, more preferably 30-50 minutes, and further preferably 40 minutes; the cooling method of the diffusion heat treatment is preferably air cooling. The present invention performs diffusion heat treatment on the rolled slab, which can reduce the internal stress after rolling on the one hand, and can make the chemical components between carbon steel and high chromium cast iron diffuse with each other on the other hand, thereby further improving the bonding strength of carbon steel and high chromium cast iron.

[0060] After the diffusion heat treatment is completed, the product of the diffusion heat treatment is preferably subjected to trimming treatment to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material. The present invention has no special restrictions on the operation and size of the trimming treatment, and the trimming operation well known to those skilled in the art can be used. The present invention can remove the edge parts that have problems such as cracking and internal stress concentration due to rolling through the trimming treatment.

[0061] The present invention adopts high chromium cast iron as the substrate reinforcement material. High chromium cast iron has excellent wear resistance but poor toughness, while carbon steel has good impact toughness but poor wear resistance and hardness. Through the combination of the two, their respective performance advantages can be brought into play, and the wear resistance of the composite material can be comprehensively improved on the basis of maintaining the good toughness of carbon steel; by first prefabricating regularly arranged cylindrical through holes in the middle carbon steel plate, and then pouring high chromium cast iron melt into the cylindrical through holes, the initial solid-liquid composite of carbon steel and high chromium cast iron can be achieved, and then the further high-quality metallurgical bonding between the two metals can be achieved through coating hot rolling; the cylindrical through holes can avoid After solidification, high-chromium cast iron will have stress concentration problem at the hole wall, so that the stress distribution inside the high-chromium cast iron is uniform. After the high-chromium cast iron in the cylindrical hole solidifies, the surrounding carbon steel can form a canning effect on the high-chromium cast iron, so that the high-chromium cast iron is in a triaxial compressive stress state during the subsequent rolling process, thereby reducing stress damage; through regularly arranged cylindrical through holes, high-hardness high-chromium cast iron materials can be controllably and regularly distributed in carbon steel, thereby enhancing the hardness and wear resistance of carbon steel plates; through welding carbon steel composite plates, carbon steel can form a support and stress buffering effect on brittle high-chromium cast iron materials that are more sensitive to stress, A carbon steel layer is formed on the upper and lower surfaces of the composite material. The carbon steel layer is first used as a working surface. After the surface is worn, the high-chromium cast iron reinforcement layer with excellent wear resistance is exposed, further exerting its wear-resistant effect, thereby achieving the purpose of improving the overall wear resistance of the composite material while maintaining the excellent toughness of carbon steel. At the same time, the presence of the carbon steel composite plate can also avoid direct contact between the brittle high-chromium cast iron and the rollers during subsequent hot rolling, further reducing the probability of cracks in the high-chromium cast iron during thermal deformation. Through hot rolling treatment, the carbon steel and high-chromium cast iron can be tightly combined together under the action of external force. Since the hard and brittle high-chromium cast iron is formed on the carbon steel during the hot rolling process, The thermal deformation is achieved under the condition of peripheral coating. At this time, the high chromium cast iron realizes overall coordinated thermoplastic deformation under triaxial compressive stress, which helps to inhibit the initiation and expansion of cracks in the high chromium cast iron during thermal deformation, reduces the stress damage degree of the high chromium cast iron, and ensures the orderly and regular distribution of the high chromium cast iron material, improves the low bonding strength between the bimetallic and the serious damage of the high chromium cast iron caused by direct composite; by subjecting the rolled slab to diffusion heat treatment, on the one hand, the internal stress after rolling can be reduced, and on the other hand, the chemical components between carbon steel and high chromium cast iron can be diffused with each other, thereby further improving the bonding strength between carbon steel and high chromium cast iron.

[0062] The invention provides a high-chromium cast iron reinforced carbon steel wear-resistant composite material prepared by the preparation method described in the above technical scheme.

[0063] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0064] Example 1

[0065] A method for preparing a high-chromium cast iron reinforced carbon steel wear-resistant composite material comprises the following steps:

[0066] (1) Prepare on carbon steel slab Figure 1 The cylindrical through holes are arranged regularly at equal intervals to obtain an intermediate substrate; the carbon steel slab is Q235 carbon steel, the length of the carbon steel slab is 100 mm, the width is 50 mm, and the thickness is 10 mm; the diameter of the cylindrical through hole is 8 mm, the center distance between two adjacent cylindrical through holes is 14 mm, and the distance between the center of the cylindrical through hole and the edge of the carbon steel slab is 10 mm;

[0067] (2) The upper surface, the lower surface and the inner wall of the cylindrical through hole of the intermediate substrate obtained in step (1) are polished and cleaned, and then preheated, and then KmTBCr26 high chromium cast iron melt is poured into the cylindrical through hole of the intermediate substrate, and finally naturally cooled to room temperature to obtain an intermediate slab; the preheating temperature is 450°C, and the preheating time is 30 minutes; the pouring temperature is 1450°C, the pouring method is bottom pouring, and the pouring is carried out in a vacuum environment, and the vacuum degree of the vacuum environment is 0.003Pa;

[0068] (3) taking two carbon steel composite plates, then grinding and cleaning the surfaces to be bonded of the carbon steel composite plates, and finally welding a layer of carbon steel composite plates on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab; the carbon steel composite plates are Q235 carbon steel, and the length of the carbon steel composite plates is 100 mm, the width is 50 mm, and the thickness is 6 mm; the welding method is: placing the intermediate slab and the surfaces to be bonded of the carbon steel composite plates opposite to each other, then sealing and welding them all around, and then evacuating from a reserved pipe to a vacuum degree of ≤0.003 Pa, and finally heat-sealing the reserved pipe;

[0069] (4) hot rolling the composite slab obtained in step (3) on a flat roll mill, then performing diffusion heat treatment, and finally performing edge trimming treatment to obtain a high chromium cast iron reinforced carbon steel wear-resistant composite material; the hot rolling start temperature is 1200°C, the hot rolling finish temperature is 1100°C, the hot rolling single pass reduction is 10%, the hot rolling pass number is 3, the hot rolling total deformation is 30%, and the hot rolling rolling speed is 1 m / s; the diffusion heat treatment temperature is 700°C, the diffusion heat treatment holding time is 40 min, and the diffusion heat treatment cooling method is air cooling.

[0070] Example 2

[0071] A method for preparing a high-chromium cast iron reinforced carbon steel wear-resistant composite material comprises the following steps:

[0072] (1) Prepare on carbon steel slab Figure 1 The cylindrical through holes are arranged regularly at equal intervals to obtain an intermediate substrate; the carbon steel slab is Q235 carbon steel, the length of the carbon steel slab is 150 mm, the width is 70 mm, and the thickness is 20 mm; the diameter of the cylindrical through hole is 15 mm, the center distance between two adjacent cylindrical through holes is 26 mm, and the distance between the center of the cylindrical through hole and the edge of the carbon steel slab is 18 mm;

[0073] (2) The upper surface, the lower surface and the inner wall of the cylindrical through hole of the intermediate substrate obtained in step (1) are polished and cleaned, and then preheated, and then KmTBCr26 high chromium cast iron melt is poured into the cylindrical through hole of the intermediate substrate, and finally naturally cooled to room temperature to obtain an intermediate slab; the preheating temperature is 450°C, and the preheating time is 30 minutes; the pouring temperature is 1450°C, the pouring method is bottom pouring, and the pouring is carried out in a vacuum environment, and the vacuum degree of the vacuum environment is 0.003Pa;

[0074] (3) taking two carbon steel composite plates, then grinding and cleaning the surfaces to be bonded of the carbon steel composite plates, and finally welding a layer of carbon steel composite plates on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab; the carbon steel composite plates are Q235 carbon steel, and the length of the carbon steel composite plates is 150 mm, the width is 70 mm, and the thickness is 12 mm; the welding method is: placing the intermediate slab and the surfaces to be bonded of the carbon steel composite plates opposite to each other, then sealing and welding them around, and then evacuating from a reserved pipe to a vacuum degree of ≤0.003 Pa, and finally heat-sealing the reserved pipe;

[0075] (4) hot rolling the composite slab obtained in step (3) on a flat roll mill, then performing diffusion heat treatment, and finally performing edge trimming treatment to obtain a high chromium cast iron reinforced carbon steel wear-resistant composite material; the hot rolling start temperature is 1200°C, the hot rolling finish temperature is 1100°C, the hot rolling single pass reduction is 10%, the hot rolling pass number is 3, the hot rolling total deformation is 30%, and the hot rolling rolling speed is 1 m / s; the diffusion heat treatment temperature is 700°C, the diffusion heat treatment holding time is 40 min, and the diffusion heat treatment cooling method is air cooling.

[0076] Example 3

[0077] A method for preparing a high-chromium cast iron reinforced carbon steel wear-resistant composite material comprises the following steps:

[0078] (1) Prepare on carbon steel slab Figure 1 The cylindrical through holes are arranged regularly at equal intervals to obtain an intermediate substrate; the carbon steel slab is Q235 carbon steel, the length of the carbon steel slab is 150 mm, the width is 70 mm, and the thickness is 20 mm; the diameter of the cylindrical through hole is 15 mm, the center distance between two adjacent cylindrical through holes is 26 mm, and the distance between the center of the cylindrical through hole and the edge of the carbon steel slab is 18 mm;

[0079] (2) The upper surface, the lower surface and the inner wall of the cylindrical through hole of the intermediate substrate obtained in step (1) are polished and cleaned, and then preheated, and then KmTBCr26 high chromium cast iron melt is poured into the cylindrical through hole of the intermediate substrate, and finally naturally cooled to room temperature to obtain an intermediate slab; the preheating temperature is 400°C, and the preheating time is 20 minutes; the pouring temperature is 1450°C, the pouring method is bottom pouring, and the pouring is carried out in a vacuum environment, and the vacuum degree of the vacuum environment is 0.003Pa;

[0080] (3) taking two carbon steel composite plates, then grinding and cleaning the surfaces to be bonded of the carbon steel composite plates, and finally welding a layer of carbon steel composite plates on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab; the carbon steel composite plates are Q235 carbon steel, and the length of the carbon steel composite plates is 150 mm, the width is 70 mm, and the thickness is 12 mm; the welding method is: placing the intermediate slab and the surfaces to be bonded of the carbon steel composite plates opposite to each other, then sealing and welding them around, and then evacuating from a reserved pipe to a vacuum degree of ≤0.003 Pa, and finally heat-sealing the reserved pipe;

[0081] (4) hot rolling the composite slab obtained in step (3) on a flat roll mill, then performing diffusion heat treatment, and finally performing edge trimming treatment to obtain a high chromium cast iron reinforced carbon steel wear-resistant composite material; the hot rolling start temperature is 1150°C, the hot rolling finish temperature is 1100°C, the hot rolling single pass reduction is 10%, the hot rolling pass number is 3, the hot rolling total deformation is 30%, and the hot rolling rolling speed is 1.5 m / s; the diffusion heat treatment temperature is 600°C, the diffusion heat treatment holding time is 20 min, and the diffusion heat treatment cooling method is air cooling.

[0082] Comparative Example 1

[0083] A method for preparing a high-chromium cast iron reinforced carbon steel composite material comprises the following steps:

[0084] (1) Take two carbon steel slabs and one high chromium cast iron slab, grind and clean them respectively, and then weld a layer of carbon steel composite plate on the upper and lower surfaces of the high chromium cast iron slab to obtain a composite slab; the carbon steel slab is Q235 carbon steel, the length of the carbon steel slab is 100 mm, the width is 50 mm, and the thickness is 10 mm; the high chromium cast iron slab is KmTBCr26 high chromium cast iron, the length of the high chromium cast iron slab is 100 mm, the width is 50 mm, and the thickness is 8 mm; the welding method is: place the intermediate slab and the surface to be bonded of the carbon steel composite plate opposite to each other, then seal and weld them all around, evacuate from a reserved pipe to a vacuum degree of ≤0.003 Pa, and finally heat seal the reserved pipe;

[0085] (2) hot rolling the composite slab obtained in step (1) on a flat roll mill, then performing diffusion heat treatment, and finally performing trimming treatment to obtain a high chromium cast iron reinforced carbon steel composite material; the hot rolling start temperature is 1200°C, the hot rolling finish temperature is 1100°C, the hot rolling single pass reduction is 10%, the hot rolling pass number is 3, the hot rolling total deformation is 30%, and the hot rolling rolling speed is 1 m / s; the diffusion heat treatment temperature is 700°C, the diffusion heat treatment holding time is 40 min, and the diffusion heat treatment cooling method is air cooling.

[0086] Comparative Example 2

[0087] The Chinese invention patent application with patent number CN111715691A is selected to prepare a high chromium cast iron dispersed composite material by preparing a 9-layer composite slab composed of high chromium cast iron KmTBCr26 and carbon steel Q235, and the preparation steps are as follows:

[0088] 1) Take carbon steel plates T1, T2, T3, T4, T5 with a length of 150 mm, a width of 100 mm, and a thickness of 1 mm, and high chromium cast iron plates G1, G2, G3, G4 with a length of 150 mm, a width of 100 mm, and a thickness of 2.5 mm, respectively. The two plates have the same shape and size, and their surfaces are mechanically polished to remove oxide scale and impurities, and then cleaned and dried with dilute nitric acid and alcohol. The two plates are alternately stacked together, with the top layer being carbon steel plate T1 and the bottom layer being carbon steel plate T5;

[0089] 2) Prefabricate a blank assembly frame 1, whose internal dimensions are slightly larger than the length and width of the blank assembly plate, and whose height is the same as the thickness of the laminated plate. A suction hole 3 connected to the suction pipe 2 is formed on the long side of the blank assembly frame;

[0090] 3) The 9 layers of alternately stacked blank plates 5 are placed into the blank frame 1, and the gaps between the blank frame 1 and the upper carbon steel plate T1 and the lower carbon steel plate T5 are welded and sealed to form a weld (4), and vacuum is drawn through the exhaust pipe 2. When the vacuum degree reaches 0.001 Pa, the exhaust pipe is sealed;

[0091] 4) placing the multi-layer composite slab into a furnace and heating it to 1500° C. and keeping it warm for 1 hour, then rolling it with a rolling mill, the rolling temperature is between 1100° C. and 1000° C., and 6 hot rolling passes are performed, each pass has a reduction of 20%, and the rolling speed is 0.1 m / s, the carbon steel is deformed by rolling deformation, and the high chromium cast iron plate is necked and fractured and partially broken to form a dispersed high chromium cast iron 9, and the broken high chromium cast iron is covered with a deformed carbon steel layer 10 to form a composite material 8 of a high chromium cast iron dispersed carbon steel matrix;

[0092] 5) After rolling, air cool and remove the frame around the composite material.

[0093] The properties of the composite materials provided in Examples 1 to 3 and Comparative Examples 1 to 2 were tested respectively, wherein the test method for wear resistance was ASTM G99-05, and the test method for impact toughness was GBT 1817-1995. The results are shown in Table 1:

[0094] Table 1 Properties of the composite materials provided by Examples 1 to 3 and Comparative Examples 1 to 2

[0095]

[0096] It can be seen from Table 1 that the high chromium cast iron reinforced carbon steel wear-resistant composite material obtained by the preparation method provided by the present invention has better impact toughness and wear resistance, indicating that the technical scheme of the present invention achieves the purpose of improving the overall wear resistance of the composite material while maintaining the excellent toughness of carbon steel by controlling the controllable regular distribution of high chromium cast iron material in carbon steel and reducing the degree of stress damage of high chromium cast iron after rolling.

[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high chromium cast iron reinforced carbon steel wear-resistant composite material, comprising the following steps: (1) Regularly arranged cylindrical through holes are prepared on a carbon steel slab to obtain an intermediate substrate; (2) pouring high chromium cast iron melt into the cylindrical through hole in the intermediate substrate obtained in step (1) to obtain an intermediate slab; (3) welding a layer of carbon steel composite plate on the upper and lower sides of the intermediate slab obtained in step (2) to obtain a composite slab; (4) The composite slab obtained in step (3) is subjected to hot rolling and diffusion heat treatment in sequence to obtain a high-chromium cast iron reinforced carbon steel wear-resistant composite material.

2. The preparation method according to claim 1, characterized in that: In the step (1), the size of the cylindrical through hole and the size of the carbon steel slab satisfy the following relationship: H / D<2, 1.5D<E<2D, D<T<1.5D, wherein H is the thickness of the carbon steel slab, D is the diameter of the cylindrical through hole, E is the center distance between two adjacent cylindrical through holes, and T is the distance between the center of the cylindrical through hole and the edge of the carbon steel slab.

3. The preparation method according to claim 1, characterized in that: In the step (2), the intermediate substrate is preheated before pouring, the preheating temperature is 400-500° C., and the preheating time is 20-30 minutes.

4. The preparation method according to claim 1, characterized in that: The pouring temperature in step (2) is 1400-1500° C., and the pouring method is bottom pouring.

5. The preparation method according to claim 1, characterized in that: The relationship between the thickness h of the carbon steel composite plate in step (3) and the thickness H of the carbon steel slab in step (1) is: 0.2H<h<H.

6. The preparation method according to claim 1, characterized in that: The welding method in step (3) is as follows: the intermediate slab and the surfaces to be joined of the carbon steel composite plate are placed opposite to each other, then the slab is sealed and welded all around, vacuum is drawn from the reserved pipe, and finally the reserved pipe is heat-sealed.

7. The preparation method according to claim 1, characterized in that: In the step (4), the starting temperature of hot rolling is 1150-1200°C, and the final temperature of hot rolling is ≥1100°C.

8. The preparation method according to claim 1, characterized in that: In the step (4), the hot rolling single pass reduction is ≤10%, and the hot rolling speed is 0.5-2 m / s.

9. The preparation method according to claim 1, characterized in that: The temperature of the diffusion heat treatment in step (4) is 600-800° C., and the insulation time of the diffusion heat treatment is 20-60 min.

10. The high chromium cast iron reinforced carbon steel wear-resistant composite material prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Carbon steel-high-chromium cast iron composite high-wear-resistance plate and preparation method thereof

    CN121402444A

  • Carbon steel-high chromium cast iron composite high wear-resistant plate and preparation method thereof