Injectable fat decellularized biological material and preparation method thereof
By compounding the fat decellularized matrix with carboxymethyl cellulose sodium, the problem of stable dispersion and filling effect of the fat decellularized matrix in terms of water solubility is solved, uniform filling and efficient repair in soft tissue are achieved, and the biocompatibility is improved. capacity and industrialization potential.
Patent Information
- Application Number
- CN202410329234.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fat acellular matrix materials have challenges in stable dispersion and immediate filling effect in terms of water solubility, which limits their application in soft tissue repair and regeneration.
By compounding the fat decellularized matrix with sodium carboxymethylcellulose (CMC-Na), an injectable fat decellularized biomaterial is formed. The polymer properties of CMC-Na are used to improve the stable dispersion of collagen and the viscosity of the material. Forms a uniform, stable gel that provides an effective support and growth framework.
It achieves stable dispersion of fat decellularized biomaterials in water and uniform filling in soft tissues, improves the efficiency and effect of soft tissue repair, reduces surgical risks and patient recovery time, and enhances the biocompatibility and industrialization potential of the material.
Smart Images

Figure BDA0004752967000000091 
Figure BDA0004752967000000161 
Figure BDA0004752967000000171
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomedical materials and medical devices, and in particular relates to an injectable fat decellularized biomaterial and a preparation method thereof. Background Art
[0002] Autologous tissue transplantation is generally considered the gold standard for tissue repair, but the limited amount of autologous materials and the secondary damage to patients make autologous tissue transplantation have certain limitations. The best scaffold for tissue repair is the extracellular matrix of the target tissue. So far, the allogeneic extracellular matrix products that have been commercialized are mainly dermis, tendon, nerve and bone tissue. Compared with xenogeneic materials, human tissue is very valuable and usually comes from body donation projects. In liposuction surgery, a large amount of adipose tissue is often discarded as medical waste. Studies have shown that adipose decellularized matrix extracted from fat is used for in vitro adipose tissue engineering and in vivo adipose tissue regeneration, and is not limited to adipose tissue engineering. It also has potential applications in healing wounds, regenerating bones, supporting breast tissue reconstruction and promoting nerve repair.
[0003] In the field of tissue engineering and regenerative medicine, adipose-derived decellularized matrix materials have become a hot topic of research due to their unique properties. This material is derived from adipose tissue and is specially treated to remove cellular components while retaining the extracellular matrix. Due to its wide range of sources and easy access, adipose-derived decellularized matrix shows great potential in medical applications. Adipose-derived decellularized matrix materials have excellent biocompatibility and maintain the extracellular matrix structure of natural tissues, which can support the regeneration of adipocytes and have broad application potential in the field of soft tissue defect repair. However, one of the main components of adipose-derived decellularized matrix is collagen, a protein with a triple helical structure, which has certain challenges in the stable dispersion in water. This characteristic of collagen limits its application in water solubility, especially in medical applications that require high dispersion stability. In addition, low-concentration forms of adipose-derived decellularized matrix, such as when injected in saline or phosphate buffered solution, are difficult to achieve immediate and lasting filling effects in soft tissue sites. These limitations in physical properties pose certain challenges in clinical applications.
[0004] A Chinese patent (application publication number: CN 113577388 A) discloses a method for preparing a decellularized fat matrix. It belongs to the technical field of medical biomaterials. It includes the following steps: adipose tissue preservation treatment; freeze-thaw process treatment; oil separation; descaling; cell removal and hydrolysis; extraction; washing and draining to obtain a decellularized fat matrix. The material is clean and free of impurities, contains the main active ingredients of the decellularized fat scaffold, has no immune response, and has excellent physical and mechanical properties, and can be well applied to soft tissue injury repair. A Chinese patent (application publication number: CN 115463264 A) discloses a temperature-sensitive interpenetrating polymer network hydrogel and its preparation method and application. The ex vivo fat is defatted, decellularized, denucleic acidized, freeze-dried, ground and dissolved in a pepsin hydrochloric acid solution to prepare a fat-decellularized extracellular matrix pre-gel solution, which is then mixed with unactivated temperature-controlled platelet-rich plasma under low temperature conditions. The temperature-controlled injectable hydrogel is rich in collagen and fibrin, and has an excellent effect in promoting tissue regeneration by releasing platelets and growth factors. It is suitable for the treatment of irregular wounds and filling of soft tissue defects.
[0005] The above patents respectively propose different methods for preparing decellularized fat matrices. However, although these methods have shown innovation in some aspects, they are still limited in cost-effectiveness, processing time or scope of application. In particular, there are challenges in the ability to stably disperse in water and achieve instant filling of soft tissue. Due to these limitations in physical properties, current fat decellularized matrix materials are limited in clinical use, especially when rapid and effective soft tissue repair and regeneration are required. Therefore, the development of a fat decellularized matrix material that has good biocompatibility and can be stably dispersed in water has become an important goal for researchers and clinicians. The development of this new material will not only enhance the efficiency and effectiveness of soft tissue repair, but also is expected to reduce patients' postoperative recovery time and improve their quality of life. Summary of the invention
[0006] The purpose of the present invention is to provide an injectable adipose decellularized biomaterial, wherein the injectable adipose decellularized biomaterial is prepared by compounding adipose decellularized matrix and sodium carboxymethyl cellulose. The injectable adipose decellularized biomaterial prepared by the present invention has excellent stability and biocompatibility, and can be injected for soft tissue volume loss caused by aging, disease or trauma.
[0007] On the one hand, the present invention provides a novel injectable adipose decellularized biomaterial to solve the problems existing in the prior art. The material not only has excellent biocompatibility, but also can be stably dispersed in water, which improves the feasibility in clinical application. The goal of the present invention is to provide a more effective and safe material option for soft tissue injury repair and regenerative medicine.
[0008] Natural cellulose is the most widely distributed and most abundant polysaccharide in nature, and its sources are very abundant. Sodium carboxymethyl cellulose (CMC-Na) is obtained by etherification modification of cellulose. Its aqueous solution has the functions of thickening, film-forming, bonding, water retention, colloid protection, emulsification and suspension. It is mostly used in the treatment of skin wounds in clinical practice and is an excellent carrier material. The injectable adipose decellularized biomaterial described in the present invention is prepared by the composite of adipose decellularized matrix and sodium carboxymethyl cellulose. The formed injectable tissue material can quickly form a gel and provide effective support after being injected into the soft tissue filling site. This material not only has a high degree of biocompatibility, but also can promote the formation of fat, angiogenesis and granulation tissue, thereby achieving long-term repair and regeneration of soft tissue volume.
[0009] As one of the main components of adipose decellularized matrix, collagen faces significant challenges in its stable dispersion in aqueous solution. The triple helix structure of collagen is prone to form unstable aggregates in water, which is particularly problematic in medical applications because non-uniformly dispersed collagen may lead to local inhomogeneity after injection, affecting the performance and safety of the material. Existing methods, such as simple physical stirring or adding surfactants, often fail to effectively solve the problem of stable dispersion of collagen because these methods cannot fully break the strong interaction between collagen molecules. Compared with the prior art, the present invention significantly improves the stable dispersion of collagen through a composite preparation method of adipose decellularized matrix and sodium carboxymethyl cellulose (CMC-Na). Compared with traditional physical stirring, the present invention utilizes the polymer characteristics of CMC-Na to effectively increase the viscosity and dispersibility of the solution and prevent the aggregation between collagen molecules. Compared with the method of adding surfactants, the preparation process of the present invention does not require the use of additional chemical additives, avoiding potential biosafety risks. From a cost-effectiveness perspective, using CMC-Na as a biocompatible thickener is both economical and efficient, significantly reducing the production cost and processing time of the material, and has a wider range of applications, including but not limited to the fields of soft tissue repair and regenerative medicine. Specifically, the addition of CMC-Na significantly increases the viscosity of the solution, prevents the aggregation of collagen molecules, and ensures that the material can quickly form a uniform and stable gel after injection, providing an ideal three-dimensional growth framework for cells, thereby significantly improving the efficiency and effectiveness of soft tissue repair.
[0010] By finely controlling the particle size of the decellularized matrix and the viscosity and concentration of sodium carboxymethyl cellulose, the material prepared by the present invention can be evenly dispersed after re-dissolution, which greatly facilitates clinical injection operations, ensures the uniform distribution of fillers in the target area, reduces surgical risks, and improves the repair effect. By precisely controlling the particle size and chemical composition of the decellularized matrix, as well as the viscosity and concentration of the sodium carboxymethyl cellulose solution, the present invention can produce materials with excellent physical properties and biological functions. This innovative preparation process, especially the fine control of particle size and chemical composition, provides a scientific basis for the uniform dispersion and injection of materials, ensuring the maximization of the therapeutic effect.
[0011] By adjusting the mixing ratio of adipose decellularized matrix and sodium carboxymethyl cellulose, the present invention provides a method to control the degradation rate of the material to meet the specific needs of different soft tissue parts. This adjustable degradability is not only beneficial to the long-term stability of the material and the performance of its biological functions, but also provides new possibilities for personalized medical treatment. By adjusting the chemical composition and physical structure of the material, the present invention achieves precise control of the degradation rate of the material. This control not only affects the persistence of the material in the body, but is also directly related to the growth rate and quality of the repaired tissue. An appropriate degradation rate can ensure that the material does not fail prematurely, while providing sufficient time and space for the formation of new tissue.
[0012] The preparation process adopted by the present invention is simple and effective, and a fat-free cell biomaterial with a sponge-like porous structure can be produced through freeze-drying technology. This structure is not only conducive to gel formation and intracellular penetration of the material after injection, but also convenient for long-term storage and transportation, significantly improving the industrialization potential of the product.
[0013] Furthermore, the method for preparing the injectable adipose decellularized biomaterial comprises the following steps:
[0014] S1. The adipose tissue is washed, broken, separated, virus inactivated, decellularized, and crushed to obtain adipose decellularized matrix;
[0015] S2. adding the obtained sodium carboxymethyl cellulose to water to form a uniform solution with or without refining or cross-linking treatment;
[0016] S3. Add the adipose decellularized matrix to the sodium carboxymethyl cellulose solution in proportion and mix evenly, add or not add excipients and mix evenly, inject and freeze-dry to prepare the injectable adipose decellularized biomaterial;
[0017] Furthermore, the injectable adipose decellularized biomaterial can be sterilized by low-temperature plasma sterilization, ethylene oxide sterilization, or irradiation sterilization;
[0018] Furthermore, the injectable adipose decellularized biomaterial can be mixed with physiological saline, phosphate buffer, etc. and injected into the soft tissue volume loss area in practical applications;
[0019] Furthermore, the method for preparing the adipose decellularized matrix in step S1 includes but is not limited to: washing, crushing, separation, virus inactivation, decellularization, pulverization and other processes;
[0020] Furthermore, in step S1, the collagen content in the adipose decellularized matrix is 10-60%, the glycosaminoglycan content is 0.1-2%, and the total growth factor content is 0-1000 pg / mg;
[0021] Furthermore, the particle size of the adipose decellularized matrix in step S1 is 0.5-1000 μm, preferably 5-500 μm;
[0022] Furthermore, the sodium carboxymethyl cellulose treatment method in step S2 is mainly a refining method, a physical crosslinking method and a chemical crosslinking method, wherein the refining method includes but is not limited to: an alcohol washing method, an acid-alcohol solution precipitation method and other processes, the physical crosslinking method includes but is not limited to: irradiation, ultraviolet irradiation and other processes, and the chemical crosslinking method includes but is not limited to: a crosslinking process using acrylamide, sodium trimetaphosphate, 1,3-propylenediamine, chloromethylpyridine iodide, EDC and NHS and other crosslinking agents;
[0023] Furthermore, in step S2, the sodium carboxymethyl cellulose solution has a viscosity of 50-100000 mPa·s and a concentration of 0.01-30%, preferably, a viscosity of 6000-14000 mPa·s and a concentration of 0.1-10%;
[0024] Furthermore, the excipients in step S3 include lyophilization protective agents, disintegrants, and suspending agents, wherein the lyophilization protective agents include but are not limited to: mannitol, trehalose and other reagents, wherein the disintegrants include but are not limited to: sodium carboxymethyl starch, cross-linked sodium carboxymethyl cellulose and other reagents, wherein the suspending agents include but are not limited to: glycerol, polyethylene glycol and Tween 80 and other reagents;
[0025] Furthermore, the drying process conditions in step S3 are: pre-freezing for 1-24 hours, pre-freezing temperature of -80-40°C, and freeze drying for 12-80 hours.
[0026] The injectable adipose decellularized biomaterial of the present invention, in addition to showing significant application potential in the repair of soft tissue volume loss, can also play an important role in other medical fields. For example, due to its excellent biocompatibility and gel-forming ability, the material can be used to treat specific diseases, such as promoting the healing of difficult-to-heal wounds, as a drug delivery system in tumor treatment, or as a scaffold material in minimally invasive surgery. These potential applications not only expand the scope of application of the present invention, but also provide new strategies for solving specific medical problems.
[0027] In order to verify the safety and biocompatibility of the proposed material, the present invention has conducted a series of in vitro and in vivo experiments. In vivo application research, by injecting the material of the present invention into an animal model and conducting long-term follow-up observations, no obvious inflammatory reaction was found, the tissue around the material was good, and there was no abnormal cell infiltration or fibrosis, which further proved the good biocompatibility and long-term stability of the material of the present invention, providing a solid safety guarantee for clinical application.
[0028] Compared with the prior art, the injectable tissue material and the preparation method thereof disclosed in the present invention have the following positive effects:
[0029] (1) The injectable tissue material of the present invention has good biocompatibility and can quickly form a gel. After injection, it plays a supporting role in the soft tissue filling site. The fat decellularized matrix encapsulated in the injectable tissue material has biological activity and can promote the formation of fat and blood vessels and granulation tissue, thus playing a long-term role in soft tissue volume filling and repair.
[0030] (2) The adipose decellularized matrix in the injectable tissue material of the present invention can be evenly dispersed after re-dissolving, which is convenient for clinical injection.
[0031] (3) During use, the degree of material degradation can be controlled by adjusting the mixing ratio of adipose decellularized matrix and sodium carboxymethyl cellulose to meet the needs of filling different parts of soft tissue.
[0032] (4) The injectable adipose decellularized biomaterial of the present invention has a simple preparation process, has a sponge-like porous structure, can be stored for a long time after freeze-drying, and is easy to realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a physical picture of the freeze-dried dosage form of the injectable adipose decellularized biomaterial of the present invention, showing the storage condition of the material in the form of a freeze-dried sponge in a vial.
[0034] Figure 2 This is a real picture of the injectable adipose decellularized biomaterial of the present invention after being mixed with physiological saline.
[0035] Figure 3 This is a photo of using a 30G needle to extrude a mixture of injectable adipose decellularized biomaterial and saline.
[0036] Figure 4 This is a scanning electron microscope (SEM) image of the injectable fat decellularized biomaterial of the present invention, revealing the mesh structure of the material, with the surface of the skeleton structure covered with a smooth sodium carboxymethyl cellulose layer.
[0037] Figure 5 The scanning electron microscope (SEM) image of the injectable fat decellularized biomaterial of the present invention is further shown, and by increasing the sodium carboxymethylcellulose content, the sodium carboxymethylcellulose layer on the surface of the material after freeze-drying is made more uniform.
[0038] Figure 6 It is a stability test diagram of the injectable adipose decellularized biomaterials of different concentrations of the present invention, showing the dispersion stability of materials of different concentrations within 30 minutes.
[0039] Figure 7 This is the scanning electron microscope (SEM) image of the pure fat decellularized matrix of Control Example 1.
[0040] Figure 8 This is a real picture of the control example 1 after mixing with normal saline.
[0041] Fig. 9 This is a picture of the control example 1 mixed with physiological saline and then squeezed out.
[0042] Fig.10 This is a stability test diagram of Control Example 1 after mixing with normal saline.
[0043] Fig.11 It is a degradation experiment diagram of the injectable fat decellularized biomaterial of the present invention and control example 1, showing the changes in the content of released protein of the injectable fat decellularized biomaterial and the pure fat decellularized biomaterial within 24 hours, and the injectable fat decellularized biomaterial shows a lower degradation rate.
[0044] Fig.12 It is a stability test diagram of the injectable adipose decellularized biomaterials with different viscosities of the present invention, showing the dispersion stability of materials with different viscosities within 30 minutes.
[0045] Fig.13 It is a diagram showing the re-dissolution of injectable adipose decellularized biomaterials of different concentrations according to the present invention.
[0046] Fig.14 It is a diagram showing the re-dissolution of injectable adipose decellularized biomaterials with different viscosities according to the present invention.
[0047] Fig.15It is a diagram showing the re-dissolution of the injectable adipose decellularized biomaterial with different excipients added thereto according to the present invention.
[0048] Fig.16 It is a general observation diagram of the animal experiment of the present invention.
[0049] Fig.17 It is a diagram of the animal experimental materials of the present invention.
[0050] Fig.18 It is a histological evaluation diagram of the animal experimental material of the present invention, showing the degradation and cell infiltration of the injectable tissue material and the pure fat decellularized biomaterial in the body.
[0051] Fig.19 This is a histological evaluation diagram of the animal experimental material of the present invention, showing the degradation and fat hyperplasia of the injectable tissue material in the body at one month.
[0052] Related definitions
[0053] In the present invention, unless otherwise specified, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. Meanwhile, in order to better understand the present invention, the definitions and explanations of the relevant terms are provided below.
[0054] As used herein, "injectable adipose decellularized biomaterial" refers to a specially treated material, which is a composite of a matrix obtained after decellularization of adipose tissue and sodium carboxymethyl cellulose (CMC-Na), has good water solubility and the ability to form a stable gel, and can be used for soft tissue repair or augmentation by injection.
[0055] As used herein, "sodium carboxymethyl cellulose (CMC-Na)" refers to a water-soluble cellulose derivative, which has the functions of thickening, gel formation, stabilizing dispersion systems, etc., and is widely used in the fields of medicine, food, and cosmetics. In the present invention, CMC-Na, as a substance with good biocompatibility and the ability to enhance material stability and support, is used in the composite adipose decellularized matrix to improve the performance of the material.
[0056] As used herein, "adipose decellularized matrix" refers to the matrix remaining after the cell components are removed from adipose tissue through a specific process, retaining the main components of the extracellular matrix, such as collagen and glycosaminoglycans. This matrix has the potential to promote adipogenesis, angiogenesis, and granulation tissue formation, and is an important material in repair and regenerative medicine.
[0057] As used herein, "stabilizing effect" refers to the mechanism of action of sodium carboxymethyl cellulose (CMC-Na) in a solution, which can increase the viscosity of the solution, form a stable gel or colloidal system, prevent precipitation or separation of components, and thus improve the stability of the entire system.
[0058] As used herein, "biocompatibility" refers to the compatibility of a material when in contact with an organism, including not causing adverse immune responses, inflammation or other harmful reactions, being suitable for long-term existence in the organism, and not affecting its normal function and tissue repair process.
[0059] As used herein, "stability" refers to the ability of a material to maintain its chemical and physical properties without significant changes during storage or use.
[0060] As used herein, "degradation rate" refers to the speed at which a material breaks down and disappears in a living body, which is usually related to the chemical composition and structure of the material as well as the external environment (such as the presence of enzymes).
[0061] As used herein, "gel formation" refers to a physical or chemical process in which molecules in a solution form a three-dimensional network structure by cross-linking or interaction, causing the entire system to transform from a fluid state to a gel state with a certain mechanical strength and shape stability.
[0062] As used herein, "soft tissue volume loss" refers to a condition in which the volume of soft tissue (such as skin, fat, muscle, etc.) is reduced or damaged due to disease, trauma, surgery or aging, and medical intervention is required to restore its original volume or function. DETAILED DESCRIPTION
[0063] The present invention is described below through specific embodiments. Unless otherwise specified, the technical means used in the present invention are methods known to those skilled in the art. In addition, the embodiments should be understood as illustrative rather than limiting the scope of the present invention, and the essence and scope of the present invention are limited only by the claims. For those skilled in the art, various changes or modifications to the material components and dosages in these embodiments, without departing from the essence and scope of the present invention, also belong to the protection scope of the present invention. The sodium carboxymethyl cellulose used in the present invention was purchased from Shanghai McLean Biochemical Technology Co., Ltd., Jiangsu Alpha Pharmaceutical Group and Anhui Shanhe Pharmaceutical Excipients Co., Ltd.; physiological saline was purchased from Shandong Hualu Pharmaceutical Co., Ltd.; distilled water was purchased from Watsons; excipients and cross-linking agents were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. and Sigma-Aldrich (Shanghai) Trading Co., Ltd.; experimental animals were purchased from Zhejiang Weitong Lihua Experimental Animal Co., Ltd.
[0064] In one embodiment, an injectable adipose decellularized biomaterial with excellent physical stability and biocompatibility is prepared by precisely controlling the ratio of adipose decellularized matrix to sodium carboxymethyl cellulose (CMC-Na). The material preparation process, appearance characteristics, solubility, microstructure and dispersion stability are demonstrated, proving that through precise material design, biomaterials suitable for clinical injection can be obtained.
[0065] In one embodiment, the effect of increasing the amount of CMC-Na added on the performance of injectable adipose decellularized biomaterials was explored, especially in terms of improving the microstructure and uniformity of the material. By using scanning electron microscopy, it was revealed that increasing the CMC-Na content can effectively improve the microstructure of the material, making the CMC-Na layer on the surface of the material more uniform, thereby potentially improving its effectiveness and safety in medical applications.
[0066] In one embodiment, the material performance evaluation of different carboxymethyl cellulose sodium (CMC-Na) addition amounts further explored the effect of CMC-Na content on material performance. By adjusting the CMC-Na content, the performance of materials with different concentrations in terms of dispersion stability was demonstrated, indicating that a higher content of CMC-Na can provide better dispersion stability and material uniformity, which is of great significance for clinical applications.
[0067] Furthermore, through the analysis of the control examples, the present invention also emphasizes the positive role of CMC-Na in improving the dispersion stability, degradation rate and long-term stability of injectable fat decellularized biomaterials. The comparison of the control experimental results with the CMC-Na addition example clarifies the effectiveness of CMC-Na as a biomaterial modifier and its key role in optimizing material properties.
[0068] Furthermore, the present invention explores the effect of different viscosities of sodium carboxymethyl cellulose (CMC-Na) on the re-dissolution performance of the material, and reveals that CMC-Na with appropriate viscosity can optimize the re-dissolution process, improve the material's handling convenience and clinical application potential, and selecting the appropriate viscosity and concentration of CMC-Na is crucial to obtaining ideal material properties.
[0069] Furthermore, the present invention explores the effects of different excipients on the re-dissolution performance of the material and reveals the effect of the addition of excipients on the re-dissolution.
[0070] In one embodiment, the effect of the adjusted CMC-Na concentration and viscosity on the volume retention rate and tissue compatibility of the material after subcutaneous injection was evaluated through the implementation of the biocompatibility experiment. The results of Example 8 and the control experiment showed that the improved material showed better stability and biocompatibility, providing an effective material choice for soft tissue repair.
[0071] In general, the specific embodiments collectively demonstrate that by precisely controlling the ratio of adipose decellularized matrix to sodium carboxymethyl cellulose and processing conditions, the performance of injectable adipose decellularized biomaterials can be significantly optimized, providing a new type of material with potential application value for the repair of soft tissue volume loss.
[0072] Example 1 Preparation and performance evaluation of injectable adipose decellularized biomaterials
[0073] The steps for preparing injectable adipose decellularized biomaterials are as follows:
[0074] (1) Weigh 5 mg of adipose decellularized matrix;
[0075] (2) Weigh 5 mg of sodium carboxymethyl cellulose with a viscosity of 6000-14000 mPa·s and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer (GL-5250C, Qilin Bell, China) at 900 rpm for 3 h until it is completely dissolved.
[0076] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 2:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried (Pilot2-4T, China Biomedical Technology Co., Ltd.) for 78.5 h, and sterilized.
[0077] The freeze drying parameters are shown in Table 1:
[0078] Table 1 Freeze drying parameters
[0079] Freeze drying step Temperature(℃) Heating time (min) Holding time (min) Vacuum setting (Pa) Step 1 -45 10 1500 0 Step 2 -5 80 60 0 Step 3 25 60 3000 0
[0080] Material characterization
[0081] Appearance: The freeze-dried material is stored in a vial in a sponge-like form with a smooth appearance. Figure 1 shown.
[0082] Solubility: After injecting 1 ml of saline into the vial, let it stand for 5 minutes to re-dissolve, shake to mix and draw into a 1 ml injection needle. When the mixed solution is squeezed out with a 30G needle, the material is evenly distributed in the droplets, such as Figure 2 and Figure 3 As shown, it demonstrates good injectability and dispersibility.
[0083] Viscosity: measured by rotational rheometer (DHR20, TA, USA) at 25°C and a shear rate of 1s -1 The shear viscosity of the reconstituted material was measured and found to be 475.94 mPa·s.
[0084] Microstructure: Scanning electron microscopy (SEM) (GeminiSEM 360, Zeiss, Germany) observation shows that the material obtained in this example presents a reticular structure, and the surface of the skeleton is covered with a smooth sodium carboxymethyl cellulose layer, such as Figure 4 shown.
[0085] Data analysis
[0086] Dispersion stability: The results of laser particle size analyzer (Mastersizer 2000, Malvern, UK) showed that d(0.1), d(0.5) and d(0.9) were 6.160 μm, 23.141 μm and 53.616 μm, respectively. According to the free sedimentation formula of Stokes' law (1), the sedimentation rate of injectable adipose decellularized biomaterial was 2.549×10 -6 cm / s, and can remain stable for a certain period of time. At the same time, the good dispersibility in physiological saline shows that the material prepared in this example has excellent physical stability and is suitable for medical injection. Through static observation, no obvious sedimentation or separation was found, indicating that the material remains stable under physiological conditions, which is very important for clinical application.
[0087]
[0088] Where: V is the particle settling velocity (cm / s); d is the particle diameter (cm); ρ is the particle density (g / cm 3 );ρ1 is the base liquid density (g / cm 3 );η is the base fluid viscosity (Pa·s)
[0089] Sterilization effect: Sterilization is carried out by low-temperature plasma sterilization, ethylene oxide sterilization, irradiation sterilization, etc. The sterility of the material is verified by sterility testing to ensure its safety in medical applications.
[0090] Contribution of microstructure to biocompatibility: The reticular structure and smooth layer of sodium carboxymethylcellulose may facilitate cell attachment and growth, improving the biocompatibility of the material.
[0091] In summary, Example 1 demonstrates that by precisely controlling the ratio of adipose decellularized matrix to sodium carboxymethylcellulose, an injectable adipose decellularized biomaterial with a smooth appearance, good dispersibility and excellent biocompatibility potential can be prepared. The preparation method of the material is simple, and its safety in clinical application is ensured by sterilization.
[0092] Example 2 Effect of increasing the amount of sodium carboxymethyl cellulose (CMC-Na) added
[0093] This example aims to explore the effect of the amount of sodium carboxymethylcellulose (CMC-Na) added on the performance of injectable adipose decellularized biomaterials. The preparation steps are as follows:
[0094] (1) Weigh 5 mg of adipose decellularized matrix;
[0095] (2) Weigh 10 mg of carboxymethyl cellulose with a viscosity of 6000-14000 mPa·s and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0096] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 2:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0097] The shear viscosity of Example 2 is 834.11 mPa·s, which is greater than that of Example 1, indicating that increasing the content of sodium carboxymethyl cellulose can increase the overall viscosity of the material.
[0098] The microstructure of the material obtained in this example was observed using a scanning electron microscope (SEM). Figure 5 As shown in the figure, as the content of sodium carboxymethyl cellulose increases to 10 mg, the sodium carboxymethyl cellulose layer on the surface of the freeze-dried material becomes more uniform. Under 20,000 times magnification, the matrix fiber structure under the sodium carboxymethyl cellulose layer can be clearly seen, indicating that increasing the content of sodium carboxymethyl cellulose can effectively improve the microstructure and uniformity of the material.
[0099] Example 3 Material Performance Evaluation of Different Addition Amounts of Sodium Carboxymethyl Cellulose (CMC-Na)
[0100] This series of examples continues to explore the effect of the amount of sodium carboxymethylcellulose (CMC-Na) added on the performance of injectable adipose decellularized biomaterials. The basic preparation steps are as follows:
[0101] Example 3-1
[0102] (1) Weigh 5 mg of adipose decellularized biomaterial;
[0103] (2) Weigh 50 mg of sodium carboxymethyl cellulose (viscosity 6000-14000 mPa·s) and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0104] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0105] Example 3-2
[0106] The preparation steps are as follows:
[0107] (1) Weigh 5 mg of adipose decellularized biomaterial;
[0108] (2) Weigh 30 mg of sodium carboxymethyl cellulose with a viscosity of 6000-14000 mPa·s and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0109] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0110] Example 3-3
[0111] The preparation steps are as follows:
[0112] (1) Weigh 5 mg of adipose decellularized biomaterial;
[0113] (2) Weigh 25 mg of sodium carboxymethyl cellulose (viscosity 6000-14000 mPa·s) and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0114] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0115] Embodiment 3-4
[0116] The preparation steps are as follows:
[0117] (1) Weigh 5 mg of adipose decellularized biomaterial;
[0118] (2) Weigh 15 mg of sodium carboxymethyl cellulose (viscosity 6000-14000 mPa·s) and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0119] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0120] Inject 5 ml of normal saline into the vials of Examples 3-1 to 3-4, let stand for 5 min to re-dissolve, shake and mix, draw in a 10 ml injection needle, add a stopper and let stand for 30 minutes. In Examples 3-1 to 3-4, the contents of CMC-Na were 50 mg, 30 mg, 25 mg and 15 mg, respectively, and measure their shear viscosities and calculate their sedimentation rates (see Table 2). Figure 6 As shown, the materials of different concentrations in all embodiments maintained good dispersion stability within 30 minutes, corresponding to their sedimentation rates. This series of embodiments shows that the content of CMC-Na plays an important role in improving the microstructure, uniformity and dispersion stability of injectable fat decellularized biomaterials. A higher content of CMC-Na can provide better dispersion stability and material uniformity, which is beneficial to the clinical application of the material. However, it should also be noted that the increase in CMC-Na content may affect other properties of the material (such as biocompatibility, mechanical strength, etc.), so various performance indicators should be considered comprehensively when optimizing the CMC-Na content to achieve the best application effect.
[0121] Table 2 Materials with different CMC-Na addition amounts
[0122] Example CMC-Na content / mg Shear viscosity / mPa·s <![CDATA[Settling rate / cm·s -1 > 3-1 50 876.57 <![CDATA[6.717×10 -7 ]]> 3-2 30 513.69 <![CDATA[1.300×10 -6 ]]> 3-3 25 441.76 <![CDATA[1.557×10 -6 ]]> 3-4 15 249.94 <![CDATA[2.915×10 -6 ]]>
[0123] Control Example 1 Effect of adding sodium carboxymethyl cellulose on the basic properties of adipose decellularized biomaterials
[0124] This control experiment is intended to evaluate the injection, dispersion stability and degradation performance of adipose decellularized biomaterials that have not been modified with CMC-Na, so as to compare with the examples (such as Example 3-1) in which CMC-Na is added. The preparation steps are as follows:
[0125] (1) Weigh 5 mg of adipose decellularized biomaterial;
[0126] (2) Add 1 ml of distilled water to the adipose decellularized matrix and vortex on a vortex oscillator (YM-H10, Michael, China) at 2000 r / min for 1 min until the mixture is evenly mixed; the resulting matrix solution is poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0127] Microstructure: Scanning electron microscope observation shows that the material obtained in this comparative example presents a network structure, such as Figure 7 shown.
[0128] Dispersion stability
[0129] The average sedimentation rate of control example 1 is 7.846×10 -4 cm / s, which is significantly higher than that of Example 3-1, and from the actual image ( Figure 8 , 9, 10) observed that the material in Control Example 1 showed poor dispersion stability compared with Example 3-1 after mixing with physiological saline, extruding and placing for 30 minutes. The CMC-Na added in Example 3-1 significantly improved the dispersibility and stability of the material, resulting in a more uniform material after extrusion and less sedimentation within 30 minutes. This result shows that the addition of CMC-Na effectively prevents the aggregation of the material and promotes better dispersion performance.
[0130] Degradation experiment
[0131] Degradation test results within 24 hours ( Fig.11 ) shows that although the content of protein released by the injectable fat decellularized biomaterial and the pure fat decellularized biomaterial in Control Example 1 increases with time, the water-soluble protein release content of the injectable fat decellularized biomaterial with the addition of CMC-Na is lower, indicating that the fat decellularized biomaterial retains more nutrients and is more conducive to cell adhesion and proliferation. Specifically, at 24 hours, the material in Example 3-1 exhibited a lower degradation rate and degradation rate (2.14% vs. 1.88%) compared to Control Example 1. This finding means that the presence of CMC-Na can slow down the degradation of the material to a certain extent.
[0132] Long-term stability and active substance retention
[0133] Comparison of Control Example 1 with Example 3-1 further reveals that freeze-drying is essential for improving the long-term stability of injectable adipose decellularized biomaterials and the retention of effective substances (such as proteins). In particular, in the presence of CMC-Na, freeze-dried materials can more effectively maintain their structure and functionality, which is extremely important for future clinical applications.
[0134] In summary, the results of Control Example 1 compared with Example 3-1 clearly show the positive effect of CMC-Na in improving the dispersion stability, slowing down the degradation rate and enhancing the long-term stability of injectable fat decellularized biomaterials. This finding not only confirms the effectiveness of CMC-Na as a biomaterial modifier, but also provides an important experimental basis for the further development and optimization of injectable biomaterials. The actual picture of this control example after mixing with physiological saline, the actual picture of extrusion and the picture after 30 minutes of placement are shown in the figure. Figure 8 , 9 , 10. Compared with adipose acellular matrix, injectable tissue material is more uniform after extrusion, has less sedimentation within 30 minutes, and is more stable.
[0135] Example 4 Material Performance Evaluation of Different Viscosities of Sodium Carboxymethyl Cellulose (CMC-Na)
[0136] This series of examples aims to explore the effect of changes in the viscosity of sodium carboxymethylcellulose (CMC-Na) on the properties of injectable adipose decellularized biomaterials, including changes in dispersion stability and microstructure. The basic preparation steps are as follows:
[0137] (1) Weigh 5 mg of adipose decellularized biomaterial;
[0138] (2) Weigh 30 mg of sodium carboxymethyl cellulose with a viscosity of 6000-14000 mPa·s and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0139] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0140] Example 4-1: Basic viscosity
[0141] Viscosity range: 6000-14000mPa·s
[0142] CMC-Na content: 30mg
[0143] Example 4-2: Low viscosity
[0144] Viscosity range: 50-500mPa·s
[0145] CMC-Na content: 30mg
[0146] Example 4-3: Medium Viscosity
[0147] Viscosity range: 500-3100mPa·s
[0148] CMC-Na content: 30mg
[0149] Example 4-4: Medium to high viscosity
[0150] Viscosity range: 3100-6000mPa·s
[0151] CMC-Na content: 30mg
[0152] Example 4-5: High Viscosity
[0153] Viscosity range: 14000-20000mPa·s
[0154] CMC-Na content: 30mg
[0155] Examples 4-6: Very high viscosity
[0156] Viscosity range: 20000-100000mPa·s
[0157] CMC-Na content: 30mg
[0158] Inject 5 ml of normal saline into the vial of the above embodiment, let it stand for 5 min to re-dissolve, shake and mix, draw in 1 ml of injection needle, add a stopper and let it stand. Fig.12 The left picture in the middle shows 0 minutes of standing, and the right picture shows 30 minutes of standing. The injectable adipose decellularized biomaterials containing sodium carboxymethyl cellulose with different viscosities all maintain good dispersion stability within 30 minutes. The shear viscosity and sedimentation rate of Examples 4-1 to 4-6 were measured and calculated (see Table 3), respectively, indicating that the higher the viscosity of CMC-Na, the longer the time it maintains a stable state. In clinical applications, choosing the right CMC-Na viscosity is crucial for balancing the injectability, stability and bioactivity of the material. CMC-Na in the medium to medium-high viscosity range has been shown to be an ideal choice for achieving this balance.
[0159] Table 3 Materials with different CMC-Na viscosities
[0160] Example CMC-Na viscosity / mPa·s Shear viscosity / mPa·s <![CDATA[Settling rate / cm·s -1 > 4-1 6000-14000 493.42 <![CDATA[1.543×10 -6 ]]> 4-2 50-500 13.76 <![CDATA[5.854×10 -5 ]]> 4-3 500-3100 97.15 <![CDATA[7.846×10 -6 ]]> 4-4 3100-6000 251.55 <![CDATA[3.032×10 -6 ]]> 4-5 14000-20000 837.64 <![CDATA[9.092×10 -7 ]]> 4-6 20000-100000 10996.71 <![CDATA[6.921×10 -8 ]]>
[0161] Example 5 Effect of Changes in the Concentration of Sodium Carboxymethyl Cellulose (CMC-Na)
[0162] This series of examples aims to explore the effect of sodium carboxymethylcellulose (CMC-Na) concentration on the performance of injectable adipose decellularized biomaterials, focusing on the resolubility of the material. The basic preparation steps are as follows:
[0163] (1) Weigh 3 mg of adipose decellularized biomaterial;
[0164] (2) Weigh 30 mg of sodium carboxymethyl cellulose with a viscosity of 6000-14000 mPa·s and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0165] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0166] Example 5-1: Standard concentration
[0167] CMC-Na content: 30mg
[0168] At standard concentrations, the material exhibits excellent resolubility and can be quickly and evenly resolubilized after mixing with saline. The solution after manual shaking is well uniform, with no obvious aggregation or sedimentation, demonstrating the effectiveness of higher concentrations of CMC-Na in improving the material's handling and ease of use.
[0169] Example 5-2: High concentration
[0170] CMC-Na content: 50mg
[0171] Increasing the concentration of CMC-Na to 50 mg, the material can maintain good re-dissolution performance, but compared with 30 mg, the re-dissolution standing time and re-dissolution operation time are increased to a certain extent. At the same time, the uniformity and stability after re-dissolution are similar to those in Example 5-1, indicating that the increase in CMC-Na content improves the material performance to a certain extent but increases the difficulty of re-dissolution.
[0172] Example 5-3: Medium concentration
[0173] CMC-Na content: 18mg
[0174] When the concentration of CMC-Na was reduced to 18 mg, the material still maintained good re-dissolution performance, but compared with 30 mg, the re-dissolved solution was slightly thinner, indicating that the concentration had a significant effect on the re-dissolution performance. Despite this, the material was still re-dissolved quickly and evenly, indicating that good performance could be maintained even with a reduced CMC-Na content.
[0175] Example 5-4: Low concentration
[0176] CMC-Na content: 3mg
[0177] When the concentration of CMC-Na is greatly reduced to 3 mg, the re-dissolution performance of the material is reduced. Although it can still be re-dissolved, the uniformity and stability after re-dissolution are weakened compared with the case of higher concentrations. It can be seen that the supporting effect of low concentration CMC-Na on material performance is limited.
[0178] Control Example 2 Effect of adding sodium carboxymethyl cellulose on the solubility of adipose decellularized biomaterials
[0179] Control Example 2 is intended to evaluate the basic properties of adipose decellularized biomaterials, especially their resolubility, when sodium carboxymethylcellulose (CMC-Na) is not added. The basic preparation steps are as follows:
[0180] (1) Weigh 3 mg of adipose decellularized biomaterial;
[0181] (2) Add 1 ml of distilled water to the adipose decellularized matrix and vortex at 2000 rpm for 1 min until the mixture is evenly mixed; the resulting matrix solution is poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0182] 1 ml of normal saline was injected into the vials of Examples 5-1 to 5-3 and Comparative Example 2, and the reconstitution conditions were shown in Table 3. The reconstitution observation results were as follows: Fig.13 Shown are diagrams of reconstitution of injectable tissue materials containing different concentrations of sodium carboxymethylcellulose.
[0183] Redissolution performance: In the case of no addition of CMC-Na, the material in Control Example 2 needs to be left to stand for 10 minutes for redissolution and shaken manually for 90 seconds. The redissolution process is difficult, and the solution after redissolution shows a certain degree of aggregation, indicating that its dispersion stability is poor. In contrast, different concentrations of CMC-Na are added to Examples 5-1 to 5-3, which significantly improves the redissolution performance and dispersion stability of the materials, especially Example 4-1 (standard concentration 30 mg) shows the best redissolution performance and uniformity.
[0184] Table 4 Effect of CMC-Na concentration changes
[0185]
[0186] Operational convenience: Control Example 2 without CMC-Na requires longer time and more operation effort during manual reconstitution to achieve a more uniform mixing effect, which may cause inconvenience in clinical applications. Examples 5-1 to 5-3 not only simplify the reconstitution process, but also shorten the reconstitution time and improve the operational convenience by adding CMC-Na.
[0187] As an effective thickener and stabilizer, CMC-Na helps improve the microstructure of the material, thereby enhancing its overall performance. Manual reconstitution of injectable tissue materials is simpler than that of pure fat decellularized biomaterials, with a shorter reconstitution time and more uniform reconstituted particles. As the concentration of sodium carboxymethylcellulose increases, the reconstitution effect of injectable tissue materials is better.
[0188] Example 6 Effect of viscosity change of sodium carboxymethylcellulose (CMC-Na)
[0189] This series of examples aims to explore the effect of different viscosities of sodium carboxymethylcellulose (CMC-Na) on the resolubility of injectable adipose decellularized biomaterials. By adjusting the viscosity of CMC-Na, the optimal resolubility conditions are found to simplify the clinical application process of the material. The basic preparation steps are as follows:
[0190] (1) Weigh 30 mg of adipose decellularized biomaterial;
[0191] (2) Weigh 5 mg of sodium carboxymethyl cellulose (viscosity 6000-14000 mPa·s) and dissolve it in 10 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0192] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; 1 ml of the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0193] Example 6-1: Basic Viscosity
[0194] CMC-Na viscosity range: 6000-14000mPa·s
[0195] CMC-Na content: 5mg
[0196] Under the basic viscosity condition, the reconstitution process of the material is relatively simple, the reconstitution time is short, and the particle distribution of the reconstituted solution is uniform. This shows that the basic viscosity of CMC-Na is sufficient to provide good reconstitution performance and is suitable for quick preparation and application.
[0197] Example 6-2: High Viscosity
[0198] CMC-Na viscosity range: 14000-20000mPa·s
[0199] CMC-Na content: 5mg
[0200] When the viscosity of CMC-Na was increased to 14000-20000 mPa·s, it was observed that the re-dissolution process was still rapid, but the re-dissolved solution showed higher uniformity. This may be because the higher viscosity CMC-Na is more stable in water and can more evenly wrap the adipose decellularized matrix, thereby improving the uniformity after re-dissolution.
[0201] Example 6-3: Low Viscosity
[0202] CMC-Na viscosity range: 50-500mPa·s
[0203] CMC-Na content: 5mg
[0204] When the viscosity of CMC-Na is reduced to 50-500 mPa·s, although the reconstitution process is still fast, the uniformity of particle distribution in the reconstituted solution decreases slightly. This indicates that the lower viscosity may lead to a weakened combination of CMC-Na and adipose decellularized matrix, affecting the uniformity of the final reconstituted solution.
[0205] 1 ml of normal saline was injected into the vials of Examples 6-1 to 6-3 and shaken manually. Table 5 shows the effect of the viscosity change of CMC-Na. Fig.14 Shown is the reconstitution diagram of injectable tissue materials containing sodium carboxymethylcellulose with different viscosities. As the concentration of sodium carboxymethylcellulose increases, the injectable tissue material is easier to reconstitute, the reconstitution time is shorter, and the reconstituted particles are more uniform. This series of results shows that the viscosity of CMC-Na affects the reconstitution performance of injectable fat-decellularized biomaterials to a certain extent. CMC-Na with higher viscosity can provide better uniformity of the reconstituted solution. However, even under low viscosity conditions, CMC-Na still shows good reconstitution ability, indicating that even CMC-Na with lower viscosity is sufficient to meet the needs of rapid reconstitution.
[0206] Table 5 Effect of CMC-Na viscosity change
[0207]
[0208] In summary, the selection of CMC-Na with appropriate viscosity is crucial for optimizing the preparation and application of injectable adipose-decellularized biomaterials. High-viscosity CMC-Na is more suitable for applications that require a highly uniformly distributed reconstituted solution, while low-viscosity CMC-Na is suitable for situations where rapid reconstitution is desired.
[0209] Example 7 Effect of Adding Excipients on Redissolution
[0210] This series of examples aims to explore the effect of the addition of excipients on the performance of injectable adipose decellularized biomaterials, focusing on the resolubility of the materials. The basic preparation steps are as follows:
[0211] (1) Weigh 3 mg of adipose decellularized biomaterial;
[0212] (2) Weigh 5 mg of sodium carboxymethyl cellulose (viscosity 6000-14000 mPa·s) and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0213] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; the auxiliary materials were added, and stirred for 10 min with a magnetic stirrer at 900 rpm until uniform; the obtained composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0214] Example 7-1: Basic formulation
[0215] Excipients: None
[0216] Content: None
[0217] Example 7-2: Reconstitution Formula 2
[0218] Excipients: Mannitol
[0219] Content: 29mg
[0220] Example 7-3: Reconstitution Formula 3
[0221] Excipients: Polyethylene glycol 300
[0222] Content: 5mg
[0223] Example 7-4: Reconstitution Formula 4
[0224] Excipients: Cross-linked carboxymethyl cellulose sodium
[0225] Content: 10mg
[0226] 1 ml of normal saline was injected into the vials of Examples 7-1 to 7-4 and shaken manually. Table 6 shows the effect of the viscosity change of CMC-Na. Fig.15 Shown is the reconstitution of injectable tissue materials with different excipients. Different excipients can help with reconstitution.
[0227] Table 6 Effect of adding different excipients on re-dissolution
[0228] Case Standing re-dissolution time / min Shaking time / s Example 7-1 5 20 Example 7-2 4 30 Example 7-3 5 20 Example 7-4 4 20
[0229] Example 8 Animal Experiment
[0230] This example aims to evaluate the effect of the adjusted concentration and viscosity of sodium carboxymethyl cellulose on the volume retention rate and tissue compatibility of injectable adipose decellularized biomaterials after subcutaneous injection. The basic preparation steps are as follows:
[0231] (1) Weigh 12 mg of adipose decellularized biomaterial;
[0232] (2) Weigh 10 mg of sodium carboxymethyl cellulose (viscosity 6000-14000 mPa·s) and dissolve it in 1 ml of distilled water preheated at 60°C. Stir with a magnetic stirrer at 900 rpm for 3 h until it is completely dissolved.
[0233] (3) The adipose decellularized matrix and sodium carboxymethyl cellulose solution were mixed at a mass volume ratio of 1:1 (w / v), and stirred for 1 h with a magnetic stirrer at 900 rpm until uniform; 1 ml of the resulting composite solution was poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0234] Control Example 3 Effect of adding sodium carboxymethyl cellulose on the biocompatibility of adipose decellularized materials
[0235] Control Example 3 is intended to evaluate the volume retention rate and tissue compatibility of adipose decellularized biomaterials after subcutaneous injection when sodium carboxymethylcellulose (CMC-Na) is not added. The basic preparation steps are as follows:
[0236] (1) Weigh 12 mg of adipose decellularized biomaterial;
[0237] (2) Add 1 ml of distilled water to the adipose decellularized matrix and vortex at 2000 rpm for 1 min until the mixture is evenly mixed; the resulting matrix solution is poured into a vial, pre-frozen at -80°C for 1 h, freeze-dried for 78.5 h, and sterilized.
[0238] 1 ml of normal saline was injected into the vials of Example 8 and Control Example 3, and the solution was drawn into a 1 ml syringe. Subcutaneous injection experiments were performed on nude mice, with 0.2 ml injected. The gross observations and material status of the animals after 2 weeks and 1 month of the experiment are shown in the figure below. Fig.16 , 17 As shown in the figure. At 2 weeks, the injectable tissue material was observed to be round and full, and the observed volume was larger than that of pure fat decellularized biomaterial. At 1 month, the volume of the injectable tissue material and pure fat decellularized biomaterial was significantly reduced, and the volume of the injectable tissue material was slightly larger. Fig.17 The surface area of the material shown in is evaluated.
[0239] Volume retention rate: In the subcutaneous injection experiment on nude mice, the material of Example 8 was generally observed to be round and full, and its volume was slightly larger than that of the pure adipose decellularized biomaterial of Control Example 3. As shown in Table 7, the apparent area and cross-sectional area of the injectable tissue material at 2 weeks and 1 month were both larger than those of the pure adipose decellularized biomaterial, and the retention rates were similar, indicating that the material of Example 8 had a good volume retention rate and a larger apparent volume.
[0240] Table 7 Effect of adding sodium carboxymethyl cellulose on the biocompatibility of adipose decellularized materials
[0241]
[0242] Histological evaluation: After one month of animal experiment, the histological evaluation chart ( Fig.18 ) observed that the material of Example 8 and Control Example 3 both degraded to varying degrees, and there was cell infiltration, no obvious inflammatory reaction, fibrosis occurred around the material, fibroblasts and collagen fibers proliferated, and no obvious necrosis was observed. It is worth noting that the degradation degree of the material of Example 8 was lower than that of Control Example 3, and the fibrosis, fibroblasts and collagen fiber proliferation around it were better than those of pure fat decellularized biomaterials, indicating that the material of Example 8 has better stability and biocompatibility. At the same time, in Example 8, obvious fat cell regeneration can be seen at 1 month, such as Fig.19As shown in the figure (the right picture is a magnified black box), it can be seen that the material is promoting fat production (black arrow). Injectable adipose decellularized biomaterials have excellent stability and biocompatibility and can be used for soft tissue volume loss.
[0243] The injectable adipose decellularized biomaterial modified by adding sodium carboxymethylcellulose (CMC-Na) in Example 8 showed excellent stability and biocompatibility in the repair of soft tissue volume loss. Compared with the control example 3 without adding CMC-Na, the material of Example 8 had a higher volume retention rate and a lower degradation rate, and promoted tissue regeneration during the tissue repair process, showing its potential advantages for soft tissue engineering applications. This finding emphasizes the important role of CMC-Na as a biomaterial modifier in improving material performance and provides an important scientific basis for the development of future soft tissue repair materials.
Claims
1. An injectable adipose decellularized biomaterial, in, The material comprises adipose decellularized matrix and sodium carboxymethylcellulose.
2. The material according to claim 1, in, The mass ratio of the adipose decellularized matrix to sodium carboxymethyl cellulose is (1-99):(1-99), preferably (13-79):(20-86), preferably (23-71):(28-76).
3. The material according to claim 1 or 2, in, The mass percentage of the adipose decellularized matrix in the material is 20-80%, preferably 20-60%, preferably 23-55%.
4. The material according to any one of claims 1 to 3, in, The mass percentage of sodium carboxymethyl cellulose in the material is 20-80%, preferably 40-80%, preferably 45-77%.
5. The material according to any one of claims 1 to 4, in, The collagen content in the adipose decellularized matrix is 10-60%, preferably 20-40%; Preferably, the glycosaminoglycan content in the adipose decellularized matrix is 0.1-2%, preferably 1.3-2%; Preferably, the total content of growth factors in the adipose decellularized matrix is 0-1000 pg / mg, preferably 300-800 pg / mg. 6 . The material according to claim 1 , wherein the particle size of the adipose decellularized matrix used to prepare the material is 0.5-1000 μm, preferably 5-500 μm.
7. The material according to any one of claims 1 to 6, wherein the sedimentation rate of the material is 9×10 -10 cm / s-9×10 -3 cm / s, preferably 9×10 -8 cm / s-8×10 -4 cm / s.
8. The material according to any one of claims 1 to 7, wherein the material can be uniformly extruded through a 20-40G needle after preparation, preferably, the material can be uniformly extruded through a 20-34G needle after preparation.
9. The material according to any one of claims 1 to 8, in, The preparation method of the material comprises the following steps: S1. Adipose tissue processing: including washing, crushing, separation, virus inactivation, decellularization, pulverization and other processes to obtain adipose decellularized matrix; S2. Preparation of sodium carboxymethyl cellulose solution: Sodium carboxymethyl cellulose with or without refining or cross-linking treatment is dissolved in water to form a uniform sodium carboxymethyl cellulose solution; S3. Mixing and molding: adding the adipose decellularized matrix to the sodium carboxymethyl cellulose solution in proportion and mixing evenly, adding or not adding auxiliary materials and mixing evenly, injection molding, and freeze-drying to prepare the injectable adipose decellularized biomaterial; Preferably, the material preparation method further comprises sterilization treatment, and preferably, the sterilization treatment adopts low-temperature plasma sterilization, ethylene oxide sterilization or radiation sterilization method; Preferably, the injectable adipose decellularized biomaterial is mixed with physiological saline or phosphate buffer and then injected into the soft tissue volume loss area; preferably, in step S2, the viscosity of the sodium carboxymethyl cellulose solution is 50-100000 mPa·s, and the concentration is 0.01-30%; preferably, the viscosity of the sodium carboxymethyl cellulose solution is 6000-14000 mPa·s, and the concentration is 0.1-10%; Preferably, the sodium carboxymethyl cellulose treatment method in step S2 is mainly a refining method, a physical crosslinking method and a chemical crosslinking method, wherein the refining method includes but is not limited to: alcohol washing method, acid alcohol solution precipitation method and other processes, the physical crosslinking method includes but is not limited to: irradiation, ultraviolet irradiation and other processes, and the chemical crosslinking method includes but is not limited to: a crosslinking process using acrylamide, sodium trimetaphosphate, 1,3-propylenediamine, chloromethylpyridine iodide, EDC and NHS and other crosslinking agents; Preferably, in step S3, the auxiliary materials include lyophilization protective agents, disintegrants, and suspending agents, wherein the lyophilization protective agents include but are not limited to: mannitol, trehalose and other reagents, wherein the disintegrants include but are not limited to: sodium carboxymethyl starch, cross-linked sodium carboxymethyl cellulose and other reagents, wherein the suspending agents include but are not limited to: glycerol, polyethylene glycol, Tween 80 and other reagents; Preferably, in step S3, the freeze-drying process conditions in the mixing and forming step are: pre-freezing for 1-24 hours, the pre-freezing temperature range is -80 to 0°C, and the freeze-drying time is 12-80 hours; Preferably, in step S3, the mixing ratio of the adipose decellularized matrix and the sodium carboxymethyl cellulose solution is adjusted to control the degradation rate of the material to meet the needs of filling different soft tissue parts; preferably, the mass volume ratio of the adipose decellularized matrix and the sodium carboxymethyl cellulose solution is 1:10-5:1, and the preferred ratios are 1:1 and 2:
1.
10. Use of the material according to any one of claims 1 to 8 in the preparation of medical materials or preparations. Preferably, the medical materials or preparations are used for the repair of soft tissue injuries, including but not limited to the treatment of skin burns, bone defects, and cartilage degeneration. They are also suitable for the field of regenerative medicine, especially in promoting nerve tissue repair, cardiac tissue regeneration, and liver injury recovery, showing significant application potential, providing more effective and safe material options.
Citation Information
Patent Citations
Preparation method of acellular fat matrix
CN113577388A
Temperature-sensitive interpenetrating polymer network hydrogel as well as preparation method and application thereof
CN115463264A
An injectable decellularized fat-matrix microparticle and applications thereof in implants
CN106492288A
Medical composition comprising adipose tissue-derived extracellular matrix and method for producing same
CN114206405A
Acellular matrix particle filler and preparation method thereof
CN114949359A
Cited By
Acellular matrix particle freeze-dried implant as well as preparation method and application thereof
CN119236183A
An acellular matrix microparticle freeze-dried implant and its preparation method and application
CN119236183B