Metal ceramic composite material

By impregnating the silicon carbide ceramic phase with alloys and/or intermetallic compounds containing Cu and Si, and adjusting the proportion of added elements, a good dispersion state of the ceramic phase and the metal phase is formed, which solves the problems of antibacterial and mechanical properties of existing composite materials. Insufficient performance, achieving highly effective antibacterial and antiviral effects.

CN118715192AActive Publication Date: 2024-09-27MITSUI MINING & SMELTING CO LTD

Patent Information

Application Number
CN202280091610.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2022-12-19
Publication Date
2024-09-27
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

It is difficult for existing composite materials containing silicon carbide and copper to balance strength, hardness and antibacterial properties, and existing antibacterial floor materials are not effective in preventing infectious diseases.

Method used

By impregnating the silicon carbide ceramic phase with alloys and/or intermetallic compounds containing Cu and Si, and adjusting the proportion of added elements, a good dispersion state of the ceramic phase and the metal phase is formed to improve the antibacterial effect of the composite material.

Benefits of technology

A new type of metal-ceramic composite material with excellent mechanical properties and antibacterial effect has been realized, which is suitable for antibacterial and antiviral applications in construction and medical environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118715192A
    Figure CN118715192A
Patent Text Reader

Abstract

The purpose of the present invention is to provide a novel cermet composite material having an antibacterial effect in which a ceramic phase containing silicon carbide and a metal phase containing Cu and Si are dispersed and mixed with each other. Disclosed is a cermet composite material containing a ceramic phase of silicon carbide and a metal phase containing an alloy of Cu and Si and / or an intermetallic compound in a mutually dispersed state, the metal phase containing at least one metal additive element M other than Cu or Si, the silicon carbide occupying more than half of the total mass of the constituent materials of the ceramic phase, when an image having an area of 256 [mu] m * 192 [mu] m is acquired at 500 magnification using a scanning electron microscope (SEM), the area ratio A / B of the ceramic phase / metal phase is 2-60, and when a is the mass fraction (%) of Si in the metal phase and m is the mass fraction (%) of the added element M, the relational expressions 0.01 < = m / a < = 1.4 and 0.3 < = m < = 20 are satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal-ceramic composite material, and more specifically, to a metal-ceramic composite material having an antibacterial effect, wherein a ceramic phase containing silicon carbide and a metal phase containing Cu and Si are dispersed and mixed with each other. Background Art

[0002] Ceramic materials formed of silicon carbide (SiC) are lightweight and have excellent wear resistance, high-temperature mechanical strength, and corrosion resistance. On the other hand, since silicon carbide is a brittle material with low toughness, the development of composite materials with an excellent balance of toughness and thermal conductivity is promoted by combining silicon carbide with copper (Cu) or copper alloys as high thermal conductivity materials. It is known that such composite materials containing silicon carbide and copper can be used in a wide range of applications such as heat sealing materials, packaging materials, semiconductor substrates, brake discs, etc. for electronic equipment, semiconductor devices, etc. (for example, refer to Patent Document 1).

[0003] For example, Patent Document 2 discloses a metal-ceramic composite material containing a Si-Cu alloy and a SiC ceramic, wherein the Si-Cu alloy has a Si:Cu content of 60 to 30% by mass: 40 to 70% by mass. According to the document, it is reported that by having such a Si:Cu content, a composite material having improved toughness and suppressed reduction in Young's modulus and increase in density can be provided.

[0004] In addition, Patent Document 3 discloses a high thermal conductivity composite material in which Cu is infiltrated into a porous SiC preform constituting a skeleton structure and an anti-reaction layer is formed between the two. According to this document, it is reported that a composite material having high thermal conductivity and low thermal expansion coefficient suitable for use as a thermal diffusion material for electronic devices and semiconductor devices can be provided.

[0005] However, from the perspective of promoting the health and hygiene of humans and animals, and preventing infectious diseases, attempts have been made to develop materials with improved antibacterial and antiviral properties as plate-like components used in various articles, structural materials constituting buildings, bridges, ships, railways, roads, ports, etc., floor materials, wall materials, ceilings and other building materials. In addition, in recent years, under the social conditions where malignant colds and infectious diseases are prevalent, such demands are increasing. For example, in livestock sheds such as cattle, pigs, and birds, in order to mainly prevent infectious diseases and achieve a stable supply of products, it is necessary to improve the sanitary environment by preventing the growth and reproduction of bacteria. As floor materials for livestock sheds, grid-like floor materials made of concrete or castings have been used, and attempts have been made to improve durability and antibacterial properties. However, such grid-like floor materials made of concrete or castings cannot fully exert their antibacterial and antiviral properties.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-165787

[0009] Patent Document 2: Japanese Patent Application Publication No. 2004-035307

[0010] Patent Document 3: Japanese Patent Application Publication No. 2003-002770 Summary of the invention

[0011] Problems to be solved by the invention

[0012] A composite material containing silicon carbide and copper that has been proven to have sufficient antibacterial properties has not been reported so far. The present inventors have conducted research and found that since it is difficult to infiltrate copper or copper alloys, especially materials forming metal phases containing Cu and Si, into the ceramic phase of silicon carbide, the infiltration is low, and thus it is difficult to achieve both mechanical properties such as strength and hardness and antibacterial properties in the composite material, and internal cracks may occur in some cases. Therefore, it is desirable to develop a composite material containing silicon carbide and copper that has good mechanical properties such as strength and hardness and exhibits excellent antibacterial properties.

[0013] Therefore, the first problem that the present invention aims to solve is to provide a novel metal-ceramic composite material which is not available in the prior art and in which a ceramic phase containing silicon carbide and a metal phase containing Cu and Si are mutually dispersed and mixed and which has an antibacterial effect.

[0014] Another problem to be solved by the present invention is to provide a novel metal-ceramic composite material having good mechanical properties such as strength and hardness and excellent antibacterial properties, in which a ceramic phase containing silicon carbide and a metal phase containing Cu and Si are dispersed and mixed with each other.

[0015] Means for solving problems

[0016] The present inventors conducted intensive research and found that when a ceramic containing silicon carbide is impregnated with an alloy and / or an intermetallic compound containing Cu and Si, by adjusting the alloy and / or the intermetallic compound so that a specified amount of at least one metal additive element other than Cu or Si is contained, and the ceramic phase and the metal phase in the resulting metal-ceramic composite material have a specified area ratio, a metal-ceramic composite material having a greatly improved impregnation state and an excellent antibacterial effect is formed, thereby completing the present invention.

[0017] That is, the main aspects of the present invention as a means for solving the above-mentioned problems are as follows.

[0018] A metal-ceramic composite material, comprising a ceramic phase and a metal phase in a mutually dispersed state, wherein the ceramic phase comprises silicon carbide, and the metal phase comprises an alloy and / or an intermetallic compound containing Cu and Si.

[0019] The metal phase contains at least one metal additive element M other than Cu or Si, and

[0020] The silicon carbide accounts for more than half of the total mass of the constituent materials of the ceramic phase.

[0021] Here,

[0022] When an image of an area of ​​256 μm×192 μm is obtained at 500 times using a scanning electron microscope (SEM) for the above-mentioned metal-ceramic composite material, with respect to the area of ​​the entire image, the percentage (%) of the total area of ​​the above-mentioned ceramic phase is set as A, and the percentage (%) of the total area of ​​the above-mentioned metal phase is set as B, the area ratio A / B of the ceramic phase / metal phase is greater than 2 and less than 60, and

[0023] In the above-mentioned metal phase, when the mass percentage (%) of Si is set to a and the mass percentage (%) of the added element M is set to m relative to the total mass, the following relationship is satisfied:

[0024] 0.01≤m / a≤1.4, and

[0025] 0.3≤m≤20.

[0026] Effects of the Invention

[0027] According to the present invention, a novel metal-ceramic composite material which is not available in the prior art and in which a ceramic phase containing silicon carbide and a metal phase containing Cu and Si are dispersed and mixed with each other and has antibacterial and antiviral effects can be provided.

[0028] According to a preferred embodiment of the metal-ceramic composite material of the present invention, the presence of a specified amount of additional element M in the metal phase containing Cu and Si brings about a good infiltration state of the metal-ceramic composite material. Furthermore, due to this good infiltration state, while exerting excellent mechanical properties such as strength and hardness, the excellent antibacterial and antiviral properties brought by copper can be exerted.

[0029] According to another preferred embodiment of the metal-ceramic composite material of the present invention, by adjusting the area ratio of the ceramic phase containing silicon carbide and the metal phase containing Cu and Si, the mass ratio of the added element M in the metal phase relative to Si, and the mass ratio of Cu in the metal phase relative to Si to the specified range, the infiltration state of the metal-ceramic composite material becomes better, and the improved mechanical properties, especially the porosity (density of the sintered body), bending strength and hardness (for example, Vickers hardness: indentation hardness) and excellent antibacterial and antiviral effects can be achieved in a well-balanced manner. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is an example of an image of the metal-ceramic composite material according to one embodiment of the present invention obtained by a scanning electron microscope (SEM) at a magnification of 500. DETAILED DESCRIPTION

[0031] 1. Metal-ceramic composites

[0032] The metal-ceramic composite material of the present invention contains a ceramic phase and a metal phase in a mutually dispersed state, wherein the ceramic phase contains silicon carbide (SiC), and the metal phase contains an alloy and / or an intermetallic compound containing Cu and Si, and the metal phase contains at least one metal additive element M other than Cu or Si, and the silicon carbide occupies more than half of the total mass of the constituent materials of the ceramic phase.

[0033] The respective amounts (mass %) of silicon carbide, free carbon, Cu, Si and added elements M constituting the metal phase, and inevitable impurities in the metal-ceramic composite material can be identified using XRF (fluorescent X-ray analysis method), ICP emission spectrometer and carbon analysis device (combustion-infrared absorption method).

[0034] In this specification, the portion obtained by removing silicon carbide and free carbon from the total analyzed elements (each mass %) thus identified is regarded as a metal phase containing inevitable impurities, and the ratio of the elements in the metal phase is calculated.

[0035] There is no limitation except that silicon carbide in the ceramic phase containing silicon carbide of the metal-ceramic composite material accounts for more than half of the total mass of the constituent materials of the ceramic phase, that is, more than 50 mass %.

[0036] The ceramic phase of the metal-ceramic composite material may contain less than 50% by mass of ceramic materials other than silicon carbide. Examples of such ceramic materials other than silicon carbide are not particularly limited, but include silicon nitride (Si3N4), aluminum nitride (AlN), boron nitride (BN), titanium nitride (TiN), zirconium nitride (ZrN), boron carbide (B4C), tantalum carbide (TaC), niobium carbide (NbC), titanium carbide (TiC), zirconium carbide (ZrC), chromium carbide (Cr3C2), molybdenum carbide (Mo2C), tungsten carbide (WC), etc.

[0037] The proportion of silicon carbide in the ceramic phase of the metal-ceramic composite material can be more preferably 55 mass %, 60 mass %, 65 mass %, 70 mass %, 75 mass %, 80 mass %, 85 mass %, 90 mass %, 95 mass %, 96 mass %, 97 mass %, 98 mass %, 99 mass %, or substantially 100 mass %. In one embodiment, the ceramic phase can be formed only by silicon carbide (excluding other ceramic materials) except a small amount of free carbon. The higher the proportion of silicon carbide in the ceramic phase is within the range of more than 50 mass %, the higher the wear resistance, corrosion resistance and strength of silicon carbide as the characteristics of the metal-ceramic composite material can be embodied.

[0038] The ceramic phase of the metal-ceramic composite material may contain a small amount of free carbon. Free carbon refers to carbon atoms that exist independently without forming chemical bonds with silicon atoms or other metal atoms in the ceramic phase or near the interface between the ceramic phase and the metal phase. The content of free carbon in the ceramic phase is not particularly limited. For example, it can usually be less than 5% by mass, and typically, it can be less than 3% by mass, relative to the total weight of the ceramic phase.

[0039] The ratio of Cu to the total mass of the metal phase of the metal-ceramic composite material can usually be 60 mass % or more and 95 mass % or less, preferably 65 mass % or more and 90 mass % or less. In addition, the ratio of Si to the total mass of the metal phase of the metal-ceramic composite material can usually be 3 mass % or more and 35 mass % or less, preferably 5 mass % or more and 30 mass % or less.

[0040] The ratio of the alloy and / or intermetallic compound comprising Cu and Si relative to the total mass of the metal phase of the metal-ceramic composite material can usually be more than 70 mass %, preferably more than 71 mass %, more than 72 mass %, more than 73 mass %, more than 74 mass %, more than 75 mass %, more than 76 mass % or more than 77 mass %. In addition, the ratio can usually be less than 99.7 mass %, preferably less than 99.5 mass %, less than 99 mass %, less than 98 mass %, less than 97 mass %, less than 96 mass %, less than 95 mass %, less than 94 mass %, less than 93 mass %, less than 92 mass %, less than 91 mass %, less than 90 mass %, less than 88 mass %, less than 86 mass % or less than 84 mass %. By making the ratio of the alloy and / or intermetallic compound comprising Cu and Si in the metal phase within the above range, the strength and thermal conductivity as copper characteristics, as well as antibacterial and antiviral properties can be more highly embodied in the metal-ceramic composite material.

[0041] The ratio of the alloy and / or intermetallic compound containing Cu and Si to the total mass of the metal phase of the metal-ceramic composite material can generally be more than 70% by mass to less than 99.7% by mass, preferably 70% by mass to 99.5% by mass, 70% by mass to 99% by mass, 70% by mass to 98% by mass, 70% by mass to 97% by mass, 70% by mass to 96% by mass, 70% by mass to 95% by mass, 70% by mass to 94% by mass, 70% by mass to 93% by mass, ...8% by mass, 70% by mass to 99% by mass, 70% by mass to 99% by mass, 70% by mass to 99% by % to 92% by mass, 70% to 91% by mass, 70% to 90% by mass, 70% to 88% by mass, 70% to 86% by mass, 70% to 84% by mass, 71% to less than 99.7% by mass, 71% to 99.5% by mass, 71% to 99% by mass, 71% to 98% by mass, 71% to 97% by mass, 71% to 96% by mass, 71% to 95% by mass % by mass or less, 71% by mass or more and 94% by mass or less, 71% by mass or more and 93% by mass or less, 71% by mass or more and 92% by mass or less, 71% by mass or more and 91% by mass or less, 71% by mass or more and 90% by mass or less, 71% by mass or more and 88% by mass or less, 71% by mass or more and 86% by mass or less, 71% by mass or more and 84% by mass or less, 72% by mass or more and less than 99.7% by mass, 72% by mass or more and 99.5% by mass or less, 72% by mass or more and 99% by mass or less, 72% by mass or more and 98% by mass or less, 7 2 mass % to 97 mass %, 72 mass % to 96 mass %, 72 mass % to 95 mass %, 72 mass % to 94 mass %, 72 mass % to 93 mass %, 72 mass % to 92 mass %, 72 mass % to 91 mass %, 72 mass % to 90 mass %, 72 mass % to 88 mass %, 72 mass % to 86 mass %, 72 mass % to 84 mass %, 73 mass % to less than 99.7 mass %, 73 mass % to 99.5 mass % or less, 73 mass % or more to 99 mass % or less, 73 mass % or more to 98 mass % or less, 73 mass % or more to 97 mass % or more, 73 mass % or more to 96 mass % or less, 73 mass % or more to 95 mass % or less, 73 mass % or more to 94 mass % or more, 73 mass % or more to 93 mass % or less, 73 mass % or more to 92 mass % or less, 73 mass % or more to 91 mass % or less, 73 mass % or more to 90 mass % or less, 73 mass % or more to 88 mass % or less, 73 mass % or more to 86 mass % or less, 73 mass % or more to 84 mass % or less, 74 mass % or more to less than 99.7 mass %, 74 mass % or more to 99. 5 mass % or less, 74 mass % or more to 99 mass % or less, 74 mass % or more to 98 mass % or less, 74 mass % or more to 97 mass % or more, 74 mass % or more to 96 mass % or less, 74 mass % or more to 95 mass % or less, 74 mass % or more to 94 mass % or less, 74 mass % or more to 93 mass % or less, 74 mass % or more to 92 mass % or less, 74 mass % or more to 91 mass % or less, 74 mass % or more to 90 mass % or less, 74 mass % or more to 88 mass % or less, 74 mass % or more to 86 mass % or less, 74 mass % or more to 84 mass % or less, 75 mass % or more to less than 99.7 mass %, 75 mass % or more to 99. 5 mass % or less, 75 mass % or more to 99 mass % or less, 75 mass % or more to 98 mass % or less, 75 mass % or more to 97 mass % or more, 75 mass % or more to 96 mass % or less, 75 mass % or more to 95 mass % or less, 75 mass % or more to 94 mass % or more, 75 mass % or more to 93 mass % or less, 75 mass % or more to 92 mass % or less, 75 mass % or more to 91 mass % or more, 75 mass % or more to 90 mass % or less, 75 mass % or more to 88 mass % or less, 75 mass % or more to 86 mass % or less, 75 mass % or more to 84 mass % or more, 76 mass % or more to less than 99.7 mass %, 76 mass % or more to 99. 5 mass % or less, 76 mass % or more to 99 mass % or less, 76 mass % or more to 98 mass % or less, 76 mass % or more to 97 mass % or less, 76 mass % or more to 96 mass % or more, 76 mass % or more to 95 mass % or less, 76 mass % or more to 94 mass % or less, 76 mass % or more to 93 mass % or less, 76 mass % or more to 92 mass % or less, 76 mass % or more to 91 mass % or less, 76 mass % or more to 90 mass % or less, 76 mass % or more to 88 mass % or less, 76 mass % or more to 86 mass % or less, 76 mass % or more to 84 mass % or less, 77 mass % or more to less than 99.7 mass %, 77 mass % or more to 99.5 mass % or less, 77 mass % or more to 99 mass % or less, 77 mass % or more to 98 mass % or less, 77 mass % or more to 97 mass % or less, 77 mass % or more to 96 mass % or more, 77 mass % or more to 95 mass % or less, 77 mass % or more to 94 mass % or less, 77 mass % or more to 93 mass % or less, 77 mass % or more to 92 mass % or less, 77 mass % or more to 91 mass % or more, 77 mass % or more to 90 mass % or less, 77 mass % or more to 88 mass % or less, 77 mass % or more to 86 mass % or less, or 77 mass % or more to 84 mass %.

[0042] At least one metal additive element M other than Cu or Si in the metal phase of the metal-ceramic composite material is an element other than Cu or Si, and is not particularly limited thereto, and may contain at least one selected from the group consisting of Ni (nickel), Pd (palladium), Mg (magnesium), Ca (calcium), Zn (zinc), Ti (titanium), Zr (zirconium), S (sulfur), Mo (molybdenum), W (tungsten), Fe (iron), Mn (manganese), V (vanadium), Nb (niobium), Ta (tantalum) and Y (yttrium). Preferably, the additive element M may contain at least one selected from the group consisting of Ni, Mg, Zn and Ti. The additive element M more preferably contains Ni.

[0043] The additional element M may contain a combination of two elements or a combination of three or more elements among the above-exemplified Ni, Pd, Mg, Ca, Zn, Ti, Zr, S, Mo, W, Fe, Mn, V, Nb, Ta and Y. Preferably, the additional element M may contain a combination of two elements or a combination of three or more elements among Ni, Mg, Zn and Ti. In the case where the additional element M contains a combination of two elements, for example, the combination may be Ni / Mg, Ni / Zn, Ni / Ti, Mg / Zn, Mg / Ti, or Zn / Ti. In the case where the additional element M contains a combination of three elements, for example, the combination may be Ni / Mg / Zn, Ni / Mg / Ti, or Mg / Zn / Ti.

[0044] In one embodiment, the additional element M is only at least one selected from the group consisting of Ni, Pd, Mg, Ca, Zn, Ti, Zr, S, Mo, W, Fe, Mn, V, Nb, Ta and Y, and does not include any other elements. In a preferred embodiment, the additional element M is only at least one selected from the group consisting of Ni, Mg, Zn and Ti, and does not include any other elements. In another embodiment, the additional element M is a combination of two elements of Ni, Pd, Mg, Ca, Zn, Ti, Zr, S, Mo, W, Fe, Mn, V, Nb, Ta and Y, and does not include any other elements; or is a combination of two elements of Ni / Mg, Ni / Zn, Ni / Ti, Mg / Zn, Mg / Ti, or Zn / Ti, and does not include any other elements. In another embodiment, the added element M is a combination of three elements selected from the group consisting of Ni, Pd, Mg, Ca, Zn, Ti, Zr, S, Mo, W, Fe, Mn, V, Nb, Ta, and Y, and does not include any other elements; or is a combination of three elements selected from the group consisting of Ni / Mg / Zn, Ni / Mg / Ti, or Mg / Zn / Ti, and does not include any other elements.

[0045] When the added element M includes Ni, the mass ratio of Ni relative to the total mass of the added element M can be 5 mass% or more and 100 mass% or less (i.e., only Ni), preferably 10 mass% or more and 100 mass% or less, 20 mass% or more and 100 mass% or less, 30 mass% or more and 100 mass% or less, 40 mass% or more and 100 mass% or less, 50 mass% or more and 100 mass% or less, 60 mass% or more and 100 mass% or less, 70 mass% or more and 100 mass% or less, 80 mass% or more and 100 mass% or less, or 90 mass% or more and 100 mass% or less.

[0046] The metal phase of the metal-ceramic composite material contains Cu, Si, and at least one metal additive element M other than Cu or Si, and also contains impurities inevitably mixed in without active addition operation, so-called unavoidable impurities.

[0047] The inevitable impurities may also include any impurities known to be included in known metal-ceramic composite materials. The inevitable impurities are not particularly limited, and examples thereof include Mn, Sr, Sn, P, Cr, etc. The content of the inevitable impurities in the metal phase is not particularly limited, and may be 5% by mass or less relative to the total mass of the metal phase.

[0048] For the metal-ceramic composite material of the present invention, when an image of an area of ​​256 μm×192 μm is obtained at 500 times using a scanning electron microscope (SEM), when the percentage (%) of the total area of ​​the ceramic phase is set to A and the percentage (%) of the total area of ​​the metal phase is set to B relative to the area of ​​the entire image, the area ratio A / B of the ceramic phase / metal phase is greater than 2 and less than 60.

[0049] In addition, in the metal phase of the metal-ceramic composite material of the present invention, when the mass percentage (%) of Si is a and the mass percentage (%) of the additive element M is m relative to the total mass, the following relationship holds.

[0050] 0.01≤m / a≤1.4, and

[0051] 0.3≤m≤20.

[0052] According to the metal-ceramic composite material of the present invention, by fully satisfying the area ratio A / B of the ceramic phase / metal phase within the above-mentioned specific range and the above-mentioned two relationship formulas, it becomes easy to form a good infiltration state in which the ceramic phase containing silicon carbide and the metal phase containing Cu and Si are fully dispersed and mixed with each other. Since the metal phase has a good infiltration state with respect to the ceramic phase, the original characteristics of the silicon carbide contained in the ceramic phase, namely wear resistance, corrosion resistance and strength, and the original characteristics of the copper of the copper alloy contained in the metal phase, namely strength, thermal conductivity, antibacterial and antiviral properties can be more effectively exerted. Therefore, in the present invention, by fully satisfying the area ratio A / B of the ceramic phase / metal phase within the above-mentioned specific range and the above-mentioned two relationship formulas, it is preferred that the infiltration state of the metal phase with respect to the ceramic phase becomes good, thereby obtaining a metal-ceramic composite material with improved mechanical properties, especially porosity (density of the sintered body), bending strength and hardness (such as Vickers hardness: indentation hardness), and antibacterial effect and antiviral effect.

[0053] The metal-ceramic composite material of the present invention contains a ceramic phase and a metal phase in a mutually dispersed state, wherein the ceramic phase contains silicon carbide, and the metal phase contains an alloy and / or an intermetallic compound containing Cu and Si, that is, the ceramic phase and the metal phase are mutually dispersed and mixed. Therefore, for the metal-ceramic composite material, when a scanning electron microscope (SEM) is used to obtain an image of an area of ​​256 μm×192 μm at a magnification of 500, due to the dispersion and mixing state of the ceramic phase and the metal phase, the calculated reproducibility of the area ratio A / B of the percentage A(%) of the total area of ​​the ceramic phase / the percentage B(%) of the total area of ​​the metal phase in the image is generally high, so it is sufficient to use only one field of view for the image usually obtained. From the viewpoint of further improving the accuracy of the calculated reproducibility of A / B, it is also possible to obtain images in any two or more fields of view, calculate the average value of the area ratio A / B in these images, and then regard the average value as the area ratio A / B of the material.

[0054] exist Figure 1 An example of an image of a metal-ceramic composite material according to an embodiment of the present invention obtained by a scanning electron microscope (SEM) at a magnification of 500 is shown in FIG. The embodiment of the image is an example in which Ni is added as an additive element M at a ratio of 5 mass % relative to the total mass of the metal phase of the composite material. In the image, the white portion is a metal phase containing a copper alloy and the additive element Ni, and the gray portion is a ceramic phase with SiC as the main component, and it can be observed that the two phases are dispersed and mixed with each other.

[0055] For the metal-ceramic composite material of the present invention, when an image with an area of ​​256 μm×192 μm is obtained at a magnification of 500 using a scanning electron microscope (SEM), the area ratio A / B of the ceramic phase / metal phase relative to the area of ​​the entire image is 2 or more and 60 or less, preferably 2.5 or more and 50 or less, and more preferably 3 or more and 45 or less, 3 or more and 40 or less, 3 or more and 35 or less, 3 or more and 30 or less, 3 or more and 25 or less, 3 or more and 20 or less, 3 or more and 15 or less, 3 or more and 10 or less, 3 or more and 8 or less, 3.3 or more and 8 or less, 3.5 or more and 8 or less, 3.7 or more and 8 or less, 3 or more and 5 or less, 3.3 or more and 5 or less, 3.5 or more and 5 or less, 3.7 or more and 5 or less, 3 or more and 4.5 or less, 3.3 or more and 4.5 or less, 3.5 or more and 4.5 or less, or 3.7 or more and 4.5 or less.

[0056] By making the area ratio A / B of the ceramic phase / metal phase relative to the overall area of ​​the above-mentioned scanning electron microscope (SEM) image within the above-mentioned range, it is preferred that the infiltration of the metal into the ceramic phase is well performed, thereby obtaining a metal-ceramic composite material in which the reduction of porosity (density of the sintered body), bending strength and hardness (for example, Vickers hardness: indentation hardness) and any one of the antibacterial effect and antiviral effect is effectively suppressed and which has a good balance of properties.

[0057] In the metal phase of the metal-ceramic composite material of the present invention, when the mass percentage (%) of the added element M relative to the total mass is defined as m, 0.3≤m≤20 holds true. In another embodiment, the range of m is not particularly limited, and for example, it can be selected from the range of 0.5≤m≤20, 1≤m≤20, 2≤m≤20, 3≤m≤20, 4≤m≤20, 5≤m≤20, 0.3≤m≤18, 0.5≤m≤18, 1≤m≤18, 2≤m≤18, 3≤m≤18, 4≤m≤18, 5≤m≤18, 0.3≤m≤16, 0.5≤m≤16, 1≤m≤16, 2≤m≤16, 3≤m≤16, 4≤m≤16, or 5≤m≤16.

[0058] In addition, in the metal phase of the metal-ceramic composite material of the present invention, relative to the total mass, when the mass percentage (%) of Si is set to a and the mass percentage (%) of the added element M is set to m, the relationship of 0.01≤m / a≤1.4 holds true, preferably 0.05≤m / a≤1.2, and more preferably 0.1≤m / a≤1, 0.15≤m / a≤1, 0.2≤m / a≤1, 0.25≤m / a≤1, 0.3≤m / a≤1, 0.35≤m / a≤1, 0.4≤m / a≤1, 0.45≤m / a≤1, 0.5≤m / a≤1, 0.1≤m / a<1, 0.15≤m / a<1, 0.2≤m / a<1, 0.25≤m / a<1, 0.3≤m / a<1, 0.35≤m / a <1, 0.4≤m / a<1, 0.45≤m / a<1, 0.5≤m / a<1, 0.1≤m / a≤0.9, 0.15≤m / a≤0.9, 0.2≤m / a≤0.9, 0.25≤m / a≤0.9, 0.3≤m / a≤0.9, 0.35≤m / a≤0.9, 0.4≤m / a≤0.9, 0.45≤m / a ≤0.9, 0.5≤m / a≤0.9, 0.1≤m / a≤0.8, 0.15≤m / a≤0.8, 0.2≤m / a≤0.8, 0.25≤m / a≤0.8, 0.3≤m / a≤0.8, 0.35≤m / a≤0.8, 0.4≤m / a≤0.8, 0.45≤m / a≤0.8, or 0.5≤m / a≤0.8.

[0059] By making the ratio m / a of the mass percentage a(%) of Si to the mass percentage m(%) of the added element M within the above range, the infiltration of the metal relative to the ceramic phase is preferably carried out well, so that the porosity (density of the sintered body) is maintained at an appropriate value, resulting in the further improvement of the characteristic balance of good bending strength and hardness (for example, Vickers hardness: indentation hardness).

[0060] In another embodiment, in the metal-ceramic composite material of the present invention, when the area ratio A / B of the ceramic phase / metal phase relative to the entire area of ​​the above-mentioned scanning electron microscope (SEM) image is greater than 5 (and less than 60), the ratio of the mass percentage m (%) of the added element M to the mass percentage a (%) of Si is preferably m / a<1. In addition, when the above-mentioned area ratio A / B is greater than 5 (and less than 60), it is more preferably 0.1≤m / a<1, 0.15≤m / a<1, 0.2≤m / a<1, 0.25≤m / a<1, 0.3≤m / a<1, 0.35≤m / a<1, 0.4≤m / a<1, 0.45≤m / a<1, 0.5≤m / a<1, 0.1≤m / a≤0.9, 0.15≤m / a≤0.9, 0.2≤m / a≤0.9, 0.25≤m / a≤0.9 , 0.3≤m / a≤0.9, 0.35≤m / a≤0.9, 0.4≤m / a≤0.9, 0.45≤m / a≤0.9, 0.5≤m / a≤0.9, 0.1≤m / a≤0.8, 0.15≤m / a≤0.8, 0.2≤m / a≤0.8, 0.25≤m / a≤0.8, 0.3≤m / a≤0.8, 0.35≤m / a≤0.8, 0.4≤m / a≤0.8, 0.45≤m / a≤0.8, or 0.5≤m / a≤0.8.

[0061] In a metal-ceramic composite material, when the area ratio A / B of the ceramic phase / metal phase is greater than 5 (and less than 60), that is, even when the proportion of the metal phase impregnated in the ceramic phase is relatively small, by m / a<1, or satisfying the above-mentioned more preferred ratio, the infiltration of the two phases will become easier, and the porosity (density of the sintered body), bending strength and hardness (for example, Vickers hardness: indentation hardness) and the balance of antibacterial and antiviral effects can be appropriately maintained.

[0062] In the metal phase of the metal-ceramic composite material of the present invention, when the mass percentage (%) of Cu is set to b and the mass percentage (%) of Si is set to a relative to the total mass as described above, it is preferred that the relationship of b / a ≥ 2.5 holds. In the metal phase, by making the mass ratio of Cu to Si satisfy this relationship, a metal-ceramic composite material with further improved porosity (density of the sintered body), bending strength and hardness, and a balance between antibacterial and antiviral effects can be obtained.

[0063] From the viewpoint of improving the balance of the above characteristics, the mass percentage (%) b of Cu in the metal phase and the mass percentage (%) a of Si are more preferably b / a≥3, more preferably b / a≥3.5, and even more preferably b / a≥4. In particular, from the viewpoint of improving the porosity (density of the sintered body) and bending strength, the mass percentage (%) b of Cu in the metal phase and the mass percentage (%) a of Si are more preferably b / a≥4.5, and even more preferably b / a≥5.

[0064] The upper limit of the ratio b / a of the mass percentage (%) b of Cu to the mass percentage (%) a of Si in the metal phase is not particularly limited, but from the viewpoint of fully obtaining the effect of improving the hardness (e.g., Vickers hardness: indentation hardness), the relationship of b / a≤20 is preferably established, and b / a≤18, b / a≤16, or b / a≤14 is more preferably established.

[0065] In another embodiment, the ratio b / a of the mass percentage (%) b of Cu to the mass percentage (%) a of Si in the metal phase may be preferably 2.5≤b / a≤20, 2.5≤b / a≤18, 2.5≤b / a≤16, 2.5≤b / a≤14, 3≤b / a≤20, 3≤b / a≤18, 3≤b / a≤16, 3≤b / a≤14, 3.5≤b / a≤20, 3.5≤b / a≤18, 3.5≤b / a≤16, 3.5≤b / a≤14, 4≤b / a≤20, 4≤b / a≤18, 4≤b / a≤16, 4≤b / a≤14, 4.5≤b / a≤20, 4.5≤b / a≤18, 4.5≤b / a≤16, or 4.5≤b / a≤14.

[0066] As described above, the metal phase of the metal-ceramic composite material contains Cu, Si and the additive element M, and in addition, contains inevitable impurities such as Mn, Sr, Sn, P, Cr, etc. Therefore, the sum of the mass percentage a (%) of Si, the mass percentage b (%) of Cu and the mass percentage m (%) of the additive element M in the metal phase is not 100 mass%. In the metal phase of the metal-ceramic composite material, from the viewpoint of forming a good infiltration state in which the ceramic phase containing silicon carbide and the metal phase containing Cu and Si are fully dispersed and mixed with each other, and effectively exerting the wear resistance, corrosion resistance and strength inherent in silicon carbide and the strength, thermal conductivity and antibacterial and antiviral properties inherent in copper of the copper alloy, it is preferably a+b+m≥95 (mass%), more preferably a+b+m≥96 (mass%), and further preferably a+b+m≥97 (mass%), a+b+m≥98 (mass%) or a+b+m≥99 (mass%).

[0067] From the viewpoint of further improving the infiltration state of the metal relative to the ceramic phase and further improving the resulting porosity (density of the sintered body), bending strength and hardness (for example, Vickers hardness: indentation hardness) and the balance of antibacterial and antiviral effects, it is more preferred that: in the metal-ceramic composite material of the present invention, the area ratio A / B of the ceramic phase / metal phase relative to the overall area of ​​the above-mentioned scanning electron microscope (SEM) image is 5 or less (and 2 or more), and the ratio of the mass percentage m (%) of the element M added in the metal phase to the mass percentage a (%) of Si is m / a<1 (and 0.01 or more), and the ratio of the mass percentage b (%) of Cu to the mass percentage a (%) of Si is b / a≥3.

[0068] It is further preferred that: in the metal-ceramic composite material, the area ratio A / B of the ceramic phase / metal phase is 4.5 or less, and the ratio of the mass percentage m(%) of the added element M to the mass percentage a(%) of Si is m / a≤0.9, and the ratio of the mass percentage b(%) of Cu to the mass percentage a(%) of Si is b / a≥3.5. It is further preferred that: in the metal-ceramic composite material, the area ratio A / B of the ceramic phase / metal phase is 4.5 or less, and the ratio of the mass percentage m(%) of the added element M to the mass percentage a(%) of Si is m / a≤0.8, and the ratio of the mass percentage b(%) of Cu to the mass percentage a(%) of Si is b / a≥4.

[0069] In a preferred embodiment, the metal-ceramic composite material of the present invention can be used as an anti-pathogen material that exerts antibacterial and antiviral effects, that is, can be used as an antibacterial and antiviral material.

[0070] Examples of the target bacteria include Staphylococcus aureus, Klebsiella pneumoniae, Pseudomonas aeruginosa, Escherichia coli, Moraxella osloensis, and methicillin-resistant Staphylococcus aureus.

[0071] In addition, examples of target viruses include bacteriophage Qβ, bacteriophage Φ6, influenza virus, coronavirus, and human immunodeficiency virus.

[0072] The antibacterial effect and the antiviral effect can be specifically evaluated by the test described below.

[0073] In a preferred embodiment, the antibacterial effect R of the metal-ceramic composite material of the present invention can be 2.0 or more when measured using Staphylococcus aureus as the test bacteria according to JIS Z2801:2012 and JIS R1752:2020 cited therein. It should be noted that, as the culture conditions of the test piece inoculated with the test bacterial solution in the determination of the antibacterial effect, JIS Z2801:2012 stipulates that the action temperature is 35±1°C and the action time is 24±1 hours, but the culture and measurement here are carried out in the dark under the conditions of the action temperature of 25°C and the action time of 6 hours. In addition, JIS R1752:2020 stipulates that the light irradiation time of the test piece inoculated with the test bacterial solution is 8 hours, but the culture and measurement here are carried out in the dark under the condition of 6 hours without light irradiation.

[0074] Specific measurement conditions for the antibacterial effect can be typically set as follows.

[0075] · Unprocessed product name: SLG glass

[0076] ·Test product size: 50mm×50mm×5mm

[0077] ·N number: n=2

[0078] Test bacteria: Staphylococcus aureus (NBRC12732)

[0079] Sterilization of test products: heating in a dry sterilizer (80°C, 15 minutes)

[0080] ·Action conditions: Action temperature: 25°C, Action time: 6 hours, in the dark

[0081] · Bacterial count measurement using agar medium

[0082] The antibacterial effect R is more preferably 2.5 or more, further preferably 3.0 or more, further preferably 3.5 or more, further preferably 3.9 or more, further preferably 4.2 or more, and most preferably 4.5 or more. The upper limit of the antibacterial effect R is not particularly limited, and in practice, about 5.5 to 6 can be the upper limit.

[0083] When the antibacterial effect R of the metal-ceramic composite material of the present invention is 2.0 or more, or preferably within the above range, the composite material can be more suitably used in a wide range of applications as a material having antibacterial properties.

[0084] In a preferred embodiment, the antiviral effect R of the metal-ceramic composite material of the present invention can be 2.5 or more when measured using bacteriophage Qβ or bacteriophage Φ6 as a test phage according to ISO18071:2016 and JIS R1756:2020. It should be noted that in the determination of the antiviral effect, as the culture conditions of the test piece inoculated with the test solution, ISO18071:2016 and JIS R1756:2020 stipulate that the action time of visible light irradiation is 4 hours, but the culture and measurement here are carried out in the dark without light irradiation and under the condition of an action time of 6 hours.

[0085] Specific conditions for measuring the antiviral effect can be typically set as follows.

[0086] · Unprocessed product name: SLG glass

[0087] ·Test product size: 50mm×50mm×4mm

[0088] ·N number: n=2

[0089] Test phage: phage Qβ (NBRC20012) or phage Φ6 (NBRC105899)

[0090] Sterilization of test products: heating in a dry sterilizer (80°C, 15 minutes)

[0091] ·Action conditions: Action temperature: 25°C, Action time: 6 hours, in the dark

[0092] Infectivity value measurement using agar medium

[0093] The antiviral effect R is more preferably 3.0 or more, further preferably 3.5 or more, further preferably 4.0 or more, further preferably 4.5 or more, further preferably 4.6 or more, and most preferably 4.7 or more. The upper limit of the antiviral effect R is not particularly limited, and in practice, about 6.5 to 7 can be the upper limit.

[0094] When the antiviral effect R of the metal-ceramic composite material of the present invention is 2.5 or more, or preferably within the above range, the composite material can be more suitably used as a material having antiviral properties in a wide range of applications.

[0095] In another embodiment, the above-mentioned action temperature and action time in the culture conditions for measuring the antibacterial effect and the antiviral effect can be changed according to the bacteria and viruses used. The action temperature can be appropriately selected within the range of 10°C to 40°C. For example, in the case of testing by culturing Escherichia coli, the action temperature can be set to 37°C where its growth and reproduction are active for culturing. In addition, it can be cultured with an appropriate action time in the range of 2 hours to 72 hours or more according to the growth and reproduction rate of the bacteria and viruses used. For example, in the case of a virus with a slow growth and reproduction rate, the action time can be set to 96 hours for culturing.

[0096] It is very advantageous that the metal-ceramic composite material of the preferred embodiment of the present invention can be used as an antipathogen material that can fully exert antibacterial and antiviral effects even in the dark. That is, according to the metal-ceramic composite material of the preferred embodiment, an antipathogen material that can exert antibacterial and antiviral effects regardless of the illumination can be provided.

[0097] In a preferred embodiment, the porosity of the metal-ceramic composite material of the present invention measured by the Archimedean method according to JIS R1634:1998 can be 10% or less. The porosity is more preferably 9% or less, further preferably 8% or less, further preferably 7% or less, further preferably 6% or less, further preferably 5% or less, and most preferably 4% or less. The lower limit of the porosity (as long as it is 0% or more) is not particularly limited, and in practice, about 2 to 3% can be the lower limit.

[0098] By setting the porosity of the metal-ceramic composite material of the present invention to 10% or less, or preferably within the above range, it is easy to obtain a composite material having a further improved density of a sintered body and a higher hardness.

[0099] In a preferred embodiment, when the metal-ceramic composite material of the present invention is measured by the Archimedean method according to JIS R1634:1998, the relative density [D1 / D2]×100 of the bulk density D1 of the metal-ceramic composite material relative to the true density D2 of the metal phase of the metal-ceramic composite material can be 90% or more. The relative density is more preferably 91% or more, further preferably 92% or more, further preferably 93% or more, further preferably 94% or more, and most preferably 95% or more.

[0100] When the relative density of the metal-ceramic composite material of the present invention is 90% or more, or preferably within the above range, it is easy to obtain a composite material having a higher hardness and further improved density of the sintered body, similarly to the case where the porosity is not more than the prescribed upper limit.

[0101] In a preferred embodiment, the flexural strength of the metal-ceramic composite material of the present invention measured by a three-point flexural strength test according to JIS R1601: 2008 may be 230 MPa or more. The flexural strength is more preferably 250 MPa or more, further preferably 270 MPa or more, further preferably 280 MPa or more, further preferably 290 MPa or more, and most preferably 300 MPa or more.

[0102] By setting the bending strength of the metal-ceramic composite material of the present invention to 230 MPa or more, or preferably within the above range, the mechanical strength against bending operation is further improved, and the metal-ceramic composite material can be more suitably used in a wide range of applications requiring high bending resistance.

[0103] In a preferred embodiment, the metal-ceramic composite material of the present invention may have a Vickers hardness of 25 GPa or more as measured by a 5-point average using a 1-point load test according to JIS R1610: 2003. The Vickers hardness is more preferably 26 GPa or more, further preferably 26.5 GPa or more, further preferably 27 GPa or more, further preferably 27.5 GPa or more, and most preferably 28 GPa or more.

[0104] By setting the Vickers hardness of the metal-ceramic composite material of the present invention to 25 GPa or more, or preferably within the above range, the robustness against pressing operation is further improved, and the metal-ceramic composite material can be more suitably used in a wide range of applications requiring high rigidity.

[0105] The metal-ceramic composite material of the present invention can be processed into various shapes for use. The shape is not particularly limited and can be a film, a sheet, a thin plate, a thick plate, a roughly prism, a roughly cylindrical, etc.

[0106] In addition, the metal-ceramic composite material of the present invention can be applied to a wide range of applications requiring antibacterial and antiviral properties. For example, the composite material can be suitably used as a component of various articles, a structural material constituting buildings, bridges, ships, railways, roads, ports, etc., a floor material of a building including a floor material of a livestock house, a wall material, a ceiling, and other building materials.

[0107] 2. Manufacturing method of metal-ceramic composite material

[0108] The method for producing the metal-ceramic composite material of the present invention is not particularly limited as long as a metal-ceramic composite material having the above-mentioned structure and characteristics can be obtained as a result. The metal-ceramic composite material of the present invention can be produced, for example, as described below.

[0109] For example, as a first step, a preform of a porous ceramic sintered body is formed from a ceramic phase forming material containing a majority of silicon carbide (SiC), and as a subsequent second step, the preform is infiltrated with a metal phase forming material under pressure, thereby manufacturing the metal-ceramic composite material of the present invention, wherein the metal phase forming material contains an alloy and / or an intermetallic compound containing Cu and Si melted at a high temperature and an additive element M. The types of other substances that may be contained in the ceramic phase forming material in addition to silicon carbide, the additive element M contained in the metal phase forming material, and the inevitable impurities are as described above with respect to the metal-ceramic composite material.

[0110] By appropriately adjusting the mass ratio of the ceramic phase forming material used in the above-mentioned first step and the metal phase forming material used in the above-mentioned second step, the mass ratio of Cu and Si in the alloy and / or intermetallic compound, and the mass ratio of the alloy and / or intermetallic compound containing Cu and Si and the added element M in the metal phase forming material, it is possible to obtain the metal-ceramic composite material of the present invention that satisfies the area ratio A / B of the ceramic phase / metal phase within the specified range, the mass percentage m(%) of the added element M within the specified range, the ratio of the mass percentage m(%) of the added element M within the specified range / the mass percentage a(%) of Si, and preferably the ratio of the mass percentage b(%) of Cu / the mass percentage a(%) of Si within the specified range.

[0111] In the first step, the silicon carbide contained as the main component in the ceramic phase forming material can be a commercially available high-purity silicon carbide raw material powder. The preform of the porous ceramic sintered body can be produced, for example, by a so-called recrystallization method, which means that a ceramic phase forming material containing a majority of silicon carbide is molded by a molding method such as mold molding, and then maintained at a high temperature of usually 2000°C or more, preferably 2200°C or more.

[0112] Alternatively, a mixture containing high-purity silicon (Si) particles and carbon (C) particles is heated at a temperature above 1400°C to react and sinter, thereby obtaining a preform of a porous ceramic sintered body containing silicon carbide. In the case of the reaction sintering method, from the viewpoint of formability and high density of the preform, it is also preferred to use a binder such as phenolic resin and asphalt (a substance carbonized by sintering) together with the high-purity carbon powder. Carbon fiber can also be used as a carbon source. The porosity of the preform of the porous ceramic sintered body obtained in the first step is not particularly limited, and can be, for example, 10% to 70%.

[0113] In the above-mentioned second step, the metal phase forming material containing the alloy and / or intermetallic compound containing Cu and Si and the additional element M can be melted in advance at a high temperature of usually more than 1000° C., preferably more than 1200° C. The metal phase forming material containing the alloy and / or intermetallic compound containing Cu and Si and the additional element M melted at such a high temperature can be impregnated into the preform of the porous ceramic sintered body obtained in the above-mentioned first step in a high pressure container under a pressure of usually more than 1 MPa, preferably more than 3 MPa.

[0114] As another method, a preform serving as a precursor of a ceramic sintered body can be formed from a ceramic phase-forming material containing a majority of silicon carbide (SiC), and the preform is then sintered and simultaneously impregnated with a metal phase-forming material containing an alloy and / or intermetallic compound containing Cu and Si melted at a high temperature and an added element M.

[0115] The alloy and / or intermetallic compound containing Cu and Si is not particularly limited, and may be any known alloy and / or intermetallic compound. For example, as the alloy, Cu3Si, Cu5Si, Cu6Si, Cu7Si, etc. may be used.

[0116] As a non-limiting specific example, a preform of a porous ceramic sintered body is immersed in a metal phase forming material containing an alloy and / or an intermetallic compound containing Cu and Si melted at a high temperature and an additive element M and maintained for a predetermined time (e.g., 10 seconds to 200 seconds), and then the preform that has been immersed is placed under pressure for a predetermined time (e.g., 30 seconds to 300 seconds), thereby allowing the preform to be impregnated as a whole. Before immersing the preform of a porous ceramic sintered body in the metal phase forming material melted at a high temperature, the preform may be preheated separately by heating and melting the metal phase forming material.

[0117] Preferably, in the second step, the preform of the porous ceramic sintered body is immediately cooled after the metal phase forming material molten at a high temperature is impregnated into the preform. The cooling can be performed quickly by introducing a cooling gas into a high-pressure container for melt infiltration and circulating the gas. Alternatively, the preform after melt infiltration can be cooled by contacting the preform with a cooling metal.

[0118] With respect to the metal-ceramic composite material and the method for manufacturing the same, the present invention has been described with reference to a number of embodiments, but it should be understood that the various constituent elements of these embodiments can be arbitrarily combined within the scope of the present invention. That is, it should be noted that the present invention is not limited to these embodiments, and the scope of the present invention is limited only by the appended claims.

[0119] Example

[0120] The present invention is further illustrated below with reference to examples, but the present invention is not limited to these examples.

[0121] Example 1

[0122] The metal-ceramic composite material of Example 1 was produced in the following manner.

[0123] <1st step>

[0124] 10% by mass (3% by mass in terms of carbon) of phenolic resin as an organic binder is mixed with 70% by mass of commercially available SiC powder fine particles (manufactured by Saint-Gobain, with an average particle size of 3 μm) and 30% by mass of coarse particles (manufactured by Shinano Electric Refining Co., Ltd., with an average particle size of 20 μm), and the mixture is preformed and then heat-treated at 1000°C for 3 hours in a nitrogen atmosphere to form a preform having a filling rate of 75% by volume after carbonizing the phenolic resin.

[0125] <Step 2>

[0126] Commercially available copper powder (manufactured by High Purity Chemical Research Institute, average particle size 3 μm), silicon powder (manufactured by High Purity Chemical Research Institute, average particle size 100 μm) and nickel powder (manufactured by High Purity Chemical Research Institute, average particle size 3 μm) were used and mixed in a crucible. At this time, the mass ratio of the ceramic phase forming material used in the first step and the metal phase forming material used in the second step was set to 1:1, the ratio of copper (Cu) to silicon (Si) in the metal phase forming material was set to 7:3, and the mass ratio of the added element Ni relative to the total mass of the metal phase forming material was set to 0.5 mass%. The preform obtained in the first step was infiltrated with the molten Cu-Si-Ni alloy under an argon atmosphere at a temperature of 1500°C for 3 hours to produce a metal-ceramic composite material.

[0127] The area ratio A / B of the ceramic phase / metal phase of the obtained metal-ceramic composite material (the determination method is described later) is 3.5, and the mass ratio b / a of Cu to Si in the metal phase (the determination method is described later) is 4.0. In addition, relative to the total mass of the metal phase forming material, the mass ratio of Si is 19.8 mass%, the mass ratio of Cu is 79.6 mass%, and the mass ratio of the added element Ni is 0.5 mass% (the determination method is described later).

[0128] Example 2

[0129] The metal ceramic composite material was manufactured in the same manner as in Example 1 except that the mass ratio of the added element Ni relative to the total mass of the metal phase forming material was changed to 5.0 mass %. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.6, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 4.2. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 18.0 mass %, the mass ratio of Cu was 76.0 mass %, and the mass ratio of the added element Ni was 5.0 mass % (the determination method is described later).

[0130] Example 3

[0131] The metal ceramic composite material was manufactured in the same manner as in Example 1 except that the mass ratio of the added element Ni relative to the total mass of the metal phase forming material was changed to 16.0 mass %. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 4.7, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 5.7. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 11.8 mass %, the mass ratio of Cu was 67.2 mass %, and the mass ratio of the added element Ni was 16.0 mass % (the determination method is described later).

[0132] Example 4

[0133] As an additive element, Mg powder (manufactured by High Purity Chemical Research Institute, with a particle size of 180 μm or less) was used instead of Ni powder, and the mass ratio of the additive element Mg relative to the total mass of the metal phase forming material was changed to 5.0 mass %. The metal ceramic composite material was manufactured in the same manner as in Example 1. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.6, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 4.3. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 17.8 mass %, the mass ratio of Cu was 76.0 mass %, and the mass ratio of the additive element Mg was 5.0 mass % (the determination method is described later).

[0134] Example 5

[0135] As an additive element, Zn powder (produced by High Purity Chemical Research Institute, with a particle size of 75 μm or less) was used instead of Ni powder, and the mass ratio of the additive element Zn relative to the total mass of the metal phase forming material was changed to 5.0 mass%. The metal ceramic composite material was manufactured in the same manner as in Example 1. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.9, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 4.2. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 18.0 mass%, the mass ratio of Cu was 76.0 mass%, and the mass ratio of the additive element Zn was 5.0 mass% (the determination method is described later).

[0136] Example 6

[0137] As an additive element, Ti powder (produced by High Purity Chemical Research Institute, with a particle size of 45 μm or less) was used instead of Ni powder, and the mass ratio of the additive element Ti relative to the total mass of the metal phase forming material was changed to 5.0 mass%. The metal ceramic composite material was manufactured in the same manner as in Example 1. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.6, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 4.1. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 18.7 mass%, the mass ratio of Cu was 76.0 mass%, and the mass ratio of the additive element Ti was 5.0 mass% (the determination method is described later).

[0138] Example 7

[0139] As an additive element, a mixture of Ni / Ti powder (mass ratio 2:1) was used instead of Ni powder, and the mass ratio of the additive element Ni / Ti mixture relative to the total mass of the metal phase forming material was changed to 6.0 mass %. The metal ceramic composite material was manufactured in the same manner as in Example 1. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.7, and the mass ratio b / a of Cu to Si in the metal phase (the determination method is described later) was 4.8. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 15.8 mass %, the mass ratio of Cu was 75.2 mass %, and the mass ratio of the additive element Ni / Ti was 6.0 mass % (the determination method is described later).

[0140] Example 8

[0141] The ratio of copper (Cu) to silicon (Si) in the metal phase forming material was set to 6:4, and the mass ratio of the additive element Ni relative to the total mass of the metal phase forming material was changed to 5.0 mass %. The metal ceramic composite material was manufactured in the same manner as in Example 1. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.5, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 2.7. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 25.1 mass %, the mass ratio of Cu was 67.9 mass %, and the mass ratio of the additive element Ni was 5.0 mass % (the determination method is described later).

[0142] Example 9

[0143] The ratio of copper (Cu) to silicon (Si) in the metal phase forming material was set to 8:2, and the mass ratio of the additive element Ni relative to the total mass of the metal phase forming material was changed to 5.0 mass %. The metal ceramic composite material was manufactured in the same manner as in Example 1. The area ratio A / B of the ceramic phase / metal phase of the obtained metal ceramic composite material (the determination method is described later) was 3.7, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 13.2. In addition, relative to the total mass of the metal phase of the obtained metal ceramic composite material, the mass ratio of Si was 6.5 mass %, the mass ratio of Cu was 85.5 mass %, and the mass ratio of the additive element Ni was 5.0 mass % (the determination method is described later).

[0144] Comparative Example 1

[0145] The metal-ceramic composite material was manufactured in the same manner as in Example 1 except that the mass ratio of the ceramic phase forming material used in the first step and the metal phase forming material used in the second step was changed, and the mass ratio of the additive element Ni relative to the total mass of the metal phase forming material was changed to 23 mass %. The area ratio A / B of the ceramic phase / metal phase of the obtained metal-ceramic composite material (the determination method is described later) was 15.0, and the mass ratio b / a of Cu relative to Si in the metal phase (the determination method is described later) was 5.7. In addition, relative to the total mass of the metal phase of the obtained metal-ceramic composite material, the mass ratio of Si was 15 mass %, the mass ratio of Cu was 85 mass %, and the mass ratio of the additive element Ni was 23 mass % (the determination method is described later).

[0146] Comparative Example 2

[0147] The metal-ceramic composite material was manufactured in the same manner as in Example 1 except that the mass ratio of the ceramic phase forming material used in the first step and the metal phase forming material used in the second step was changed and the additive element M was not added. The area ratio A / B of the ceramic phase / metal phase of the obtained metal-ceramic composite material (the determination method is described later) was 1.5, and the mass ratio b / a of Cu to Si in the metal phase (the determination method is described later) was 4.0. In addition, the mass ratio of Si was 20 mass % and the mass ratio of Cu was 80 mass % (the determination method is described later) relative to the total mass of the metal phase of the obtained metal-ceramic composite material.

[0148] Comparative Example 3

[0149] The metal-ceramic composite material was manufactured in the same manner as in Example 1 except that the mass ratio of the ceramic phase forming material used in the first step and the metal phase forming material used in the second step was changed and the additive element M was not added. The area ratio A / B of the ceramic phase / metal phase of the obtained metal-ceramic composite material (the determination method is described later) was 63.3, and the mass ratio b / a of Cu to Si in the metal phase (the determination method is described later) was 4.0. In addition, the mass ratio of Si was 20 mass % and the mass ratio of Cu was 80 mass % (the determination method is described later) relative to the total mass of the metal phase of the obtained metal-ceramic composite material.

[0150] Comparative Example 4

[0151] A silicon carbide (SiC) sintered body was produced from the ceramic phase forming material by the same procedure as in Example 1. For comparison, the properties were measured and evaluated without impregnating the ceramic phase forming material.

[0152] Determination of various properties of composite materials

[0153] (1) Determination and calculation of the area ratio A / B of the ceramic phase / metal phase

[0154] Using a scanning electron microscope (SEM) ("JSM-IT200" manufactured by JEOL Ltd.), images of an area of ​​256 μm × 192 μm were obtained at a magnification of 500 for each metal-ceramic composite material of Examples 1 to 9 and Comparative Examples 1 to 3. Relative to the area of ​​the entire image, the percentage (%) of the total area of ​​the ceramic phase (gray area) is set as A, and the percentage (%) of the total area of ​​the metal phase (white area) is set as B, and the area ratio A / B of the ceramic phase / metal phase is calculated. In principle, the total area percentage of each of the two phases is measured from the image of one field of view to calculate the area ratio. As an additional step selected at will, images can be obtained from any two or more fields of view, and the average value of the area ratio A / B in these images can be calculated, and it is confirmed that the average value is substantially the same as the area ratio obtained from the image of the above-mentioned one field of view. In the case of calculating the average value in this way, when it is found that there is a difference of 0.1 or more between the area ratio of the former (one field of view) and the area ratio of the latter (the average value of multiple fields of view), the latter value is adopted as the area ratio.

[0155] Table 1 shows the area ratio A / B of the ceramic phase / metal phase of each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 3.

[0156] (2) Identification and determination of the composition of the metal phase

[0157] Using XRF (fluorescent X-ray analysis), ICP emission spectrometer and carbon / sulfur analyzer (combustion-infrared absorption method), the amounts (mass %) of silicon carbide, free carbon, Cu, Si and added element M constituting the metal phase, and inevitable impurities in each metal-ceramic composite material of Examples 1 to 9 and Comparative Examples 1 to 3 were identified. When performing the above three measurements, the sample of the metal-ceramic composite material was crushed into powder and analyzed.

[0158] XRF (X-ray fluorescence analysis) is to place the crushed sample in a cup holder dedicated to powder analysis and identify the main components and impurity elements such as ceramics, copper, silicon, and added metals contained in the sample. The fluorescent X-ray analyzer used is "Supermini20" manufactured by Rigaku Corporation.

[0159] ICP emission spectrometry is to add hydrochloric acid to the pulverized sample to decompose the components at room temperature, and use an ICP emission spectrometer to measure the emission intensity of each element, thereby performing quantitative analysis on the elements measured by XRF. The ICP emission spectrometer used is "Agilent 5110" manufactured by Agilent Technologies, Inc.

[0160] Free carbon and silicon carbide (SiC) were measured using a carbon / sulfur analyzer (combustion-infrared absorption method). The measurement was performed in accordance with JIS R 2011:2007 "Chemical analysis method for refractory materials containing carbon and silicon carbide". It should be noted that for silicon carbide (SiC), an indirect method (total carbon and free carbon were measured, and the difference in carbon was converted to silicon carbide) was used. The carbon / sulfur analyzer used was "EMIA-810W" manufactured by Horiba, Ltd., which utilizes combustion in an oxygen flow (tubular electric furnace method)-infrared absorption method.

[0161] In addition, based on these identification and measurement results, the ratio m / a of the mass percentage m(%) of the added element M / the mass percentage a(%) of Si in the metal phase of the metal-ceramic composite material and the ratio b / a of the mass percentage b(%) of Cu / the mass percentage a(%) of Si are calculated.

[0162] The mass percentage a(%) of Si, the mass percentage b(%) of Cu, the mass percentage m(%) of the added element M, the ratio m / a of the mass percentage m(%) of the added element M / the mass percentage a(%) of Si, and the ratio b / a of the mass percentage b(%) of Cu / the mass percentage a(%) of Si in the metal phase of each metal-ceramic composite material of Examples 1 to 9 and Comparative Examples 1 to 3 are shown in Table 1 together with the type of the added element M.

[0163] It should be noted that in the manufacture of metal-ceramic composites, the amount of metal in the metal phase-forming material prepared as a powder mixture before infiltration is greater than the amount of metal in the preform infiltrated with the ceramic phase-forming material, and it is also possible that the various metal species including the additional element M constituting the metal phase-forming material are not completely evenly mixed during infiltration. Therefore, it is considered that theoretically it is also possible that the mass percentage of the additional element M in the metal phase-forming material is not completely consistent with the mass percentage of the additional element M in the metal phase of the metal-ceramic composite material actually manufactured.

[0164] In each of Examples 1 to 9 and Comparative Example 1 described above, the mass percentage of the additive element M in the metal phase forming material is consistent with the mass percentage of the additive element M in the metal phase of the metal-ceramic composite material actually produced.

[0165] (3) Evaluation of impregnation status

[0166] The impregnation state of each metal-ceramic composite material of Examples 1 to 9 and Comparative Examples 1 to 3 was observed by the appearance after the impregnation treatment. The evaluation criteria of the impregnation state are shown below. The evaluation results are shown in Table 2.

[0167] ○ (good): The whole surface is impregnated.

[0168] △(moderate): No local penetration.

[0169] × (bad): No penetration.

[0170] (4) Whether there are internal cracks in the composite material

[0171] In the scanning electron microscope (SEM) images of each metal-ceramic composite material of Examples 1 to 9 and Comparative Examples 1 to 3 obtained in the same manner as in (1) above, the presence or absence of internal cracks was confirmed. When no internal cracks were confirmed in the image at a magnification of 250, the image at a magnification of 500 was also confirmed. The evaluation criteria are shown below. The evaluation results are shown in Table 2.

[0172] ○ (good): No internal cracks were generated even in an image at a magnification of 500 times.

[0173] × (bad): Internal cracks occurred in the image at a magnification of 250 or 500 times.

[0174] (5) Determination of antibacterial activity (antibacterial effect R)

[0175] For each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 4, the antibacterial effect R was measured in the dark at an action temperature of 25° C. and an action time of 6 hours using Staphylococcus aureus as a test bacteria according to JIS Z2801: 2012 and JIS R1752: 2020. Specific conditions for measuring the antibacterial effect R are as follows.

[0176] · Unprocessed product name: SLG glass

[0177] ·Test product size: 50mm×50mm×5mm

[0178] ·N number: n=2

[0179] Test bacteria: Staphylococcus aureus (NBRC12732)

[0180] Sterilization of test products: heating in a dry sterilizer (80°C, 15 minutes)

[0181] ·Action conditions: Action temperature: 25°C, Action time: 6 hours, in the dark

[0182] · Bacterial count measurement using agar medium

[0183] Table 2 shows the measurement results of the antibacterial effect R.

[0184] (6) Determination of antiviral activity (antiviral effect R)

[0185] The antiviral effect R of each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 4 was measured using bacteriophage Qβ as a test virus in the dark at an action temperature of 25° C. and an action time of 6 hours according to ISO 18071: 2016 and JIS R 1756: 2020. Specific conditions for measuring the antiviral effect R are as follows.

[0186] · Unprocessed product name: SLG glass

[0187] ·Test product size: 50mm×50mm×4mm

[0188] ·N number: n=2

[0189] Test phage: bacteriophage Qβ (NBRC20012)

[0190] Sterilization of test products: heating in a dry sterilizer (80°C, 15 minutes)

[0191] ·Action conditions: Action temperature: 25°C, Action time: 6 hours, in the dark

[0192] Infectivity value measurement using agar medium

[0193] Table 2 shows the results of measuring the antiviral effect R.

[0194] (7) Determination of porosity

[0195] The porosity of each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 4 was measured by the Archimedean method in accordance with JIS R1634: 1998. Table 2 shows the measurement results.

[0196] (8) Determination of true density and relative density

[0197] For each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 4, the relative density [D1 / D2]×100 of the bulk density D1 of the composite material relative to the true density D2 of the metal phase (theoretical density of the metal phase calculated based on the ratio of SiC to the metal phase) was measured by the Archimedean method according to JIS R1634:1998. The measurement results are shown in Table 2.

[0198] (9) Determination of flexural strength

[0199] For each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 4, according to JIS R1601:2008, the distance between the external fulcrums is 30±0.1 mm, the test fixture is 3p-30, the form of the support is a rotating type, the test piece is a standard test piece I, and the standard test piece I is less than the total length (L T The bending strength was measured by a three-point bending strength test under the conditions of: 36 mm or more and less than 45 mm, width (w): 4.0±0.1 mm, thickness (t): 3.0±0.1 mm>. The measurement results are shown in Table 2.

[0200] (10) Determination of Vickers hardness

[0201] The Vickers hardness of each of the metal-ceramic composite materials of Examples 1 to 9 and Comparative Examples 1 to 4 was measured by a 5-point average using a test force of 2.942 N (HV 0.3) in a one-point load test in accordance with JIS R1610:2003.

[0202]

[0203]

[0204] It can be seen from the results of the above-mentioned Examples 1 to 9 that the preferred metal-ceramic composite material according to the present invention brings about a good infiltration state, and thereby exerts excellent mechanical properties such as excellent strength and hardness while exerting excellent antibacterial and antiviral properties brought by copper. In particularly preferred examples, the porosity (density of the sintered body), bending strength and hardness (for example, Vickers hardness: indentation hardness), and antibacterial and antiviral effects are all well-balanced and excellent at a high level.

[0205] On the other hand, according to Comparison Example 1 in which the metal phase contains an excessive amount of the added element M, Comparison Example 2 in which the area of ​​the ceramic phase is relatively small relative to the metal, and Comparison Example 3 in which the area of ​​the ceramic phase is relatively large relative to the metal, a good infiltration state cannot be obtained, the porosity becomes high and a dense sintered body cannot be obtained, or the desired degree of antibacterial activity, antiviral activity, etc. cannot be obtained, resulting in results that are inappropriate for practical use.

[0206] It should be noted that the present invention may include many schemes or many implementation methods which are summarized as follows.

[0207] [1] A metal-ceramic composite material comprising a ceramic phase and a metal phase in a mutually dispersed state, wherein the ceramic phase comprises silicon carbide and the metal phase comprises an alloy and / or an intermetallic compound containing Cu and Si,

[0208] The metal phase contains at least one metal additive element M other than Cu or Si, and

[0209] The silicon carbide accounts for more than half of the total mass of the constituent materials of the ceramic phase.

[0210] Here,

[0211] When an image of an area of ​​256 μm×192 μm is obtained at 500 times using a scanning electron microscope (SEM) for the above-mentioned metal-ceramic composite material, with respect to the area of ​​the entire image, the percentage (%) of the total area of ​​the above-mentioned ceramic phase is set as A, and the percentage (%) of the total area of ​​the above-mentioned metal phase is set as B, the area ratio A / B of the ceramic phase / metal phase is greater than 2 and less than 60, and

[0212] In the above-mentioned metal phase, when the mass percentage (%) of Si is set to a and the mass percentage (%) of the added element M is set to m relative to the total mass, the following relationship is satisfied:

[0213] 0.01≤m / a≤1.4, and

[0214] 0.3≤m≤20.

[0215] [2] The metal-ceramic composite material according to item 1 above, wherein in the metal phase, when the mass percentage (%) of Cu relative to the total mass is b and the mass percentage (%) of Si is a as described above, the following relationship is satisfied:

[0216] b / a≥2.5.

[0217] [3] The metal-ceramic composite material according to item 2 above, wherein the area ratio A / B of the ceramic phase / metal phase is less than 5, and m / a<1, and b / a≥3.

[0218] [4] The metal-ceramic composite material according to any one of items 1 to 3 above, wherein the additional element M includes at least one selected from the group consisting of Ni, Mg, Zn and Ti.

[0219] [5] The metal-ceramic composite material according to any one of items 1 to 4 above, wherein the antibacterial effect R measured in accordance with JIS Z 2801:2012 using Staphylococcus aureus as a test bacterium is 2.0 or more.

[0220] [6] The metal-ceramic composite material according to any one of items 1 to 5 above, characterized in that the metal-ceramic composite material is used as an anti-pathogen material.

[0221] [7] The metal-ceramic composite material according to any one of items 1 to 6 above, wherein the porosity measured by the Archimedean method according to JIS R 1634:1998 is 10% or less.

[0222] [8] A metal-ceramic composite material according to any one of items 1 to 7 above, wherein, when measured using the Archimedean method according to JIS R 1634: 1998, the relative density [D1 / D2] × 100 of the bulk density D1 of the metal-ceramic composite material to the true density D2 of the metal phase of the metal-ceramic composite material is 90% or more.

[0223] [9]. The metal-ceramic composite material according to any one of items 1 to 8 above, wherein the flexural strength measured by a three-point flexural strength test according to JIS R 1601: 2008 is 230 MPa or more.

[0224]

[10] . The metal-ceramic composite material according to any one of items 1 to 9 above, wherein the Vickers hardness measured by a 5-point average in a 1-point load test according to JIS R1610:2003 is 25 GPa or more.

[0225]

[11] . The metal-ceramic composite material according to any one of items 1 to 10 above, wherein the ceramic phase further contains free carbon.

Claims

1. A metal-ceramic composite material, comprising a ceramic phase and a metal phase in a mutually dispersed state, wherein the ceramic phase comprises silicon carbide, and the metal phase comprises an alloy and / or an intermetallic compound containing Cu and Si, The metal phase contains at least one metal additive element M other than Cu or Si, and The silicon carbide occupies more than half of the total mass of the constituent materials of the ceramic phase, Here, For the metal-ceramic composite material, when an image of an area of ​​256 μm×192 μm is obtained at 500 times using a scanning electron microscope (SEM), with respect to the entire area of ​​the image, the percentage (%) of the total area of ​​the ceramic phase is set to A, and the percentage (%) of the total area of ​​the metal phase is set to B, the area ratio A / B of the ceramic phase / metal phase is greater than 2 and less than 60, and In the metal phase, relative to the total mass, when the mass percentage (%) of Si is a and the mass percentage (%) of the additive element M is m, the following relationship is satisfied: 0.01≤m / a≤1.4, and 0.3≤m≤20。 2. The metal-ceramic composite material according to claim 1, in, In the metal phase, when the mass percentage (%) of Cu relative to the total mass is b and the mass percentage (%) of Si is a as described above, the following relationship is satisfied: b / a≥2.

5.

3. The metal-ceramic composite material according to claim 2, in, The area ratio A / B of the ceramic phase / metal phase is 5 or less, and m / a<1, and b / a≥3.

4. The metal-ceramic composite material according to any one of claims 1 to 3, in, The additional element M includes at least one selected from the group consisting of Ni, Mg, Zn, and Ti.

5. The metal-ceramic composite material according to any one of claims 1 to 3, in, The antibacterial effect R measured according to JIS Z2801:2012 using Staphylococcus aureus as a test bacterium is 2.0 or more.

6. The metal-ceramic composite material according to any one of claims 1 to 3, It is characterized in that The metal-ceramic composite material is used as an anti-pathogen material.

7. The metal-ceramic composite material according to any one of claims 1 to 3, in, The porosity measured by the Archimedes method according to JIS R1634:1998 is 10% or less.

8. The metal-ceramic composite material according to any one of claims 1 to 3, in, When measured by the Archimedean method according to JIS R1634:1998, the relative density [D1 / D2]×100 of the bulk density D1 of the metal-ceramic composite material to the true density D2 of the metal phase of the metal-ceramic composite material is 90% or more.

9. The metal-ceramic composite material according to any one of claims 1 to 3, in, The flexural strength measured by a three-point flexural strength test in accordance with JIS R1601:2008 is 230 MPa or more.

10. The metal-ceramic composite material according to any one of claims 1 to 3, in, The Vickers hardness measured at 5 points by a one-point load test in accordance with JIS R1610:2003 is 25 GPa or more.

11. The metal-ceramic composite material according to any one of claims 1 to 3, in, The ceramic phase also contains free carbon.

Citation Information

Patent Citations

  • Highly thermal conductive composite material and production method therefor

    JP2003002770A

  • Composite material

    JP2003165787A

  • Metal-ceramic composite material

    JP2004035307A

  • Method for preparing high volume-fraction carborundum granule-reinforced copper-based composite material

    CN101157993A

  • Composite material and preparation method and application thereof

    CN110396616A

Cited By

  • High-strength high-thermal-conductivity silicon carbide composite material and preparation method thereof

    CN119371207A