Silicon monoxide negative electrode material and preparation method thereof

By using a double carbon layer-coated silicon oxide negative electrode material preparation method in lithium-ion batteries, the problems of low cycle performance and Coulombic efficiency of silicon oxide materials are solved, and the energy density and cycle stability of the battery are significantly improved.

CN118693258AActive Publication Date: 2024-09-24HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410731111.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-09-24
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Silicone oxide anode materials have low cycle performance and Coulombic efficiency in lithium-ion batteries, resulting in insufficient energy density and cycle stability, and cannot effectively replace traditional graphite anode materials.

Method used

A preparation method is adopted, which includes stirring an organic carbon source with silicon oxide and metal powder in an organic solvent and then sintering, and then drying it in an acid solvent, and forming a double layer under microwave heating by mixing a high molecular polymer and a conductive agent. Carbon layer coating improves the electrochemical performance of the material.

Benefits of technology

It improves the first Coulombic efficiency and long-term cycle stability of silicon oxide anode materials, enhances the mechanical properties and electrical properties of the material, and significantly improves the energy density and cycle life of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118693258A
    Figure CN118693258A
Patent Text Reader

Abstract

The invention discloses a silicon monoxide negative electrode material and a preparation method thereof. The preparation method comprises the following steps: mixing an organic carbon source and an organic solvent, stirring and dissolving to obtain a mixed solution, mixing the mixed solution with silicon monoxide and metal powder, stirring, standing, and sintering in inert gas to obtain a sintered material; mixing the sintered material, a solvent and acid, stirring, performing solid-liquid separation, and drying; mixing the dried material, a high-molecular polymer, an organic solvent and a conductive agent, stirring, and carrying out microwave heating in inert gas; according to the preparation method, the organic carbon source fully wraps the silicon monoxide under the liquid phase condition, so that the agglomeration of the material is reduced, and the uniformity of a coating layer is improved; siO2 can be partially reduced through high-temperature sintering of metal powder, volatilization of metal steam can be reduced through coating of an organic carbon layer, the reduction proportion of SiO2 is increased, and the first effect of a silicon monoxide material is improved; and a secondary coating layer with high integrity and good mechanical property is formed on the surface of the material through microwave heating, so that the long-cycle stability of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a silicon oxide negative electrode material and a preparation method thereof. Background Art

[0002] With the widespread application of lithium-ion batteries in power batteries and energy storage power stations, traditional graphite anode materials are currently unable to meet the market demand for high-energy-density lithium-ion batteries due to their own capacity limitations. Silicon-based anode materials have the advantages of abundant reserves and high capacity, and are considered to be one of the most promising anode materials for next-generation lithium-ion batteries. x ) is one of the most promising materials to replace traditional graphite anode as anode material for lithium-ion batteries due to its high theoretical specific capacity (1700mAh / g) and more stable cycle performance than other silicon-based anode materials. x The amorphous SiO2 phase (a-SiO2) reacts with lithium ions in an irreversible electrochemical reaction after the first few cycles to generate lithium silicates (Li2SiO3, Li4SiO4) and Li2O, which in turn causes poor first coulombic efficiency and irreversible consumption of lithium ions from the positive electrode in the entire battery, thereby reducing the actual energy density of lithium-ion batteries. In addition, another problem with silicon-based negative electrode materials is their poor cycle performance, which cannot replace commercial graphite negative electrode materials. The volume change of silicon oxide materials during the cycle (≈160%) is smaller than that of silicon-based negative electrode materials (≈300%), but it is still much higher than that of graphite materials (≈10%). This severe volume change is the main reason for the poor long-term cycle stability of silicon-based negative electrode materials.

[0003] At present, in terms of improving the first coulombic efficiency, the main method is to pre-lithiate the silicon-based negative electrode, including directly adding lithium powder, electrochemical pre-embedding lithium, etc., which can improve the first coulombic efficiency to a certain extent. However, the above modification methods still have many problems. In terms of improving the cycle performance of materials, carbon coating is often used in industry to improve the long cycle life of materials.

[0004] The Chinese patent application document with publication number CN111434609A provides a pre-lithiation lithium battery negative electrode material and a preparation method thereof, wherein a metal lithium source is added to an organic solvent, the obtained mixture is heated until the metal lithium source is melted, and the melted metal lithium source is stirred to disperse into particles to obtain a metal lithium source particle dispersion; a negative electrode active material is added to the metal lithium source particle dispersion, and the reaction is stirred for a predetermined time to obtain a pre-lithiation negative electrode active material, wherein the negative electrode active material includes a silicon-based material. However, there are still problems such as a complicated pre-lithiation process and poor cycle enhancement effect. Summary of the invention

[0005] The technical problem to be solved by the present invention is how to improve the cycle performance and coulombic efficiency of silicon monoxide negative electrode materials.

[0006] The present invention solves the above technical problems through the following technical means:

[0007] A method for preparing a silicon oxide negative electrode material comprises the following steps:

[0008] S1, mixing an organic carbon source and an organic solvent and stirring and dissolving them to obtain a mixed solution;

[0009] S2, mixing the mixed solution, silicon dioxide and metal powder, stirring and then letting it stand;

[0010] S3, sintering the material after standing in S2 in an inert gas to obtain a sintered material;

[0011] S4, mixing the sintering material, the solvent and the acid, stirring, separating the solid and the liquid and drying;

[0012] S5, mixing the dried material in S4, the high molecular polymer, the organic solvent and the conductive agent, stirring them, and heating them by microwave in an inert gas to obtain the silicon iodide negative electrode material.

[0013] Preferably, in S1, the organic carbon source is a mixture of one or more of polyvinyl alcohol, polyvinyl butyral, phenolic resin, tar, and glucose; and the organic solvent is a mixture of one or more of anhydrous ethanol, acetone, dichloromethane, tetrahydrofuran, and ethyl acetate.

[0014] Preferably, in S1, the mass ratio of the organic carbon source to the organic solvent is 1:8 to 1:19; and the stirring time is 1 to 2 hours.

[0015] Preferably, in S2, the median particle size of the silicon oxide is 3-5 μm; and the metal powder is a mixture of one or more of magnesium, aluminum, tin, iron, antimony, lithium and zinc powder.

[0016] Preferably, in S2, the mass ratio of silicon oxide to metal powder is 5:1-10:1; the mass ratio of silicon oxide to the organic carbon source in S1 is 40-50:5-16; the stirring time is 2-4 hours; and the standing time is 1-3 hours.

[0017] Preferably, in S3, the inert gas is a mixture of one or more of helium, argon and nitrogen; the sintering temperature is 600-800°C, the heating rate is 2-5°C / min, and the sintering time is 4-12h.

[0018] Preferably, in S4, the mass ratio of the solvent to the sintering material is 2:1 to 5:1; the mass ratio of the acid to the solvent is 1:4 to 1:10; the stirring time is 1 to 3 hours; the solvent is a mixture of one or more of water, acetone, anhydrous ethanol, dichloromethane and ethyl acetate; the acid is a mixture of one or more of acetic acid, sulfuric acid, hydrochloric acid and nitric acid.

[0019] Preferably, in S5, the high molecular polymer is at least one of polyacrylonitrile, polyacrylic acid, polyethylene glycol, and polyacrylamide; the organic solvent is at least one of dimethylformamide, dimethyl sulfoxide, cyclopentane, ethyl nitrate, and anhydrous ethanol; the conductive agent is at least one of Super-P, acetylene black, carbon nanotubes, and Ketjen black; the mass ratio of the high molecular polymer to the organic solvent is 1:5 to 1:12; the mass ratio of the high molecular polymer to the conductive agent is 19:1 to 9:1; the mass ratio of the dried material to the high molecular polymer is 20-30:5; in S5, the inert gas is a mixture of one or more of helium, argon, and nitrogen; the frequency of the microwave heating is 2450 MHz; and the microwave heating time is 3 to 5 min.

[0020] Preferably, in S4, the drying time is 6 to 12 hours, and the drying temperature is 60 to 100°C.

[0021] Preferably, in S5, the stirring time is 10 to 30 minutes.

[0022] The present invention also provides a silicon 2 oxide negative electrode material, which is prepared by adopting the preparation method of the silicon 2 oxide negative electrode material.

[0023] The present invention also provides a lithium ion battery, the negative electrode of which contains the silicon monoxide negative electrode material and graphite.

[0024] Preferably, the mass ratio of the silicon monoxide negative electrode material to graphite is 3:7.

[0025] The advantages of the present invention are:

[0026] The present invention provides a method for preparing a silicon oxide negative electrode material, wherein the silicon oxide negative electrode material is coated with a double carbon layer. The present invention uniformly stirs silicon oxide material, metal powder and organic carbon source in an organic solvent, and then sinters the mixture in an inert atmosphere, and obtains silicon oxide negative electrode material with improved electrical performance through secondary coating. The method allows the organic carbon source to fully wrap the silicon oxide material under liquid phase conditions, reduces the agglomeration of the material, and increases the uniformity of the coating layer; high-temperature sintering of metal powder will partially reduce SiO2, and the coating of the organic carbon layer will reduce the volatilization of metal vapor, increase the reduction ratio of SiO2, and improve the primary effect of the silicon oxide material; after the reaction, microwave heating technology can be used to form a secondary coating layer with high integrity and good mechanical properties on the surface of the material, forming a double carbon layer, and improving the long-cycle stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a SEM image of the silicon dioxide negative electrode material prepared in Example 1 of the present invention;

[0028] Figure 2 The first charge and discharge curves of the batteries prepared with the materials of Example 1 and Comparative Example 1 of the present invention at a current density of 0.1C;

[0029] Figure 3 The cycle performance curves of the full battery prepared with the materials of Example 1 of the present invention and Comparative Example 1 at a current density of 1C / 1C. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0032] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0033] Example 1

[0034] A method for preparing a silicon oxide negative electrode material comprises the following steps:

[0035] In a dry environment, weigh 45g of acetone solvent and pour it into a beaker, then add 5g of PVB powder and stir with a magnetic stirrer for 1h. Add 50g of silicon oxide powder with a median particle size of 3μm and 5g of magnesium powder to the obtained solution, continue stirring for 4h and let it stand for 2h. Transfer the material after standing to a tube furnace, heat it to 800℃ at a heating rate of 2℃ / min under argon atmosphere, sinter it at a constant temperature for 4h, and take it out after cooling to room temperature to obtain a sintered material. Take 50g of the sintered material and pour it into a beaker containing 250g of deionized water and 25g of acetic acid. After stirring for 1h, filter it for 20min and transfer it to a vacuum oven and dry it at 60℃ for 12h. Take 20g of the dried material, put it into a beaker, add 5g of polyacrylonitrile, 45g of dimethyl sulfoxide and 0.5g of Super-P, stir for 30min, pour it into an alumina crucible, transfer it to an argon atmosphere microwave heating furnace and heat it for 3min before taking it out, where the heating frequency is 2450MHz, and grind to obtain the silicon oxide negative electrode material.

[0036] Figure 1 The SEM image of the silicon oxide negative electrode material prepared in Example 1 shows that the particle size of the material is relatively uniform, and the particle size is about 5 μm. The prepared silicon oxide negative electrode material is slurried and coated according to the mass ratio of silicon oxide negative electrode material: SP: PAA = 8:1:1, and a CR2032 button battery is assembled. The electrolyte uses 1 mol / L LiPF6 EC+DMC+DEC (mass ratio is 1:1:1) solution, and the electrochemical performance is tested. The results are as follows Figure 2 As shown in Table 1, at a current density of 0.1C, the battery made of the material prepared in Example 1 has a first discharge capacity of 1560.3 mAh / g, a charge capacity of 1329.2 mAh / g, and a first coulombic efficiency of 85.2%.

[0037] Comparative Example 1

[0038] Commercial SiO / C material was used as the negative electrode material, and the slurry was mixed and coated according to the mass ratio of commercial SiO / C material: SP: PAA = 8:1:1, and CR2032 button batteries were assembled. The electrolyte used was 1 mol / L LiPF6 EC+DMC+DEC (mass ratio of 1:1:1) solution, and the electrochemical performance was tested. The results are as follows Figure 2As shown in Table 1, at a current density of 0.1C, the first discharge specific capacity of the battery made of the material of Comparative Example 1 is 2311.1mAh / g, the charging specific capacity is 1600.5mAh / g, and the first coulombic efficiency is 69.3%. By comparing Example 1 with Comparative Example 1, it can be found that the first coulombic efficiency of the battery made of the negative electrode material of Example 1 is improved by about 15.9%. Using NCM622 as the positive electrode, 30wt% of the negative electrode material of Comparative Example 1 and 70wt% of conventional graphite mixed material or 30wt% of the material prepared in Example 1 and 70wt% of conventional graphite mixed material as the negative electrode, 7Ah soft-pack batteries were assembled by slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The results are as follows: Figure 3 As shown, after 300 cycles of the full battery, the battery capacity retention rate made of the material in Comparative Example 1 is 89.5%. Figure 3 By comparing Example 1 with Comparative Example 1, it can be found that the cycle performance of the material prepared in Example 1 is improved by about 5.8% in the full battery. This is because the metal powder partially reduces SiO2 in the silicon oxide material, improves the first coulombic efficiency, and the double carbon layer coating further improves the cycle life of the battery.

[0039] Example 2

[0040] A method for preparing a silicon oxide negative electrode material comprises the following steps:

[0041] In a dry environment, weigh 140g of ethyl acetate solvent and pour it into a beaker, then add 10g of glucose powder and stir with a magnetic stirrer for 1h. Add 40g of silicon oxide powder with a median particle size of 4μm and 5g of aluminum powder to the obtained solution, continue stirring for 4h and let it stand for 2h. Transfer the material after standing to a tube furnace, heat it to 700℃ at a heating rate of 3℃ / min under argon atmosphere, sinter it at a constant temperature for 4h, and take it out after cooling to room temperature to obtain a sintered material. Take 50g of the sintered material and pour it into a beaker containing 150g of anhydrous ethanol and 25g of dilute hydrochloric acid. After stirring for 1h, filter it for 30min and transfer it to a vacuum oven and dry it at 60℃ for 12h. Take 20g of the dried material, put it into a beaker, add 5g of polyacrylonitrile, 45g of cyclopentane sulfone and 0.5g of Super-P, stir for 30min, pour it into an alumina crucible, transfer it to an argon atmosphere microwave heating furnace and heat it for 4min before taking it out, wherein the heating frequency is 2450MHz, and grind to obtain the silicon oxide negative electrode material.

[0042] The prepared silicon oxide negative electrode material was slurried and coated according to the mass ratio of silicon oxide negative electrode material: SP: PAA = 8:1:1, and CR2032 button batteries were assembled. The electrolyte used was 1 mol / L LiPF6 EC+DMC+DEC (mass ratio of 1:1:1) solution, and the electrochemical performance test was performed. The results are shown in Table 1. At a current density of 0.1C, the battery made of the material prepared in Example 2 has a first discharge capacity of 1500.7mAh / g, a charge capacity of 1257.6mAh / g, and a first coulombic efficiency of 83.8%.

[0043] Example 3

[0044] A method for preparing a silicon oxide negative electrode material comprises the following steps:

[0045] In a dry environment, weigh 160g of tetrahydrofuran solvent and pour it into a beaker, then add 16g of PVA powder and stir with a magnetic stirrer for 1h. Add 50g of silicon oxide powder with a median particle size of 5μm and 5g of lithium powder to the obtained solution, continue stirring for 3h and let it stand for 2h. Transfer the material after standing to a tube furnace, heat it to 600℃ at a heating rate of 5℃ / min under argon atmosphere, sinter it at a constant temperature for 8h, and take it out after cooling to room temperature to obtain a sintered material. Take 50g of the sintered material and pour it into a beaker containing 120g of anhydrous ethanol and 30g of acetic acid. After stirring for 1h, filter it for 30min and transfer it to a vacuum oven and dry it at 60℃ for 12h. Take 20g of the dried material, put it into a beaker, add 5g of polyacrylonitrile, 60g of cyclopentane sulfone and 0.5g of carbon nanotubes and stir for 20min, pour it into an alumina crucible, transfer it to an argon atmosphere microwave heating furnace and heat it for 5min before taking it out, wherein the heating frequency is 2450MHz, and grind to obtain the silicon oxide negative electrode material.

[0046] The prepared silicon oxide negative electrode material was slurried and coated according to the mass ratio of silicon oxide negative electrode material: SP: PAA = 8: 1: 1, and CR2032 button batteries were assembled. The electrolyte used was 1 mol / L LiPF6 EC+DMC+DEC (mass ratio of 1: 1: 1) solution, and the electrochemical performance test was performed. The results are shown in Table 1. At a current density of 0.1C, the battery made of the material prepared in Example 3 had a first discharge capacity of 1486.8 mAh / g, a charge capacity of 1344.1 mAh / g, and a first coulombic efficiency of 90.4%.

[0047] Example 4

[0048] A method for preparing a silicon oxide negative electrode material comprises the following steps:

[0049] In a dry environment, weigh 120g of tetrahydrofuran solvent and pour it into a beaker, then add 15g of phenolic resin powder and stir with a magnetic stirrer for 2h. Add 40g of silicon oxide powder with a median particle size of 3μm and 5g of tin powder to the obtained solution, continue stirring for 2h and let it stand for 3h. Transfer the material after standing to a tube furnace, heat it to 800℃ at a heating rate of 4℃ / min under argon atmosphere, sinter it at a constant temperature for 8h, and take it out after cooling to room temperature to obtain a sintered material. Take 50g of the sintered material and pour it into a beaker containing 150g of acetone and 30g of acetic acid. After stirring for 1h, filter it for 30min and transfer it to a vacuum oven and dry it at 60℃ for 12h. Take 30g of the dried material, put it into a beaker, add 5g of polyacrylic acid, 45g of cyclopentane sulfone and 0.5g of Ketjen black and stir for 30min, pour it into an alumina crucible, transfer it to an argon atmosphere microwave heating furnace and heat it for 3min before taking it out, wherein the heating frequency is 2450MHz, and grind to obtain the silicon oxide negative electrode material.

[0050] The prepared silicon oxide negative electrode material was slurried and coated according to the mass ratio of silicon oxide negative electrode material: SP: PAA = 8: 1: 1, and a CR2032 button battery was assembled. The electrolyte used was a 1 mol / L LiPF6 EC+DMC+DEC (mass ratio of 1: 1: 1) solution, and the electrochemical performance test was performed. The results are shown in Table 1. At a current density of 0.1C, the battery made of the material prepared in Example 4 has a first discharge capacity of 1509.3 mAh / g, a charge capacity of 1269.3 mAh / g, and a first coulombic efficiency of 84.1%.

[0051] Table 1

[0052] First discharge specific capacity / mAh / g First charge specific capacity / mAh / g First coulombic efficiency Comparative Example 1 2311.1 1600.5 69.3% Example 1 1560.3 1329.2 85.2% Example 2 1500.7 1257.6 83.8% Example 3 1486.8 1344.1 90.4% Example 4 1509.3 1269.3 84.1%

[0053] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a silicon oxide negative electrode material, Features: The following steps are involved: S1, mixing an organic carbon source and an organic solvent and stirring and dissolving them to obtain a mixed solution; S2, mixing the mixed solution, silicon dioxide and metal powder, stirring and then letting it stand; S3, sintering the material after standing in S2 in an inert gas to obtain a sintered material; S4, mixing the sintering material, the solvent and the acid, stirring, separating the solid and the liquid and drying; S5, mixing the dried material in S4, the high molecular polymer, the organic solvent and the conductive agent, stirring them, and heating them by microwave in an inert gas to obtain the silicon iodide negative electrode material.

2. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S1, the organic carbon source is a mixture of one or more of polyvinyl alcohol, polyvinyl butyral, phenolic resin, tar, and glucose; the organic solvent is a mixture of one or more of anhydrous ethanol, acetone, dichloromethane, tetrahydrofuran, and ethyl acetate.

3. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S1, the mass ratio of the organic carbon source to the organic solvent is 1:8 to 1:19; and the stirring time is 1 to 2 hours.

4. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S2, the median particle size of the silicon oxide is 3 to 5 μm; and the metal powder is a mixture of one or more of magnesium, aluminum, tin, iron, antimony, lithium, and zinc powder.

5. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S2, the mass ratio of silicon oxide to metal powder is 5:1-10:1; the mass ratio of silicon oxide to the organic carbon source in S1 is 40-50:5-16; the stirring time is 2-4 hours; and the standing time is 1-3 hours.

6. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S3, the inert gas is a mixture of one or more of helium, argon, and nitrogen; the sintering temperature is 600-800°C, the heating rate is 2-5°C / min, and the sintering time is 4-12h.

7. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S4, the mass ratio of the solvent to the sintering material is 2:1 to 5:1; the mass ratio of the acid to the solvent is 1:4 to 1:10; the stirring time is 1 to 3 hours; the solvent is a mixture of one or more of water, acetone, anhydrous ethanol, dichloromethane and ethyl acetate; the acid is a mixture of one or more of acetic acid, sulfuric acid, hydrochloric acid and nitric acid.

8. The method for preparing the silicon 2 oxide negative electrode material according to claim 1, Features: In S5, the high molecular polymer is at least one of polyacrylonitrile, polyacrylic acid, polyethylene glycol, and polyacrylamide; the organic solvent is at least one of dimethylformamide, dimethyl sulfoxide, cyclopentane, ethyl nitrate, and anhydrous ethanol; the conductive agent is at least one of Super-P, acetylene black, carbon nanotubes, and Ketjen black; the mass ratio of the high molecular polymer to the organic solvent is 1:5 to 1:12; the mass ratio of the high molecular polymer to the conductive agent is 19:1 to 9:1; the mass ratio of the dried material to the high molecular polymer is 20-30:5; the inert gas is a mixture of one or more of helium, argon, and nitrogen; the frequency of the microwave heating is 2450 MHz; and the time of the microwave heating is 3 to 5 minutes.

9. A silicon oxide negative electrode material, Features: The silicon monoxide negative electrode material is prepared by the method for preparing the silicon monoxide negative electrode material according to any one of claims 1 to 8.

10. A lithium ion battery, Features: The negative electrode thereof contains the silicon monoxide negative electrode material as claimed in claim 9 and graphite.

Citation Information

Patent Citations

  • Lithium-ion battery silicon monoxide negative electrode material, preparation method and application thereof

    CN110767877A

  • Silicon-based negative electrode material, preparation method thereof and lithium ion battery

    CN111342020A

  • Modified conductive polymer coated silicon-based anode material and preparation method and application thereof

    CN111785949A

  • Pre-lithiated silicon monoxide negative electrode material, preparation method thereof, negative electrode and lithium ion battery

    CN116062759A

  • Preparation method of pre-lithiated silicon monoxide negative electrode material

    CN116177553A